Aluminum alloy coated plate for tab
The aluminum alloy coated plate with controlled Si, Fe, Cu, Mn, and Mg composition and subgrain structure addresses the challenge of reduced tear resistance in thinner tabs, ensuring strong and tear-resistant can opening.
Patent Information
- Application Number
- JP2024148649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-06-30
AI Technical Summary
Aluminum alloy plates for tabs have become thinner for cost reduction, leading to reduced bending stress and tab tear resistance, necessitating improved tab tearability while maintaining strength.
An aluminum alloy coated plate with specific compositions of Si, Fe, Cu, Mn, and Mg, and a structured subgrain formation through cold rolling and heat treatment, enhancing tab tear resistance.
The solution provides high tab tear resistance and strength, ensuring effective can opening without breakage or tearing, even with reduced wall thickness.
Smart Images

Figure 2024161621000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated aluminum alloy sheet for use in a tub. [Background technology]
[0002] Beverage cans and food cans, such as canned goods, are widely distributed as packaging containers used for beverages and food. Currently, the so-called pull-top type, which uses an easy-open end (EOE) that allows the can to be easily opened by hand without using a tool such as a can opener, is widely used for the ends of these cans, and the stay-on tab (SOT) type, in which the tab does not come off the lid body, is becoming more popular due to safety and environmental concerns.
[0003] Tab materials for forming tabs are required to have not only moldability but also high strength, repeated bending property and high tab tear resistance. On the other hand, particularly in recent years, the thickness of tabs has been reduced in order to reduce costs, and a material strength higher than ever before is required to ensure the tab breaking strength. In addition, the reduction in thickness and the associated increase in strength have significantly reduced tab tear resistance, and there is an increasing demand for materials with high tab tear resistance.
[0004] For example, Patent Document 1 describes an aluminum alloy sheet for packaging container tabs, which contains predetermined amounts of Si, Fe, Cu, Mn, and Mg, the contents of Fe and Mn satisfy a predetermined relationship, and further specifies the sum of the area ratios of Al-Fe-Mn-based crystallized particles and Mg-Si-based crystallized particles in the center of the sheet thickness and the maximum sizes of these crystallized particles. Tabs formed from such an aluminum alloy sheet are said to be free from tearing and cracking when the can is opened.
[0005] For example, Patent Document 2 describes an aluminum alloy sheet for packaging container tabs, which contains predetermined amounts of Mg, Cu, Fe, Si, and Mn, the contents of Fe and Mn satisfy a predetermined relationship, and specifies the total area ratio of Al-Fe-Mn intermetallic compounds and M-Si intermetallic compounds having a maximum length of 1 μm or more at the center of the sheet thickness. Tabs formed from such an aluminum alloy sheet are said to be resistant to tearing when opening a can even when thinned, and to have excellent repeated bending properties.
[0006] For example, Patent Document 3 describes an aluminum alloy sheet for tabs that contains predetermined amounts of Mg, Cu, Fe, Si, Mn, and Cr and has a texture in which the Cube orientation density is 1.5 times or more that of a random orientation sample over the entire range from the center of the sheet to the surface in the thickness direction. Such an aluminum alloy sheet is said to be capable of achieving both high strength and excellent bendability. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2005-200754 A [Patent Document 2] JP 2011-225977 A [Patent Document 3] JP 2017-66458 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in recent years, from the viewpoints of cost reduction, CO2 reduction, resource conservation, etc., aluminum alloy sheets for tabs have become thinner than ever before, and the bending stress on the surface layer of the bent part where it breaks due to repeated bending has decreased, making it relatively easy to ensure repeated bending properties, which was a problem in the past. In addition, the tab breaking strength can be addressed by increasing the strength of the material. On the other hand, the progress in thinner and stronger materials has made it necessary to further improve the tab breaking resistance.
[0009] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a coated aluminum alloy sheet for tabs which has high resistance to tab cracking even when made thin. [Means for solving the problem]
[0010] The coated aluminum alloy sheet for tabs according to the present invention comprises an aluminum alloy sheet containing 0.05% by mass to 0.40% by mass of Si, 0.05% by mass to 0.50% by mass of Fe, 0.01% by mass to 0.30% by mass of Cu, 0.1% by mass to 0.6% by mass of Mn, 4.0% by mass to 6.0% by mass of Mg, with the balance being Al and unavoidable impurities, and a resin layer. When the structure of the coated aluminum alloy sheet for tabs is observed in a region 50 nm thick from the center of the sheet thickness in both thickness directions from the normal direction of the rolled surface, the coated aluminum alloy sheet has a diameter of 205×10 in an image taken by a transmission electron microscope at a magnification of 50,000. -12 m 2 The grain size is 40 or more subgrains in total. Effect of the Invention
[0011] According to the present invention, it is possible to provide a coated aluminum alloy sheet for tabs which has high resistance to tab cracking even when made thin. [Brief description of the drawings]
[0012] [Figure 1] 1A and 1B are diagrams illustrating the appearance of a stay-on-tab type can lid and the can-opening operation, in which FIG. 1A is a plan view, FIG. 1B is a cross-sectional view taken along the line AA of FIG. 1A, and FIG. 1C is a cross-sectional view and a plan view of the main parts explaining the can-opening operation. [Diagram 2] 1 is an example of a transmission electron microscope image of the structure of an aluminum alloy plate. [Diagram 3] FIG. 4 is a schematic diagram illustrating a method for measuring a tab tearing simulated load. [Figure 4] 13 is an example of the measurement results of a tab tearing simulated load. [Diagram 5] 1 is a graph showing the relationship between a tab cracking simulated load and a plate threading interval. [Figure 6]1 is a graph showing the relationship between a tab tearing simulated load and the number of subgrains. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an aluminum alloy coated sheet for a tab according to one embodiment of the present invention will be described. However, the embodiment shown below is an example for embodying the technical idea of the present invention, and the present invention is not limited to the following embodiment. The size and positional relationship of the members shown in each drawing may be exaggerated for clarity of explanation. In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Furthermore, the content of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified. Furthermore, the upper and lower limits of the numerical ranges described in this specification can be arbitrarily selected and combined.
[0014] As shown in FIG. 1A, the stay-on-tab type lid is composed of a lid material 2 and a tab 1, and the tab 1 is attached to the lid material 2 by crimping a rivet part 21 formed at approximately the center of the disk-shaped lid material 2 (part of which is shown in FIG. 1A) into a rivet hole 11 in the tab 1. The rivet hole 11 is formed at a position closer to one end than the center in the longitudinal direction of the tab 1, and a ring-shaped hook part 12 is formed at the other end so that a finger can be easily hooked. As shown in FIG. 1B, the tab 1 is increased in rigidity and ensured in safety by bending the outer periphery of the cut plate material (aluminum alloy plate) and the inner periphery of the hook part 12 downward. Meanwhile, the region where the rivet hole 11 and the U-shaped hole (slit)-like inner lance 14 are formed on the outer side of the rivet hole 11 is formed as a single flat plate, making it easily deformable. Generally, aluminum alloy plates such as 5182 alloy are widely used as the material for such a tab 1. The aluminum alloy plate is coated and baked on the surface, then cut and formed into a prescribed shape to manufacture the tub 1, and the tub 1 is attached by rivets to a lid material 2 formed by forming another plate material. An opening region 23 for forming a drinking spout after the can is opened is provided on the extension of the one end side of the tub 1, surrounded by scores 25. This score 25 does not go completely around the periphery of the opening region 23, but is formed so as to be discontinuous at one point (the region where the tub 1 overlaps in FIG. 1A).
[0015] In opening the can, when the hooking portion 12 of the tab 1 is pulled upward, as shown in FIG. 1C, this becomes a force point E, and the vicinity of the rivet portion 21 becomes a fulcrum F, and the tab 1 is raised, leaving the area fixed by the rivet portion 21. In detail, the tab 1 is divided by the inner lance 14, and the outer area such as the hooking portion 12 is raised while the inner area (the area around the rivet hole 11) is fixed to the lid material 2. Then, one end of the tab 1 (the opposite side of the hooking portion 12 across the rivet hole 11) becomes a point of action L, and is strongly pushed downward by the lever action, and a part of the opening area 23 of the lid material 2 directly below this one end is pushed down together. Then, the lid material 2 is cracked along the score 25 from the vicinity of the pushed-down part, and the opening area 23 is separated from the other part of the lid material 2 leaving a part and pushed downward (into the inside of the can), and a drinking spout (opening) is formed in the lid material 2. The opening region 23 easily bends where the lid material 2 does not have the scores 25 formed, maintaining the connection with the other parts of the lid material 2, and the tab 1 easily bends between both ends of the inner lance 14 around the rivet hole 11, and is connected to the rivet part 21 outside the opening region 23 of the lid material 2. Therefore, the opening region 23 and the tab 1 do not separate from the can body (can trunk).
[0016] Thus, the tab acts as a lever and is subjected to a strong external force when the can is opened. Therefore, if the tab is not strong enough, it may bend at the thin part of the hook 12 near the center between the fulcrum F and the force point E shown in Fig. 1C or at the thin part around the inner lance 14 (see the bent part 4 in the lower right of Fig. 1C), making it difficult to open the can (tab breakage) or even tearing off. In addition, when the outer area of the inner lance 14, such as the hook 12, is raised, the end of the inner lance 14 may tear along the movement direction (tab tear) (see the tear part 5 in the lower right of Fig. 1C).
[0017] In particular, in the case of a stay-on-tab end, if the opening region 23 is not pushed deep enough into the beverage can, it will be an obstacle when taking out (drinking) the beverage in the beverage can. For this reason, the tab 1 (hooking portion 12) is raised to nearly vertical, and then raised even more (tilted to the opposite side) to open the can. After opening the can, the tab 1 is generally returned (tilted) to its original state so that only the opening region 23 of the lid member 2 is pushed inward, as shown by the dashed line in FIG. 1C, so that the raised tab 1 does not hinder drinking the beverage in the beverage can. That is, the tab 1 is bent to an angle of nearly 90° or more near both ends of the inner lance 14 around the rivet hole 11, and then returned to its original state (bent back). In addition, if the opening region 23 is not sufficiently pushed in by bending and bending back the tab 1 once, it is necessary to repeat the bending and bending back operations again, so that the tab 1 is required to have formability that can withstand at least four deformations and does not break at the bending point (see the breaking portion 6 in the lower right of FIG. 1C). This property is called repeated bending property.
[0018] As described above, tab materials are required to have not only moldability but also high strength, repeated bending property and high tab tear resistance. On the other hand, particularly in recent years, the thickness of tabs has been reduced in order to reduce costs, and a material strength higher than ever before is required to ensure the tab breaking strength. In addition, the reduction in thickness and the associated increase in strength have significantly reduced tab tear resistance, and there is an increasing demand for materials with high tab tear resistance.
[0019] Aluminum alloy coated plate for tub The coated aluminum alloy sheet for tabs according to one embodiment of the present invention comprises an aluminum alloy sheet and a resin layer provided on one or both sides of the aluminum alloy sheet. When the coated aluminum alloy sheet for tabs is subjected to a paint baking treatment and the structure of a region 50 nm thick in both thickness directions from the center of the sheet thickness (hereinafter sometimes referred to as the center of the sheet thickness) is observed from the normal direction of the rolled surface, the region has a thickness of 205×10 in an image taken by a 50,000-power transmission electron microscope. -12 m 2 The grain size is 40 or more subgrains in total.
[0020] Aluminum Alloy Composition The aluminum alloy plate constituting the aluminum alloy coated plate for the tab is made of, for example, an Al-Mg alloy, for example, a general JIS alloy such as 5182.
[0021] Specifically, the aluminum alloy plate contains Si: 0.05% by mass to 0.40% by mass, Fe: 0.05% by mass to 0.50% by mass, Cu: 0.01% by mass to 0.30% by mass, Mn: 0.1% by mass to 0.6% by mass, Mg: 4.0% by mass to 6.0% by mass, and the balance is Al and inevitable impurities. The content of each component contained in the aluminum alloy plate and the reason for limiting the content will be described below.
[0022] (Si: 0.05 mass% or more and 0.40 mass% or less) If the Si content is less than 0.05% by mass, high-purity aluminum ingot is required during casting, which increases costs. If the Si content exceeds 0.40% by mass, a large number of intermetallic compounds are formed during casting and hot rolling, which promotes the generation and propagation of cracks, resulting in a decrease in repeated bending properties and tab crack resistance. The Si content is preferably 0.30% by mass or less, more preferably 0.25% by mass or less, and even more preferably 0.20% by mass or less. The Si content is preferably 0.06% by mass or more.
[0023] (Fe: 0.05 mass% or more and 0.50 mass% or less) If the Fe content is less than 0.05% by mass, high-purity aluminum ingot is required during casting, which increases costs. On the other hand, if the Fe content exceeds 0.50% by mass, the amount of Al-Fe-Mn intermetallic compounds increases, promoting the generation and propagation of cracks, thereby reducing repeated bending properties and tab crack resistance. The Fe content is preferably 0.10% by mass or more, more preferably 0.15% by mass or more. The Fe content is preferably 0.40% by mass or less, more preferably 0.35% by mass or less, even more preferably 0.30% by mass or less, and particularly preferably 0.25% by mass or less.
[0024] (Cu: 0.01 mass% or more and 0.30 mass% or less) If the Cu content is less than 0.01% by mass, the strength is insufficient, and the tab folding strength is insufficient. On the other hand, if the Cu content exceeds 0.30% by mass, the strength becomes too high, and the tab is easily torn off due to bending deformation such as repeated bending. The Cu content is preferably 0.02% by mass or more, and more preferably 0.03% by mass or more. The Cu content is preferably 0.25% by mass or less, more preferably 0.20% by mass or less, even more preferably 0.15% by mass or less, and particularly preferably 0.10% by mass or less.
[0025] (Mn: 0.1 mass% or more and 0.6 mass% or less) If the Mn content is less than 0.1% by mass, the strength is insufficient, and the tab breaking strength is insufficient. On the other hand, if the Mn content exceeds 0.6% by mass, the strength becomes too high and the amount of Al-Fe-Mn intermetallic compounds increases, so that the tab crack resistance decreases. The Mn content is preferably 0.2% by mass or more. The Mn content is preferably 0.55% by mass or less, more preferably 0.45% by mass or less, and particularly preferably 0.35% by mass or less.
[0026] (Mg: 4.0 mass% or more and 6.0 mass% or less) If the Mg content is less than 4.0% by mass, the strength is insufficient, resulting in insufficient tab breaking strength. On the other hand, if the Mg content exceeds 6.0% by mass, the strength becomes excessive and formability decreases. As the Mg content increases, the strength and work hardening ability improve, making the material more likely to break due to repeated bending. The Mg content is preferably 4.5% by mass or more. The Mg content is preferably 5.5% by mass or less, more preferably 5.0% by mass or less.
[0027] (Ti: 0.1% by mass or less) The aluminum alloy plate may contain Ti. Ti is added as necessary for the purpose of refining the ingot structure, and the effect is obtained by adding 0.01 mass% or more. If the Ti content exceeds 0.1 mass%, coarse compounds may be formed, which may reduce the tab tear load. Therefore, the Ti content in the aluminum alloy may be limited within the above range. When Ti is added, for example, an ingot refiner (Al-Ti-B) with a mass ratio of Ti to B of 5:1 is added. Since it is added to the molten metal before casting in the form of a waffle or rod, B is inevitably added according to the content ratio. The Ti content may be preferably 0.08 mass% or less, more preferably 0.06 mass% or less.
[0028] (balance: Al and unavoidable impurities) The aluminum alloy plate may contain inevitable impurities in addition to Al and the above alloy components. Examples of inevitable impurities include Cr, Zn, Zr, B, V, Na, Ca, Ni, In, Sn, and Ga. The allowable content of inevitable impurities is, for example, 0.1 mass% or less for Cr, preferably 0.05 mass% or less. For example, 0.3 mass% or less for Zr, preferably 0.1 mass% or less, more preferably 0.05 mass% or less. For example, each of the other elements may be 0.05 mass% or less and a total of 0.15 mass% or less. If the content is within the above range, the effect of the present invention is suppressed from being hindered even when the above elements are added, not limited to when they are contained as inevitable impurities.
[0029] The thickness of the aluminum alloy plate constituting the coated aluminum alloy plate for the tab may be, for example, 0.18 mm or more and 0.40 mm or less.
[0030] Aluminum alloy plate structure In one embodiment of the present invention, the aluminum alloy sheet has the above-mentioned alloy composition, and is cold-rolled without intermediate annealing, and then heat-treated by paint baking treatment. The structure of the aluminum alloy sheet has 40 or more subgrains in a predetermined region in the center of the sheet thickness. By making the aluminum alloy sheet have a predetermined number of subgrains or more, it is possible to solve a problem that has been difficult to solve in the past, that is, the tab breaking load can be improved while maintaining strength. The subgrains of the aluminum alloy sheet have a density of 205×10 when observed from the normal direction of the rolled surface in a 100 nm thick structure in the center of the sheet thickness. -12 m 2 They are counted by observing them under a transmission electron microscope (TEM) at 50,000 magnification.
[0031] Subgrains, also known as subcrystal grains, are small, irregular grains that arise when a material (structure) into which dislocations have been introduced by cold rolling or other methods undergoes recovery to a lower energy structure under given temperature, time, and strain.
[0032] That is, in the case of coated aluminum alloy sheets for tabs, subgrains with sharp boundaries are formed when dislocations in dislocation-dense regions such as dislocation cell walls and deformation bands introduced by cold rolling coalesce and annihilate and rearrange. When many dislocation-dense regions are formed, the probability of them coalescing and annihilat- ing with newly moving dislocations increases, lowering the work hardening exponent (n value), but the formation of a subgrain structure improves the work hardening exponent (n value). When the work hardening exponent (n value) is improved, the plastic deformation region in the stress concentration area expands, improving tab crack resistance. For this reason, the more subgrains there are, the higher the tab crack load.
[0033] An example of an observed subgrain is shown in Figure 2. Figure 2 is an example of a transmission electron microscope (TEM) image at 50,000 times magnification. Dislocation-dense regions 100 and subgrains 200 are mixed together, and the subgrains 200 are identified within the crystal grains as small, individual, irregular grains with a sharp (clear and distinct) outer edge shape that is the boundary and few dislocations inside.
[0034] In this way, the number of individual subgrains can be counted in the observation field of the transmission electron microscope. It is also possible to measure the area ratio of the subgrains instead of the number of subgrains present in a given observation field, but in that case, the size of the subgrains is not taken into consideration, so a high subgrain area ratio can be obtained even in the case of a coarse subgrain structure. Since a coarse subgrain structure has a lower dislocation density than a fine subgrain structure, the strength is reduced and the strength required for a tab cannot be obtained.
[0035] Therefore, in one embodiment, the size of the subgrain is, for example, 1000 nm or less, preferably 800 nm or less, more preferably 600 nm or less in terms of the equivalent circle diameter. The lower limit of the equivalent circle diameter of the subgrain is, for example, 50 nm or more. The equivalent circle diameter is calculated by measuring the boundary length of the subgrain and calculating it as the diameter of a circle having a circumference length equal to the boundary length.
[0036] In one embodiment, the number of subgrains in a predetermined region in the sheet thickness center of the aluminum alloy plate constituting the aluminum alloy coated sheet for tabs may be 40 or more, preferably 50 or more, and more preferably 60 or more. The upper limit of the number of subgrains is, for example, 600 or less, or 400 or less.
[0037] When subgrain formation in a predetermined region in the thickness center of an aluminum alloy sheet is not advanced, that is, when the number of subgrains is as small as less than 40, the aluminum alloy sheet has high strength, but on the other hand, it may not be possible to achieve both excellent tab crack resistance and tab breaking strength (high strength). That is, it may not be possible to improve the tab crack resistance while maintaining the high strength of the aluminum alloy coated sheet for tabs.
[0038] The aluminum alloy coated sheet for tabs has excellent strength and tab crack resistance. The sheet strength of the aluminum alloy coated sheet for tabs may be, for example, 300 MPa or more as 0.2% proof stress, preferably 320 MPa or more, more preferably 330 MPa or more, and even more preferably 340 MPa or more. The upper limit of the sheet strength of the aluminum alloy coated sheet for tabs is, for example, 390 MPa or less as 0.2% proof stress. The tab crack resistance of the aluminum alloy coated sheet for tabs can be evaluated by a tab crack simulation load obtained by, for example, the method shown in FIG. 3. The tab crack simulation load by the method shown in FIG. 3 may be, for example, 65 N or more, preferably 67 N or more, more preferably 68 N or more, and even more preferably 70 N. The upper limit of the tab crack simulation load is, for example, about 100 N or less. If the 0.2% proof stress is 300 MPa or more and the tab breaking simulated load is 65 N or more, the can can be opened while maintaining sufficient strength without causing tab bending, tab breaking, etc. The method for evaluating the tab breaking simulated load will be described in detail later.
[0039] The structure and properties of the aluminum alloy sheet described above are those of a painted aluminum alloy sheet (precoated sheet) after painting and paint baking treatments are performed on a cold-rolled sheet (sheet after cold rolling). Note that such structure and properties may be those of an aluminum alloy sheet after heat treatment under specific conditions simulating paint baking treatment is performed on a cold-rolled sheet without painting and paint baking treatments or without forming into a tab. These structures and properties are the same or can be considered to be the same with only a slight difference if the conditions of the paint baking treatment and the heat treatment are the same.
[0040] The aluminum alloy coated sheet for tabs may be a precoated sheet having a resin layer provided on one or both sides of the aluminum alloy sheet. The resin layer may be a baked resin layer formed by applying an organic paint such as an epoxy-based, vinyl chloride-based, or polyester-based paint and then subjecting it to a heat treatment. The aluminum alloy sheet to which the organic paint is applied may be a surface-treated aluminum alloy sheet that has been surface-treated or chemically treated with a surface treatment agent such as a chromate-based or zircon-based agent. The temperature of the heat treatment may be, for example, a temperature at which the peak metal temperature (PMT) is about 200°C or higher and 290°C or lower. The thickness of the resin layer may be, for example, about 0.5 μm or higher and 15 μm or lower.
[0041] Manufacturing method An example of a method for producing an aluminum alloy sheet constituting an aluminum alloy coated sheet for a tab will be described. The method for producing an aluminum alloy sheet includes a casting step as a first step, a homogenization heat treatment step as a second step, a hot rolling step as a third step, and a cold rolling step as a fourth step, and these steps are carried out in this order.
[0042] (1st to 3rd processes: casting process, homogenization heat treatment process, hot rolling process) The first step is to produce an ingot having a target composition by a semi-continuous casting method, and the second step is to perform a homogenization heat treatment on the aluminum alloy ingot produced in the first step.
[0043] In the first step, an aluminum alloy is cast by a semi-continuous casting method (DC (direct chill) casting) to obtain an ingot. Next, a step of removing the region of the ingot surface that will become a non-uniform structure by facing and a step of performing a homogenization heat treatment are performed. This homogenization heat treatment is performed, for example, in the range of 400°C to 570°C, and also serves as preheating for the subsequent hot rolling.
[0044] The third step is hot rolling the aluminum alloy ingot that has been subjected to the homogenization heat treatment in the second step. The thickness of the hot-rolled plate obtained by hot rolling is usually set by calculating backward the total rolling reduction ratio by cold rolling from the thickness of the product plate obtained by cold rolling.
[0045] The coiling temperature, which is the end temperature of the hot rolling, is, for example, 300° C. to 400° C., preferably 320° C. to 370° C. When the coiling temperature is 300° C. or higher, the recrystallization rate of the hot-rolled sheet is improved, and the tab tearing simulated load of the aluminum alloy sheet after paint baking is further improved. On the other hand, when the coiling temperature is 400° C. or lower, the occurrence of a surface defect called seizure on the sheet surface is suppressed, and the properties of the sheet surface are improved.
[0046] The fourth step is a step of cold rolling the hot-rolled sheet obtained in the third step. In the fourth step, the hot-rolled sheet is cold-rolled without intermediate annealing to finish it into an aluminum alloy sheet of a predetermined thickness. The cold rolling is performed by setting multiple passes with a predetermined total rolling ratio so that the hot-rolled sheet is rolled to the thickness of the product sheet within an appropriate load range. Note that a pass refers to a single pass of the sheet between a pair of work rolls to be rolled.
[0047] The total rolling reduction ratio of the cold rolling is preferably 85.0% or more and 95.0% or less, more preferably 87.0% or more and 93.0% or less. When the total rolling reduction ratio of the cold rolling is 85.0% or more and 95.0% or less, the strength of the aluminum alloy sheet is sufficiently obtained, the dislocation density is increased, the formation of subgrains after paint baking is promoted, and the number of subgrains can be set within the range specified in the present invention. As a result, the tab crack resistance tends to be improved.
[0048] In addition to keeping the total rolling reduction rate of the cold rolling within a predetermined range, it is preferable to keep the sheet passing interval between the final rolling pass and the rolling pass immediately preceding it within 0.33 seconds. By keeping the sheet passing interval within 0.33 seconds, dynamic recovery in the final rolling pass is further promoted, and the formation of subgrains is further promoted in the dislocation-dense region, so that more subgrains are formed than in the past during the next paint baking process. The sheet passing interval is preferably within 0.32 seconds, more preferably within 0.31 seconds.
[0049] The aluminum alloy sheet manufactured by the above process is subjected to a chemical conversion treatment using a surface treatment agent such as a chromate-based or zircon-based agent. Then, an organic paint containing an epoxy-based resin, a vinyl chloride-based agent, a polyester-based agent, etc. is applied to form a coating film. The formed coating film is then painted and baked at a PMT (metal temperature) of about 200°C to 290°C to produce a precoated aluminum alloy coated sheet for tabs. EXAMPLES
[0050] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0051] (Preparation of test materials) An aluminum alloy having the composition shown in Table 1 was cast by a semi-continuous casting method, and was subjected to facing and homogenization heat treatment by the methods shown as the first and second steps, and was hot rolled without cooling. The end temperature of the hot rolling was set to 300°C or more and 370°C or less as the coiling temperature. The obtained hot rolled sheet was then cold rolled under the conditions shown in Table 1 without intermediate annealing to obtain an aluminum alloy sheet as a cold rolled sheet having a sheet thickness of 0.25 mm. The balance of the composition shown in Table 1 is Al and unavoidable impurities. The cold rolling ratio is the total rolling ratio in cold rolling, and the sheet passing interval is the time required between the final rolling pass and the rolling pass immediately before it in cold rolling.
[0052] Next, the obtained aluminum alloy plate was subjected to a chemical conversion treatment, and then coated with an epoxy-based paint and baked in a continuous baking furnace at a PMT of 200° C. to 290° C. The baking temperature and baking time were the same for all of the manufacturing examples No. 1 to No. 3.
[0053] [Table 1]
[0054] The produced aluminum alloy coated sheets were used as test materials, and the number of subgrains, 0.2% proof stress, and tab cracking simulated load (tab cracking resistance) were measured by the following methods. The results are shown in Table 1.
[0055] Number of subgrains The structure of each test material was observed in a region 50 nm thick in both thickness directions from the center of the sheet thickness using a transmission electron microscope (TEM) at 50,000 times magnification from the normal direction of the rolled surface, and the number of subgrains was counted to calculate the number of subgrains.
[0056] Specifically, the test material was mechanically polished to a thickness of 0.05 mm (0.1 mm) from the center of the plate thickness in both thickness directions, and then a twin-jet electrolytic polishing method was used to make a thin film with a thickness of approximately 100 nm. This thin film was then examined with a transmission electron microscope at a magnification of 50,000 times and a magnification of 205 × 10 -12 m 2 The area was photographed. The number of subgrains measured within the field of view was summed up to calculate the number of subgrains. There is no particular upper limit on the number of subgrains, but the upper limit is usually around 400 to 600.
[0057] Measurement of 0.2% proof stress For each test material, a JIS-5 tensile test piece was prepared with the tensile direction parallel to the rolling direction, and a tensile test was performed according to the JIS Z2241 regulations. The plate thickness was calculated by subtracting the coating thickness, and the 0.2% yield strength was obtained. The appropriate range for 0.2% yield strength is 300 MPa or more, and within this range, even a thin-walled tab will satisfy the tab breaking strength. There is no particular upper limit for 0.2% yield strength, but considering the adverse effects on formability, the upper limit is usually around 390 MPa.
[0058] Tab tearing simulated load measurement A test piece shown in FIG. 3A was prepared from each test material, and a tear test simulating tab tearing was performed to obtain the tab tearing simulated load. As shown in FIG. 3B, the test piece was clamped at parts 26 and 27 in the tensile tester by one side of the chuck, and the part 28 was clamped and fixed by the other side of the chuck, and the tear test was performed at a tensile test chuck speed of 10 mm / min. The inner diameter of the holes in the test piece was 2.0 mm in both cases. In this tear test, the peak loads at which cracks occurred in the holes 31 and 32 of the test piece were measured as shown in FIG. 4. The test was performed eight times using test pieces prepared from the same test material, and the minimum measurement results of the two peak loads measured in each test were extracted and averaged to obtain the tab tearing simulated load. In addition, there are cases where the holes 31 and 32 tear simultaneously in the tear test, in which case the peak load obtained in one test is one and the peak load is also high. In the present invention, cases where only one peak load was obtained in the tear test were excluded from the test results. The appropriate range of the tab tearing simulated load was set to 65 N or more. If the tab tearing simulated load is 65 N or more, the can opening operation can be completed without causing tab tearing during the can opening operation, and the can has excellent tab tearing resistance.
[0059] As shown in Table 1, No. 1 to No. 3, in which the composition of the aluminum alloy coated sheet is within the range specified by the present invention, correspond to examples because the number of subgrains is within the range specified by the present invention. In all of No. 1 to No. 3, the sheet passing interval between the final pass of cold rolling and the pass immediately before is within 0.33 seconds, and the tab cracking simulated load (tab cracking resistance) also reaches the acceptable value. As shown in FIG. 5, the tab cracking simulated load and the sheet passing interval are approximately proportional to each other, and the slope of the linear approximation line indicates that the sheet passing interval at which the tab cracking simulated load is 65 N or more is expected to be about 0.33 seconds. As shown in FIG. 6, the tab cracking simulated load and the number of subgrains are approximately proportional to each other, and the slope of the linear approximation line indicates that the number of subgrains at which the tab cracking simulated load is 65 N or more is expected to be about 40 or more. [Explanation of symbols]
[0060] 1 Tab 2 Lid material 11 Rivet holes 14 Inner Lance 21 Rivet section 100 Dislocation-dense region 200 subgrains
Claims
1. An aluminum alloy plate comprising: Si: 0.05% by mass or more and 0.40% by mass or less; Fe: 0.05% by mass or more and 0.50% by mass or less; Cu: 0.01% by mass or more and 0.30% by mass or less; Mn: 0.1% by mass or more and 0.6% by mass or less; Mg: 4.0% by mass or more and 6.0% by mass or less; and the balance being Al and inevitable impurities; and a resin layer; When observing the structure of a region 50 nm thick in both thickness directions from the center of the sheet thickness in the normal direction of the rolled surface, the image taken by a 50,000-times transmission electron microscope shows a 205×10 -12 m 2 The coated aluminum alloy plate for tabs has a total of 50 or more subgrains in an area of 10 mm.
2. 2. The aluminum alloy coated sheet for tabs according to claim 1, wherein the total number of said subgrains in said region is 60 or more.
3. 3. The coated aluminum alloy sheet for tabs according to claim 1, wherein the aluminum alloy sheet has a Ti content of 0.1 mass % or less.
Citation Information
Patent Citations
Aluminum alloy sheet for tab, and method for manufacturing the same
JP2011225977A
Aluminum alloy sheet for can-top
JP2016079501A
Aluminum alloy sheet for can-top
JP2016079502A
Aluminum alloy sheet for can-top
JP2016079503A
Aluminum alloy sheet for can top
JP2017066430A