Negative electrode active material for lithium-ion secondary battery

A sintered powder of benzimidazole-amide copolymer with specific molar ratios addresses the limitations of existing nitrogen-doped carbon materials by providing enhanced discharge capacity, durability, and high-speed charging capabilities for lithium ion secondary batteries.

JP2024161718APending Publication Date: 2024-11-20JAPAN ADVANCED INST OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023076674
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20

Smart Images

  • Figure 2024161718000005
    Figure 2024161718000005
  • Figure 2024161718000006
    Figure 2024161718000006
  • Figure 2024161718000007
    Figure 2024161718000007
Patent Text Reader

Abstract

To provide a sintered powder for a negative electrode active material for a lithium-ion secondary battery, which has a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and also excellent high-speed charging properties, a method for manufacturing the same, a negative electrode active material for a lithium-ion secondary battery containing the sintered powder for the negative electrode active material for the lithium-ion secondary battery, a negative electrode containing the negative electrode active material for the lithium-ion secondary battery, and a lithium-ion secondary battery having the negative electrode.SOLUTION: A sintered powder is a sintered powder of a benzimidazole-amide copolymer having benzimidazole units and amide units, and the molar ratio of the benzimidazole units to the amide units (benzimidazole units / amide units) is 75 / 25 to 95 / 5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode active material for a lithium ion secondary battery. More specifically, the present invention relates to a negative electrode active material for a lithium ion secondary battery, a sintered powder for a negative electrode active material for a lithium ion secondary battery that can be suitably used for the negative electrode active material for the lithium ion secondary battery and a method for producing the same, a negative electrode containing the negative electrode active material for the lithium ion secondary battery, and a lithium ion secondary battery having the negative electrode. [Background technology]

[0002] Nitrogen-doped carbon is used as an electrochemical catalyst in reactions such as redox reactions and oxygen evolution reactions, a material for supercapacitors, etc. It is generally believed that the higher the nitrogen content in nitrogen-doped carbon, the higher the redox activity of the nitrogen-doped carbon (see, for example, paragraph

[0002] of Patent Document 1).

[0003] A method for producing nitrogen-containing carbon has been proposed, which includes the steps of using a sintering vessel made of quartz to sinter carbon in an atmosphere containing carbon dioxide gas, lowering the internal temperature of the sintering vessel to 100°C or lower, and replacing the internal atmosphere of the sintering vessel with an ammonia-containing gas atmosphere and sintering the carbon (see, for example, claim 1 of Patent Document 1).

[0004] However, since the nitrogen content in the nitrogen-containing carbon obtained by the above-mentioned method for producing nitrogen-containing carbon is about 1.5% by weight (for example, see paragraph

[0013] and FIG. 2 of Patent Document 1), the redox activity of the nitrogen-containing carbon cannot be said to be particularly high, and improvement in the discharge capacity is desired.

[0005] Nitrogen-doped carbon particles having a nitrogen atom content of 15 mass % or more have been proposed as nitrogen-doped carbon that has a large discharge capacity, excellent durability against charging and discharging, and excellent high-speed charging ability that allows charging in a short time (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-67487 A [Patent Document 2] Patent Publication No. 2022-40599 Summary of the Invention [Problem to be solved by the invention]

[0007] The negative electrode of a lithium ion secondary battery in which the nitrogen-doped carbon particles are used has a large discharge capacity, excellent durability against charging and discharging, and excellent high-speed charging ability, which allows charging in a short time. However, in recent years, there has been a demand for the development of a negative electrode active material for a lithium ion secondary battery that has a large initial discharge capacity and a large discharge capacity even after 500 charge and discharge cycles.

[0008] The present invention has been made in view of the above-mentioned conventional techniques, and has an object to provide a sintered powder for a negative electrode active material of a lithium ion secondary battery, which has a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and also excellent high-speed chargeability, and a method for producing the same, a negative electrode active material for a lithium ion secondary battery containing the sintered powder for a negative electrode active material of a lithium ion secondary battery, a negative electrode containing the negative electrode active material for a lithium ion secondary battery, and a lithium ion secondary battery having the negative electrode. [Means for solving the problem]

[0009] The present invention relates to (1) A sintered powder for use as a negative electrode active material of a lithium ion secondary battery, the sintered powder being a sintered powder of a benzimidazole-amide copolymer having benzimidazole units and amide units, the molar ratio of the benzimidazole units to the amide units (benzimidazole units / amide units) being 75 / 25 to 95 / 5. (2) A method for producing a sintered powder for a negative electrode active material of a lithium ion secondary battery according to the above (1), comprising sintering a benzimidazole-amide copolymer at a temperature of 750 to 1500° C.; (3) A negative electrode active material for a lithium ion secondary battery, comprising the sintered powder for a negative electrode active material for a lithium ion secondary battery according to (1) above. (4) A negative electrode containing the negative electrode active material for a lithium ion secondary battery according to (3) above, and (5) A lithium ion secondary battery having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, the negative electrode containing the negative electrode active material of the lithium ion secondary battery according to (4) above. Regarding. Effect of the Invention

[0010] According to the present invention, there are provided a sintered powder for a negative electrode active material of a lithium ion secondary battery, which has a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and also excellent high-speed chargeability, and a method for producing the same; a negative electrode active material for a lithium ion secondary battery containing the sintered powder for a negative electrode active material of a lithium ion secondary battery; a negative electrode containing the negative electrode active material of a lithium ion secondary battery; and a lithium ion secondary battery having the negative electrode. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is an X-ray diffraction diagram of the sintered powders for negative electrode active material obtained in Examples 1 to 3 and Comparative Examples 1 to 3. [Diagram 2] 1 is a graph showing Raman spectra of the sintered bodies for negative electrode active material obtained in Example 1 and Comparative Examples 1 to 3. [Diagram 3] 2 is a graph showing the results of investigating the cycle characteristics of the discharge capacity and the charge / discharge efficiency (Coulombic efficiency) of a coin battery produced using the sintered body for negative electrode active material obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] As described above, the sintered powder for use as a negative electrode active material for a lithium ion secondary battery of the present invention is a sintered powder of a benzimidazole-amide copolymer having benzimidazole units and amide units, and is characterized in that the molar ratio of the benzimidazole units to the amide units (benzimidazole units / amide units) is 75 / 25 to 95 / 5.

[0013] The sintered powder for negative electrode active material of the lithium ion secondary battery of the present invention is a sintered powder of a benzimidazole-amide copolymer having benzimidazole units and amide units, and since the molar ratio of the benzimidazole units to the amide units (benzimidazole units / amide units) is 75 / 25 to 95 / 5, the initial discharge capacity is large, durability against charge and discharge (cycle characteristics) is excellent, and further, high-speed charging properties that enable charging in a short time are excellent.

[0014] The sintered powder for use as a negative electrode active material for a lithium ion secondary battery of the present invention can be produced, for example, by sintering a benzimidazole-amide copolymer having a molar ratio of benzimidazole units to amide units (benzimidazole units / amide units) of 75 / 25 to 95 / 5 in a nitrogen gas atmosphere at a temperature of 750 to 1500°C.

[0015] [Benzimidazole-amide copolymer] As raw material monomers that provide the benzimidazole units of the benzimidazole-amide copolymer, 3,4-diaminobenzoic acid compounds and 4-aminobenzoic acid compounds can be used. Both 3,4-diaminobenzoic acid compounds and 4-aminobenzoic acid compounds can be prepared using glucose obtained by enzymatic hydrolysis of cellulose contained in plants as a raw material (see, for example, Ultrahigh Thermoresistant Lightweight Bioplastics Developed from Fermentation Products of Cellulosic Feedstock, Adv. Sus. Sys. 5(1), 2000193 (2021)).

[0016] Therefore, since the benzimidazole-amide copolymer used as the raw material of the sintered powder for the negative electrode active material of the lithium ion secondary battery of the present invention can be prepared by using cellulose contained in plants, the sintered powder for the negative electrode active material of the lithium ion secondary battery of the present invention has the advantage of being environmentally friendly.

[0017] The 3,4-diaminobenzoic acid compound is a compound that provides the benzimidazole unit of the benzimidazole-amide copolymer. Examples of the 3,4-diaminobenzoic acid compound include 3,4-diaminobenzoic acid and its salts.

[0018] The benzene ring of the 3,4-diaminobenzoic acid compound may have one or two substituents within the scope of the present invention. Examples of the substituents include an alkyl group having 1 to 8 carbon atoms, preferably 1 to 4 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, preferably 1 to 4 carbon atoms, a hydroxyl group, a carboxyl group, an amino group, a halogen atom such as a fluorine atom, a chlorine atom, or a bromine atom, but the present invention is not limited to these examples. Suitable 3,4-diaminobenzoic acid compounds include 3,4-diaminobenzoic acid and 3,4-diaminobenzoic acid dihydrochloride. 3,4-diaminobenzoic acid dihydrochloride can be easily prepared, for example, by reacting 3,4-diaminobenzoic acid with hydrochloric acid.

[0019] The 4-aminobenzoic acid compound is a compound that provides the amide unit of the benzimidazole-amide copolymer. Examples of the 4-aminobenzoic acid compound include 4-aminobenzoic acid and its salts.

[0020] The benzene ring of the 4-aminobenzoic acid compound may have one or two substituents within the scope of the present invention. Examples of the substituents include an alkyl group having 1 to 8 carbon atoms, preferably 1 to 4 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, preferably 1 to 4 carbon atoms, a hydroxyl group, a carboxyl group, an amino group, a halogen atom such as a fluorine atom, a chlorine atom, or a bromine atom, but the present invention is not limited to these examples. Suitable 4-aminobenzoic acid compounds include 4-aminobenzoic acid and 4-aminobenzoic acid hydrochloride. 4-aminobenzoic acid hydrochloride can be easily prepared, for example, by reacting 4-aminobenzoic acid with hydrochloric acid.

[0021] The molar ratio of the 3,4-diaminobenzoic acid compound to the 4-aminobenzoic acid compound [3,4-diaminobenzoic acid compound / 4-aminobenzoic acid compound] is 75 / 25 to 95 / 5, preferably 80 / 20 to 90 / 10, from the viewpoint of obtaining a negative electrode active material for a lithium ion secondary battery having a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and excellent high-speed chargeability that allows charging in a short time.

[0022] The benzimidazole-amide copolymer can be easily prepared, for example, by copolymerizing a 3,4-diaminobenzoic acid compound and a 4-aminobenzoic acid compound in the presence of polyphosphoric acid at a temperature of about 80 to 150°C until a sufficient amount of the benzimidazole-amide copolymer is produced.

[0023] Examples of the method for polymerizing a 3,4-diaminobenzoic acid compound and a 4-aminobenzoic acid compound include bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization, but the present invention is not limited to these examples. Among these polymerization methods, from the viewpoint of efficiently preparing a benzimidazole-amide copolymer with a small amount of impurities, bulk polymerization and solution polymerization are preferred, and solution polymerization is preferred because it is easy to operate when polymerizing a 3,4-diaminobenzoic acid compound and a 4-aminobenzoic acid compound.

[0024] When 3,4-diaminobenzoic acid compounds and 4-aminobenzoic acid compounds are copolymerized by solution polymerization, an organic solvent is used. The organic solvent is preferably an organic solvent that can dissolve 3,4-diaminobenzoic acid compounds and 4-aminobenzoic acid compounds at the polymerization reaction temperature and is poorly soluble or insoluble in the benzimidazole-amide copolymer produced. Examples of the organic solvent include aliphatic alcohols having 1 to 3 carbon atoms such as methanol, ethanol, and propanol, ketone compounds such as acetone and methyl ethyl ketone, ethyl acetate, tetrahydrofuran, dioxane, chloroform, dichloromethane, chlorobenzene, phenol, and cresol, but the present invention is not limited to these examples. These organic solvents may be used alone or in combination of two or more kinds. The amount of the organic solvent is not particularly limited as long as it is an amount that can efficiently polymerize the 3,4-diaminobenzoic acid compound and the 4-aminobenzoic acid compound, but is usually preferably about 3 to 20 times (mass) the total amount (mass) of the 3,4-diaminobenzoic acid compound and the 4-aminobenzoic acid compound, and more preferably about 5 to 15 times (mass).

[0025] When polymerizing a 3,4-diaminobenzoic acid compound and a 4-aminobenzoic acid compound, a heat stabilizer can be used in an appropriate amount. Examples of the heat stabilizer include phenylphosphonic acid (PPA), dimethyl phenylphosphonate, diethyl phenylphosphonate, and diphenylphosphonic acid, but the present invention is not limited to these examples.

[0026] The polymerization reaction temperature between the 3,4-diaminobenzoic acid compound and the 4-aminobenzoic acid compound is not particularly limited, but from the viewpoint of increasing the reaction efficiency, it is preferably about 120 to 220° C. The polymerization reaction temperature may be constant or may be increased stepwise.

[0027] The polymerization reaction time between the 3,4-diaminobenzoic acid compound and the 4-aminobenzoic acid compound cannot be generally determined because it varies depending on the polymerization reaction temperature, etc., but is usually about 10 to 40 hours. The atmosphere during the polymerization reaction between the 3,4-diaminobenzoic acid compound and the 4-aminobenzoic acid compound is preferably an inert gas such as nitrogen gas or argon gas, from the viewpoint of not being affected by oxygen contained in the air.

[0028] As described above, a benzimidazole-amide copolymer can be obtained by copolymerizing a 3,4-diaminobenzoic acid compound with a 4-aminobenzoic acid compound. When the 3,4-diaminobenzoic acid compound is prepared using cellulose contained in plants as a raw material for the 3,4-diaminobenzoic acid compound, the benzimidazole-amide copolymer is a bio-based polymer that is friendly to the global environment.

[0029] The resulting benzimidazole-amide copolymer may be washed, dried, and pulverized to a desired particle size, if necessary.

[0030] Suitable benzimidazole-amide copolymers include those having the formula (I):

[0031] [ka]

[0032] (In the formula, R 1 and R 2 each independently represents a hydrogen atom, an alkyl group, an alkoxy group, a hydroxyl group, a carboxyl group, an amino group, or a halogen atom. and a benzimidazole unit represented by formula (II):

[0033] [ka]

[0034] (In the formula, R 3and R 4 each independently represents a hydrogen atom, an alkyl group, an alkoxy group, a hydroxyl group, a carboxyl group, an amino group, or a halogen atom. and the molar ratio of the benzimidazole units to the amide units (amide units / benzimidazole units) is from 75 / 25 to 95 / 5.

[0035] In the benzimidazole unit of formula (I), R 1 and R 2 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxyl group, a carboxyl group, an amino group, or a halogen atom. 3 and R 4 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxyl group, a carboxyl group, an amino group or a halogen atom.

[0036] Of the alkyl groups, alkyl groups having 1 to 8 carbon atoms are preferred, and alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, and tert-butyl, are more preferred. Of the alkoxy groups, alkoxy groups having 1 to 8 carbon atoms are preferred, and alkoxy groups having 1 to 4 carbon atoms, such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, isobutoxy, and tert-butoxy, are more preferred. As the halogen atom, a fluorine atom, a chlorine atom, and a bromine atom are preferred, and a fluorine atom and a chlorine atom are more preferred.

[0037] R 1 ~R 4 are each preferably independently a hydrogen atom, an alkyl group or a halogen atom, and more preferably a hydrogen atom.

[0038] From the viewpoint of obtaining a negative electrode active material for a lithium ion secondary battery having a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and excellent high-speed chargeability that enables charging in a short time, the number average molecular weight of the benzimidazole-amide copolymer is preferably 2000 to 100,000, more preferably 3000 to 100,000 when it does not have a crosslinked structure, and is preferably 2000 to 1,000,000, more preferably 3000 to 1,000,000 when it has a crosslinked structure.

[0039] The number average molecular weight of the benzimidazole-amide copolymer is a value measured by gel permeation chromatography (GPC) under the following measurement conditions: However, when the benzimidazole-amide copolymer has a crosslinked structure, the benzimidazole-amide copolymer having the crosslinked structure is difficult to dissolve in a solvent, so that it may be difficult to measure the number average molecular weight of the benzimidazole-amide copolymer having the crosslinked structure by gel permeation chromatography (GPC).

[0040] [Measurement conditions] Equipment: Showa Denko Co., Ltd., product name: Shodex-101 Injection concentration: 0.01% by mass ·Injection volume: 100μL ·Flow rate: 1mL / min Solvent: N,N-dimethylformamide Column: Showa Denko K.K., product name: Shodex KD-803 and product name: Shodex KD-804 Column temperature: 40℃ Standard: Polymethylmethacrylate

[0041] The benzimidazole-amide copolymer may contain repeating units other than the benzimidazole unit and the amide unit as long as the object of the present invention is not impaired.

[0042] [Sintered powder for negative electrode active material of lithium ion secondary battery] The sintered powder for use as a negative electrode active material in a lithium ion secondary battery of the present invention can be obtained by sintering the benzimidazole-amide copolymer.

[0043] In addition, when the benzimidazole-amide copolymer is sintered, it is preferable to pulverize the copolymer in advance in order to increase the sintering efficiency of the benzimidazole-amide copolymer and to use the copolymer as a negative electrode active material. The particle size of the pulverized benzimidazole-amide copolymer is not particularly limited, but is preferably 1 mm or less, more preferably 500 μm or less, and even more preferably 300 μm or less, in order to increase the sintering efficiency of the benzimidazole-amide copolymer.

[0044] When the benzimidazole-amide copolymer is calcined, for example, an electric furnace can be used. The atmosphere when the benzimidazole-amide copolymer is calcined is not particularly limited, but from the viewpoint of avoiding the influence of oxygen contained in the air, it is preferable to use an inert gas atmosphere such as argon gas or nitrogen gas.

[0045] The heating rate when the benzimidazole-amide copolymer is baked is not particularly limited. The heating rate when the benzimidazole-amide copolymer is baked may be changed stepwise or may be kept constant. The baking temperature of the benzimidazole-amide copolymer is preferably 700 to 1200°C, more preferably 750 to 1100°C, and even more preferably 750 to 1000°C, from the viewpoint of obtaining a negative electrode active material for a lithium ion secondary battery having a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and excellent high-speed charging property that allows charging in a short time, and from the viewpoint of improving energy efficiency. The baking temperature of the benzimidazole-amide copolymer can be measured using a thermocouple.

[0046] The baking time of the benzimidazole-amide copolymer cannot be generally determined because it varies depending on the baking temperature of the benzimidazole-amide copolymer, but is usually about 1 to 6 hours. After baking the benzimidazole-amide copolymer, the baked benzimidazole-amide copolymer is allowed to cool to preferably 60° C. or less, more preferably 40° C. or less, and even more preferably room temperature.

[0047] By calcining the benzimidazole-amide copolymer as described above, a calcined powder for use as a negative electrode active material for a lithium ion secondary battery can be obtained. If the calcined powder for use as a negative electrode active material for a lithium ion secondary battery obtained is aggregated, the calcined powder for use as a negative electrode active material for a lithium ion secondary battery may be crushed, if necessary, using a pin mill, a hammer mill, or the like.

[0048] The spacing of the crystal planes of the sintered powder for the negative electrode active material of the lithium ion secondary battery of the present invention can be examined by powder X-ray diffraction. It has been confirmed in the following examples that the spacing of the crystal planes of the sintered powder for the negative electrode active material of the lithium ion secondary battery of the present invention is 3.8 Å, which is wider than the spacing of the crystal planes (d-spacing) of graphite (3.3 Å) when the molar ratio of benzimidazole units to amide units is 85 / 15.

[0049] The average particle diameter of the sintered powder for the negative electrode active material of the lithium ion secondary battery when observed with a transmission electron microscope is usually within the range of 50 nm to 10 μm. The average particle diameter of the sintered powder for the negative electrode active material of the lithium ion secondary battery means a value obtained by arbitrarily selecting 100 sintered powders for the negative electrode active material of the lithium ion secondary battery from an image taken with a scanning electron microscope, calculating the average value of the maximum length and the minimum length of the sintered powder for the negative electrode active material of each lithium ion secondary battery, summing up the average values ​​for the 100 sintered powders for the negative electrode active material of the lithium ion secondary battery, and dividing the total value by 100.

[0050] [Negative electrode active material for lithium ion secondary battery] The negative electrode active material of the lithium ion secondary battery of the present invention contains the sintered powder for the negative electrode active material of the lithium ion secondary battery. Since the negative electrode active material of the lithium ion secondary battery of the present invention contains the sintered powder for the negative electrode active material of the lithium ion secondary battery, the use of the negative electrode active material makes it possible to obtain a lithium ion secondary battery that has a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and also excellent high-speed chargeability.

[0051] The negative electrode active material of the lithium ion secondary battery of the present invention may be composed of only the sintered powder for the negative electrode active material of the lithium ion secondary battery, or may contain other negative electrode active materials within the scope of the present invention. Examples of other negative electrode active materials include powders of carbon materials such as graphite, graphite, and coke, but the present invention is not limited to only these examples.

[0052] [Lithium-ion secondary battery] The lithium ion secondary battery of the present invention has a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and a negative electrode containing the negative electrode active material of the lithium ion secondary battery of the present invention is used as the negative electrode.

[0053] The lithium ion secondary battery of the present invention uses a negative electrode containing the negative electrode active material of the lithium ion secondary battery of the present invention as the negative electrode, and therefore has a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and also excellent high-speed chargeability.

[0054] The basic structure of the lithium ion secondary battery of the present invention is similar to that of commonly used lithium secondary ion batteries.

[0055] The lithium ion secondary battery of the present invention usually has a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte. The shape of the lithium ion secondary battery may be, for example, a cylindrical type or a laminated type, but the present invention is not limited to these examples.

[0056] When the lithium ion secondary battery of the present invention is, for example, a CR2025 lithium ion secondary battery, the negative electrode, the separator, and the non-aqueous electrolyte are housed in a case. In the following, an embodiment in which the lithium ion secondary battery is a CR2025 lithium ion secondary battery will be described, but the present invention is not limited to only this embodiment.

[0057] The case used in the CR2025 lithium-ion secondary battery is hollow, has an opening, and also serves as a positive electrode container. A lid is provided at the opening of the case, and the lid also serves as a negative electrode lid. A gasket is provided between the case and the lid to maintain an insulating and sealed state between the case and the lid. An electrode and a non-aqueous electrolyte are accommodated in the space between the case and the lid.

[0058] (1) Electrode The electrodes include a positive electrode, a separator, and a negative electrode, arranged in that order. The positive electrode is in contact with the inner surface of the case, and the negative electrode is in contact with the inner surface of the lid.

[0059] The positive electrode may be the same as a positive electrode used in a commonly used lithium secondary ion battery, and the present invention is not limited by the composition and structure of the positive electrode.

[0060] The positive electrode can be produced, for example, by mixing a positive electrode active material, a conductive material, and a binder in a predetermined ratio, adding a solvent, and optionally activated carbon, a viscosity adjusting additive, and the like, to the resulting mixture, kneading the resulting mixture to prepare a positive electrode composite paste, applying the paste to the surface of a current collector, and optionally press-molding and drying the paste.

[0061] Representative examples of the positive electrode active material include lithium, lithium-manganese composite oxide, and lithium-nickel-cobalt-aluminum composite oxide, but the present invention is not limited to these examples. Examples of the conductive material include carbon black such as acetylene black, natural graphite, artificial graphite, and expanded graphite, but the present invention is not limited to these examples. Examples of the binder include polyvinylidene fluoride (PVDF), 1-methyl-2-pyrrolidone (NMP), polytetrafluoroethylene (PTFE), fluororubber, and ethylene propylene diene rubber, but the present invention is not limited to these examples. Examples of the solvent include N-methyl-2-pyrrolidone, but the present invention is not limited to these examples.

[0062] The negative electrode is made of the negative electrode active material of the present invention. The negative electrode can be produced, for example, by mixing the negative electrode active material of the present invention with a binder, adding a solvent to the resulting mixture to prepare a paste-like negative electrode mixture, applying the negative electrode mixture to the surface of a metal foil current collector such as copper foil, drying, and, if necessary, press-molding and drying.

[0063] The negative electrode active material is the negative electrode active material of the lithium ion secondary battery of the present invention, but as described above, powders such as graphite and carbon black may be included as necessary. Examples of binders include polyvinylidene fluoride (PVDF), 1-methyl-2-pyrrolidone (NMP), polytetrafluoroethylene (PTFE), fluororubber, and ethylene propylene diene rubber, but the present invention is not limited to these examples. Examples of solvents include N-methyl-2-pyrrolidone, but the present invention is not limited to these examples.

[0064] The separator is used between the positive electrode and the negative electrode. The separator separates the positive electrode and the negative electrode, holds the electrolyte, and forms a path for lithium ions to move between the positive electrode and the negative electrode. The separator can be a foil film of a polyolefin resin such as polyethylene or polypropylene, and the thin film has many micropores formed therein.

[0065] (2) Nonaqueous electrolyte Examples of non-aqueous electrolytes include cyclic carbonates such as ethylene carbonate (EC), diethylene carbonate (DEC), propylene carbonate, butylene carbonate, and trifluoropropylene carbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; and ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane, but the present invention is not limited to these examples. These non-aqueous electrolytes may be used alone, or two or more of them may be used in combination, such as a combination of ethylene carbonate (EC) and diethylene carbonate (DEC).

[0066] As described above, the lithium ion secondary battery of the present invention uses a negative electrode containing the negative electrode active material of the lithium ion secondary battery of the present invention as the negative electrode active material, and therefore has a large initial discharge capacity, excellent durability against charge and discharge (cycle characteristics), and also has excellent high-speed chargeability, which enables charging in a short period of time. EXAMPLES

[0067] Next, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0068] The physical properties measured in the following examples were measured according to the following methods. [X-ray powder diffraction] Powder X-ray diffraction was performed using a powder / thin film X-ray diffractometer (Rigaku Corporation, product name: SmartLab) with CuKα radiation having a wavelength (λ) of 0.154 nm in the measurement range (2θ) of 10 to 80°.

[0069] [Raman Spectroscopic Analysis] Raman spectroscopic analysis was performed using a Raman spectrometer (Renishaw Ltd., microscopic laser Raman spectrometer, light source: HeNe).

[0070] [X-ray photoelectron spectroscopy (XPS)] X-ray photoelectron spectroscopy was performed using an X-ray photoelectron spectrometer (manufactured by Fison Instruments, product name: S-PROBE™ 2803).

[0071] [Cycle characteristics] The cycle characteristics of the coin batteries were investigated using an automatic battery evaluation device (manufactured by Electrofield Co., Ltd., product number: ABE1024-05RI) and a battery cycler (manufactured by Biologic Co., Ltd., product number: BCS) as the charge / discharge device, adjusting the potential range to 0.1 to 2.1 V (vs. Li / Li+) and at a constant current of 1 C.

[0072] Preparation Example 1 [Preparation of 3,4-diaminobenzoic acid dihydrochloride] 3.0 g (19.72 mmol) of 3,4-diaminobenzoic acid was placed in a 100 mL beaker at room temperature, 30 mL of methanol was added to the beaker, and the contents of the beaker were stirred for about 1 hour to obtain a suspension. 12 N hydrochloric acid was added dropwise to the suspension obtained above while stirring until the 3,4-diaminobenzoic acid contained in the suspension was completely dissolved, and after the color of the suspension changed from pink to dark red, the suspension was further stirred at room temperature for 4 hours to obtain a reaction solution.

[0073] The reaction solution obtained above was filtered through a Buchner funnel to remove unreacted precipitate, and the filtrate was collected.

[0074] The solvent (methanol) was removed from the filtrate obtained above using a rotary evaporator to recover a solid content, which was then dried under reduced pressure for 5 to 6 hours to obtain 5.4 g of 3,4-diaminobenzoic acid dihydrochloride (yield: 94%).

[0075] Preparation Example 2 [Preparation of 4-aminobenzoic acid hydrochloride] 3.0 g (21.88 mmol) of 4-aminobenzoic acid was placed in a beaker at room temperature, 30 mL of methanol was added to the beaker, and the contents of the beaker were stirred for about 1 hour to obtain a suspension. 12 N hydrochloric acid was added dropwise to the suspension obtained above while stirring until the 4-aminobenzoic acid contained in the suspension was completely dissolved, and after the color of the suspension changed from pink to dark red, the suspension was stirred at room temperature for 4 hours to obtain a reaction solution.

[0076] The reaction solution obtained above was filtered through a Buchner funnel to remove unreacted precipitate, and the filtrate was collected.

[0077] The solvent (methanol) was removed from the filtrate obtained above using a rotary evaporator to recover a solid content, which was then dried under reduced pressure for 5 to 6 hours to obtain 3.2 g of 4-aminobenzoic acid hydrochloride (yield: 94%).

[0078] Example 1 (1) Preparation of benzimidazole-amide copolymer powder Into a 100 mL three-necked round-bottom flask, 30 g of polyphosphoric acid was added with stirring while introducing nitrogen gas, and the polyphosphoric acid was heated at 120° C. for 1 hour to remove moisture from the polyphosphoric acid.

[0079] Next, while introducing nitrogen gas into the flask, 1.887 g (8.5 mmol) of 3,4-diaminobenzoic acid dihydrochloride obtained above and 0.237 g (1.5 mmol) of 4-aminobenzoic acid hydrochloride were added to the flask [molar ratio of 3,4-diaminobenzoic acid dihydrochloride to 4-aminobenzoic hydrochloride: 85 / 15], and the mixture was stirred at a temperature of 120°C for 1 hour. After that, the temperature of the contents of the flask was raised to 160°C and heated for 4 hours, and then heated at 220°C for 16 hours, thereby obtaining a benzimidazole-amide copolymer.

[0080] The benzimidazole-amide copolymer obtained above was added to 200 mL of distilled water in a beaker at room temperature and left for about 24 hours to dissolve the remaining unreacted 3,4-diaminobenzoic acid dihydrochloride in water, thereby purifying the benzimidazole-amide copolymer. The number average molecular weight of the benzimidazole-amide copolymer obtained above was 34,000.

[0081] Next, the benzimidazole-amide copolymer was removed from the beaker, placed in a dryer, and dried for about 4 hours under reduced pressure at a temperature of 100° C. The dried benzimidazole-amide copolymer was pulverized for 20 minutes at a rotation speed of 1430 rpm in a pulverizer (manufactured by Japan Analytical Industry Co., Ltd., product number: JF-300) to obtain a powder of the benzimidazole-amide copolymer.

[0082] The benzimidazole-amide copolymer powder obtained above was added to a 10% potassium hydroxide aqueous solution at room temperature, and after stirring for about 12 hours, the benzimidazole-amide copolymer powder was thoroughly washed with deionized water.The benzimidazole-amide copolymer powder was then filtered through a fluororesin (polytetrafluoroethylene) filter membrane with a pore size of 0.1 μm, and the resulting residue was placed in a dryer and dried at a temperature of 100° C. for about 12 hours to obtain a purified benzimidazole-amide copolymer powder.

[0083] (2) Preparation of sintered powder for negative electrode active material About 100 mg of the benzimidazole-amide copolymer obtained above was placed in a silica-alumina boat, which was then placed in a furnace core tube of a tubular electric furnace having a ceramic furnace core tube equipped with an inert gas replacement unit. Nitrogen gas was introduced into the furnace core tube at a flow rate of 100 mL / min for 20 minutes to create a nitrogen gas atmosphere inside the furnace core tube.

[0084] The powder of the benzimidazole-amide copolymer was heated in a nitrogen gas atmosphere from room temperature to 200°C at a heating rate of 10°C / min, and maintained at 200°C for 20 minutes to remove moisture and the like contained in the powder of the benzimidazole-amide copolymer. Subsequently, while flowing nitrogen gas into the furnace tube, the benzimidazole-amide copolymer was heated from 200°C to 800°C at a heating rate of 10°C / min, and heated at 800°C for 60 minutes, and then the obtained sintered body of the benzimidazole-amide copolymer was allowed to cool to room temperature to obtain a sintered body for negative electrode active material (yield: 95%). The sintered body for negative electrode active material obtained above was washed with 1M hydrochloric acid at room temperature for about 30 minutes, washed with pure water, and then dried.

[0085] Since the sintered body for the negative electrode active material obtained above was agglomerated, the sintered body for the negative electrode active material was pulverized using an agate mortar and pestle to obtain a powder of the sintered body for the negative electrode active material.

[0086] Example 2 A benzimidazole-amide copolymer (number average molecular weight: 35,000) was prepared in the same manner as in Example 1, except that the molar ratio of 3,4-diaminobenzoic acid dihydrochloride and 4-aminobenzoic hydrochloride in Example 1 was changed to 90 / 10, and a sintered powder for negative electrode active material was obtained.

[0087] Example 3 A benzimidazole-amide copolymer (number average molecular weight: 33,000) was prepared in the same manner as in Example 1, except that the molar ratio of 3,4-diaminobenzoic acid dihydrochloride and 4-aminobenzoic hydrochloride in Example 1 was changed to 80 / 20, and a sintered powder for negative electrode active material was obtained.

[0088] Comparative Example 1 A sintered powder for a negative electrode active material was obtained in the same manner as in Example 1, except that the molar ratio of 3,4-diaminobenzoic acid dihydrochloride and 4-aminobenzoic hydrochloride in Example 1 was changed to 50 / 50.

[0089] Comparative Example 2 A sintered powder for a negative electrode active material was obtained in the same manner as in Example 1, except that 4-aminobenzoic hydrochloride was not used.

[0090] Comparative Example 3 A sintered powder for a negative electrode active material was obtained in the same manner as in Example 1, except that the molar ratio of 3,4-diaminobenzoic acid dihydrochloride and 4-aminobenzoic hydrochloride in Example 1 was changed to 70 / 30.

[0091] Comparative Example 4 As a conventional negative electrode active material, graphite powder was used.

[0092] [X-ray powder diffraction] 1 shows powder X-ray diffraction patterns of the sintered powder for negative electrode active material obtained in Examples 1 to 3 and Comparative Examples 1 to 3. In FIG. 1, (a) is an X-ray diffraction pattern of the sintered powder for negative electrode active material obtained in Comparative Example 2, (b) is an X-ray diffraction pattern of the sintered powder for negative electrode active material obtained in Example 1, (c) is an X-ray diffraction pattern of the sintered powder for negative electrode active material obtained in Comparative Example 3, (d) is an X-ray diffraction pattern of the sintered powder for negative electrode active material obtained in Comparative Example 1, (e) is an X-ray diffraction pattern of the sintered powder for negative electrode active material obtained in Example 2, and (f) is an X-ray diffraction pattern of the sintered powder for negative electrode active material obtained in Example 3.

[0093] From the results shown in Figure 1, the Miller indices of the sintered powder for negative electrode active material obtained in each Example are (002), and the broad peak indicates that amorphous carbon is produced. nλ=2dsinθ (In the formula, n is a positive integer, λ is the wavelength of the X-ray, d is the spacing between the crystal planes, and θ is the angle between the crystal planes and the X-ray.) The crystal plane spacing (d-spacing) of the sintered powder for negative electrode active material obtained based on the above was 3.80 Å in Example 1, 3.74 Å in Example 2, 3.63 Å in Example 3, 3.74 Å in Comparative Examples 1 and 3, 3.60 Å in Comparative Example 2, and 3.30 Å in Comparative Example 4.

[0094] From the above results, it can be seen that the spacing between the crystal planes of the sintered powder for negative electrode active material obtained in Example 1 is larger than those of the sintered powder for negative electrode active material obtained in each Comparative Example and the graphite powder of Comparative Example 4. Therefore, the sintered powder for negative electrode active material obtained in Example 1 has more active sites for lithium ion absorption than the sintered powder for negative electrode active material obtained in each Comparative Example and the graphite powder of Comparative Example 4, and is therefore superior in lithium ion diffusibility and absorption properties.

[0095] [Raman Spectroscopic Analysis] Raman spectroscopy was performed on the sintered powders for negative electrode active material obtained in Example 1 and Comparative Examples 1 to 3. The results are shown in Fig. 2. In Fig. 2, (a) to (d) are graphs showing the Raman spectra of the sintered powders for negative electrode active material obtained in Comparative Example 2, Example 1, Comparative Example 3, and Comparative Example 1, respectively.

[0096] As shown in FIG. 2(b), the sintered powder for the negative electrode active material obtained in Example 1 had a wave number of about 1350 cm -1 The D band is located in the region with a wavenumber of approximately 1570 cm -1 It can be seen that the G band exists in this region.

[0097] In addition, the negative electrode active material sintered powder obtained in Example 1 was D / I G The ratio (corresponding to Id / Ig in FIG. 2) was 1.06, and the I D / I GSince the ratio is larger than the above, the introduction rate of structural defects in the sintered powder for negative electrode active material obtained in Example 1 is higher than that in the sintered powder for negative electrode active material obtained in each comparative example, and therefore it is considered that the sintered powder for negative electrode active material obtained in Example 1 has excellent diffusibility of lithium ions.

[0098] In addition, the graphite powder I of Comparative Example 4 D / I G Since the ratio was 0.18, the graphite powder is considered to have extremely few structural defects.

[0099] [X-ray photoelectron spectroscopy (XPS)] X-ray photoelectron spectroscopy (XPS) was performed on the sintered powders for negative electrode active material obtained in Example 1 and Comparative Examples 1 to 3. As a result, the content of nitrogen atoms in the sintered powders for negative electrode active material was 11.2 atom% in Example 1, 10.5 atom% in Example 2, 10.6 atom% in Example 3, 8.0 atom% in Comparative Example 1, 14.8 atom% in Comparative Example 2, and 9.9 atom% in Comparative Example 3.

[0100] The results of X-ray photoelectron spectroscopy analysis of the sintered powder for negative electrode active material show that the nitrogen atom content in the sintered powder for negative electrode active material increases in proportion to the amide unit content in the benzimidazole-amide copolymer used as the raw material for the sintered powder for negative electrode active material.

[0101] In addition, the results of X-ray photoelectron spectroscopy (XPS) of the sintered powders for negative electrode active material obtained in Examples 1 to 3 confirmed that the nitrogen atom content in the sintered powders for negative electrode active material obtained in each Example was in the range of 10 to 12 atom %.

[0102] [Cycle characteristics] 80 g of any one of the sintered powders for negative electrode active material obtained in Examples 1 to 3 and Comparative Examples 1 to 3, 10 g of acetylene black, 10 g of polyvinylidene fluoride as a binder, and 400 g of N-methyl-2-pyrrolidone were mixed to a uniform composition, and the resulting slurry was applied to a copper foil (length: 20 mm, width: 100 mm, thickness: 20 μm) with a doctor blade, dried at a temperature of 80° C. under reduced pressure for about 12 hours, and pressed with a roll to produce an electrode with a coating thickness of 0.06 mm after drying.

[0103] In order to incorporate the electrode obtained above into a CR2025 lithium ion secondary battery, it was punched out to a disk with a diameter of 15 mm, and the disk obtained above was used as the negative electrode, lithium foil was used as the counter electrode, a polypropylene separator (manufactured by Asahi Kasei Corporation, product name: Celgard 2500, thickness: 25 μm) was used as the separator, and an electrolyte obtained by dissolving LiPF6 to a concentration of 1 M in a solvent mixed with ethylene carbonate and diethylene carbonate in a 1:1 mass ratio was used as the electrolyte, and an anode half cell was assembled in an argon gas atmosphere. The obtained anode half cell was left at room temperature for 12 hours for stabilization.

[0104] The negative electrode half cell obtained above was repeatedly charged and discharged at a current density of 3.7 A / g during charging, and the discharge capacity and capacity retention rate of the negative electrode half cell were examined at room temperature using a secondary battery charge / discharge tester (Hokuto Denko Corporation, product number: HJ-SD8). The results are shown in Table 1.

[0105] The capacity retention rate is calculated using the formula: [Capacity maintenance rate (%)] = ([Discharge capacity after a given number of cycles] ÷ [Initial discharge capacity]) × 100 The initial discharge capacity is the discharge capacity when the discharge capacity starts to stabilize after the start of charging and discharging.

[0106] [Table 1]

[0107] From the results shown in Table 1, it can be seen that the initial discharge capacity when the sintered powder for negative electrode active material obtained in each Example was used was 100 mAh / g or more, which is significantly higher than the initial discharge capacity (52 to 93 mAh / g) when the sintered powder for negative electrode active material obtained in each Comparative Example was used. In addition, it can be seen that the sintered powder for negative electrode active material obtained in each Example has excellent long-term cycle characteristics, since the capacity retention rate after 1000 cycles is 80% or more.

[0108] [Full cell performance] The negative electrode was prepared in the same manner as described in the "Cycle Characteristics" section. A positive electrode (active material: lithium-nickel-cobalt-aluminum composite oxide) manufactured by Biotrek Co., Ltd. was used as the positive electrode, which was punched out to have a disk with a diameter of 15 mm for incorporation into a CR2025 lithium-ion secondary battery. The negative electrode and positive electrode were each set to a current of 0.065 mA / cm 2 All the batteries were used after 10 cycles of charging and discharging at a current density of 1000 mAh.

[0109] A coin battery (full battery) was assembled in a glove box filled with argon gas using the negative electrode, the positive electrode, a 1M LiPF6 non-aqueous electrolyte (volume ratio of ethylene carbonate:diethylene carbonate = 1:1) solution as an electrolyte, and a polypropylene separator having a thickness of 25 μm as a separator. The obtained coin battery was left at room temperature for 12 hours for stabilization.

[0110] The coin battery obtained above was charged at 2.6 to 4.2 V, then discharged, for a total of 58 cycles, and the discharge capacity and charge / discharge efficiency (Coulomb efficiency) were examined. The results are shown in Figure 3(a). The coin battery obtained above was also charged at a potential of 4.2 V using a constant current / constant voltage charging (CCCV) method, and then discharged, for a total of 120 cycles, and the discharge capacity and charge / discharge efficiency (Coulomb efficiency) were examined. The results are shown in Figure 3(b).

[0111] 3, (a) is a graph showing the relationship between the number of charge / discharge cycles and the discharge capacity and charge / discharge efficiency (Coulomb efficiency) when the C rate is changed in the charge / discharge cycle of the entire battery, and (b) is a graph showing the relationship between the number of charge / discharge cycles and the discharge capacity and charge / discharge efficiency (Coulomb efficiency) at a constant rate of 0.1 C. In FIG. 3, the symbol A is a graph showing the discharge capacity, and the symbol B is a graph showing the charge / discharge efficiency (Coulomb efficiency).

[0112] From the results shown in FIG. 3(a), it can be seen that the whole battery using the sintered powder for negative electrode active material obtained in Example 2 exhibits very good rate characteristics, and the discharge capacity does not decrease significantly even when the rate of the whole battery is increased.

[0113] In addition, from the results shown in FIG. 3(b), all the batteries using the sintered powder for negative electrode active material obtained in Example 2 had a capacity retention rate of about 94% and a capacity of about 0.8 mAh even after 110 cycles of charge and discharge at a potential of 4.2 V using a constant current / constant voltage charging (CCCV) method, indicating excellent battery performance.

[0114] [Fast charging performance] A negative electrode half cell was prepared in the same manner as above using any one of the negative electrode active material sintered powders obtained in Examples 1 to 3 as the negative electrode active material sintered powder, and the current density during charging of the cell was adjusted to 4000mA / g, and the cell was charged and discharged 1000 times, after which the discharge capacity, charge and discharge efficiency (Coulomb efficiency), and time required for charging (charging time) were examined. The results are shown in Table 2.

[0115] [Table 2]

[0116] From the results shown in Table 2, it can be seen that the negative electrode half-cells using the sintered powder for negative electrode active material obtained in each Example have a high discharge capacity of 60 to 120 mAh / g even after repeated charging and discharging, and the charge and discharge efficiency (Coulombic efficiency) is almost constant at about 100%, so that the quality is stable. It can also be seen that the durability against charge and discharge (cycle characteristics) is significantly superior to that of conventional negative electrodes using carbon as the electrolyte, which have a high durability of 500 cycles at most.

[0117] Furthermore, the negative electrode half-cells using the sintered powders for negative electrode active material obtained in each Example can be charged in a very short time of about 2 minutes or less, which shows that they have outstanding high-speed charging properties.

[0118] Therefore, since the lithium ion secondary battery of the present invention has a large discharge capacity, excellent durability against charging and discharging, and high-speed charging ability, it is believed that it will contribute to the rapid charging of EVs in short periods of time at places such as service areas on highways. [Industrial Applicability]

[0119] The sintered powder for negative electrode active material of a lithium ion secondary battery of the present invention, the negative electrode active material of a lithium ion secondary battery containing the sintered powder for negative electrode active material of a lithium ion secondary battery, and a lithium ion secondary battery having a negative electrode containing the negative electrode active material of a lithium ion secondary battery have large discharge capacities, excellent durability against charging and discharging, and excellent high-speed charging properties that enable charging in a short period of time, and are therefore expected to be used in, for example, smartphones, tablet personal computers, hybrid automobiles, electric automobiles, and the like.

Claims

1. The sintered powder for use as a negative electrode active material for a lithium ion secondary battery is characterized in that the sintered powder is a sintered powder of a benzimidazole-amide copolymer having benzimidazole units and amide units, and the molar ratio of the benzimidazole units to the amide units (benzimidazole units / amide units) is 75 / 25 to 95 / 5.

2. A method for producing a sintered powder for a negative electrode active material of a lithium ion secondary battery according to claim 1, characterized in that the benzimidazole-amide copolymer is sintered at a temperature of 750 to 1500°C.

3. A negative electrode active material for a lithium ion secondary battery, comprising the sintered powder for a negative electrode active material for a lithium ion secondary battery according to claim 1 .

4. A negative electrode of a lithium ion secondary battery comprising the negative electrode active material according to claim 3.

5. A lithium ion secondary battery having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, the negative electrode being an anode containing the anode active material of the lithium ion secondary battery according to claim 4.

Citation Information

Patent Citations

  • Method of producing nitrogen-containing carbon

    JP2015067487A

  • Negative-electrode active material for lithium-ion secondary battery

    JP2022040599A