Metal products with improved bond durability and related methods

Mechanical modification of near-surface microstructures in aluminum alloys, combined with a silicon-containing layer, addresses defects to enhance durability and reduce corrosion, improving the overall performance of aluminum alloy products.

JP2024161384APending Publication Date: 2024-11-19NOVELIS INC(US)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024115709
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-03-23
Filing Date
2024-07-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing aluminum alloy products suffer from near-rolled surface microstructural defects such as entrained oxides, voids, cracks, and non-uniform alloying element distribution, which affect mechanical and chemical performance, including increased corrosion sensitivity and reduced bond durability.

Method used

Mechanically modify the near-surface microstructure of aluminum alloy products to create a microparticle subsurface structure with a uniform composition and reduced defects, using processes like grinding, laser ablation, or sandblasting, followed by depositing a silicon-containing layer to enhance bonding sites.

Benefits of technology

The modified microstructure improves mechanical and chemical performance by reducing defects, enhancing bond durability, and minimizing corrosion sensitivity, resulting in more robust and reliable aluminum alloy products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161384000002
    Figure 2024161384000002
  • Figure 2024161384000003
    Figure 2024161384000003
  • Figure 2024161384000004
    Figure 2024161384000004
Patent Text Reader

Abstract

To provide aluminum alloy products having a bulk and a micro-grained subsurface structure, and methods of processing the aluminum alloy products.SOLUTION: The aluminum alloy products may exhibit superior bonding character and may comprise or have a silicon-containing layer thereon. The bulk may include a matrix including grains of an aluminum alloy and may comprise aluminum and one or more alloying elements such as zinc, magnesium, copper, chromium, silicon, iron, and manganese. A micro-grained subsurface structure may be devoid or substantially devoid of one or more defects (e.g., voids, transfer cracks, or fissures) or organic compounds, oils, hydrocarbons, soils, inorganic residues, rolled-in oxides, or anodic oxides, which may commonly be present in rolled near-surface microstructures. The micro-grained subsurface structure may include or have thereon a first oxide layer having a thickness of 1 nm to 20 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of and priority to U.S. Provisional Application No. 62 / 978,767, filed February 19, 2020, U.S. Provisional Application No. 62 / 984,555, filed March 3, 2020, and U.S. Provisional Application No. 62 / 993,365, filed March 23, 2020, each of which is incorporated by reference in its entirety.

[0002] The present disclosure relates generally to metallurgy, and more specifically to techniques for improving the near-surface structure of rolled aluminum alloy products and the mechanical and chemical performance of aluminum alloy products. [Background technology]

[0003] During processing of aluminum alloy products, the generation of near-rolled surface microstructures that may contain defects may occur. For example, the defects may be entrapped oxides, entrapped oil, transfer cracks, surface cracks, internal cracks, fissures, or dense clusters of alloying elements. The defects in the near-rolled surface microstructure may affect the mechanical and chemical performance of the aluminum alloy product. There is a lack of technology that addresses defects in or associated with the near-rolled surface microstructure. Summary of the Invention

[0004] The terms "embodiments" and similar terms are intended to broadly refer to all of the subject matter of the present disclosure and the following claims. Statements containing these terms should be understood neither to limit the subject matter described herein nor to limit the meaning or scope of the following claims. The embodiments of the present disclosure covered herein are defined by the following claims, not this Summary. This Summary is a broad overview of various aspects of the disclosure and introduces some of the concepts that are further described in the Detailed Description section below. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to determine the scope of the claimed subject matter. The subject matter should be understood by reference to the entire specification of this disclosure, any or all drawings, and appropriate portions of each claim.

[0005] In one aspect, an aluminum alloy product is described. The aluminum alloy product includes or can be a rolled aluminum alloy product having a bulk, a first surface region, and a second surface region. The first surface region can include a near-surface microstructure (NSM) having a thickness of less than 500 nm. The near-surface microstructure can include one or more defects. The second surface region can be free of near-surface microstructure or substantially free of near-surface microstructure. The second surface region can have a thickness of 1 nm to 2 μm, such as 1 nm to 5 nm, 5 nm to 10 nm, 10 nm to 25 nm, 25 nm to 50 nm, 50 nm to 100 nm, 100 nm to 250 nm, 250 nm to 500 nm, 500 nm to 1 μm, or 1 μm to 2 μm. The second surface region can include an oxide layer and a micro-grain subsurface structure. In some embodiments, the first surface region and the second surface region can be discontinuous. For example, in some cases, "islands" of a first surface region may form within a second surface region, or "islands" of a second surface region may form within a first surface region. In some embodiments, the ratio of the area of ​​the first surface region to the area of ​​the second surface region may be less than 50%. For example, in a 100 μm 2 rolled aluminum alloy product, 2In the case of a surface area of ​​at least 51% (e.g., greater than 55%, 60%, 65%, 70%, or 75%) of the surface area may be or include the second surface region. In some cases, only the second surface region may be present in the aluminum alloy product.

[0006] In an embodiment, the rolled aluminum alloy product may include at least one of a 7xxx series aluminum alloy product, a 6xxx series aluminum alloy product, and a 5xxx series aluminum alloy product. Optionally, the rolled aluminum alloy product may be a hot rolled aluminum alloy product or a cold rolled aluminum alloy product. The bulk may include a matrix having grains of aluminum alloy, and the bulk may have a first composition. The first composition may include aluminum and one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese. The one or more alloying elements may be spatially uniformly distributed within the bulk.

[0007] The micro-grain subsurface structure may exist between the oxide layer and the bulk, may have a different or the same composition as the bulk, but may have a thickness of, for example, 1 nm to 2 μm, and may have a limited number of defects.

[0008] The micrograin subsurface structure may be different from the near-surface microstructure (also referred to herein as the rolled near-surface microstructure) that is produced during the creation of the rolled aluminum alloy product, e.g., the micrograin subsurface structure may be referred to herein as being or including an altered near-surface microstructure, since it is a subsurface or near-surface structure that may be produced when modifying the surface of a rolled aluminum alloy product having a rolled near-surface microstructure. The micrograin subsurface structure may be free or substantially free of one or more defects that may be present in the rolled near-surface microstructure. As used herein, the term substantially free refers to the absolute absence of an object or structure within the material, or to an object or structure within the material being present in such a small amount that it does not generally affect the mechanical properties, material properties, or performance of the material. As an example, if an aluminum alloy product is substantially free of defects, some defects may be present, but those defects may be present in a concentration that is, on average, 100 nm or more away from another defect. In some cases, when the defects are small, the defects may be present in a concentration where the defects are spaced much closer together on average, e.g., 25-50 nm.

[0009] By way of example, the one or more defects may correspond to or include one or more voids, transmission cracks, or fissures, which may be referred to herein as structural defects. The microparticle subsurface structure may have a second composition. The second composition may include aluminum and one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese. In some embodiments, the concentration of magnesium in the aluminum alloy may be less than 10% by weight, or the concentrations of magnesium and zinc in the aluminum alloy may be less than 20% by weight, and the ratio of zinc to magnesium in the concentration may be 0.1 to 10.0. Optionally, the concentration of magnesium in the first composition (i.e., bulk) is greater than the second composition (i.e., microparticle subsurface structure), the concentration of copper in the first composition is greater than the second composition, or the concentration of zinc in the first composition is greater than the second composition. The second composition (i.e., the microparticle subsurface structure) may be substantially free of organic matter, oil, hydrocarbons, soil, inorganic residues, entrained oxides, or anodic oxides, which may be referred to herein as compositional defects.

[0010] In some embodiments, the second composition (i.e., microparticle subsurface structure) may contain more defects than the first composition (i.e., bulk). However, in other embodiments, the second composition may be substantially the same as the first composition. In some cases, the second composition may include a grain structure uniformity or distribution uniformity of alloying elements different from that of the first composition. In some embodiments, the second composition may have a grain structure different from that of the first composition. For example, the grain structure of the second composition may include aluminum alloy particles having an average diameter of 10 nm to 500 nm. In some cases, the second composition may include homogenous ultrafine particles having a grain size or average grain size of about 10 nm to about 200 nm, such as 10 nm to 25 nm, 25 nm to 50 nm, 50 nm to 100 nm, 100 nm to 150 nm, or 150 nm to 200 nm. The second composition may include or may include precipitates (precipitates). In some examples, the precipitates may have an average diameter of 10 nm to 2 μm. In some embodiments, the precipitates may include one or more alloying elements selected from the group including zinc, magnesium, copper, chromium, silicon, iron, and manganese.

[0011] The oxide layer on the micrograin subsurface structure may have a thickness of 1 nm to 20 nm. The oxide layer may be a native oxide layer in some instances, or may be thicker than a native oxide layer due to heating that may occur when forming the micrograin subsurface structure or during subsequent processing. In some embodiments, the aluminum alloy product may further include a silicon-containing layer or oxide layer on the micrograin subsurface structure. The silicon-containing layer may modify some of the bonding sites in the micrograin subsurface structure. In some cases, the weight percent of aluminum in the second composition may be less than the weight percent of aluminum in the first composition. In some embodiments, the aluminum alloy product having the micrograin subsurface structure may exhibit bond durability of 22 cycles to 100 cycles or more according to FLTMBV101-07 Standard Test, Stress Durability Test for Adhesive Lap Shear Bonds (2017), which is incorporated herein by reference. The bond durability can be at least 22, at least 30, at least 35, at least 40, at least 45, at least 50, at least 55, at least 60, at least 65, at least 70, at least 75, at least 80, at least 85, at least 90, at least 95, or at least 100 cycles.

[0012] In another aspect, a method of processing an aluminum alloy product is described. The method of this aspect may include providing a rolled aluminum alloy product having a bulk and a near-rolled surface microstructure. In some embodiments, the rolled aluminum alloy product may include at least one of a 7xxx series aluminum alloy product, a 6xxx series aluminum alloy product, or a 5xxx series aluminum alloy product. In some embodiments, the rolled aluminum alloy product may be a hot rolled aluminum alloy product or a cold rolled aluminum alloy product. The bulk may include a matrix having grains of aluminum alloy, and the bulk may have a first composition. The first composition may include aluminum and one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese. The one or more alloying elements may be spatially uniformly distributed within the bulk. The near-rolled surface microstructure may include one or more defects. For example, in some embodiments, the one or more defects may correspond to or include one or more voids, transmission cracks, or fissures.

[0013] The method may also include modifying the near-surface microstructure (i.e., near-surface microstructure) to produce a first surface region and a second surface region. The first surface region may comprise a near-surface microstructure having a thickness of less than 500 nm, which may correspond to a reduction in the thickness of the near-surface microstructure upon modification. The second surface region may be free of the near-surface microstructure. The second surface region may comprise an oxide layer, such as an oxide having a thickness of 1 nm to 20 nm, and a microparticle subsurface structure, also referred to herein as the modified near-surface microstructure. In some embodiments, the first surface region and the second surface region may be discontinuous. For example, in some cases, "islands" of the first surface region may form in the second surface region, or vice versa. In some embodiments, the ratio of the area of ​​the first surface region to the area of ​​the second surface region may be less than 50%. For example, the ratio of the area of ​​the first surface region to the area of ​​the second surface region may be 40% or less, 35% or less, 33% or less, 30% or less, 25% or less, 20% or less, 15% or less, 10% or less, or 5% or less. In some cases, only the second surface region may be present in the aluminum alloy product.

[0014] The subsurface structure of the microparticle may be substantially free of one or more defects. The microparticle subsurface structure may be between the oxide layer and the bulk and may have a second composition. The second composition may include aluminum and one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese. In some embodiments, the concentration of magnesium in the aluminum alloy may be less than 10% by weight, or the concentrations of magnesium and zinc in the aluminum alloy may be less than 20% by weight, and the concentration of zinc to magnesium may be 0.1 to 10.0. In some cases, the concentration of magnesium in the first composition may be greater than the second composition, or the concentration of copper in the first composition may be greater than the second composition, or the concentration of zinc in the first composition may be greater than the second composition. The second composition may be substantially free of oil, hydrocarbons, soil, inorganic residue, entrained oxides, or anodic oxides. The second composition may comprise a grain structure that is different from the grain structure of the first composition. For example, the particle structure of the second composition may include aluminum alloy particles having an average diameter of 10 nm to 500 nm.

[0015] In some embodiments, modifying the near-rolled surface microstructure may include integrating the near-rolled surface microstructure to produce a second composition and eliminate at least a portion of one or more defects. In some cases, the second composition of the micrograin subsurface structure may have fewer defects than the near-rolled surface microstructure. In some cases, the second composition may have more defects than the first composition. However, in some embodiments, the second composition may be substantially the same as the first composition. In some cases, the second composition may include a grain structure uniformity or alloying element distribution uniformity that is different from that of the near-rolled surface microstructure or the first composition.

[0016] The second surface region may include a first oxide layer having a thickness of 1 nm to 20 nm. In some embodiments, the micrograin subsurface structure may exhibit or provide an aluminum alloy product comprising the micrograin subsurface structure with a bond durability of 22 cycles to 100 cycles or more according to the FLTMBV101-07 standard test. In some embodiments, modifying the near-rolled surface microstructure may include depositing a silicon-containing layer when generating the micrograin subsurface structure. The silicon-containing layer may be present on the micrograin subsurface structure and / or on a portion of the micrograin subsurface structure or on an oxide layer corresponding thereto. The silicon-containing layer may modify some of the bond sites in the micrograin subsurface structure. In some cases, modifying the near-rolled surface microstructure may include coating at least a portion of the micrograin subsurface structure and / or an oxide layer thereon with a silicon-containing material to modify some of the bond sites in the micrograin subsurface structure. The coating may include transferring the silicon-containing material from the silicon-containing grit used to modify the near-rolled surface microstructure. Examples of silicon-containing grits can include SACO grit. Optionally, modifying the near-rolled surface microstructure to produce a fine grain subsurface structure can include producing homogenous ultrafine grains.

[0017] In some embodiments, the method of this aspect may further include subjecting the near-rolled surface microstructure to one or more mechanical modification processes. The mechanical modification may include grinding the near-rolled surface microstructure, physically ablating the near-rolled surface microstructure, laser ablation of the near-rolled surface microstructure, sandblasting the near-rolled surface microstructure, or polishing the near-rolled surface microstructure. In some cases, physically ablating the near-rolled surface microstructure may include grit blasting the near-rolled surface microstructure. In some embodiments, the mechanical modification may include subjecting the near-rolled surface microstructure to a first modification process and subjecting the near-rolled surface microstructure to a second modification process. In some cases, the mechanical modification may further include subjecting the near-rolled surface microstructure to a third modification process. In some examples, a first modification process may include exposing the near-surface microstructure to a first grit, a second modification process may include exposing the near-surface microstructure to a second grit, and a third modification process may include exposing the near-surface microstructure to a third grit, where the first grit may be coarser than the second grit, and the second grit may be coarser than the third grit.

[0018] In some embodiments, modification of the near-rolled surface microstructure may occur during final gauging of the rolled aluminum alloy product. In some cases, modification of the near-rolled surface microstructure may occur after a hot rolling process. In some cases, modification of the near-rolled surface microstructure may occur before a cold rolling process. In some cases, modification of the near-rolled surface microstructure may occur before a pre-working process.

[0019] In some embodiments, the method may further include subjecting the microparticle subsurface structure to a pre-fabrication process. In some cases, the pre-fabrication process may include etching the microparticle subsurface structure.

[0020] In another aspect, an aluminum alloy product is described, such as an aluminum alloy product produced according to the methods described herein. In yet another aspect, a method for producing an aluminum alloy product as described herein is described.

[0021] Other objects and advantages will become apparent from the following detailed description of non-limiting examples.

[0022] This specification refers to the following accompanying figures, in which the use of like reference numbers in different figures is intended to illustrate the same or similar components. [Brief description of the drawings]

[0023] [Figure 1A] 1 provides a schematic representation of an aluminum alloy product having a near-rolled surface microstructure that includes one or more defects. [Figure 1B] 1 provides an SEM image of an aluminum alloy product having a near-rolled surface microstructure that includes one or more defects. [Figure 2A] 1 provides an exemplary graph illustrating elemental distribution of alloying elements and distribution of aluminum as a function of depth for an aluminum alloy product having a near-rolled surface microstructure that includes one or more defects. [Figure 2B] 1 provides an exemplary graph showing elemental distribution of alloying elements and distribution of aluminum as a function of depth for an aluminum alloy product having a micrograin subsurface structure. [Figure 2C] 1 provides an exemplary graph showing elemental distribution of copper as a function of depth for an aluminum alloy product having a rolled near surface structure compared to an aluminum alloy product having a micrograin subsurface structure; [Figure 2D] 1 provides an exemplary graph showing elemental distribution of zinc as a function of depth for an aluminum alloy product having a near-rolled surface structure compared to an aluminum alloy product having a micrograin subsurface structure; [Figure 3A]1 provides an exemplary graph illustrating the distribution of defects as a function of depth in an aluminum alloy product having a near-rolled surface microstructure that includes one or more defects. [Figure 3B] 1 provides an exemplary graph showing the distribution of defects as a function of depth in an aluminum alloy product having a micro-grain subsurface structure. [Figure 4A] 1 provides an exemplary graph illustrating grain size distribution as a function of depth in an aluminum alloy product having a near-rolled surface microstructure that includes one or more defects. [Figure 4B] 1 provides an exemplary graph showing grain size distribution as a function of depth in an aluminum alloy product having a micrograin subsurface structure. [Diagram 5] A, B, and C provide a schematic of mechanically modifying the near-rolled surface microstructure to generate a micrograin subsurface structure. [Figure 6] 1A, B, and C provide schematics of mechanically altering the near-rolled surface microstructure to produce a micrograin subsurface structure according to another embodiment. [Figure 7] 1A, B, and C provide schematics of mechanically altering the near-rolled surface microstructure to produce a micrograin subsurface structure according to another embodiment. [Figure 8] A, B, C, D, and E provide schematics of mechanically modifying the near-rolled surface microstructure via a multi-modification process to generate a micrograined subsurface structure. [Figure 9] 1 provides exemplary images of elemental distribution of an aluminum alloy product sample modified according to the techniques and methods provided herein. [Figure 10A] 1 is an exemplary image of an aluminum alloy product sample having a surface region with a micrograin subsurface structure. [Figure 10B] 1 is an exemplary image of an aluminum alloy product sample having a surface region without a micro-grain subsurface structure. [Figure 11] 1 provides exemplary images of surface regions of various aluminum alloy product samples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Described herein are aluminum alloy products produced by casting and / or rolling processes in which the near-rolled surface microstructure of the rolled product is mechanically altered to produce a micrograin subsurface structure, as well as processes for producing such products. The near-rolled surface microstructure may occupy a region to the majority of the depth of the rolled product and may include one or more defects. The micrograin subsurface structure may be produced by mechanically altering the near-rolled surface microstructure. The micrograin subsurface structure may have a composition that is different from the composition of the near-rolled surface microstructure.

[0025] The aluminum alloy product may be cast and rolled to produce a rolled product having a near-surface microstructure. The generation of the near-surface microstructure may occur in a sub-surface layer of the aluminum alloy product, also known as the "surface layer" or "Beerby layer." Defects in the near-surface microstructure may be generated, for example, during the rolling process. Exemplary defects include entrapped oil, entrapped oxides, voids, crevices, and cracks. For example, the presence of dense populations of amorphous carbon and / or aluminum carbide may be generated from the incorporation of rolling lubricant into the surface layer of the rolled product during the rolling process. Similarly, dense populations of oxides in the near-surface microstructure may be generated from a combination of the incorporation of rolling lubricant and shear strain generated during the rolling process, which may result in, for example, the incorporation of surface oxides into the near-surface microstructure.

[0026] Defects in the near-rolled surface microstructure can affect the mechanical and chemical performance of aluminum alloy products, for example, they can increase the corrosion sensitivity of aluminum alloy products or reduce the quality of bonds between aluminum alloy products that are bonded together, such as with adhesives or epoxies.

[0027] As another example, the presence of oxides and / or voids at or near the boundary between the subsurface layer and the bulk can cause or induce crack propagation. Boundary voids and oxides can provide preferential crack propagation paths between the subsurface layer and the bulk, so that stresses on the region, either during processing or end use, can result in shearing of the subsurface layer from the bulk. Cracks propagated within the rolled near-surface microstructure can then nucleate new cracks. Secondary cracks can originate from the primary crack, so the presence of defects within the near-surface microstructure compromises the possibility of a chain reaction.

[0028] Defects can also cause the near-surface microstructure to have different mechanical and chemical properties than the bulk. For example, a dense population of oxides in the near-surface microstructure can result in the near-surface microstructure having a relatively low ductility compared to the bulk. This can mean that the near-surface microstructure may deform less than the bulk during processing or use. Different ductility can lead to mechanical failure of the aluminum alloy product, for example, fracture, cracking, or even shearing between the near-surface microstructure and the bulk.

[0029] Other defects that may result from the rolling and casting process include non-uniformity in composition and grain structure. In some embodiments, non-uniform element distribution (e.g., alloying element distribution) is of concern because it may result in, for example, increased corrosion sensitivity of the aluminum alloy product. During processing of the aluminum alloy product, certain elements may diffuse faster than other elements into the near-rolled surface microstructure of the rolled product. This may result in a denser population of certain alloying elements in the near-rolled surface microstructure than the population in the bulk. Furthermore, the presence of dense populations of some alloying elements may increase the corrosion sensitivity of the aluminum alloy product. Due to low activation energy and the presence of defects, the diffusion rate of the dense alloying elements in the near-rolled surface microstructure may be greater than the diffusion rate of the alloying elements in the bulk. This may cause the near-rolled surface microstructure to react. In a corrosive environment, increased diffusion rates or the presence of near-surface alloying elements, as well as the presence of other defects in the near-rolled surface microstructure, may cause more vigorous corrosion propagation conditions.

[0030] Mechanically altering the rolled near-surface microstructure may provide many advantages, including producing a new (modified) near-surface microstructure or a micrograin subsurface structure that has a different composition than the rolled near-surface microstructure. As a particular example, the modified composition of the micrograin subsurface structure, also referred to herein as the second composition, may be free or substantially free of defects present in the rolled composition. In some cases, the second composition of the micrograin subsurface structure may have a reduced number of defects compared to the number of defects in the composition of the rolled near-surface microstructure.

[0031] Another advantage of creating micro-grained subsurface structures may be reduced corrosion sensitivity. By creating a uniform elemental distribution within the micro-grained subsurface structure, the reactivity of the surface can be controlled (e.g., reduced). Furthermore, the micro-grained subsurface structure can be mechanically modified to have the appropriate mechanical interlock and cleanliness (e.g., defect-free) to withstand cyclic or repeated corrosion exposure.

[0032] Overall, the mechanical and chemical performance of aluminum alloy products can be improved by mechanically modifying the near-rolled surface microstructure as described herein. Creating a homogenous elemental distribution and homogenous grain structure, as well as creating a substantially defect-free near-surface composition, can improve subsequent etching and pre-fabrication processes, and extend the life and usefulness of the aluminum alloy product. Advantageously, bonding between alloy products having a micrograin subsurface structure according to the present disclosure can be more durable than bonding between alloy products having a near-rolled surface microstructure.

[0033] Definitions and Explanations As used herein, the terms "invention," "the invention," "this invention," and "the present invention" are intended to refer broadly to all subject matter of this patent application and the claims that follow. Statements containing these terms should not be understood as limiting the subject matter described herein or the meaning or scope of the claims that follow.

[0034] References are made herein to alloys identified by AA numbers and other related designations, such as "series" or "7xxx." For an understanding of the numbering systems most commonly used to name and identify aluminum and its alloys, see "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Compositions Limits for Aluminum Alloys in the Form of Castings and Ingot" (both published by The Aluminum Association).

[0035] As used herein, a plate generally has a thickness of greater than about 15 mm. For example, a plate can refer to an aluminum product having a thickness of greater than about 15 mm, greater than about 20 mm, greater than about 25 mm, greater than about 30 mm, greater than about 35 mm, greater than about 40 mm, greater than about 45 mm, greater than about 50 mm, or greater than about 100 mm.

[0036] As used herein, a shade (also referred to as a sheet plate) generally has a thickness of about 4 mm to about 15 mm. For example, a shade may have a thickness of about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm, or about 15 mm.

[0037] As used herein, sheet generally refers to an aluminum product having a thickness of less than about 4 mm. For example, the sheet may have a thickness of less than about 4 mm, less than about 3 mm, less than about 2 mm, less than about 1 mm, less than about 0.5 mm, or less than about 0.3 mm, (e.g., about 0.2 mm).

[0038] As used herein, terms such as "cast metal product," "cast product," "cast aluminum alloy product," and the like, are used interchangeably and may refer to products made by direct chill casting (including direct chill simultaneous casting) or semi-continuous casting, continuous casting (including, for example, by use of a twin belt caster, twin roll caster, block caster, or any other casting machine), electromagnetic casting, hot top casting, or any other casting process, including the processes disclosed herein.

[0039] As used herein, the meaning of "room temperature" can include a temperature of about 15° C. to about 30° C., e.g., about 15° C., about 16° C., about 17° C., about 18° C., about 19° C., about 20° C., about 21° C., about 22° C., about 23° C., about 24° C., about 25° C., about 26° C., about 27° C., about 28° C., about 29° C., or about 30° C. As used herein, the meaning of "ambient conditions" can include a temperature of about room temperature, a relative humidity of about 20% to about 100%, and an atmospheric pressure of about 975 millibars (mbar) to about 1050 mbar. For example, the relative humidity may be about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about It can be 1%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, or anything therebetween. For example, the air pressure can be about 975 mbar, about 980 mbar, about 985 mbar, about 990 mbar, about 995 mbar, about 1000 mbar, about 1005 mbar, about 1010 mbar, about 1015 mbar, about 1020 mbar, about 1025 mbar, about 1030 mbar, about 1035 mbar, about 1040 mbar, about 1045 mbar, about 1050 mbar, or anything therebetween.

[0040] All ranges disclosed herein should be understood to include any and all subranges subsumed therein. For example, a stated range "1-10" should be considered to include any and all subranges between a minimum value of 1 and a maximum value of 10 (and inclusive), i.e., all subranges begin with a minimum value of 1 or more (e.g., 1-6.1) and end with a maximum value of 10 or less (e.g., 5.5-10). Unless otherwise indicated, the term "maximum" when referring to a compositional amount of an element means that the element is optional and includes a zero percent composition of that particular element. Unless otherwise indicated, all compositional percentages are weight percent (wt%).

[0041] As used herein, the meanings of "a," "an," and "the" include singular and plural references unless the context clearly dictates otherwise.

[0042] FIG. 1A illustrates a schematic diagram of an aluminum alloy product 100. The aluminum alloy product 100 may be a rolled product, such as a plate, a sheet, or a sheet. The aluminum alloy product 100 may be produced by any suitable casting and / or rolling process. Exemplary casting processes include direct chill casting (including direct chill co-casting), semi-continuous casting, continuous casting (including, for example, using a twin belt caster, a twin roll caster, a block caster, or any other continuous caster), electromagnetic casting, hot top casting, or other casting methods. The aluminum alloy product 100 may include or correspond to a rolled product. The rolled product may be a cold rolled product or a hot rolled product, depending on the casting process and / or the application of the aluminum alloy product 100.

[0043] In embodiments, the rolled product may be relatively rectangular in cross-section and may have a width W and a thickness T, which may be selected based on the application of the aluminum alloy product 100. In various embodiments, the rolled product may have a width W of about 0.1 m to about 10 m, e.g., 0.1 m to 1 m, 1 m to 2 m, 2 m to 3 m, 3 m to 5 m, or 5 m to 10 m. In other embodiments, the rolled product may have a width W in the range of 0.1 m to 0.2 m, 0.2 m to 0.3 m, 0.3 m to 0.4 m, or 0.4 m to 0.5 m. The rolled product may have a thickness T of 0.2 mm to 1 mm, 1 mm to 4 mm, 4 mm to 10 mm, 4 mm to 15 mm, 15 mm to 25 mm, 25 mm to 40 mm, 40 mm to 50 mm, 50 mm to 100 mm, or in embodiments, greater than 100 mm. The rolled product may be in the form of, for example, a plate, a sheet, or a sheet. It will be understood that FIG. 1 is not to scale.

[0044] The rolled product may include a near-surface microstructure 110 and a bulk 120. As described herein, the near-surface microstructure may also be referred to as a near-surface microstructure (NSM). The generation of the near-surface microstructure 110 may occur as part of the rolled product during the rolling process. The near-surface microstructure 110 may occur in a subsurface layer of the rolled product. The subsurface layer, also known as the "surface layer" or "Beerby layer," may include a portion of the rolled product that occupies a space from the surface of the rolled product to a depth of the thickness of the rolled product. In an embodiment, the rolled product may include two or more surfaces and / or have two or more subsurface layers. In such an embodiment, the near-surface microstructure 110 may occur in each subsurface layer. For example, the rolled product may have a thickness such that two surfaces are generated, one surface at the top of the rolled product and one surface at the bottom of the rolled product, each surface directly facing each other. The other four sides or edges of the rolled product that extend circumferentially around the side / edge of the rolled product may not be thick enough or may not have a large enough area to create a subsurface layer, and / or may not be subjected to a sufficient rolling process to generate a rolled near-surface microstructure, and / or may not be evaluated for near-surface microstructure. In some cases, the side edges may be scalped, trimmed, or otherwise removed. In some examples, each of the top and bottom surfaces may have a corresponding subsurface layer. In each of the corresponding subsurface layers, the rolled near-surface microstructure 110 may be present. Thus, in various embodiments, the rolled product may have multiple surfaces with rolled near-surface microstructure 110.

[0045] In embodiments, the near-surface microstructure 110 may occupy the entire subsurface layer. The near-surface microstructure 110 may occupy the space from the surface of the rolled product to a depth to the bulk 120 or to a depth within the bulk 120. The depth may be greater than 500 nm. In some cases, the depth may be 500 nm to 700 nm, 500 nm to 800 nm, 200 nm to 800 nm, 800 nm to 1 μm, 1 μm to 5 μm, 5 μm to 10 μm, 10 μm to 15 μm, 15 μm to 20 μm, or any subrange thereof. In other embodiments, the depth may be less than 500 nm. For example, the depth can be 50 nm to 100 nm, 100 nm to 150 nm, 150 nm to 200 nm, 200 nm to 250 nm, 250 nm to 300 nm, 300 nm to 350 nm, 350 nm to 400 nm, 400 nm to 450 nm, 450 nm to 500 nm, or any subrange thereof.

[0046] The rolled products may include 7xxx series aluminum alloy products. Exemplary 7xxx series aluminum alloy products include AA7011, AA7019, AA7020, AA7021, AA7039, AA7072, AA7075, AA7085, AA7108, AA7108A, AA7015, AA7017, AA7018, AA7019A, AA7024, AA7025, AA7028, AA7030, AA7031, AA7033, AA7035, AA7035A, AA7046, AA7046A, AA7003, AA7004, AA7005, AA7009, AA701 0, AA7011, AA7012, AA7014, AA7016, AA7116, AA7122, AA7023, AA7026, AA7029, AA7129, AA7229 , AA7032, AA7033, AA7034, AA7036, AA7136, AA7037, AA7040, AA7140, AA7041, AA7049, AA7049 A, AA7149, AA7204, AA7249, AA7349, AA7449, AA7050, AA7050A, AA7150, AA7250, AA7055, AA71 55, AA7255, AA7056, AA7060, AA7064, AA7065, AA7068, AA7168, AA7175, AA7475, AA7076, AA7178, AA7278, AA7278A, AA7081, AA7181, AA7185, AA7090, AA7093, AA7095, or AA7099 products.

[0047] In various embodiments, the rolled product may include a 5xxx series aluminum alloy product, for example, AA5182, AA5183, AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA5119, AA5119A, AA5021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA5049, AA5149, AA5249, AA5 349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, AA5251, AA5251A, AA5351, AA 5451, AA5052, AA5252, AA5352, AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454, AA5554, AA5654, AA 5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5556, AA5456A, AA5456B, AA5556, AA5556A, AA5556B, These may include AA5556C, AA5257, AA5457, AA5557, AA5657, AA5058, AA5059, AA5070, AA5180, AA5180A, AA5082, AA5182, AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187, or AA5088 products.

[0048] In various embodiments, the rolled product may include a 6xxx series aluminum alloy product. For example, the rolled product may include AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015, AA6016, AA6016A, AA611 6, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA6027, AA6028, AA6031, AA6032 , AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA6053, AA6055, AA6056 , AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A, AA6261, AA636 1, AA6162, AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092 products.

[0049] In yet other embodiments, the rolled product may include a 1xxx series aluminum alloy product, a 2xxx series aluminum alloy product, a 3xxx series aluminum alloy product, a 4xxx series aluminum alloy product, or an 8xxx series aluminum alloy product.

[0050] A boundary 115 may exist between the near-rolled surface microstructure 110 and the bulk 120. The boundary 115 may indicate a depth where the rolled composition of the near-rolled surface microstructure 110 transitions to the composition of the bulk 120, also referred to as the bulk composition or first composition. The boundary 115 may exist at a depth where the near-rolled surface microstructure 110 occupies in the bulk 120. The boundary 115 may extend parallel or nearly parallel to the surface of the rolled product and may extend the full width or lateral dimension of the rolled product. In some embodiments, the boundary 115 may occur at a discrete depth or may occur over a range of depths. In an embodiment, the boundary 115 may be a grain boundary between the near-rolled surface microstructure 110 and the bulk 120. The grain boundary may be a boundary that delineates between two different grain structures of the near-rolled surface microstructure 110 and the bulk 120. For example, the near-rolled surface microstructure 110 may have a heterogeneous grain structure, such as a heterogeneous distribution of both large and small grain sizes. In contrast, the bulk 120 may have a homogeneous (e.g., uniformly distributed) grain structure, such as a uniform distribution of grain sizes, which may be large and small. In such an example, the boundary 115 may be a grain boundary between the heterogeneous grain structure of the near-rolled surface microstructure 110 and the homogeneous grain structure of the bulk 120. In an embodiment, the bulk 120 having a bulk grain size may occur at a depth from the surface of 10 μm to 45 μm in the rolled product, depending on the alloy and process. In some cases, a homogeneous grain structure may mean that a certain percentage of any given volume of the bulk 120 may have the same or approximately the same grain size. For example, a homogeneous grain structure may mean that about 70% or more of any given volume of the bulk 120 has approximately the same grain size, such as an average grain size in the range of 5 μm to 50 μm. The different uniformity of the grain structure can be illustrated by FIG. 1A and other figures, where the packing patterns differ between the near-rolled surface microstructure 110 and the bulk 120.

[0051] As noted above, the rolled near surface microstructure 110 has a composition that may be referred to herein as the "rolled composition," which may include one or more defects 130a-130e (collectively, defects 130). The one or more defects 130 may affect the mechanical and chemical performance of the aluminum alloy product 100. For example, the one or more defects 130 may increase corrosion sensitivity, reduce bond durability performance, and reduce the tensile and shear strength of the aluminum alloy product 100.

[0052] As shown in FIG. 1A, the one or more defects 130 may include various defects. In some embodiments, the one or more defects 130 may include one or both of compositional and structural defects. For example, the defects 130 may include one or more internal cracks 130a or surface cracks 130d. The internal cracks 130a and surface cracks 130d may include propagation cracks, fissures, and microcracks. The internal cracks 130a and surface cracks 130d may be generated by stress or strain conditions applied to the rolled product during the rolling process, such as normal shear stress applied to the rolled product by the rollers. As shown in FIG. 1A, the surface cracks 130d may be generated at the surface of the rolled surface near microstructure 110, resulting in an uneven or irregular surface. In contrast, the internal cracks 130a may be generated within the rolled surface near microstructure 110. In an embodiment, the internal cracks 130a may extend horizontally through the near-rolled surface microstructure 110, parallel to the surface of the near-rolled surface microstructure 110, or in any other direction relative to the surface of the near-rolled surface microstructure 100.

[0053] In an embodiment, the voids 130b may induce the development of internal cracks 130a and surface cracks 130d. Weak sites created by defects 130 such as voids 130b may be sites where cracks are more likely to initiate. The voids 130b may include or consist of spaces in the near-rolled surface microstructure 110 that are devoid of solid material. The absence of solid material may be due to steam entrapment in the near-rolled surface microstructure 110 during processing or due to the mechanical structure and / or grain composition of the rolled product material.

[0054] The one or more defects 130 may also include entrained material 130c. The entrained material 130c may include hot mill pick-ups, such as, for example, entrained oxides and / or entrained oil. The entrained material 130c may include oxides and lubricants incorporated and trapped in the near-rolled surface microstructure 110 during the rolling process, as well as any other entrained impurities. For example, rolling lubricants may be incorporated into the near-rolled surface microstructure 110 during rolling of the aluminum alloy product. Amorphous carbon and / or aluminum carbide trapped in the near-rolled surface microstructure 110 may indicate or correspond to entrained lubricants. The entrained oxides may include metal oxides, such as, for example, aluminum oxide or magnesium oxide. Metal oxides may be generated when metal elements at or near the surface of the rolled product oxidize during processing and are then incorporated into the rolled product.

[0055] The presence of voids 130b and / or entrapped material 130c near the boundary 115 may induce crack propagation. Weak spots at the boundary 115, such as voids 130b and entrapped material 130c, may provide crack propagation paths between the near-rolled surface microstructure 110 and the bulk 120. Such paths between defects may be preferential crack propagation paths, and any stress condition may induce the creation of internal cracks 130a between the near-rolled surface microstructure 110 and the bulk 120. Stress exposure may result in partial or complete shearing of the near-rolled surface microstructure 110 from the bulk 120. Additionally, any internal cracks 130a may initiate further cracks. Thus, the presence of defects 130 may cause a detrimental chain reaction of defect creation within the near-rolled surface microstructure 110 and potentially within the bulk 120.

[0056] In an embodiment, the bulk 120 may have a composition, referred to herein as a "first composition," which may include primarily aluminum and alloying elements 140. Exemplary alloying elements 140 may include zinc, magnesium, copper, chromium, silicon, iron, and / or manganese, and may depend on or define a particular alloy. As shown in FIG. 1A, the alloying elements 140 may be spatially uniformly (e.g., evenly) distributed within the bulk 120. The uniform distribution of the alloying elements 140 shown in FIG. 1A may not imply or require that an array of alloying elements 140 occurs. Rather, the distribution of the alloying elements 140 shown in the bulk 120 of FIG. 1A is a pictorial representation of a uniform distribution of the alloying elements 140 in the bulk 120. The uniform distribution of the alloying elements 140 may mean that a certain percentage of any given volume of the first composition may include the same or substantially the same amount of the alloying elements 140.

[0057] In various embodiments, one of the defects 130 may include a non-uniform distribution of the alloying elements 140. The dense population 130e of the alloying elements 140 may occur or be created in the near-rolled surface microstructure 110 during the casting and / or rolling process. Some of the alloying elements 140 may exhibit different diffusion coefficients from one another, resulting in different diffusion rates for different alloying elements. That is, some of the alloying elements 140 may diffuse at a different rate than another alloying element 140. Thus, during casting and / or rolling of the rolled product, certain alloying elements may diffuse from the bulk 120 to the surface or near-rolled surface microstructure 110 at a faster rate than other elements present in the bulk 120. The faster diffusion rate of certain alloying elements 140 may create a non-uniform distribution of the alloying elements 140 between the near-rolled surface microstructure 110 and the bulk 120, creating a dense population 130e of certain alloying elements 140 in the near-rolled surface microstructure 110. For example, in some embodiments, zinc may have a higher diffusion rate under processing conditions than other alloying elements and may preferentially concentrate at the surface, resulting in a dense population 130e of zinc within the rolled surface near microstructure 110. Again, the dense population 130e shown in FIG. 1A is merely pictorial and is not intended to limit the dense population of alloying elements 140 to clusters of alloying elements as shown, although in some cases clusters of alloying elements 140 may be present. Rather, the presence of the dense population 130e in the rolled surface near microstructure 110 may indicate that the concentration of alloying elements in the rolled surface near microstructure 110 may be generally different (e.g., higher) than in the bulk 120.

[0058] Non-uniform distribution of alloying elements 140, and other defects 130, can affect the chemical performance of the aluminum alloy product 100. For example, the presence of defects 130 in the near-rolled surface microstructure 110 can cause pre-processing applications to be patchy or incompletely coated. Defects 130 can also interfere with etch pre-processing, as the non-uniform distribution of defects 130 and alloying elements 140 can provide an inconsistent medium for the etching process.

[0059] The dense population 130e may also, or alternatively, increase the corrosion sensitivity of the aluminum alloy product 100. At or near the surface, the diffusion rate of the alloying elements 140 may increase by a factor of one or two due to the low activation energy and the presence of other defects 130. Thus, the dense population 130e may propagate reactive pockets or regions within the rolled near surface microstructure 110 that may initiate corrosion. Certain aluminum alloy series may be more susceptible to corrosion sensitivity due to the dense population 130e of alloying elements 140. For example, the 7xxx series aluminum alloys may be more susceptible to the generation of the dense population 130e due to their high composition of alloying elements 140. The 7xxx series aluminum alloys may contain, for example, more than 10% alloying elements, while other aluminum alloy series may contain 3-4% alloying elements.

[0060] FIG. 1B shows a scanning electron micrograph (SEM) image of aluminum alloy product 105. Aluminum alloy product 105 may be similar or the same as aluminum alloy product 100. As shown, aluminum alloy product 105 may include bulk 125, which may be the same as bulk 120, and near-surface microstructure 112, which may be the same as rolled near-surface microstructure 110. Near-surface microstructure 112 shown in FIG. 1B may have a thickness between 100 nm and 300 nm, although near-surface microstructure 112 may have a thickness greater than 500 nm in other sections of aluminum alloy product 105. Near-surface microstructure 112 may have one or more defects 135. One or more defects 135 as shown may include, for example, voids or entrapped material.

[0061] Increased corrosion sensitivity may contribute to poor performance during bonding and / or during bond durability testing. Bond durability testing evaluates the strength of bonds created by and / or with the surface (e.g., near-surface) microstructure of the alloy product. During testing, two aluminum alloy products are bonded together, such as by an epoxy adhesive. The bonded aluminum alloy products are then exposed to strain and / or other conditions. For example, the bonded alloy products may be immersed in a salt solution or subjected to wet or dry conditions. After a series of cycles at one or more conditions, the bond between the aluminum alloys is evaluated for chemical and mechanical failure. The bond durability performance of an aluminum alloy product may be indicative of the reactivity and corrosion sensitivity of the product's near-rolled surface microstructure.

[0062] 2A provides an example plot of the varying elemental distribution of alloying elements 140 across the depth of an aluminum alloy product 100. The graph 200A shown in FIG. 2A is provided for example purposes only to illustrate an example elemental distribution of alloying elements 140 across the depth of the rolled product, specifically, the change in elemental distribution between the near rolled surface microstructure 110 and the bulk 120. In FIG. 2A, the range of 0 nm to 200 nm deep into the rolled product may correspond to the near rolled surface microstructure 110, while the range of 600 nm to 2400 nm or more may correspond to the bulk 120 of the rolled product.

[0063] Graph 200A includes an x-axis that corresponds to a depth into the rolled product. The origin of the x-axis, 0 nm, may correspond to the surface of the rolled product. Specifically, 0 nm may correspond to the surface or beginning of the rolled near-surface microstructure 110. The depth into the rolled product may correspond to a thickness of the rolled product. The depth may correspond to a depth into the thickness of the rolled product. In embodiments, the depth may correspond to the entire thickness, while in other embodiments, the depth may correspond to only a portion of the thickness.

[0064] Graph 200A also includes multiple y-axes that correspond to the intensity of aluminum (e.g., the amount of the element present) and the intensity of alloying elements 140 (e.g., the amount of the element present) in the rolled product at a given depth in the rolled product. As shown in Figure 2A, the left y-axis corresponds to the intensity of aluminum present in the rolled product and the right y-axis corresponds to the intensity of one or more alloying elements 140 present in the rolled product. In an embodiment, the alloying elements 140 represented in graph 200A may include zinc, magnesium, copper, chromium, silicon, iron, and / or manganese.

[0065] The aluminum distribution line 210A on the graph 200A shows an exemplary aluminum elemental profile throughout the depth of the rolled product. The depth may correspond to a depth into the thickness of the rolled product. However, in some embodiments, the depth may correspond only to the space occupied by a portion of the rolled composition and / or the first composition. As shown, the depth of the rolled product as shown in the graph 200A may be 2400 nm (i.e., 2.4 μm). In various embodiments, the depth may be greater than 2400 nm. In other embodiments, the depth may be less than 2400 nm. For example, the depth may be 2000 nm, 1200 nm, or 800 nm. The depth may depend on the cross-section of the rolled product shown (e.g., the rolled composition, the thickness of the rolled composition, etc.).

[0066] As shown in graph 200A, the aluminum concentration 210A at or near the surface of the rolled near surface microstructure 110 of FIG. 2A may be minimal. During the first 600 nm, the aluminum concentration may increase and reach a steady state near 500 nm to 600 nm. This increasing aluminum distribution may indicate the presence of one or more defects 130 near the surface of the rolled product. As the defect or defects increase, the aluminum prominence present may decrease. As the depth reaches the bulk 120, the concentration of aluminum may reach the bulk concentration indicated by the plateau of the aluminum distribution line 210.

[0067] The alloying element distribution line 220A of FIG. 2A illustrates an exemplary elemental profile of alloying element 140 within the rolled product. As illustrated, a high concentration of alloying element 140 may be present near the surface of the rolled product. The prominence of alloying element 140 may be highest near the surface and then taper off to a depth of about 600 nm of the rolled product before reaching a constant or near constant concentration. The range of depths from 0 nm to 600 nm of the rolled product in FIG. 2A may correspond to the near-rolled surface microstructure 110. Thus, in an exemplary embodiment, a high population of alloying element 140 may be present within the near-rolled surface microstructure 110 and then taper off to a lower population within the bulk 120 of the rolled product. The constant concentration of alloying element 140 illustrated by the plateau of alloying element distribution line 220A may correspond to a uniform distribution of alloying element 140 within the bulk 120, as described above. Conversely, the decreasing slope of the alloying element distribution line 220A in the first 600 nm may correspond to a non-uniform distribution of the alloying elements 140 within the near-rolled surface microstructure 110, as described above. In an embodiment, the inflection points of the aluminum and alloying elements, where the aluminum distribution line 210A and the alloying element distribution line 220A begin to stabilize at about 400 nm or 600 nm, may correspond to the boundary 115. These inflection points may indicate a transition from the near-rolled surface composition to the first composition. In an embodiment, the near-rolled surface microstructure 110 may end and the bulk 120 may begin at a depth of about 600 nm. In various embodiments, the near-rolled surface microstructure 110 may transition into the bulk 120 at a depth of about 50 nm, about 100 nm, about 150 nm, about 250 nm, about 300 nm, about 400 nm, about 500 nm, about 600 nm, about 800 nm, about 1000 nm, about 1200 nm, about 1400 nm, about 1600 nm, about 1800 nm, or greater than 1800 nm.

[0068] FIG. 2B provides an exemplary plot of the varying elemental distribution of alloying elements 140 across the depth of an aluminum alloy product 100 having a micrograin subsurface structure. The graph 200B shown in FIG. 2B is provided for exemplary purposes only to illustrate the exemplary elemental distribution of alloying elements 140 across the depth of the rolled product, specifically, the change in elemental distribution between the near-rolled surface microstructure 110 illustrated in FIG. 2A and the micrograin subsurface structure illustrated in FIG. 2B. In FIG. 2B, the range of depths of the rolled product from 0 nm to 600 nm may correspond to the micrograin subsurface structure, while the range of depths of 600 nm to 2400 nm may correspond to the bulk 120 of the rolled product. As discussed in more detail with respect to FIGS. 5-8, the micrograin subsurface structure may correspond to a rolled product having a mechanically altered near-rolled surface microstructure 110.

[0069] Graph 200B includes an x-axis that corresponds to a depth of the rolled product. The origin of the x-axis, 0 nm, may correspond to the surface of the rolled product. Specifically, 0 nm may correspond to the surface or beginning of the microparticle subsurface structure. The depth into the rolled product may correspond to a thickness of the rolled product. The depth may correspond to a depth into the thickness of the rolled product. In embodiments, the depth may correspond to the entire thickness, while in other embodiments, the depth may correspond to only a portion of the thickness.

[0070] Graph 200B also includes multiple y-axes that correspond to the intensity of aluminum (e.g., the amount of the element present) and the intensity of alloying elements 140 (e.g., the amount of the element present) in the rolled product at a given depth in the rolled product. As shown in Figure 2B, the left y-axis corresponds to the intensity of aluminum present in the rolled product and the right y-axis corresponds to the intensity of one or more alloying elements 140 present in the rolled product. In an embodiment, the alloying elements 140 represented in graph 200B may include zinc, magnesium, copper, chromium, silicon, iron, and / or manganese.

[0071] Aluminum distribution line 210B on graph 200B illustrates an exemplary aluminum elemental profile throughout the depth of the rolled product. The depth may correspond to a depth into the thickness of the rolled product. However, in some embodiments, the depth may only correspond to the space occupied by a portion of the second composition and / or the first composition. As shown, the depth of the rolled product as shown in graph 200B may be 2400 nm. In embodiments, the depth may be less than 2400 nm. The depth may depend on the cross-section of the rolled product shown (e.g., the second composition, the thickness of the second composition, etc.).

[0072] As shown in graph 200B, the aluminum concentration 210B at or near the surface of the micro-grain subsurface structure of FIG. 2B may be substantially the same as the aluminum concentration throughout the depth. For the first 600 nm, the aluminum concentration may increase and reach a steady state near 600-1200 nm, but the aluminum concentration throughout the depth of the rolled product shown in graph 200B may remain substantially constant. As discussed above, this increasing aluminum distribution may indicate the presence of one or more defects 130 near the surface of the rolled product. An increase in the one or more defects may decrease the aluminum prominence present. Conversely, an increase in the aluminum prominence may indicate the absence or reduction of one or more defects 130. Thus, a constant distribution of aluminum between the surface and bulk 120 of the micro-grain subsurface structure may indicate a lower prominence or presence of one or more defects 130.

[0073] 2B illustrates an exemplary elemental profile of alloying elements 140 within the rolled product. As shown, the density of alloying elements 140 may remain substantially the same throughout the depth of the rolled product. That is, the prominence of alloying elements 140 at or near the surface of the micrograin subsurface structure may be similar or the same as the prominence of alloying elements 140 at or within the bulk 120.

[0074] FIG. 2C provides an exemplary data plot of various distributions of copper into the depth of the rolled product. Specifically, the graph 200C shown in FIG. 2C illustrates a comparative example of copper distribution between a rolled product having a near-rolled surface microstructure and a rolled product having a micro-grain subsurface structure. The micro-grain subsurface structure line 230C illustrates an exemplary elemental profile of copper within the rolled product. As shown, a high density of copper may be present near the surface of the rolled product. The copper prominence may be highest near the surface and then decrease to a depth of about 300 nm of the rolled product before gradually increasing and reaching a constant or near constant concentration. The range of depths of the rolled product from 0 nm to 300 nm may correspond to a micro-grain subsurface structure. Thus, in an exemplary embodiment, a high density population of copper may be present within the micro-grain subsurface structure and then gradually decrease to a lower density population within the bulk (e.g., bulk 120) of the rolled product.

[0075] Near-surface microstructure lines 235C show an exemplary elemental profile of copper within a near-surface microstructure, such as near-surface microstructure 110. As shown, a high density of copper may be present near the surface of the rolled product. The presence of copper within the rolled product may gradually increase until about 1200 nm (1.2 μm) and then reach a constant or near-constant concentration. A range of depths of the rolled product from 0 nm to 1200 nm may correspond to the near-surface microstructure. Thus, in an exemplary embodiment, a low density population of copper may be present within the near-surface microstructure and then gradually increase to a higher density population within the bulk (e.g., bulk 120) of the rolled product.

[0076] FIG. 2D provides an exemplary data plot of various distributions of zinc into the depth of the rolled product. Specifically, FIG. 2D shows a graph 200D illustrating a comparative example of zinc distribution between a rolled product having a near-rolled surface microstructure and a rolled product having a micrograin subsurface structure. Micrograin subsurface line 230D illustrates an exemplary elemental profile of zinc within the rolled product. As shown in graph 200D, a high density of zinc may be present near the surface of the rolled product. The zinc prominence may be highest near the surface and then decrease to a depth of about 300 nm of the rolled product before gradually increasing and reaching a constant or near constant concentration. The range of depths of the rolled product from 0 nm to 300 nm may correspond to a micrograin subsurface structure. Thus, in an exemplary embodiment, a high density population of zinc may be present within the micrograin subsurface structure and then gradually decrease to a lower density population within the bulk (e.g., bulk 120) of the rolled product.

[0077] Near-rolled surface microstructure line 235D illustrates an exemplary elemental profile of zinc within a near-rolled surface microstructure, such as near-rolled surface microstructure 110. As shown, a high density of zinc may be present near the surface of the rolled product. The presence of zinc within the rolled product may gradually increase until about 1500 nm (1.5 μm) and then reach a constant or near-constant concentration. A range of depths of the rolled product from 0 nm to 1500 nm may correspond to the near-rolled surface microstructure. Thus, in an exemplary embodiment, a low density population of zinc may be present within the near-rolled surface microstructure and then gradually increase to a higher density population within the bulk (e.g., bulk 120) of the rolled product.

[0078] 3A provides a plot showing the distribution of defects throughout the depth of an aluminum alloy product 100. Similar to graphs 200A and 200B, graph 300A is provided for exemplary purposes to illustrate an exemplary distribution profile of defects throughout the depth of a rolled product.

[0079] Graph 300A includes an x-axis that corresponds to the depth of the rolled product. The x-axis of graph 300A may correspond to the depth of the rolled product, similar to the x-axis of graphs 200A and 200B. In an embodiment, the depth may correspond to the thickness of the rolled product. In various embodiments, the origin of the x-axis, 0 nm, may correspond to the surface of the rolled product. The surface of the rolled product may also be the surface of the near-surface microstructure 110.

[0080] Graph 300A also includes multiple y-axes. The multiple y-axes may correspond to an intensity of aluminum and an intensity of defects. The intensities of both aluminum and defects may correspond to a population density or concentration of aluminum and defects, respectively, present at a given depth in the rolled product. For example, as shown by aluminum distribution line 310A of graph 300A, a lower concentration of aluminum may be present near the surface of the rolled product. However, the concentration of aluminum may increase and reach a plateau concentration at a depth of about 600 nm in the rolled product. This increase in aluminum concentration may indicate the presence of one or more defects 130 near the surface. In other words, a low concentration of aluminum near the surface of the rolled product may indicate one or more defects 130 in the rolled near surface microstructure 110.

[0081] The defect distribution line 320A may correspond to a population density or concentration of defects throughout the depth of the rolled product. The defects may correspond to one or more of the one or more defects 130. For example, the defects may correspond to entrained material 130c, voids 130b, and / or internal cracks 130a.

[0082] A higher concentration of one or more defects 130 may be present near the surface of the rolled product, as shown by defect distribution line 320A. The higher concentration of defects near the surface may correspond to the presence of defects in the rolled near surface microstructure 110. The concentration of defects may decrease with greater depth into the rolled product. At some point, for example near a depth of 600 nm in the rolled product, the defect concentration may reach a lower steady-state concentration. In an embodiment, the point at which the concentration of defects reaches a steady-state concentration may correspond to the boundary 115 between the rolled near surface microstructure 110 and the bulk 120.

[0083] In an exemplary embodiment, the defect may correspond to entrained material 130c. For example, the defect may correspond to entrained rolling lubricant. In such an exemplary embodiment, the defect distribution line 320A may indicate or correspond to the carbon concentration throughout the depth of the rolled product. A high concentration of carbon within the first 600 nm of the rolled product may indicate rolling lubricant trapped within the near-rolled surface microstructure 110. During processing of the rolled product, rolling lubricant and other processing materials may be incorporated into the near-rolled surface microstructure 110. Thus, there may be a higher concentration of entrained material 130c near the surface of the rolled product, such as within the near-rolled surface microstructure 110. However, as one deepens toward the bulk 120, the concentration of entrained material 130c may decrease until the concentration reaches a lower steady-state concentration of the first composition, which may be zero for some defects.

[0084] Figure 3B provides a plot showing the distribution of defects throughout the depth of the aluminum alloy product 100. Similar to graph 300A, graph 300B is provided for illustrative purposes to show an exemplary distribution profile of defects throughout the depth of a rolled product, and specifically, to show the contrast between the defect distribution between the rolled near surface microstructure 110 shown in Figure 3A and the micro-grain subsurface structure shown in Figure 3B.

[0085] Graph 300B includes an x-axis that corresponds to the depth of the rolled product. The x-axis of graph 300B may correspond to the depth of the rolled product, similar to the x-axis of graph 300A. In an embodiment, the depth may correspond to the thickness of the rolled product. In an embodiment, the depth may correspond to the thickness of the rolled product. In various embodiments, the origin of the x-axis, 0 nm, may correspond to the surface of the rolled product. The surface of the rolled product may also be the surface of the micro-particle subsurface structure.

[0086] Graph 300B also includes multiple y-axes. The multiple y-axes may correspond to an intensity of aluminum and an intensity of defects. The intensities of both aluminum and defects may correspond to a population density or concentration of aluminum and defects, respectively, present at a given depth in the rolled product. For example, as shown by aluminum distribution line 310B of graph 300B, the concentration of aluminum present near the surface of the rolled product may be the same or similar to the concentration of aluminum present throughout the depth of the rolled product. As noted above, an increase in the concentration of aluminum from the surface toward the bulk 120 of the rolled product may indicate the presence of one or more defects 130 near the surface. Thus, a stable concentration of aluminum between the surface and bulk 120 of the rolled product may indicate the absence of one or more defects 130 near the surface.

[0087] The defect distribution line 320B (the straight line in FIG. 3B) may correspond to a population density or concentration of defects throughout the depth of the rolled product. The defects may correspond to one or more of the one or more defects 130. For example, the defects may correspond to entrained material 130c, voids 130b, internal cracks 130a, etc. As shown by the defect distribution line 320B, the concentration of near-surface defects between the near-surface concentration and the concentration toward the bulk 120 of the rolled product or the concentration at the depth of the rolled product may remain constant. The concentration of defects may remain substantially the same between the micro-grain subsurface structure and the depth of the rolled product. For example, the concentration of near-surface defects in the rolled product may be the same or similar to the concentration of defects around a depth of 600 nm into the rolled product, the same or similar to the concentration of defects near a depth of 1200 nm in the rolled product, the same or similar to the concentration of defects near a depth of 1800 nm in the rolled product, or the same or similar to the concentration of defects near a depth of 2400 in the rolled product.

[0088] 4A provides a plot of grain size distribution across the depth of an aluminum alloy product 100. Similar to graphs 200A and 300A above, graph 400A is provided for illustrative purposes to illustrate an example distribution of relative grain sizes as a function of depth.

[0089] Graph 400A includes an x-axis that corresponds to the depth of the rolled product. The x-axis may be the same as the x-axis of graphs 200A, 200B, 300A, and 300B. The x-axis may correspond to the depth of the rolled product, starting from a starting point of 0 nm. The starting point of 0 nm may correspond to the surface of the rolled product. The starting point may also correspond to the surface of the rolled near surface microstructure 110. The x-axis may extend to a depth of 2400 nm. Similar to the discussion of depth in graph 200A, the depth may correspond to the space occupied by the rolled composition. In an embodiment, the depth may correspond to the thickness of the rolled product. For example, as shown in graph 400A, the depth of 2400 nm may correspond to the depth of the bulk 120. However, in other embodiments, the depth may be greater than 2400 nm or less than 2400 nm.

[0090] Graph 400A also includes a y-axis. The y-axis corresponds to the grain size of the exemplary aluminum alloy product 100 throughout the depth of the rolled product. The grain size may correspond to the crystallization size of the underlying constituents of the aluminum alloy when the rolled product is created. The grain size distribution line 410A corresponds to the grain size throughout the depth of the rolled product. As shown in graph 400A, the grain size near the surface of the rolled product may be larger than the grain size closer to the bulk 120. The grain size may be largest near the surface in the near-rolled surface microstructure 110 and then decrease toward the bulk 120 where the grain size is a constant grain size. In an embodiment, the grain size may reach a constant size near about 600 nm. The point where the grain size reaches a constant size may correspond to the boundary 115 between the near-rolled surface microstructure 110 and the bulk 120. In some cases, the grain size in the bulk 120 may be larger and range from 5 μm to 50 μm. In various embodiments, the grain size can be ultra-fine at a particular depth, such as in the bulk 120. For example, the grain size can be 10 nm to 5 μm in the bulk 120. In some embodiments, a fine grain layer below the oxide layer can be formed having an ultra-fine grain. In other embodiments, the grain size can be small in the near-rolled surface microstructure 110 but larger closer to the bulk 120.

[0091] The one or more defects 130 present within the near-rolled surface microstructure 110 may also affect the chemical performance of the aluminum alloy product 100. Specifically, the high density population 130e of alloying elements 140 may increase the corrosion sensitivity of the aluminum alloy product 100. As noted above, the high density population 130e may increase the corrosion tendency of the aluminum alloy product 100, in part, because the alloying elements 140 that make up the high density population 130e may diffuse faster than adjacent elements or compounds, or because the alloying elements 140 may be more reactive than adjacent elements or compounds. In turn, the high density population 130e may create reactive pockets within the near-rolled surface microstructure 110, which may lead to favorable corrosion propagation conditions.

[0092] 4B provides a plot of grain size distribution across the depth of the aluminum alloy product 100. Similar to graphs 200A, 200B, 300A, 300B, and 400A above, graph 400B is provided for illustrative purposes to illustrate an example distribution of relative grain size as a function of depth of a micro-grain subsurface structure.

[0093] Graph 400B includes an x-axis corresponding to the depth of the rolled product. The x-axis may be the same as the x-axis of graph 400A. The x-axis may correspond to the depth of the rolled product, starting from a starting point of 0 nm. The starting point, 0 nm, may correspond to the surface of the rolled product. The starting point may also correspond to the surface of the microparticle subsurface structure. The x-axis may extend to a depth of 2400 nm. Similar to the depths of graphs 200B and 300B, the depths may correspond to the space occupied by the second configuration. In an embodiment, the depths may correspond to the thickness of the rolled product. For example, as shown in graph 400B, the depth of 2400 nm may correspond to the depth of the bulk 120. However, in other embodiments, the depths may be greater than 2400 nm or less than 2400 nm.

[0094] Graph 400B also includes a y-axis. Similar to graph 400A, the y-axis may correspond to the grain size of the aluminum alloy product 100 throughout the depth of the rolled product. The grain size may correspond to the crystallization size of the underlying constituents of the aluminum alloy when the rolled product is created. The grain size distribution line 410B corresponds to the grain size throughout the depth of the rolled product. As shown in graph 400B, the grain size near the surface of the rolled product may be substantially the same or similar to the grain size closer to the bulk 120. In an embodiment, the grain size may be a fine grain size throughout the micro-grain subsurface structure and the bulk 120. In some cases, the grain size may be ultra-fine throughout the depth. For example, the grain size may be 10 nm to 5 μm throughout the surface and bulk 120 of the rolled product. In other embodiments, the grain size may be a larger grain size throughout the micro-grain subsurface structure and the bulk 120, such as larger than the grain size of the rolled near surface microstructure 110.

[0095] The above-mentioned one or more defects 130 and different grain sizes in the near-rolled surface microstructure 110 may affect the mechanical performance of the aluminum alloy product 100. For example, the presence of entrained material 130c or other defects in the near-rolled surface microstructure 110 may cause the near-rolled surface microstructure 110 to have a different ductility than the bulk 120. The different ductility between the near-rolled surface microstructure 110 and the bulk 120 may result in mechanical failure as the near-rolled surface microstructure 110 may deform less than the bulk 120.

[0096] In an embodiment, mechanically altering the near-surface microstructure may include modifying the near-surface microstructure to produce a first surface region and a second surface region. The first surface region may be or include a near-surface microstructure (NSM) having a thickness of less than 500 nm. For example, the near-surface microstructure of the first surface region may have a thickness of 400 nm to 500 nm, 300 nm to 400 nm, 200 nm to 300 nm, 100 nm to 200 nm, 50 nm to 100 nm, 10 nm to 50 nm, or 1 nm to 10 nm. In some cases, the first surface region may be substantially free of near-surface microstructure such that only a trace amount of near-surface microstructure is present.

[0097] The second surface region may be free or substantially free of near-surface microstructures. The second surface region may include an oxide layer. The oxide layer may have a thickness of up to 1 nm to 20 nm. For example, the oxide layer may range from 1 nm to 15 nm, 1 nm to 10 nm, 1 nm to 5 nm, or 1 nm to 2 nm. In some cases, the second surface region may be free or substantially free of an oxide layer. A microparticle subsurface structure may be present between the oxide layer and the bulk. The microparticle subsurface structure may have a thickness of 1 nm to 2 μm. For example, the microparticle subsurface structure may have a thickness of 1 nm to 1 μm, 10 nm to 800 nm, 50 nm to 800 nm, 100 nm to 800 nm, 100 nm to 500 nm, or 100 nm to 400 nm.

[0098] In some embodiments, both the first surface region and the second surface region may be present after mechanical modification of the near-rolled surface microstructure. The first surface region and the second surface region may be present in a ratio of 50% or less of the first surface region to the second surface region. For example, the ratio of the area of ​​the first surface region to the area of ​​the second surface region may be 40% or less, 30% or less, 20% or less, 15% or less, 10% or less, 5% or less, or 1% or less. In some cases, the first surface region may not be present after mechanical modification of the near-rolled surface microstructure. In some embodiments, the first surface region and the second surface region may be discontinuous. For example, the second surface region may form "islands" or pockets within the first surface region.

[0099] In various embodiments, mechanically modifying the rolled near surface microstructure can include creating a new layer of modified near surface microstructure, referred to herein as micro-grain subsurface structure. For example, mechanically modifying the rolled near surface microstructure can produce a first surface region with a micro-grained surface structure. The new layer of micro-grained subsurface structure can include material from the rolled near surface microstructure and / or material from the bulk, and in some cases can optionally include material provided during the mechanical modification process. As shown in Figures 5A, 5B, and 5C, mechanically modifying the rolled near surface microstructure 510 can include creating a micro-grained subsurface structure 512. To begin with, in Figure 5A, an aluminum alloy product 500 can include a rolled product including a rolled near surface microstructure 510 and a bulk 520. The rolled near surface microstructure 510 can have a rolled composition including one or more defects 530. The one or more defects 530 can be the same as or different from the one or more defects 130 as discussed herein. Similarly, the near-rolled surface microstructure 510 and the bulk 520 can be the same as or different from the near-rolled surface microstructure 110 and the bulk 120, respectively.

[0100] The composition of the near-rolled surface microstructure 510 may include one or more defects 530, which may be the same or different from the one or more defects 130. The one or more defects 530 may include surface cracks 530d, internal cracks 530a, voids 530b, entrained material 530c, and / or dense populations 530e of alloying elements 540. Thus, the one or more defects 530 may include a non-uniform distribution of alloying elements 540 within the near-rolled surface microstructure 510, as well as a non-uniform distribution of grain size and structure. In contrast to the near-rolled surface microstructure 510, the bulk 520 may have a first composition with minimal or no defects. The first composition may include a uniform distribution of alloying elements 540, as shown, and may include a uniform distribution of grain size and structure. 5A, 5B, and 5C show a uniform distribution of alloying elements 540 as an array within bulk 520, it will be understood that the illustrated configurations are intended to show a homogenous distribution, rather than arranging alloying elements 540 as an array. In embodiments, alloying elements 540 may not be arrayed within bulk 520, but may instead be a natural but homogenous distribution.

[0101] In FIG. 5B, the near-rolled surface microstructure 510 may be mechanically altered, such as by ablation. Ablating the near-rolled surface microstructure 510 may include physically ablating the surface with grit 555. The grit 555 may be propelled toward the surface of the rolled product by an ablating device 550. As described below with respect to FIG. 7B, the ablating device 550 may be configured to blast the grit 555 at the near-rolled surface microstructure 510. The configuration (e.g., force, angle, exposure time) of the ablating device 550 may depend on the depth of alteration desired. In an embodiment, the ablating device 550 may include a sandblasting device configured to blast the grit 555. In such an embodiment, the grit 555 may include sand, glass, or other silicate-based grit. The size and composition of the grit 555 may depend on the application of the aluminum alloy product 500 and / or the degree of mechanical alteration to the near-rolled surface microstructure 510 desired.

[0102] In some embodiments, a top layer 512a may be produced on the microparticle subsurface structure 512. The top layer 512a may optionally be or include an oxide layer. Such an oxide layer may be an engineered oxide layer that may have a specific thickness, composition, and structure that may enable a strong bond with an adhesive, such as an epoxy adhesive.

[0103] In some embodiments, the top layer 512a may be or include a silicon-containing layer. The silicon-containing layer may modify some of the bonding sites on or within the near-rolled surface microstructure 510. As described above, the near-rolled surface microstructure 510 may include one or more defects 530, such as transmission cracks, voids, or fissures. By depositing a silicon-containing layer on the near-rolled surface microstructure 510, one or more of the defects 530 in the rolled composition of the near-rolled surface microstructure 510 may be addressed to form a second composition having fewer defects 530 than the rolled composition of the near-rolled surface microstructure 510.

[0104] To deposit a silicon-containing layer on the near-rolled surface microstructure 510, a silicon-containing material, such as grit 555 embodied as silicon-containing grit, may be used. In an embodiment, depositing a silicon-containing layer on the near-rolled surface microstructure 510 or a portion of the near-rolled surface microstructure 510 may include grit blasting the near-rolled surface microstructure 510 with silicon-containing grit. For example, the silicon-containing grit may be coated or machined with a silicon-containing material and configured to transfer the silicon-containing material to a surface, such as the surface of the near-rolled surface microstructure 510, upon impingement. That is, when the grit 555 impacts the near-rolled surface microstructure 510, the thermal, mechanical, and kinetic energy of the impact may cause or induce the silicon-containing material coating the grit 555 to migrate to the near-rolled surface microstructure 510. For example, when the grit 555 impacts the surface, a localized thermal transient occurs, depositing the silicon-containing material on the surface. The energy generated from the individual impact of each grit 555 particle may disrupt the native oxide of the aluminum, thereby allowing the silicon-containing material to contact and bond with both the oxide and the metal present at the surface. During the mechanical modification process or processing of the aluminum alloy product, a complex amorphous silicon-containing film may form on the surface of the rolled product, creating a silicon-containing layer as part of the micro-in, micro-on, or micro-grain subsurface structure 512. In an embodiment, the silicon-containing material may be ionized to have a positive or negative charge. In such an embodiment, the ionized state of the silicon-containing material may give the silicon-containing material an affinity for the rolled surface near microstructure 510. Thus, when the grit 555 collides with the rolled surface near microstructure 510, the grit 555 may transfer silicon to the rolled surface near microstructure 510, in part due to the ionic charge of the silicon-containing material.

[0105] As described above, the grit 555 may be processed or coated with a silicon-containing compound, including a silicon-containing material for transferring to the near-rolled surface microstructure 510. For example, the grit 555 may be a silicon oxide (e.g., a SiO 2 , SiO 3 , SiO 4 , etc.)x ), silane, hexamethyldisiloxane (HMDSO), tetramethylsilane (TMS), tetraethoxysilane (TEOS), triethoxysilane, N-sec-butyl(trimethylsilyl)amine, 1,3-diethyl-1,1,3,3,tetramethyldisilazane, methylsilane, pentamethyldisilane, tetraethylsilane, tetramethyldisilane, or other suitable organosilicon compounds. In embodiments, the silicon-containing grit 555 may also include additional materials such as adhesion promoters, corrosion inhibitors, aesthetic dopants, coupling agents, antimicrobial agents, etc., or any combination thereof. An exemplary grit 555 may include or comprise SACO grit.

[0106] The silicon-containing material can modify some of the bond sites in the near-rolled surface microstructure 510. The near-rolled surface microstructure 510 can have bond sites that do not readily bond or do not accept bonding. For example, one or more defects 530 can reduce or block the bond sites or the bond sites can be occupied by undesired material. To improve the bond sites, the silicon-containing material can open up the bond sites and make them available for bonding. For example, the silicon-containing material can impart a desired ionic charge or change the electrochemical or mechanical structure of the bond sites to improve and promote bonding at the bond sites. In an embodiment, the impingement of the grit 555 can improve the bond sites. For example, the impact of the grit 555 can compact the near-rolled surface microstructure 510 or remove undesired material that occupies some of the bond sites.

[0107] FIG. 5C illustrates a top layer 512a that may be deposited on the near-rolled surface microstructure 510 by the silicon-containing grit 555 described above. The top layer 512a may develop on the surface of the near-rolled surface microstructure 510 during the generation of the micro-grain subsurface structure 512. In an embodiment, the deposition or generation of the top layer 512a on the near-rolled surface microstructure 510 may occur simultaneously with or otherwise be associated with the generation of the micro-grain subsurface structure 512, such as when the material silicon inclusions migrate to the surface in the case of silicon-containing grit. For example, silicon within the silicon-containing material may alter or modify the near-rolled surface microstructure 510 to form the micro-grain subsurface structure 512. Altering or modifying the near-rolled surface microstructure 510 may include integrating the near-rolled surface microstructure 510 to address one or more defects 530 and / or to modify bonding sites, as described above. In embodiments, the top layer 512a may have a different composition than the second composition of the micro-particle subsurface structures 512. For example, the second composition may be closer to the first composition and include primarily an aluminum alloy with a uniform distribution of one or more alloying elements 540. In contrast, the top layer 512a may include primarily silicon, such as when using silicon-containing grits, including silanes, silicates, silicon oxides, and other silicon-based materials that adhere to oxides and / or aluminum at or near the surface. In other embodiments, the top layer 512a may have a similar composition to the second composition of the micro-particle subsurface structures 512 and may optionally include an oxide layer.

[0108] Mechanically altering the near-rolled surface microstructure to have or produce a micrograin subsurface structure is useful for improving the overall mechanical and chemical performance of an aluminum alloy product. In part, the improved mechanical and chemical performance of an aluminum alloy product may result from the removal or modification of one or more defects. Figures 6A, 6B, and 6C provide schematics of mechanically altering a near-rolled surface microstructure 610 to produce a micrograin subsurface structure 612, according to some embodiments.

[0109] 6A provides a schematic diagram of an aluminum alloy product 600. The aluminum alloy product 600 may be the same as or different from the aluminum alloy products 100 or 500. The aluminum alloy product 600 may comprise a rolled product including a bulk 620 and a near-rolled surface microstructure 610. The near-rolled surface microstructure 610 and the bulk 620 may be the same as or different from the near-rolled surface microstructure 110 or 510 and the bulk 120 or 520, respectively. There may optionally be a boundary 615 between the near-rolled surface microstructure 610 and the bulk 620. In an embodiment, the boundary 615 may be the same as or different from the boundary 115 or 515.

[0110] As shown in FIG. 6A, the near-rolled surface microstructure 610 may have a rolled composition having one or more defects 630. The one or more defects 630 may be the same as or different from the one or more defects 130 or 530. In an embodiment, the one or more defects 630 may include internal cracks 630a, surface cracks 630d, voids 630b, entrained material 630c, and / or dense populations 630e of alloying elements 640. The internal cracks 630a may correspond to cracks generated within the near-rolled surface microstructure 610, and the surface cracks 630d may correspond to cracks generated at the surface of the near-rolled surface microstructure 610. In an embodiment, the entrained material 630c may correspond to entrained lubricant or oxides incorporated into the near-rolled surface microstructure 610 during the rolling process.

[0111] As discussed with respect to aluminum alloy products 100 and 500, a dense population 630e of alloying elements 640 may be present in the near-rolled surface microstructure 610. Within the bulk 620, the alloying elements 640 may be uniformly distributed, meaning that in any given volume of the bulk 620, the alloying elements 640 may be present in the same or nearly the same concentration. In FIG. 6A, the uniform distribution of the alloying elements 640 within the bulk 620 may be depicted as an array of the alloying elements 640. In various embodiments, the alloying elements 640 may not exist in such an array, but rather may be randomly distributed throughout the bulk 620 according to the natural alloying tendencies of the alloying elements 640.

[0112] In contrast, the alloying elements 640 may not be uniformly distributed within the near-rolled surface microstructure 610. As shown in Figure 6A, the alloying elements 640 may be non-uniformly distributed within the near-rolled surface microstructure 610, creating pockets of low density populations of alloying elements 640 and pockets of high density populations 630e of alloying elements 640.

[0113] To alter the rolled composition of the near-rolled surface microstructure 610 to a more desirable composition, the near-rolled surface microstructure 610 may be mechanically altered during processing of the aluminum alloy product 600. For example, the near-rolled surface microstructure 610 may be mechanically altered at any stage before the aluminum alloy product 600 undergoes any prior processing processes. In various embodiments, the near-rolled surface microstructure 610 may be mechanically altered after a hot rolling process has been performed or after a cold rolling process has been performed. In other embodiments, the near-rolled surface microstructure 610 may be mechanically altered during a final gauging process of the aluminum alloy product 600.

[0114] The aluminum alloy product 600 may be processed according to one or more methods disclosed herein. For example, a method of processing an aluminum alloy product may include providing a rolled product having a bulk and near-rolled surface microstructure, the near-rolled surface microstructure having a rolled composition including one or more defects. For example, the one or more defects may include at least one of entrapped oxides, entrapped oil, transmitted cracks, voids, fissures, non-uniform bond sites, or alloying element non-uniformities. The method may also include mechanically modifying the near-rolled surface microstructure to produce a micrograin subsurface structure having a second composition different from the rolled composition. In some cases, the near-rolled surface microstructure may occupy spaces deep into the bulk. In other embodiments, the second composition may include fewer defects than the rolled composition, but more defects than the first composition of the bulk. For example, the second composition may be substantially the same as the first composition of the bulk, or the second composition may be substantially free of one or more defects. Additionally, the second composition may include uniformity in grain structure and uniformity in distribution of alloying elements.

[0115] According to certain embodiments of the present disclosure, a method of processing an aluminum alloy product, such as aluminum alloy product 600, may include grinding the near-rolled surface microstructure, laser ablating the near-rolled surface microstructure, sandblasting the near-rolled surface microstructure, and / or polishing the near-rolled surface microstructure. In some embodiments, mechanically modifying the near-rolled surface microstructure may include physically ablating the near-rolled surface microstructure. In some cases, physically ablating the near-rolled surface microstructure may include grit blasting the near-rolled surface microstructure. In yet other embodiments, mechanically modifying the near-rolled surface microstructure may include compressing the near-rolled surface microstructure to a controlled depth. For example, compressing the near-rolled surface microstructure may include shot peening the near-surface microstructure to a controlled depth. Mechanically modifying the second composition may also include producing a homogenous ultrafine grain.

[0116] The method of mechanically modifying the near-rolled surface microstructure may also include subjecting the near-rolled surface microstructure to a first modification process and then subjecting the near-rolled surface microstructure to a second modification process. In certain embodiments, the mechanical modification may further include subjecting the near-rolled surface microstructure to a third modification process. In some examples, the first modification process may include exposing the near-rolled surface microstructure to a first grit, the second modification process may include exposing the near-rolled surface microstructure to a second grit, and the third modification process may include exposing the near-surface microstructure to a third grit. In some examples, the first grit is coarser than the second grit, and the second grit is coarser than the third grit.

[0117] The method of processing an aluminum alloy product disclosed herein may include mechanically modifying the near-rolled surface microstructure during final gauging of the rolled product. However, in other embodiments, mechanically modifying the near-rolled surface microstructure may occur after the hot rolling process and / or before the cold rolling process. In some embodiments, mechanically modifying the near-rolled surface microstructure may occur before pre-working the rolled product. The method may further include pre-working the rolled product. For example, the method may include pre-working the rolled product by etching the rolled product.

[0118] The rolled products mechanically modified via the methods disclosed herein may include at least one of a 7xxx series aluminum alloy product, a 6xxx series aluminum alloy product, or a 5xxx series aluminum alloy product. In various embodiments, the rolled product may be a hot rolled product or a cold rolled product.

[0119] The aluminum alloy products according to the methods and techniques disclosed herein may include a rolled product having a bulk and a micrograin subsurface structure, where the rolled product has a near-rolled surface microstructure having a rolled composition including one or more defects that are first modified to mechanically alter the near-rolled surface microstructure to produce a micrograin subsurface structure having a second composition different from the rolled composition. For example, the one or more defects may include at least one of entrapped oxides, entrapped oil, transmitted cracks, voids, fissures, non-uniform bond sites, or non-uniformity of alloying elements. It may be that the near-rolled surface microstructure occupies space to the depth of the bulk. In various embodiments, the second composition may include fewer defects than the rolled composition, but more defects than the bulk first composition. For example, the second composition may be substantially the same as the bulk first composition, or the second composition may be substantially free of one or more defects. The second composition may include uniformity of grain structure and uniformity of distribution of alloying elements. For example, the second composition may include homogeneous nanoparticles.

[0120] In various embodiments, the rolled product may include at least one of a 7xxx series aluminum alloy product, a 6xxx series aluminum alloy product, and a 5xxx series aluminum alloy product. The rolled product may be a hot rolled product or a cold rolled product. In certain cases, the aluminum alloy product may be produced according to any of the methods disclosed herein.

[0121] As shown in FIG. 6B, the near-rolled surface microstructure 610 of the aluminum alloy product 600 may be mechanically modified using a variety of modification processes and devices. In various embodiments, mechanically modifying the near-rolled surface microstructure 610 may include grinding, physical ablation, laser ablation, compression, sand blasting, polishing, dry ice blasting, and / or electrolytic polishing of the near-rolled surface microstructure 610. As shown in FIG. 6B, one or more grinding elements 650 may be used to mechanically modify the near-rolled surface microstructure 610. The grinding elements 650 may extend the entire width of the aluminum alloy product 600. In an embodiment, the grinding elements 650 may extend only a portion of the width of the aluminum alloy product 600.

[0122] As shown in FIG. 6B, the composition of the near-rolled surface microstructure 610 can be modified by the grinding element 650. For example, the near-rolled surface microstructure 610 can be modified to remove internal cracks 630a as well as some of the entrained material 630c and voids 630b. Mechanical modification of the near-rolled surface microstructure 610 can be accomplished by using the grinding element 650. The grinding element 650 can include one or more abrasive surfaces. For example, the outer periphery of the grinding element 650 can include an abrasive surface. Exemplary abrasive surfaces can include, but are not limited to, silicate-based surfaces, metal surfaces, diamond or hard crystallized surfaces, stone surfaces, or ceramic surfaces. The type of abrasive surface selected can depend on the rolled composition, particularly the amount and type of one or more defects 630 present in the near-rolled surface microstructure 610, and the application of the aluminum alloy product 600. For example, a stone or ceramic surface may be selected as the abrasive surface of the grinding element 650 because one or more defects 630 may include a high density of voids 630b. By using stone or ceramic as the abrasive surface, the near-rolled surface microstructure 610 may be crushed and compressed during mechanical alteration. It may be desirable for the near-rolled surface microstructure to compress the near-rolled surface microstructure 610, which includes a high density of voids 630b, because compression may be the optimal means of removing the voids 630b.

[0123] The abrasive surface may be rotated or ground against the near-rolled surface microstructure 610 to remove material and / or redistribute the rolled composition. In various embodiments, the abrasive surface may be on a flat surface or a surface parallel to the surface of the aluminum alloy product 600. Instead of rotating to grind the surface, the abrasive surface may be agitated back and forth to achieve the desired friction between the abrasive surface and the near-rolled surface microstructure 610. The amount of friction applied during grinding of the surface may be proportional to the amount of near-rolled surface microstructure 610 that is altered. For example, higher friction applied to the surface may correspond to a higher rate of change to the near-rolled surface microstructure 610. A variety of different grit sizes of the abrasive surface on the grinding element 650 may be used to grind the surface, with the grit size optionally decreasing with successive grinds applied by the grinding element 650. A larger grit size may be desirable initially to achieve a more robust grinding or rubbing effect, and in subsequent grinds, smaller grit sizes may be desirable to cause less and less surface alteration and produce the desired micro-particle subsurface structure 612.

[0124] As described above, the near-rolled surface microstructure 610 can occupy a space from the surface of the rolled product to a depth in the bulk 620. For example, the depth can be greater than 500 nm. However, in other embodiments, the depth can be less than 500 nm. The depth can range from 200 nm to 400 nm, 300 nm to 500 nm, 400 nm to 600 nm, 200 nm to 600 nm, 500 nm to 700 nm, 500 nm to 800 nm, or 200 nm to 800 nm, 800 nm to 1 μm, 1 μm to 5 μm, 5 μm to 10 μm, 10 μm to 15 μm, or 15 μm to 20 μm. During mechanical modification, a portion of the depth of the near-rolled surface microstructure 610 can be modified. In an embodiment, a portion of the depth can be mechanically modified. For example, if the near-surface microstructure 610 has a depth of 10 μm, the mechanically altered depth portion may be the first 5 μm of the rolled near-surface microstructure 610. The mechanically altered depth portion may range from 50 nm to 100 nm, 100 nm to 200, 200 nm to 400 nm, 300 nm to 500 nm, 400 nm to 600 nm, 200 nm to 600 nm, 500 nm to 700 nm, 500 nm to 800 nm, 200 nm to 800 nm, 800 nm to 1 μm, 1 μm to 5 μm, 5 μm to 10 μm, 10 μm to 15 μm, 15 μm to 20 μm, depending on the total depth. In some embodiments, the total depth corresponding to the rolled near-surface microstructure 610 may be altered.

[0125] The micrograin subsurface structure 612 can be achieved by mechanically modifying the rolled near surface microstructure 610 as described above. As shown in FIG. 6C, the second composition of the micrograin subsurface structure may be free or substantially free of one or more defects 630. A micrograin subsurface structure substantially free of one or more defects 630 may mean that the micrograin subsurface structure 612 functions similarly to a micrograin subsurface structure 612 that does not include one or more defects 630. That is, substantially free of one or more defects 630 may mean that some defects 630 are present in the micrograin subsurface structure 612, but the defects 630 that are present do not appreciably affect the mechanical or chemical performance of the aluminum alloy product 602. The second composition may be different from the rolled composition. In various embodiments, the second composition may be between the rolled composition and the first composition. In an exemplary embodiment, the second composition may be the same or substantially the same as the first composition.

[0126] As shown in FIG. 6C, the second composition of the near-surface microstructure 612 may include a redistribution of alloying elements 640. The redistribution of alloying elements 640 may mean that the dense population 630e of alloying elements 640 has been redistributed or altered to achieve a homogenous or relatively more homogenous distribution of alloying elements 640. The redistribution of alloying elements 640 within the micrograin subsurface structure 612 may be similar to the distribution of alloying elements 640 within the bulk 620, as shown in FIG. 6C, although in various embodiments, the redistribution of alloying elements 640 within the micrograin subsurface structure 612 may be distributed differently than the distribution within the bulk 620. For example, in embodiments, alloying elements 640 may be found in a higher concentration within the bulk 620 than within the micrograin subsurface structure 612. However, regardless of the concentration or prominence of alloying elements 640 within the bulk 620 or the micrograin subsurface structure 612, the distribution of alloying elements 640 may be uniform within both. That is, the alloying elements 640 may be uniformly distributed within any given volume of the rolled product.

[0127] The second composition of the micro-grain subsurface structure 612 may also comprise a homogenous grain structure. By uniformity of grain structure, for example, the crystallite size throughout the micro-grain subsurface structure 612 may be the same or within a standard deviation of the bulk 620. In various embodiments, uniformity of grain structure may correspond to the uniformity of the grain structure of the micro-grain subsurface structure 612 being the same as the uniformity of the grain structure of the bulk 620. For example, after the rolling near-surface microstructure 610 is mechanically altered to produce the micro-grain subsurface structure, the grain structure of the micro-grain subsurface structure 612 may comprise an ultra-fine grain structure that matches (or is similar to) that of the ultra-fine grain structure in the first composition. However, in other embodiments, an ultra-fine grain structure may be created in the micro-grain subsurface structure 612, but the bulk 620 may comprise a larger homogenous grain structure. In some cases, the grain structure of the micro-grain subsurface structure 612 may include aluminum alloy grains having an average diameter of 10 nm to 500 nm. Although not shown in FIG. 6C, the microparticle subsurface structure 612 may include or have a top layer thereon, such as an oxide layer.

[0128] 7A, 7B, and 7C provide schematics of mechanically altering the near-rolled surface microstructure to achieve a micrograin subsurface structure 712, according to another embodiment. To begin with, in FIG. 7A, an aluminum alloy product 700 may include a rolled product having a bulk 720 and a near-rolled surface microstructure 710. The bulk 720 may be the same as or different from the bulk 120, the bulk 520, or the bulk 620, and the near-rolled surface microstructure 710 may be the same as or different from the near-rolled surface microstructure 110, the near-surface microstructure 510, or the near-rolled surface microstructure 610. In an embodiment, the aluminum alloy product 700 may be the same as or different from the aluminum alloy product 100, the aluminum alloy product 500, or the aluminum alloy product 600.

[0129] The rolled surface near microstructure 700 may have one or more defects 730. The one or more defects 730 may be the same as or different from the one or more defects 130, 530, or the one or more defects 630, as described herein. In an embodiment, the one or more defects 730 may include internal cracks 730a, surface cracks 730d, voids 730b, entrained material 730c, and / or dense populations 730e of alloying elements 740. As shown, the distribution of alloying elements 740 within the rolled surface near microstructure 710 may be non-uniform, resulting in pockets of dense populations 730e and pockets of minimal alloying elements 740. Similar to the first compositions discussed with respect to bulk 120, bulk 520, or bulk 620, the first composition of bulk 720 may provide a uniform distribution of alloying elements 740. Between the first composition of the bulk 720 and the rolled composition of the near-rolled surface microstructure 710 may be an optional boundary 715. The boundary 715 may be the same as or different from boundary 115, boundary 515, or boundary 615.

[0130] In FIG. 7B, the near-rolled surface microstructure 710 may be mechanically altered. Mechanically altering the near-rolled surface microstructure 710 may include ablating the near-rolled surface microstructure 710. Ablating the near-rolled surface microstructure 710 may include physically ablating, laser ablating, and / or compressing the near-rolled surface microstructure. Physical ablation may include sand or grit blasting the near-rolled surface microstructure 710. Laser ablation may include irradiating the near-rolled surface microstructure 710 with a laser beam or another high intensity beam to alter the surface. Compressing the near-rolled surface microstructure 710 may include shot peening the surface. Shot peening may include modifying the mechanical properties of the near-rolled surface microstructure 710 by impacting the surface with shot to achieve plastic deformation. Exemplary shots may include circular metal, glass, silicate, or ceramic particles.

[0131] Mechanically altering the near-rolled surface microstructure 710 may include one or more ablation devices 750. The one or more ablation devices 750 may include components for ablating the near-rolled surface microstructure 710. In an exemplary embodiment, physically ablating the near-rolled surface microstructure 710 may include sandblasting the surface. In such an embodiment, the ablation device 750 may be a grit blasting device. The ablation device 750 may be configured to blast grit 755 at the near-rolled surface microstructure 710. In an embodiment in which the ablation device 750 may be a sand blasting device, the grit 755 may include sand, glass, or other silicate-based grit. The size and composition of the grit 755 may depend on the application of the aluminum alloy product 700 and / or the degree of mechanical alteration desired in the near-rolled surface microstructure 710. In some embodiments, it may be desirable to ablate the surface using grit blasting with grits of various sizes, such as applying multiple successive grit blasts of different grit sizes. For example, a larger grit size may be desirable initially to achieve a more robust modification effect, and in subsequent grit blasts, smaller grit sizes may be desirable to cause less and less surface alteration and produce the desired micro-grain subsurface structure 712.

[0132] In an exemplary embodiment where mechanically modifying the near-rolled surface microstructure 710 includes shot peening the surface, the ablation apparatus 750 may include a peening device. Exemplary shot peening methods may include physical shot peening, ultrasonic peening, wet peening, and laser peening. In the case of physical shot peening, the ablation apparatus 750 may include a peening apparatus configured to propel a shot at the near-rolled surface microstructure 710 with sufficient force to achieve a mechanical change. In an embodiment, the mechanical change may include compressing the near-rolled surface microstructure 710 to create a plastic deformation in the outermost layer of the rolled product. In applications where less material removal is desired, shot peening may be preferred over abrasive mechanical modification. Because shot peening compresses the near-rolled surface microstructure 710 instead of removing particles and material from the near-rolled surface microstructure 710, shot peening may be a preferred means of mechanically modifying the near-rolled surface microstructure 710 in certain applications.

[0133] The microparticle subsurface structure 712 can be generated by mechanically modifying the rolled near surface microstructure 710 as described above. The newly generated microparticle subsurface structure 712 can be a thin surface layer. In an embodiment, the microparticle subsurface structure 712 can be 1 nm to 2 μm thick. For example, the microparticle subsurface structure 712 can be 25 nm to 50 nm thick, 50 nm to 100 nm thick, 50 nm to 200 thick, 50 nm to 300 nm thick, 50 nm to 400 nm thick, 50 nm to 500 nm thick, 50 nm to 100 nm thick, 100 nm to 200 nm thick, 100 nm to 400 nm thick, 100 nm to 500 nm, 500 nm to 1 μm, 800 nm to 2 μm, or 1 μm to 2 μm thick.

[0134] The micro-grain subsurface structure 712 may include a second composition that is free or substantially free of one or more defects 730. As described above, the substantial absence of one or more defects 730 allows the micro-grain subsurface structure 712 to function as if the second composition were free of the one or more defects. In an embodiment, if the micro-grain subsurface structure 712 is substantially free of one or more defects 730, any defects 730 that are present may not affect the mechanical or chemical performance of the aluminum alloy product 700. The second composition of the micro-grain subsurface structure 712 may be different from the as-rolled composition of the rolled near-surface microstructure 710. In various embodiments, the second composition may be between the as-rolled composition and the first composition of the bulk 720. In an exemplary embodiment, the second composition may be the same or substantially the same as the first composition.

[0135] Similar to the micro-grain subsurface structures 512 and 612 discussed above, the second composition of the micro-grain subsurface structure 712 can include a uniform distribution of alloying elements 740. Exemplary alloying elements 740 can include zinc, manganese, magnesium, copper, chromium, silicon, and / or iron. As shown in FIG. 7C, the alloying elements 740 can be redistributed within the micro-grain subsurface structure 712 to achieve a homogenous distribution. As described above, the redistribution of the alloying elements 740 within the micro-grain subsurface structure 712 can be similar to the uniform distribution within the bulk 720. However, in other embodiments, the redistribution of the alloying elements 740 can differ from the uniform distribution within the bulk 720. As shown in FIG. 7C, the redistribution of the alloying elements 740 within the micro-grain subsurface structure 712 can provide a uniform distribution, but the distribution can differ from the uniform distribution within the bulk 720. Although not shown in FIG. 7C, the micro-grain subsurface structure 712 can include or have a top layer thereon, such as an oxide layer.

[0136] In an exemplary embodiment, the mechanical modification of the near-rolled surface microstructure may include a multi-modification process. The multi-modification process may be a preferential means for mechanically altering the near-rolled surface microstructure. During the mechanical modification of the near-rolled surface microstructure, a disturbed layer may be generated. The disturbed layer may be a layer generated near the surface of the near-rolled surface microstructure that is deformed by the mechanical modification process. To minimize the possibility of generating a disturbed layer, a multi-modification process may be used. As shown in Figures 8A, 8B, 8C, 8D, and 8E, the multi-modification process may optionally include three modification processes. In some embodiments, only two modification processes may be used, while in other embodiments, more than three modification processes may be used.

[0137] As shown in FIG. 8A, the aluminum alloy product 800 may include a rolled product including a near-rolled surface microstructure 810 and a bulk 820. The near-rolled surface microstructure 810 and the bulk 820 may be the same as or different from the near-rolled surface microstructure 110, 510, 610, or 710, and the bulk 120, 520, 620, or 720, respectively. The near-rolled surface microstructure 810 may have a rolled composition including one or more defects 830a-e (collectively defects 830). The one or more defects 830 may include some or all of the defects described with respect to the one or more defects 130, 530, 630, and 730. For example, as shown in FIG. 8A, the one or more defects 830 may include an internal crack 830a, a void 830b, entrained material 830c, a surface crack 830d, and / or a dense population 830e of alloying elements 840. As with the other embodiments discussed, the one or more defects 830 may include a non-uniform distribution of alloying elements 840, as well as a non-uniform distribution of grain size and structure. The one or more defects 830 may not be present within the first composition of the bulk 820.

[0138] To achieve the desired second composition, the near-rolled surface microstructure 810 may be mechanically altered. As first shown in FIG. 8B, the near-rolled surface microstructure 810 may be subjected to a first alteration process. The first alteration process may include altering the near-rolled surface microstructure 810 by a first means of alteration. In various embodiments, the first alteration process may include grinding, physical ablation, laser ablation, compression, sand blasting, polishing, dry ice blasting, and / or electropolishing of the near-rolled surface microstructure 810. For illustrative purposes, the alteration process shown in FIGS. 8B, 8C, and 8D may include physically ablating the near-rolled surface microstructure 810. Specifically, the depicted alteration process may include grit blasting the near-rolled surface microstructure 810.

[0139] Each of the first modification process of FIG. 8B, the second modification process of FIG. 8C, and the third modification process of FIG. 8C may include a modification device 850 configured to blast grit 855 at the near-rolled surface microstructure 810. The grit 855 used in each of the three modification processes may be different from each other. For example, the grit 855a used in the first modification process may be larger than the grit 855b used in the second modification process, which may be larger than the grit 855c used in the third modification process. In an embodiment, the grit 855a may be a coarse 320 grit sand, the grit 855b may be a 400 grit sand, and the grit 855c may be a fine 600 grit sand. In various embodiments, the mechanical modification process may include grinding the near-rolled surface microstructure 810. In such an embodiment, a first modified process may use a 320 grit grinding surface, a second modified process may use a 400 grit grinding surface, and a third modified process may use a 600 grit grinding surface.

[0140] By using different grits 855a, 855b, and 855c, the near-rolled surface microstructure 810 can be mechanically altered to achieve the desired second composition. For example, a coarser grit 855a can be used first to alter the surface cracks 830d and voids 830b. However, the coarser grit 855a can create a disordered layer with rough and undesirable characteristics. As part of the disordered layer, a dense population 830e of alloying elements 840 can be present along with a non-uniform grain structure in the near-rolled surface microstructure 810. To achieve a smooth and uniform crystallite structure in the near-rolled surface microstructure 810, the coarse crystallites 855a can be used followed by the crystallites 855b and then the fine crystallites 855c. The grits 855b and 855c can alter the disordered layer to create a smooth and defect-free micro-grain subsurface structure 812. As noted above, the microparticle subsurface structure 812 may be free or substantially free of one or more defects 830. Although not shown in FIG. 8E, the microparticle subsurface structure 812 may include or have thereon a top layer, such as an oxide layer.

[0141] In various embodiments, different types of mechanical modification may be used in each modification process. For example, a first modification process may include shot peening the near-rolled surface microstructure 810. A second modification process may include grinding the near-rolled surface microstructure 810 with an abrasive roller. A third modification process may include sandblasting the near-rolled surface microstructure 810 with fine grit 855. Any combination of the mechanical modifications discussed herein may be used to create the micro-grain subsurface structure 812.

[0142] In an exemplary embodiment, each modification process may optionally use a loading force of 10 pounds of grit 855. Each modification process may optionally last for 2 minutes. In various embodiments, each modification process may last for more than 2 minutes or less than 2 minutes. In various embodiments, each modification process may use a load of more than 10 pounds or less than 10 pounds. The time and load applied during each modification process may depend on the desired microparticle subsurface structure 812.

[0143] In FIG. 8E, a micro-grain subsurface structure 812 may be produced. The micro-grain subsurface structure 812 may have a second composition that is different from the rolled composition. In various embodiments, the second composition may be between the rolled composition and the first composition. In an exemplary embodiment, the second composition may be the same or substantially the same as the first composition. As shown in FIG. 8E, the second composition may include a uniform distribution of alloying elements 840. The distribution of alloying elements 840 within the micro-grain subsurface structure 812 may be different from the distribution within the bulk 820, although both distributions may be uniform. Similarly, the grain size distribution within the micro-grain subsurface structure 812 may be different from the grain size distribution within the bulk 820, although both grain size distributions may be uniform.

[0144] Following mechanical modification, the resulting product can be processed by any suitable means. Processing steps can be used, if desired, for example to prepare a sheet. Such processing steps include, but are not limited to, homogenization, hot rolling, cold rolling, solution heat processing, and an optional pre-aging step. The mechanically modified product can be processed and manufactured into products such as sheets, plates, or other suitable products. Method of using the disclosed metal product

[0145] The metal products described herein can be used in automotive applications, as well as other aircraft and transportation applications, such as railroad applications, or any other desired application. For example, the disclosed metal products can be used to prepare automotive structural components, such as bumpers, side beams, roof beams, cross beams, pillar reinforcements (e.g., A-pillars, B-pillars, and C-pillars), inner panels, outer panels, side panels, inner hoods, outer hoods, or trunk lid panels. The metal products and methods described herein can also be used in aircraft or railroad vehicle applications, for example, to prepare exterior and interior panels.

[0146] The metal products and methods described herein can also be used in electronics applications. For example, the metal products and methods described herein can be used to make housings for electronic devices, including mobile phones and tablet computers. In some examples, the metal products can be used to prepare outer casings for mobile phones (e.g., smartphones), tablet bottom chassis, and housings for other portable electronic devices.

[0147] Non-limiting examples of 1xxx aluminum alloys for use in the products, systems, and methods described herein can include AA1100, AA1100A, AA1200, AA1200A, AA1300, AA1110, AA1120, AA1230, AA1230A, AA1235, AA1435, AA1145, AA1345, AA1445, AA1150, AA1350, AA1350A, AA1450, AA1370, AA1275, AA1185, AA1285, AA1385, AA1188, AA1190, AA1290, AA1193, AA1198, or AA1199.

[0148] Non-limiting examples of 2xxx series aluminum alloys for use in the products, systems, and methods described herein include AA2001, A2002, AA2004, AA2005, AA2006, AA2007, AA2007A, AA2007B, AA2008, AA2009, AA2010, AA2011, AA2011A, AA2111, AA2111A, AA2111B, AA2012, A A2013, AA2014, AA2014A, AA2214, AA2015, AA2016, AA2017, AA2017A, AA2117, AA2018, AA2218, AA2618, AA261 8A, AA2219, AA2319, AA2419, AA2519, AA2021, AA2022, AA2023, AA2024, AA2024A, AA2124, AA2224, AA2224A, AA 2324, AA2424, AA2524, AA2624, AA2724, AA2824, AA2025, AA2026, AA2027, AA2028, AA2028A, AA2028B, AA2028 C, AA2029, AA2030, AA2031, AA2032, AA2034, AA2036, AA2037, AA2038, AA2039, AA2139, AA2040, AA2041, AA20 AA2097, AA2197, AA2297, AA2397, AA2098, AA2198, AA2099, or AA2199.

[0149] Non-limiting examples of 3xxx series aluminum alloys for use in the products, systems, and methods described herein include AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3005A, AA3105, AA3105A, AA31 AA3013, AA3014, AA3015, AA3016, AA3017, AA3019, AA3020, AA3021, AA3025, AA3026, AA3030, AA3130, or AA3065.

[0150] Non-limiting examples of 4xxx series aluminum alloys for use in the products, systems, and methods described herein can include AA4004, AA4104, AA4006, AA4007, AA4008, AA4009, AA4010, AA4013, AA4014, AA4015, AA4015A, AA4115, AA4016, AA4017, AA4018, AA4019, AA4020, AA4021, AA4026, AA4032, AA4043, AA4043A, AA4143, AA4343, AA4643, AA4943, AA4044, AA4045, AA4145, AA4145A, AA4046, AA4047, AA4047A, or AA4147.

[0151] Non-limiting examples of 5xxx series aluminum alloys for use in the products, systems, and methods described herein include AA5182, AA5183, AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA 5019A, AA5119, AA5119A, AA5021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA 5043, AA5049, AA5149, AA5249, AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, A A5251, AA5251A, AA5351, AA5451, AA5052, AA5252, AA5352, AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454 , AA5554, AA5654, AA5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5456, AA5456A, AA5456B, AA5556, AA555 AA5183, AA5283A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187, or AA5088.

[0152] Non-limiting examples of 6xxx series aluminum alloys for use in the products, systems, and methods described herein include AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA601 4, AA6015, AA6016, AA6016A, AA6116, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA60 27, AA6028, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA6 053, AA6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A, A Examples of such compounds include A6261, AA6361, AA6162, AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092.

[0153] Non-limiting examples of 7xxx series aluminum alloys for use in the products, systems, and methods described herein include AA7011, AA7019, AA7020, AA7021, AA7039, AA7072, AA7075, AA7085, AA7108, AA7108A, AA7015, AA7017, AA7018, AA7019A, AA702 4, AA7025, AA7028, AA7030, AA7031, AA7033, AA7035, AA7035A, AA7046, AA7046A, AA7003, AA7004, AA7005, AA7009, AA7010, AA7011, AA7012, AA7014, AA7016, AA7116, AA7122, AA7023, AA7026, AA70 29, AA7129, AA7229, AA7032, AA7033, AA7034, AA7036, AA7136, AA7037, AA7040, AA7140, AA7041, A A7049, AA7049A, AA7149, AA7204, AA7249, AA7349, AA7449, AA7050, AA7050A, AA7150, AA7250, AA7 AA7090, AA7093, AA7095, or AA7099.

[0154] Non-limiting examples of 8xxx series aluminum alloys for use in the products, systems, and methods described herein include AA8005, AA8006, AA8007, AA8008, AA8010, AA8011, AA8011A, AA8111, AA8211, AA8112, AA8014, AA8015, AA8016, AA8017, AA8018, AA801 9, AA8021, AA8021A, AA8021B, AA8022, AA8023, AA8024, AA8025, AA8026, AA8030, AA8130, AA8040, AA8050, AA8150, AA8076, AA8076A, AA8176, AA8077, AA8177, AA8079, AA8090, AA8091, and AA8093 may be mentioned.

[0155] The examples disclosed herein will serve to further illustrate the present invention, but at the same time will not be any limitation thereof. On the contrary, it should be clearly understood that after reading the description of this specification, various embodiments, modifications thereof and equivalents that may suggest themselves to those skilled in the art can be used without departing from the spirit of the present invention. The examples and embodiments described herein can also utilize conventional procedures, unless otherwise specified. Some of the procedures are described herein for illustrative purposes.

[0156] Example 1 Table 1 below shows exemplary results illustrating the improved bond durability performance of various aluminum alloy products that have been mechanically altered to produce a micrograin subsurface structure. Bond durability results for an aluminum alloy product that retains the near-rolled surface microstructure and has not been mechanically altered are shown in Table 1 for comparison.

[0157] For the results in Table 1, sample 1 is comprised of a 7075 aluminum alloy product that has been mechanically modified using physical abrasion. Sample 1 is mechanically modified using a polished surface to produce a micrograin subsurface structure. Similarly, sample 2 is comprised of another 7xxx series aluminum alloy product that has been mechanically modified using a similar polished surface, such as S702. Samples 3 and 4 are comprised of 7075 aluminum alloy products. Samples 5, 6, and 7 are comprised of additional 7xxx aluminum alloy products. Samples 3, 4, 5, 6, and 7 are all mill finished. None of samples 3-7 have been mechanically modified, instead they retain the rolled near surface microstructure.

[0158] All specimens are subjected to an adhesion durability test. In this test, each specimen is composed of two aluminum alloy products, prepared and processed using the same conditions, and bonded through six bond sites. Each specimen is then subjected to a variety of test conditions. For example, the test conditions may include one or more of immersion in a salt solution, exposure to moist conditions, exposure to dry conditions, or application of a force that induces stress or strain. Each specimen is subjected to numerous cycles of these test conditions. The number of cycles that the specimen undergoes is either the number of cycles until mechanical failure is reached, or 60 cycles, which is the maximum number of cycles used in this particular test. Mechanical failure includes adhesion failure, metal product failure, or adhesive failure.

[0159] As can be seen from Table 1, Samples 1 and 2 performed significantly better than the unmodified Samples 3, 4, 5, 6, and 7. Samples 1 and 2 have a microparticle surfaced structure where all six bonds were intact after 60 cycles of adhesion durability testing. In contrast, all five mill-finished samples with rolled near surface microstructures suffered mechanical failure to all bonds within 10 cycles. [Table 1]

[0160] Example 2 FIG. 9 provides an exemplary image of elemental distribution of an aluminum alloy product sample modified according to the techniques and methods provided herein. The image provided in FIG. 9 was taken using energy dispersive x-ray spectroscopy (EDX). Image 910 shows a cross-sectional view of an aluminum alloy product sample. As shown, the aluminum alloy product includes a bulk 912, which may be similar or the same as bulk 820. The aluminum alloy product also includes an oxide layer 916. A deposition layer 914 covers the oxide layer 916 to preserve the surface during the sectioning and imaging process. The presence of the oxide layer 916 is highlighted in image 930. As shown, a denser oxygen population is present near the surface of the bulk 912, indicating the oxide layer 916. In this cross-sectional view of the aluminum alloy product sample, micrograin subsurface structure is not present. Micrograin subsurface structure may be present in other surface regions of the aluminum alloy product sample that are not shown.

[0161] Images 920, 940, and 950 show the distribution of various elements across the cross section of the aluminum alloy product sample. Image 920 shows the distribution of aluminum in the aluminum alloy product sample. As shown, the aluminum density is highest throughout the bulk 912 and is substantially uniform throughout the cross section depth of the bulk 912. Image 940 shows the distribution of zinc in the aluminum alloy product sample. As shown, the population of zinc is greater in the bulk 912 than in other regions of the aluminum alloy product sample. Image 950 shows the distribution of chromium in the aluminum alloy product sample. As shown, the presence of chromium is higher in the bulk 912, with a higher density population in the bulk 912.

[0162] Experimental Example 3 10A and 10B provide exemplary images of aluminum alloy product samples modified in accordance with the teachings herein. FIG. 10A provides image 1000A showing a cross-section of the aluminum alloy product. FIG. 10B provides image 1000B showing a cross-section of the aluminum alloy product. Images 1000A and 1000B are of the same sample, but were taken from different regions to show the differences in the surface regions of the aluminum alloy product sample. As shown, the surface region of the aluminum alloy product sample in image 1000A includes a micro-particle sub-surface structure 1010. The micro-particle sub-surface structure 1010 shown in FIG. 10A has a thickness of about 500 nm at its thickest point. In other areas not shown in the photograph, the micro-particle sub-surface structure 1010 may have a thickness substantially less than 500 nm, such as 150 nm, 100 nm, or 50 nm.

[0163] In some areas, the surface region of the aluminum alloy product sample may be free or substantially free of micro-particle subsurface structure 1010. One such area is shown in FIG. 10B. Image 1000B shows a surface region of the aluminum alloy product sample lacking micro-particle subsurface structure 1010. As shown, an oxide film 1020 (i.e., oxide layer 1020) is present on the surface region of the aluminum alloy product sample in image 1000B. The oxide film 1020 has a thickness of about 4 nm. Both images 1000A and 1000B were taken using a SEM. Due to the nature of the SEM, the surface of the aluminum alloy product sample in image 1000B is covered with a sputtered gold film to prevent degradation of the oxide film 1020 during imaging.

[0164] Example 4 FIG. 11 provides exemplary images of surface regions of various aluminum alloy product samples. Image 1110 corresponds to a first aluminum alloy material having a rolled near-surface microstructure. Image 1120 corresponds to a second aluminum alloy material having a micro-grain subsurface structure. Images 1110 and 1120 show the ratio of the first surface region to the second surface region. To analyze the ratio of the first surface region to the second surface region, both aluminum alloy material samples were color mapped using a chromaticity color mapping technique. More light absorption corresponds to yellow tones and less light absorption corresponds to blue tones. When viewed as a black and white image, yellow tones may appear lighter and blue tones may appear darker. The first surface region with the near-surface microstructure exhibits stronger light absorption and therefore appears yellow. The second surface region with the micro-grain subsurface structure exhibits lower light absorption and therefore appears blue.

[0165] The area percentage of the yellow and blue surface areas of each sample is evaluated to determine the ratio of the first surface area to the second surface area. Image 1110 includes a color mapping of sample 1112 and sample 1114. Samples 1112 and 1114 are samples of a mill-finished first aluminum alloy material. As shown, the surface area of ​​sample 1112 includes 47% of the first surface area and 53% of the second surface area. As shown, the surface area of ​​sample 1114 includes 54.3% of the first surface area and 45.7% of the second surface area. The increased surface percentage of the first surface area indicates a more prominent near-surface microstructure including defects. This may correspond to a lower bond durability of the first aluminum alloy material.

[0166] Image 1120 includes color mapping of sample 1122 and sample 1124. Samples 1122 and 1124 are samples of a second aluminum alloy material that have been mechanically modified in accordance with the techniques and methods herein. As shown, the surface area of ​​sample 1122 includes 32.3% of the first surface area and 67.7% of the second surface area. As shown, the surface area of ​​sample 1124 includes 22.4% of the first surface area and 77.6% of the second surface area. For samples 1122 and 1124, the surface percentage of the original surface area is reduced compared to samples 1112 and 1114, indicating a reduced near-surface microstructure that includes one or more defects. This may correspond to a higher bond durability of the second aluminum alloy material. Real-life examples

[0167] As used below, any reference to a series of examples should be understood as a disjunctive reference to each of those examples (e.g., "Examples 1-4" should be understood as "Examples 1, 2, 3, or 4").

[0168] Example 1 is an aluminum alloy product comprising: a bulk comprising a bulk grain structure including particles of aluminum alloy, the aluminum alloy including aluminum and one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese; a first surface region including a near-surface microstructure (NSM) having a thickness of less than 500 nm; a second surface region free of NSM, the second surface region including an oxide layer; and a micro-grain subsurface structure present between the oxide layer and the bulk, the micro-grain subsurface structure having a thickness of between 1 nm and 2 μm, being free or substantially free of one or more compositional defects, the one or more compositional defects including organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxides, or anodic oxides, and comprising a grain structure distinct from the bulk grain structure, the grain structure including aluminum alloy particles having an average diameter of between 10 nm and 500 nm.

[0169] Example 2 is an aluminum alloy product as described in any of the preceding or following examples, wherein the oxide layer has a thickness of 1 nm to 20 nm.

[0170] Example 3 is an aluminum alloy product of the preceding or subsequent examples, in which the oxide layer has an average thickness of 10 nm and a standard deviation of 5 nm.

[0171] Example 4 is an aluminum alloy product of any preceding or subsequent example, in which the oxide layer is free or substantially free of one or more defects.

[0172] Example 5 is the aluminum alloy product of any preceding or subsequent example, wherein the NSM includes one or more compositional defects, the one or more compositional defects including organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxide, or anodic oxide.

[0173] Example 6 is an aluminum alloy product of any preceding or subsequent example, wherein the ratio of the first surface area to the second surface area is less than 50%.

[0174] Example 7 is an aluminum alloy product of any preceding or subsequent example, wherein the first surface region and the second surface region are discontinuous.

[0175] Example 8 is the aluminum alloy product of any preceding or subsequent example, wherein the micrograin subsurface structure further comprises precipitates having an average diameter of 10 nm to 2 μm, the precipitates comprising one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese.

[0176] Example 9 is the aluminum alloy product of any preceding or subsequent example, further comprising a silicon-containing layer over the micrograin subsurface structure, the silicon-containing layer modifying a portion of the bonding sites within the micrograin subsurface structure.

[0177] Example 10 is an aluminum alloy product of any preceding or subsequent example, where the weight percent of aluminum in the micrograin subsurface structure is less than the weight percent of aluminum in the bulk.

[0178] Example 11 is an aluminum alloy product of the preceding or succeeding examples, and exhibits adhesion durability of 22 cycles to 100 cycles or more according to the FLTMBV101-07 standard test.

[0179] Example 12 is an aluminum alloy product of any preceding or subsequent example, wherein the concentrations of magnesium and zinc in the aluminum alloy are less than 20 wt. %, and the ratio of zinc to magnesium in the concentrations is 0.1 to 10.0.

[0180] Example 13 is an aluminum alloy product of any preceding or subsequent example, wherein the concentration of magnesium in the bulk is higher than in the micrograin subsurface structure, the concentration of copper in the bulk is higher than in the micrograin subsurface structure, or the concentration of zinc in the bulk is higher than in the micrograin subsurface structure.

[0181] Example 14 is an aluminum alloy product of any preceding or subsequent example, wherein the micrograin subsurface structure includes more structural defects than the bulk, the structural defects corresponding to or including voids, propagating cracks, or fissures.

[0182] Example 15 is an aluminum alloy product of the preceding or subsequent examples, in which the micrograin subsurface structure is substantially the same as the bulk.

[0183] Example 16 is an aluminum alloy product of any preceding or subsequent example, wherein the micrograin subsurface structure includes a uniformity of grain structure or uniformity of distribution of alloying elements that differs from that of the bulk.

[0184] Example 17 is a method of fabricating an aluminum alloy product, the method including providing an aluminum alloy product comprising: a bulk having a bulk grain structure including particles of an aluminum alloy, the aluminum alloy including aluminum and one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese; and a near-surface microstructure (NSM) greater than 500 nm thick; and modifying the NSM to provide a first surface region including a near-surface microstructure (NSM) less than 500 nm thick and a second surface region free of NSM. and generating a micro-grained subsurface structure between the oxide layer and the bulk, the micro-grained subsurface structure having a thickness of between 1 nm and 2 μm, free or substantially free of one or more compositional defects, the one or more compositional defects comprising organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxide, or anodic oxide, and comprising a grain structure different from the bulk grain structure, the grain structure comprising aluminum alloy grains having an average diameter of between 10 nm and 500 nm.

[0185] Example 18 is the method of any preceding or subsequent example, wherein the oxide layer has a thickness of 1 nm to 20 nm.

[0186] Example 19 is the method of the preceding or subsequent examples, where the oxide layer has an average thickness of 10 nm and a standard deviation of 5 nm.

[0187] Example 20 is the method of any preceding or subsequent example, wherein the oxide layer is free or substantially free of one or more defects.

[0188] Example 21 is the method of any preceding or subsequent example, wherein the NSM includes one or more compositional defects, and the one or more compositional defects include organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxides, or anodic oxides.

[0189] Example 22 is the method of any preceding or subsequent example, wherein the ratio of the first surface area to the second surface area is less than 50%.

[0190] Example 23 is the method of any preceding or subsequent example, wherein the first surface region and the second surface region are discontinuous.

[0191] Example 24 is the method of any preceding or subsequent example, wherein the micrograin subsurface structure further comprises precipitates having an average diameter of 10 nm to 2 μm, and the precipitates comprise one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese.

[0192] Example 25 is the method of any preceding or subsequent example, wherein the concentrations of magnesium and zinc in the aluminum alloy are less than 20 wt. %, and the ratio of zinc to magnesium in the alloy is 0.1 to 10.0.

[0193] Example 26 is the method of any preceding or subsequent example, wherein the weight percent of aluminum in the microparticle subsurface structure is less than the weight percent of aluminum in the bulk.

[0194] Example 27 is a method of any preceding or subsequent example, wherein the concentration of magnesium in the bulk is higher than in the microparticle subsurface structure, the concentration of copper in the bulk is higher than in the microparticle subsurface structure, or the concentration of zinc in the bulk is higher than in the microparticle subsurface structure.

[0195] Example 28 is the method of any preceding or subsequent example, wherein the microparticle subsurface structure provides adhesion durability of 22 cycles to 100 cycles or more according to the FLTMBV101-07 standard test.

[0196] Example 29 is the method of any preceding or subsequent example, wherein the micro-particle subsurface structure has fewer structural defects than NSM and more structural defects than bulk, and the structural defects correspond to or include voids, propagating cracks, or fissures.

[0197] Example 30 is the method of any preceding or subsequent example, wherein modifying the NSM includes depositing a silicon-containing layer when generating the microparticle subsurface structure or coating at least a portion of the microparticle subsurface structure with a silicon-containing layer, wherein the silicon-containing layer modifies a portion of the binding sites within the microparticle subsurface structure.

[0198] Example 31 is the method of any preceding or subsequent example, wherein the modification includes subjecting the NSM to mechanical modification, the mechanical modification including one or more of grinding the NSM, physically ablating the NSM, grit blasting the NSM, laser ablating the NSM, sandblasting the NSM, or polishing the NSM.

[0199] All patents, publications, and abstracts cited above are incorporated herein by reference in their entirety. The foregoing description of the embodiments, including the illustrated embodiments, has been presented for purposes of illustration and description only and is not intended to be exhaustive or to be limited to the precise forms disclosed. Numerous modifications, adaptations, and uses thereof will be apparent to those skilled in the art.

Claims

1. An aluminum alloy product, A bulk having a bulk grain structure including grains of an aluminum alloy, the aluminum alloy comprising: Aluminum, as well as the bulk comprising one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese; a first surface region including a near-surface microstructure (NSM) having a thickness of less than 500 nm; a second surface region free of the NSM, the second surface region comprising an oxide layer; a micro-grain sub-surface structure present between the oxide layer and the bulk, the micro-grain sub-surface structure comprising: having a thickness of 1 nm to 2 μm; is free or substantially free of one or more compositional defects, the one or more compositional defects including organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxides, or anodic oxides; and and said micro-grain sub-surface structure having a grain structure different from said bulk grain structure, said grain structure comprising aluminum alloy grains having an average diameter between 10 nm and 500 nm.

2. 2. The aluminium alloy product according to claim 1, wherein the oxide layer has a thickness of from 1 nm to 20 nm.

3. 3. The aluminum alloy product of claim 2, wherein the oxide layer has an average thickness of 10 nm and a standard deviation of 5 nm.

4. 10. The aluminum alloy product of claim 1, wherein said oxide layer is free or substantially free of one or more defects.

5. 10. The aluminum alloy product of claim 1, wherein the NSM comprises one or more compositional defects, the one or more compositional defects comprising organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxide, or anodic oxide.

6. 2. The aluminum alloy product of claim 1, wherein a ratio of said first surface area to said second surface area is less than 50%.

7. 2. The aluminum alloy product of claim 1, wherein the first surface region and the second surface region are discontinuous.

8. 2. The aluminum alloy product of claim 1, wherein the micrograin subsurface structure further comprises precipitates having an average diameter of 10 nm to 2 μm, the precipitates comprising one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese.

9. 10. The aluminum alloy product of claim 1, further comprising a silicon-containing layer on said micrograin subsurface structure, said silicon-containing layer modifying a portion of the bonding sites within said micrograin subsurface structure.

10. 10. The aluminum alloy product of claim 1, wherein a weight percent of aluminum in said micrograin subsurface structure is less than a weight percent of aluminum in said bulk.

11. 10. The aluminum alloy product of claim 1, exhibiting adhesion durability of 22 to 100 cycles or more according to FLTM BV101-07 standard test.

12. 2. The aluminium alloy product of claim 1, wherein the concentrations of magnesium and zinc in said aluminium alloy are less than 20% by weight, and the ratio of zinc to magnesium in said concentrations is between 0.1 and 10.

0.

13. 2. The aluminum alloy product of claim 1, wherein the concentration of magnesium in the bulk is greater than in the micrograin subsurface structure, the concentration of copper in the bulk is greater than in the micrograin subsurface structure, or the concentration of zinc in the bulk is greater than in the micrograin subsurface structure.

14. 2. The aluminum alloy product of claim 1, wherein the micro-grain subsurface structure contains more structural imperfections than the bulk, the structural imperfections corresponding to or including voids, propagating cracks, or fissures.

15. 2. The aluminum alloy product of claim 1, wherein the micrograin subsurface structure is substantially the same as the bulk.

16. 2. The aluminum alloy product of claim 1, wherein the micrograin subsurface structure comprises a grain structure uniformity or alloying element distribution uniformity different from that of the bulk.

17. 1. A method for processing an aluminum alloy product, the method comprising: To provide an aluminum alloy product, the aluminum alloy product comprising: A bulk having a bulk grain structure including grains of an aluminum alloy, the aluminum alloy comprising: Aluminum, as well as the bulk comprising one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese; a near-surface microstructure (NSM) having a thickness greater than 500 nm; The NSM is modified to a first surface region including a near-surface microstructure (NSM) having a thickness of less than 500 nm; a second surface region free of the NSM, the second surface region comprising an oxide layer; a micro-grain sub-surface structure present between the oxide layer and the bulk, the micro-grain sub-surface structure comprising: having a thickness of 1 nm to 2 μm; is free or substantially free of one or more compositional defects, the one or more compositional defects including organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxides, or anodic oxides; and and producing the micro-grain subsurface structure having a grain structure different from the bulk grain structure, the grain structure comprising aluminum alloy grains having an average diameter of 10 nm to 500 nm.

18. The method of claim 17, wherein the oxide layer has a thickness of 1 nm to 20 nm.

19. 20. The method of claim 18, wherein the oxide layer has an average thickness of 10 nm and a standard deviation of 5 nm.

20. The method of claim 17 , wherein the oxide layer is free or substantially free of one or more defects.

21. 20. The method of claim 17, wherein the NSM comprises one or more compositional defects, the one or more compositional defects comprising organic matter, oil, hydrocarbons, soil, inorganic residue, entrained oxide, or anodic oxide.

22. 20. The method of claim 17, wherein a ratio of the first surface area to the second surface area is less than 50%.

23. The method of claim 17 , wherein the first surface region and the second surface region are discontinuous.

24. 18. The method of claim 17, wherein the micro-grain subsurface structure further comprises precipitates having an average diameter of 10 nm to 2 μm, the precipitates comprising one or more alloying elements selected from the group consisting of zinc, magnesium, copper, chromium, silicon, iron, and manganese.

25. 18. The method of claim 17, wherein the concentrations of magnesium and zinc in the aluminum alloy are less than 20% by weight, and the ratio of zinc to magnesium in said concentrations is between 0.1 and 10.

0.

26. 20. The method of claim 17, wherein the weight percent of aluminum in the microparticle subsurface structure is less than the weight percent of aluminum in the bulk.

27. 18. The method of claim 17, wherein the concentration of magnesium in the bulk is greater than in the microparticle subsurface structure, the concentration of copper in the bulk is greater than in the microparticle subsurface structure, or the concentration of zinc in the bulk is greater than in the microparticle subsurface structure.

28. 18. The method of claim 17, wherein the microparticle subsurface structure provides adhesion durability of 22 to 100 cycles or more according to FLTM BV101-07 standard test.

29. 20. The method of claim 17, wherein the microparticle subsurface structure has fewer structural defects than the NSM and more structural defects than the bulk, the structural defects corresponding to or including voids, propagating cracks, or fissures.

30. 20. The method of claim 17, wherein modifying the NSM comprises depositing a silicon-containing layer when generating the microparticle subsurface structure or coating at least a portion of the microparticle subsurface structure with a silicon-containing layer, the silicon-containing layer modifying a portion of the binding sites within the microparticle subsurface structure.

31. The modifying includes subjecting the NSM to a mechanical modification, the mechanical modification comprising: grinding the NSM; physically ablating the NSM; grit blasting the NSM; laser ablating the NSM; Sandblasting the NSM; or Polishing the NSM.