All-solid-state battery including thin film current collector and method for manufacturing the same
By employing a thin film current collector with lithium-affinity metals or oxides, the interfacial resistance in all-solid-state batteries is reduced, enhancing capacity and safety.
Patent Information
- Application Number
- JP2024125929
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-07-23
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
All-solid-state batteries face issues with high interfacial resistance and reduced capacity due to the difficulty in forming a uniform interface between the electrodes and the solid electrolyte layer, leading to potential short circuits and lower performance.
The use of a thin film current collector with a thickness of less than 5 μm, made of metals or metal oxides with lithium affinity, directly facing the solid electrolyte layer, and heat-treated together with the electrolyte to reduce interfacial resistance.
This approach significantly reduces interfacial resistance, enhances battery capacity, and minimizes short circuit occurrences, thereby improving the overall performance and safety of all-solid-state batteries.
Smart Images

Figure 2024161019000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 2020-0091625 filed on July 23, 2020, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.
[0002] The present invention relates to an all-solid-state battery including a thin film current collector and a manufacturing method thereof, and more particularly to an all-solid-state battery including a thin film current collector for improving the interfacial resistance between the current collector and a solid electrolyte while increasing the overall capacity of the all-solid-state battery using the thin film current collector, and a manufacturing method thereof. [Background technology]
[0003] Secondary batteries using electrolyte have problems such as a shortened lifespan due to the electrolyte being consumed during charging and discharging, and overheating or explosion due to leakage or combustion of the electrolyte.
[0004] In order to improve the safety of secondary batteries, various methods have been considered, such as providing safety devices such as fuses and protection circuits. To solve the above problems, all-solid-state batteries in which the liquid electrolyte is changed to a solid electrolyte have been proposed.
[0005] Unlike existing secondary batteries, all-solid-state batteries have a positive electrode and a negative electrode formed on both sides of a solid electrolyte layer containing a solid electrolyte, and the solid electrolyte layer also serves as a separator.
[0006] Since solid-state batteries use a solid electrolyte instead of a liquid electrolyte, they are safe from explosions and fires because there is no electrolyte evaporation due to temperature changes or leakage due to external impact. However, the solid-state battery has the disadvantages of lower ionic conductivity than secondary batteries using liquid electrolytes, and high interface resistance because it is difficult to form interfaces between the positive electrode, negative electrode, and solid electrolyte layer. Due to these problems, the solid-state battery has the disadvantage of reduced lifespan and output.
[0007] FIG. 1 is a schematic diagram of an all-solid-state battery according to the prior art.
[0008] As shown in Fig. 1, a lithium secondary battery according to the related art includes a positive electrode 10 including a positive electrode current collector 11 and a positive electrode active material layer 12 coated on both sides of the positive electrode current collector 11, a solid electrolyte layer 20, and a negative electrode 30 including a negative electrode current collector 31 and a negative electrode active material layer 32 coated on both sides of the negative electrode current collector. Unlike Fig. 1, the negative electrode can be formed by a lithium plating and stripping technique using the negative electrode current collector alone or lithium metal without a separate negative electrode active material layer 32 in order to increase the overall capacity of the lithium secondary battery.
[0009] In conventional lithium secondary batteries, pressure F is applied from the top and bottom of the battery to reduce the interfacial resistance between the positive electrode 10, the solid electrolyte layer 20, and the negative electrode 30. If the positive electrode 10, the solid electrolyte layer 20, and the negative electrode 30 are not uniform, it is difficult to reduce the interfacial resistance by pressure alone, and short circuits may occur due to lithium dendrite growth during charging in areas with different interfacial resistances. In particular, as the capacity of the positive electrode increases to achieve high energy density, the amount of lithium deposited during charging also increases proportionally, thereby increasing the probability of short circuits.
[0010] Meanwhile, research into batteries using Li plating / stripping is ongoing to increase the energy density of batteries. Current collectors used here generally have a thickness of around 10 μm, so there is a need to further reduce the thickness to improve energy density.
[0011] In Patent Document 1, a laminate consisting of a positive electrode, a solid electrolyte layer, and a negative electrode is compressed in order to improve electrical conductivity, electronic conductivity, and lithium ion conductivity, but the document does not recognize the prevention of the cell short phenomenon of a unit cell caused by lithium dendrites during charging.
[0012] Patent Document 2 also compresses a laminate consisting of a positive electrode, a solid electrolyte layer, and a negative electrode in order to reduce the interfacial resistance, but does not recognize the point that the safety of the unit cell is improved by reducing the stress caused by lithium dendrites during charging. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] JP 2018-181451 A [Patent Document 2] JP 2019-200890 A Summary of the Invention [Problem to be solved by the invention]
[0014] The present invention is intended to solve the above problems, and aims to reduce the interfacial resistance between an electrode using a thin film current collector and a solid electrolyte layer while using the thin film current collector as a current collector.
[0015] Another object of the present invention is to increase the capacity relative to the size of the battery by using a thin film current collector. [Means for solving the problem]
[0016] In order to achieve the above object, the all-solid-state battery according to the present invention includes a positive electrode, a solid electrolyte layer, and a negative electrode, the positive electrode or the negative electrode being made of a current collector having a thickness of less than 5 μm, and the current collector can directly face the solid electrolyte layer.
[0017] The current collector may include a metal having an affinity for lithium.
[0018] Here, the metal having lithium affinity may be at least one selected from the group consisting of metals including Au, Ag, Pt, Zn, Si, and Mg, and metal oxides including CuO, ZnO, CoO, and MnO.
[0019] Here, it is preferable that the current collector does not contain lithium metal.
[0020] The current collector may be heat treated together with the solid electrolyte layer.
[0021] Also, the current collector may be formed by a deposition and transfer process.
[0022] The solid-state battery may not require the use of lithium, such as nickel-cadmium, nickel-manganese, nickel-hydrogen, or metal-air batteries.
[0023] The present invention may provide a method for manufacturing any one of the all-solid-state batteries, comprising: S1) forming a current collector by depositing a metal for a current collector on a release film; and S2) transferring the current collector of step S1) to a solid electrolyte layer and then heat-treating the same to form an electrode assembly.
[0024] Also, after step S2) or before the heat treatment of step S2), the step of removing the release film may be included.
[0025] Also, in step S2), the transfer and the heat treatment can be carried out simultaneously.
[0026] The release film may have a coating or surface treatment applied to the deposition surface on which the metal is deposited.
[0027] The deposition in step S1) may be any one of a vacuum deposition method, a chemical deposition method, a chemical vapor deposition method, and a physical deposition method.
[0028] The present invention may include a battery module or a battery pack including the all-solid-state battery, and may also include a device equipped with the all-solid-state battery.
[0029] The present invention can select and combine one or more of the above-mentioned configurations that are not contradictory to each other. Effect of the Invention
[0030] As described above, in the all-solid-state battery according to the present invention, the thin film current collector is heat-treated together with the solid electrolyte layer to reduce the interface resistance and improve the performance of the all-solid-state battery.
[0031] In addition, since the thickness of the current collector is small, the capacity relative to the size of the solid-state battery is increased. [Brief description of the drawings]
[0032] [Figure 1] FIG. 1 is a schematic diagram of an all-solid-state battery according to the prior art. [Diagram 2] FIG. 1 is a schematic diagram of an all-solid-state battery according to the present invention. [Diagram 3] FIG. 1 is a schematic diagram of a method for producing an all-solid-state battery according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings, which are provided to enable a person having ordinary skill in the art to which the present invention pertains to easily carry out the present invention. However, in describing the operation principle of the preferred embodiment of the present invention in detail, detailed description of related well-known functions or configurations will be omitted if it is determined that such detailed description may unnecessarily obscure the gist of the present invention.
[0034] In addition, the same reference numerals are used throughout the drawings for parts having similar functions and actions. Throughout the specification, when a part is said to be connected to another part, this includes not only the case where the part is directly connected to another part, but also the case where the part is indirectly connected via another element between the two parts. In addition, when a part includes a certain component, it does not mean that the other component is excluded, but that the part may further include the other component, unless otherwise specified.
[0035] Furthermore, descriptions that limit or add specific elements are applicable to all inventions and are not limited to a particular invention unless otherwise specified.
[0036] Furthermore, throughout the description of the present invention and the claims, the singular includes the plural unless otherwise stated.
[0037] In addition, throughout the description of the present invention and the claims, unless otherwise specified, "or" includes "and." Therefore, "including A or B" means three cases: including A, including B, or including both A and B.
[0038] Furthermore, all numerical ranges include the endpoints and all intermediate values therebetween unless expressly stated to the contrary.
[0039] The all-solid-state battery according to the present invention comprises a positive electrode, a solid electrolyte layer, and a negative electrode, the positive electrode or the negative electrode being made of a current collector having a thickness of less than 5 μm, and the current collector directly faces the solid electrolyte layer.
[0040] FIG. 2 is a schematic diagram of an all-solid-state battery according to the present invention.
[0041] In the all-solid-state battery according to the present invention, the positive electrode 100 may be made of a positive electrode current collector 110 having a thickness of less than 5 μm, and the positive electrode current collector 110 may directly face the solid electrolyte layer 200, and the negative electrode may be made of a negative electrode current collector 300 having a thickness of less than 5 μm, and the negative electrode current collector 300 may directly face the solid electrolyte layer 200. Alternatively, the positive electrode 100 and the negative electrode may both be made of electrode current collectors having a thickness of less than 5 μm, and the electrode current collectors may directly face the solid electrolyte layer 200. Although the positive electrode and the negative electrode may not use a thin film current collector, the following description will be given based on the case where a thin film current collector is used only in the negative electrode, with reference to FIG. 2. It goes without saying that the thin film current collector may also be applied to the positive electrode.
[0042] 2, the all-solid-state battery according to the present invention includes a cathode 100 including a cathode current collector 110 and a cathode active material layer 120 coated on at least one surface of the cathode current collector 110, a solid electrolyte layer 200, and an anode including an anode current collector 300. The cathode may include the cathode active material 120 facing the cathode current collector 110 and the solid electrolyte layer 200, and the anode may include an anode active material layer coated on at least one surface of the anode current collector 300, or both the cathode and the anode may include electrode current collectors.
[0043] The positive electrode 100 may be manufactured by, for example, applying a positive electrode mixture, which is a mixture of a positive electrode active material composed of positive electrode active material particles, a conductive material, and a binder, to a positive electrode current collector 110 to form a positive electrode active material layer 120, and a filler may be further added to the positive electrode mixture, if necessary. Also, unlike FIG. 2, the positive electrode 100 may use only the positive electrode current collector 110.
[0044] The positive electrode current collector 110 is generally manufactured to have a thickness of 3 μm to 500 μm. However, when only the positive electrode current collector 110 is heat-treated together with the solid electrolyte layer, the thickness of the positive electrode current collector 110 may be less than 5 μm.
[0045] The positive electrode current collector 110 is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and may be one selected from stainless steel, aluminum, nickel, titanium, and aluminum or stainless steel surface-treated with carbon, nickel, titanium, or silver, and may be aluminum. The current collector may have micro-irregularities on its surface to increase the adhesive strength of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0046] The positive electrode active material contained in the positive electrode active material layer 120 may be, for example, a layered compound such as lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals, in addition to the positive electrode active material particles; 1+x Mn 2-x O4 (where x is 0 to 0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M x O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x = 0.01 to 0.3); 2-x M x The lithium manganese composite oxides may be represented by Li2Mn3MO8 (wherein M is Co, Ni, Fe, Cr, Zn or Ta, and x is 0.01 to 0.1); LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion; disulfide compounds; Fe2(MoO4)3, but are not limited to these.
[0047] The positive electrode active material layer 120 may be located on at least one surface of the positive electrode current collector 110. Here, when the positive electrode current collector 110 is replaced with the current collector of the present invention, the positive electrode active material layer 120 may be located only on the surface of the positive electrode current collector 110 facing the solid electrolyte layer 200.
[0048] The conductive material is usually added in an amount of 0.1% by weight to 30% by weight based on the total weight of the mixture including the positive electrode active material. Such a conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the battery, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0049] The binder contained in the positive electrode 100 is a component that helps bind the active material and conductive material and the current collector, and is usually added in an amount of 0.1 to 30% by weight based on the total weight of the mixture including the positive electrode active material. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer, sulfonated ethylene-propylene-diene terpolymer, styrene-butadiene rubber, fluororubber, various copolymers, etc.
[0050] The solid electrolyte layer 200 may be made of, but is not limited to, an organic solid electrolyte or an inorganic solid electrolyte. The solid electrolyte layer may further include a binder such as polytetrafluoroethylene (PTFE).
[0051] Examples of the organic solid electrolyte include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups.
[0052] Examples of the inorganic solid electrolyte include a sulfide-based solid electrolyte and an oxide-based solid electrolyte.
[0053] As an oxide-based solid electrolyte, for example, Li 6.25 La3Zr2A l0 . 25 O 12 , Li3PO4, Li 3+x PO 4-x N x Nitrides and halides of Li, such as (LiPON), Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, or Li4SiO4-LiI-LiOH, can be used.
[0054] The sulfide-based solid electrolyte is not particularly limited in the present invention, and may be any known sulfide-based material used in the field of lithium batteries. The sulfide-based material may be a commercially available product, or may be prepared by a crystallization process from an amorphous sulfide-based material. For example, the sulfide-based solid electrolyte may be a crystalline sulfide-based solid electrolyte, an amorphous sulfide-based solid electrolyte, or any one or combination of these. Examples of usable composite compounds include sulfur-halogen compounds, sulfur-germanium compounds, and sulfur-silicon sulfides, and may include sulfides such as SiS2, GeS2, and B2S3, and Li3PO4, halogens, halogen compounds, and the like may be added. Preferably, 10 -4 A sulfide-based electrolyte capable of realizing lithium ion conductivity of 100 S / cm or more can be used.
[0055] Representative examples include Li6PS5Cl (LPSCl), Thio-LISICON (Li 3.25 Ge 0.25 P 0.75 S4), Li2S-P2S5-LiCl, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, Li3PS4, Li7P3S 11 , LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, Li 10 GeP2S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , and Li7P3S 11 Includes.
[0056] When the negative electrode according to the present invention uses only the negative electrode current collector 300 or the positive electrode 100 uses only the positive electrode current collector 110, a negative electrode having a negative electrode active material coated on at least one surface of the negative electrode current collector 300 may be used.
[0057] When the negative electrode is formed by applying a negative active material to at least one surface of a negative current collector, the negative current collector 300 may generally have a thickness of 3 μm to 500 μm. The negative current collector 300 is not particularly limited as long as it is conductive and does not cause a chemical change in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used. In addition, as with the positive current collector 110, the surface may be formed with minute irregularities to strengthen the binding force of the negative active material, and various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. may be used.
[0058] Examples of the negative electrode active material include carbon such as non-graphitizable carbon and graphite-based carbon; Li xFe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, 2, 3 elements of the periodic table, halogen; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8) and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials, etc. can be used.
[0059] When only the negative electrode current collector 300 is used as the negative electrode, the negative electrode current collector 300 has a thickness of less than 5 μm, and the negative electrode current collector 300 is directly facing the solid electrolyte layer 200.
[0060] The negative electrode current collector 300 can contain a metal having lithium affinity. The metal having lithium affinity can be at least one or more of substances selected from the group consisting of metals including Au, Ag, Pt, Zn, Si, and Mg, and metal oxides including CuO, ZnO, CoO, and MnO.
[0061] By having the negative electrode current collector 300 have a metal having lithium affinity, the formation position of lithium dendrites generated inside the all-solid-state battery can be adjusted.
[0062] The negative electrode current collector 300 may be heat-treated together with the solid electrolyte layer 200. When the negative electrode current collector 300 is heat-treated together with the solid electrolyte layer 200, the interface resistance between the negative electrode current collector 300 and the solid electrolyte layer 200 is reduced. Here, since the negative electrode current collector 300 is separately formed and then heat-treated together with the solid electrolyte layer 200, the negative electrode current collector 300 and the solid electrolyte layer 200 do not react with each other. Of course, the negative electrode current collector 300 may be directly deposited on the solid electrolyte layer 200.
[0063] The positive electrode current collector 110 or the negative electrode current collector 300 may not contain lithium metal. This is because, considering that the thickness of the positive electrode current collector 110 or the negative electrode current collector 300 is less than 5 μm, even if the formation of lithium dendrites is controlled, the solid electrolyte layer 200 may be damaged and a short circuit may occur. Therefore, the all-solid-state battery may be an all-solid-state battery that does not use lithium, such as a nickel-cadmium, nickel-manganese, nickel-hydrogen, or metal-air battery.
[0064] FIG. 3 is a schematic diagram of a method for producing an all-solid-state battery according to the present invention.
[0065] As shown in FIG. 3, the all-solid-state battery according to the present invention includes the steps of: S1) depositing a current collector metal 310 on a release film 320 to form a current collector; S2) transferring the current collector of step S1) to a solid electrolyte layer 200 and then heat-treating the same to form an electrode assembly; and S3) removing the release film 320 from the electrode assembly.
[0066] The metal used as the positive or negative electrode current collector may be used as the current collector metal 310. The metals used as the positive electrode current collector and the negative electrode current collector that can be used as the current collector metal 310 have been described above and will not be described further.
[0067] Any known release film may be used as the release film 320. For example, any material may be used as the release film 320 as long as it has a low surface roughness and is easily peelable so that it is not damaged when the current collector metal 310 is deposited and no residue is left when the current collector metal 310 is peeled off. For example, the release film 320 may be made of a synthetic resin film such as polyethylene, polypropylene, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyethylene terephthalate, or a metal foil.
[0068] The release film 320 may be coated or surface-treated at least on a surface facing the current collector metal 310 so that no residue is left when the current collector metal 310 is peeled off. Examples of the surface treatment include surface modification treatments such as plasma treatment and sulfonation treatment, or peeling treatments such as silicon treatment, long-ring alkyl treatment, and fluorine treatment. The release film 320 may be made of a material that evaporates by heat treatment, etc., so that step S3) of removing the release film 320 from the electrode assembly is not performed.
[0069] In addition, the release film 320 may have different adhesive strengths on both sides in order to easily remove the current collector metal 310. Here, the adhesive strength of the opposing side of the current collector metal 310 may be weaker than the adhesive strength of the opposite side.
[0070] The deposition in step S1) may be selected from vacuum deposition, chemical vapor deposition, chemical vapor deposition, physical vapor deposition, physical vapor deposition, thermal evaporation, electron beam evaporation, and sputtering, but is not limited thereto, and various deposition methods used in the art may be used.
[0071] In step S2), the current collector is transferred to the solid electrolyte layer 200 and then heat-treated to form an electrode assembly. Here, the transfer and heat-treatment can be performed simultaneously. The transfer can be performed using an apparatus such as a roll press. Here, the roll press can perform heating and pressing simultaneously.
[0072] Here, the temperature applied to the current collector and the solid electrolyte layer 200 may be 40° C. to 200° C., and more specifically, the temperature may be 100° C. to 150° C. If the temperature is less than 40° C., the contact between the current collector and the solid electrolyte layer 200 may not reach a desired degree, and if the temperature exceeds 200° C., it is not preferable because there is a risk of denaturation of materials due to side reactions, a decrease in adhesive strength due to a decrease in binder performance, or deformation of the solid electrolyte layer 200.
[0073] The heat treatment time can be about 6 to 48 hours, and more specifically, about 12 to 24 hours. If the heat treatment time is less than 6 hours, the improvement effect by the heat treatment may be small, and if it is more than 48 hours, the processability decreases, which is not preferable.
[0074] The pressure applied by the pressing can be about 1 ton to about 3 tons, and more specifically, about 1.5 to about 2 tons. If the pressure exceeds 3 tons, the solid electrolyte layer may be damaged, and if the pressure is less than 1 ton, the effect of reducing the interfacial resistance between the current collector and the solid electrolyte layer 200 may be small.
[0075] The pressing time may be about 1 minute to about 24 hours. Here, the optimal range may be about 1.5 minutes to about 2.5 minutes. If the pressing time exceeds 24 hours, structural deformation of the solid electrolyte layer 200 may occur, and if the pressing time is less than 1 minute, the effect of reducing the interfacial resistance between the current collector and the solid electrolyte layer 200 is small.
[0076] In step S3), the release film 320 is removed from the electrode assembly. The metal collector 310 may be peeled off while the release film 320 is attached to a roll or a substrate having good adhesive strength to the release film 320. The metal collector 310 may be peeled off due to the difference in adhesive strength between the surface of the release film 320 facing the metal collector 310 and the opposite surface. In addition, the release film 320 may be evaporated by the heat treatment in step S2) by using a material that is evaporated by heat treatment, etc., as described above.
[0077] The present invention will be described below by comparing experimental examples according to the present invention with comparative examples according to the prior art.
[0078] (Experimental Example 1) The electrical conductivity of silver coated by deposition to a thickness of 1 μm on a PET release film (Production Example 1), silver coated by deposition to a thickness of 2 μm on a PET release film (Production Example 2), gold coated by deposition to a thickness of 1 μm on a PET release film (Production Example 3), nickel foil with a thickness of 11 μm that was not deposited (Production Example 4), and SUS304 foil with a thickness of 10 μm that was not deposited (Production Example 5) were compared and are shown in Table 1 below. The electrical conductivity was measured using a 5×5 cm 2 Each sample was measured using a 4-point probe. Each part was divided into 25 sections, and the average resistance (R s ) was calculated, and the resistivity (ρ cal ) were calculated and are shown in Table 1 below.
[0079] ρ cal =R s ×Thickness (μm)
[0080] The electrical conductivity is the resistivity (ρ cal The smaller the resistivity, the higher the electrical conductivity.
[0081] In Table 1 below, ρ calis the specific resistivity value of the material used in Production Examples 1 to 5.
[0082] [Table 1]
[0083] Referring to Table 1, the resistivity (ρ cal ) is the specific resistivity (ρ bulk ) is almost the same as the calculated resistivity value (ρ cal ) is found to be highly reliable.
[0084] As shown in Table 1, Preparation Examples 1 and 2 in which lithium-affinity silver was thinned showed average resistance values at similar levels to Preparation Example 4 in which a general nickel current collector was used, compared with Preparation Example 3 in which gold was thinned.
[0085] In particular, in the case of Preparation Example 1, in which 1 μm-thick silver was deposited on a PET release film, the average resistance was measured to be much lower than that of the SUS304 current collector in Preparation Example 5, despite the very small thickness, so Preparation Example 1 shows very good electrical conductivity.
[0086] Therefore, it can be seen that silver coated on a PET release film and gold coated on a PET release film can also function as a current collector, just like nickel and SUS304.
[0087] (Experimental Example 2) After bonding the current collector and the solid electrolyte layer of Preparation Example 1, the interface resistance was measured before and after heat treatment in a vacuum at 100° C. for 12 hours. The results are shown in Table 2.
[0088] The solid electrolyte layer was prepared by dispersing and stirring the solid electrolyte, argyrodite (Li6PS5Cl), and the binder, PTFE, in anisole at a weight ratio of 95:5 to form a solid electrolyte layer slurry, coating the slurry on a PET release film, and vacuum drying at 100°C for 12 hours.
[0089] [Table 2]
[0090] (Experimental Example 3) Based on the above Experimental Examples 1 and 2, in Experimental Example 3, an experiment was conducted using all-solid-state batteries including the following positive electrodes, solid electrolyte layers, and negative electrodes according to Example 1, Comparative Example 1, and Comparative Example 2.
[0091] The positive electrode is a positive electrode active material NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 The cathode slurry was prepared by dispersing and stirring the cathode slurry in anisole at a weight ratio of 77.5:19.5:1.5:1.5, which consisted of 02), argyrodite (Li6PS5Cl) as a solid electrolyte, carbon as a conductive material, and PTFE as a binder. The cathode slurry was applied to an aluminum current collector with a thickness of 14 μm using a doctor blade, and then vacuum-dried at 100° C. for 12 hours to prepare the cathode.
[0092] The solid electrolyte, argyrodite (Li6PS5Cl), and the binder, PTFE, were dispersed and stirred in anisole at a weight ratio of 95:5 to form a solid electrolyte layer slurry, which was then coated onto a PET release film and vacuum dried at 100°C for 12 hours to form a solid electrolyte layer.
[0093] The positive electrode, the solid electrolyte layer, and the negative electrode according to Example 1, Comparative Example 1, and Comparative Example 2 described below were laminated in order to fabricate a battery.
[0094] In Experimental Example 3, the solid-state battery was used to perform an initial charge / discharge cycle at 60° C. (initial charge: CC, 0.05 C, 4.25 V, cut off at 0.01 C, initial discharge: CC, 0.05 C, discharge to 3 V), and the output efficiency and short circuit occurrence rate were measured. The results are shown in Table 3.
[0095] Example 1 In Example 1, an electrode assembly was manufactured using Preparation Example 1 as a negative electrode, and then heat-treated at 100° C. for 12 hours.
[0096] Comparative Example 1 In Comparative Example 1, a battery was produced in the same manner as in Example 1, except that the nickel of Production Example 4 was laminated to a thickness of 11 μm and used as the negative electrode.
[0097] Comparative Example 2 In Comparative Example 2, an electrode assembly was manufactured using Preparation Example 1 as a negative electrode, and a separate heat treatment process was not performed.
[0098] [Table 3]
[0099] Referring to Table 3, the charge and discharge capacity of the battery heat-treated as in Example 1 was superior to that of the battery not heat-treated as in Comparative Example 2 due to the improved interfacial resistance. Furthermore, the use of a lithium affinity material as the current collector reduced the rate of short circuiting during charging.
[0100] In addition, when comparing the current collectors of Example 1 and Comparative Example 1, it can be seen that the thickness ratio of Example 1 to Comparative Example 1 is at most about 9%, so that not only is the thickness smaller than Comparative Example 1, but also that in the case of a positive electrode of 50 μm and a solid electrolyte layer of 30 μm, the energy density is improved by 12.3% compared to Comparative Example 1.
[0101] The present invention also provides a battery module including the all-solid-state battery, a battery pack, and a device including the battery pack. The battery pack and device are well known in the art, and therefore, detailed description thereof will be omitted in this specification.
[0102] It goes without saying that the device can be, for example, but is not limited to, a notebook computer, a netbook computer, a tablet computer, a mobile phone, an MP3 player, a wearable electronic device, a power tool, an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), an electric bicycle (E-bike), an electric scooter (E-scooter), an electric golf cart, or a power storage system.
[0103] Those skilled in the art will appreciate that various applications and modifications within the scope of the present invention are possible based on the above content. [Industrial Applicability]
[0104] As described above, in the all-solid-state battery according to the present invention, the thin film current collector is heat-treated together with the solid electrolyte layer to reduce the interface resistance and improve the performance of the all-solid-state battery.
[0105] In addition, since the thickness of the current collector is small, the capacity is increased compared to the size of the all-solid-state battery. [Explanation of symbols]
[0106] 10, 100 positive electrode 11, 110 Positive electrode current collector 12, 120 Cathode active material layer 20, 200 solid electrolyte layer 30 negative electrode 31, 300 Negative electrode current collector 310 Collector metals 32 Negative electrode active material layer 320 Release film F Pressure
Claims
1. An electrode assembly including a positive electrode, a solid electrolyte layer, and a negative electrode, the negative electrode is made of a current collector having a thickness of 10 μm or less, the current collector being in direct contact with the solid electrolyte layer, the current collector is at least one selected from the group consisting of metals including Au, Ag, Pt, Zn, Si, and Mg; the solid electrolyte layer includes a sulfide-based solid electrolyte, The electrode assembly, wherein the interfacial resistance between the current collector and the solid electrolyte layer is reduced by heat treatment.
2. The electrode assembly according to claim 1 , wherein the current collector has a thickness of 5 μm or less.
3. The electrode assembly of claim 1 or 2, wherein the current collector does not contain lithium metal.
4. The electrode assembly according to claim 1 , wherein the positive electrode comprises a positive electrode active material comprising a lithium transition metal oxide.
5. The sulfide-based solid electrolyte is Li 6 P.S. 5 Cl (LPSCl), Thio-LISICON (Li 3.25 Ge 0.25 P 0.75 S 4 ), Li 2 S-P 2 S 5 -LiCl, Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 O 5 , LiI-Li 3 P.O. 4 -P 2 S 5 , Li 2 S-P 2 S 5 , Li 3 P.S. 4 , Li 7 P 3 S 11 , LiI-Li 2 S-B 2 S 3 , Li 3 P.O. 4 -Li 2 S-Si 2 S., Li. 3 P.O. 4 -Li 2 S-SiS 2 , LiPO 4 -Li 2 S-SiS, Li 10 GeP 2 S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 C 0.3 , and Li 7 P 3 S 11 The electrode assembly according to claim 1 , comprising one or more selected from the group consisting of:
6. 6. The electrode assembly according to claim 1, wherein the interfacial resistance between the current collector and the solid electrolyte layer is reduced by pressing simultaneously with the heat treatment.
Citation Information
Patent Citations
Lithium solid type secondary battery and method for manufacturing the same
JP2016035867A
Lithium ion secondary battery
JP2019114406A
All-solid-state battery including thin-film current collector and method for manufacturing the same
JP2023521736A
Laminate type all-solid battery and manufacturing method thereof
JP2018181451A
Method for manufacturing electrode layer
JP2019200890A