Thermal conductor and joint
The thermal conductor with a flexible joint and solder layer addresses thermal stress issues by enhancing adhesion and conductivity, ensuring effective heat dissipation in electronic devices.
Patent Information
- Application Number
- JP2023076987
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-21
AI Technical Summary
Existing thermal conductors experience peeling and insufficient adhesion due to thermal stress caused by differences in the coefficient of thermal expansion between joined members, leading to inadequate thermal conductivity.
A thermal conductor comprising a flexible material in the joint part and a solder layer that connects multiple thermal conductive parts, allowing for flexibility and adhesion to absorb thermal stress, ensuring excellent thermal conductivity.
The solution effectively alleviates thermal stress and enhances substantial thermal conductivity by absorbing the difference in thermal expansion, preventing peeling and maintaining strong adhesion between members.
Smart Images

Figure 2024161928000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermal conductor and a joint. [Background technology]
[0002] In recent years, there has been an urgent need for heat dissipation measures for heat-generating components such as electronic devices, vehicle headlights, and on-board batteries. For example, the amount of heat generated by electronic components such as central processing units of computers, image processing processors, SoCs in smartphones, DSPs and microcomputers in embedded devices, and semiconductor elements such as transistors, laser diodes, light-emitting diodes, electroluminescent devices, and liquid crystal light-emitting bodies has been decreasing in size and becoming more highly integrated. The heat generated by these electronic components has caused problems such as shortened life spans and malfunctions of devices and systems, and the demand for heat dissipation measures for electronic components is increasing year by year.
[0003] For example, Patent Document 1 discloses a semiconductor device equipped with a ceramic circuit board, which includes a ceramic board, a metal circuit plate bonded to one surface of the ceramic board and electrically connected to the semiconductor board, and a metal heat sink bonded to the other surface of the ceramic board, as a heat dissipation measure for the semiconductor board, which is a heat generating component. In this semiconductor device, heat from the semiconductor board arranged on one surface of the ceramic board is conducted to the metal heat sink, which is a heat dissipation component, and dissipated from the metal heat sink.
[0004] However, in such a structure, due to the difference in the thermal expansion coefficients of the parts being joined, thermal stress occurs at the joint, and peeling occurs at the interface, making it impossible to ensure sufficient adhesion, and it is not possible to achieve sufficient actual thermal conductivity between the heat-generating part and the heat-dissipating part. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-72281 A Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a thermal conductor capable of alleviating thermal stress caused by the difference in the thermal expansion coefficients of members joined to both sides and having excellent substantial thermal conductivity, and to provide a bonded body capable of alleviating thermal stress caused by the difference in the thermal expansion coefficients of members joined to both sides of the thermal conductor and having excellent substantial thermal conductivity. [Means for solving the problem]
[0007] The thermal conductor of the present invention is a thermal conductor including a thermal conductor body having a plurality of thermal conductive parts and a joint part including a flexible material that joins the plurality of thermal conductive parts, a solder layer covering at least a portion of an outer surface of the thermal conductor body; Of the two surfaces aligned in the thickness direction of the thermal conductor body, one surface is joined to a first member via the solder layer, and the other surface is joined to a second member via the solder layer.
[0008] The joint of the present invention includes a heat conductor body having a plurality of heat conductive parts and a joint portion including a flexible material that joins the plurality of heat conductive parts; and a first member joined to the heat conductor body via a solder layer on one of two surfaces aligned in the thickness direction of the heat conductor body. Effect of the Invention
[0009] According to the present invention, it is possible to provide a thermal conductor having excellent substantial thermal conductivity, which is capable of alleviating thermal stress caused by the difference in thermal expansion coefficients of members bonded to both sides of the thermal conductor, and it is possible to provide a bonded body having excellent substantial thermal conductivity, which is capable of alleviating thermal stress caused by the difference in thermal expansion coefficients of members bonded to both sides of the thermal conductor. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic example of a thermal conductor of the present invention. [Diagram 2] FIG. 2 is a perspective view showing a schematic example of a thermal conductor body. [Diagram 3] 4 is an enlarged cross-sectional view showing a schematic view of a laminated heat conductive portion and a bonding portion. FIG. [Figure 4] FIG. 2 is a plan view showing a schematic example of a heat conducting portion constituting a heat conductor main body. [Diagram 5] FIG. 2 is a schematic partially exploded perspective view showing a plurality of laminated heat conductive parts in an exploded state. [Figure 6] FIG. 2 is a conceptual diagram of an example of a cured product of a curable resin material that constitutes a joint. [Figure 7] FIG. 11 is a perspective view showing a schematic diagram of another example of a thermal conductor body. [Figure 8] FIG. 8 is a vertical cross-sectional view of the thermal conductor body shown in FIG. [Figure 9] 1 is an electron microscope photograph showing a thermal conductor with a portion of the solder layer penetrating into the thermal conductor body. [Figure 10] FIG. 1 is a cross-sectional view illustrating a schematic example of a bonded body of the present invention. [Figure 11] 1 is an electron microscope photograph showing a joint in which a portion of the solder layer penetrates into the thermal conductor body. [Figure 12] FIG. 2 is a perspective view illustrating a schematic diagram of another example of the bonded body of the present invention. [Figure 13] FIG. 1 is a cross-sectional view illustrating an example of an electronic device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Preferred embodiments of the present invention will now be described in detail. [1] Thermal conductor First, the thermal conductor of the present invention will be described. FIG. 1 is a cross-sectional view showing an example of the thermal conductor of the present invention. FIG. 2 is a perspective view showing an example of the thermal conductor body. FIG. 3 is a cross-sectional view showing an enlarged view of the laminated thermal conductive parts and the joint part. FIG. 4 is a plan view showing an example of the thermal conductive part constituting the thermal conductor body. FIG. 5 is a partially exploded perspective view showing a schematic exploded view of a plurality of laminated thermal conductive parts. FIG. 6 is a conceptual diagram of an example of a cured product of the curable resin material constituting the joint part. Note that the resin fibers 22 are not shown in FIG. 3.
[0012] In the drawings referred to in this specification, some parts may be shown in a reduced or enlarged form to make the relationship between the members easier to understand, and the size ratio between the members shown in the drawings does not represent the actual size ratio between the members. In this specification, the term "natural state" refers to a state in which no external force other than gravity is applied, and in particular, refers to a state in which no external force other than gravity has been applied within 24 hours. In addition, it is preferable that the thermal conductor has no history of being subjected to stress of 0.1 MPa or more after its manufacture. In addition, the measurements and treatments described in this specification are performed at 20°C unless otherwise specified. In addition, the measured values described in this specification are obtained by measurement in air at 1 atmosphere unless otherwise specified.
[0013] In this specification, the term "thermal expansion coefficient" refers to the "linear expansion coefficient" which indicates the rate at which length changes in response to an increase in temperature.
[0014] The thermal conductor 1 has a thermal conductor body 2 having a plurality of thermal conductive portions 10 and a joining portion 20 including a flexible material that joins the plurality of thermal conductive portions 10, and a solder layer 3 covering at least a portion of the outer surface of the thermal conductor body 2.
[0015] The thermal conductor 1 is joined to a first member 110 via a solder layer 3 at one of the two faces aligned in the thickness direction of the thermal conductor body 2, the first face 23, and joined to a second member 120 via a solder layer 3 at the other face, the second face 24.
[0016] In the thermal conductor 1 and thermal conductor body 2 shown in Figures 1 and 2, the two surfaces aligned in the thickness direction of the thermal conductor body 2 are, in other words, a pair of opposing surfaces, one surface (first surface 23) being the top surface and the other surface (second surface 24) being the bottom surface.
[0017] In the example shown in Figure 10, which will be described later, the thermal conductor 1 is joined to a first member 110 on its top surface (first surface 23) via a solder layer 3, and is joined to a second member 120 on its bottom surface (second surface 24) via a solder layer 3.
[0018] In the following description, the first member 110 and the second member 120 may be collectively referred to as "member joined to the thermal conductor 1", "member joined to the thermal conductor 1", or simply "members".
[0019] The thermal conductor 1 has a joint 20 including a flexible material, and a solder layer 3 having ductility and flexibility that is joined to the first member 110 and the second member 120. This gives the thermal conductor 1 flexibility as a whole, and excellent adhesion to the members to be joined and ability to follow the expansion and contraction of the members due to temperature changes. In other words, the thermal conductor 1 itself deforms to absorb and alleviate thermal stress caused by the difference in thermal expansion coefficient between the first member 110 and the second member 120 that are joined to both sides of the thermal conductor 1 via the solder layer 3. In other words, the thermal conductor 1 functions as a buffer material that exerts a buffering effect.
[0020] This makes it possible to prevent separation at the bonding interfaces between the thermal conductor 1 and the first and second members 110 and 120, and to maintain sufficient adhesion.
[0021] Furthermore, since the thermal conductor 1 is flexible, the adhesion between the thermal conductor 1 and the first member 110 and the second member 120 joined to the thermal conductor 1 can be excellent, and the actual thermal conductivity between the thermal conductor 1 and the first member 110 and the second member 120 can be excellent.
[0022] Furthermore, since the thermal conductor 1 is not only in contact with the first member 110 and the second member 120 but is also joined thereto, good adhesion can be ensured without applying surface pressure, and the substantial thermal conductivity between the first member 110 and the second member 120 and the thermal conductor 1 can be improved. Furthermore, even if at least one of the first member 110 and the second member 120 is a member to which it is difficult to apply surface pressure, the thermal conductor 1 can be applied.
[0023] [1-1] Thermal conductor body The heat conductor body 2 has a plurality of heat conductive parts 10 and joint parts 20 including a flexible material that join the plurality of heat conductive parts 10. In other words, the heat conductor body 2 is a composite laminate having a plurality of heat conductive parts 10 and the joint parts 20.
[0024] This makes it possible to improve the flexibility of the thermal conductor 1 as a whole, the adhesion between the first member 110 and the second member 120 to be joined, and the ability of the first member 110 and the second member 120 to follow the expansion and contraction due to temperature changes, and makes it possible to improve the actual thermal conductivity between the first member 110 and the second member 120 and the thermal conductor 1.
[0025] The thermal conductor body 2 may have at least one joint 20, but in the example shown in FIG. 2, it has a plurality of thermal conductive parts 10 and a plurality of joints 20, with thermal conductive parts 10 arranged at both ends in the stacking direction.
[0026] Such a heat conductor body 2 can be suitably manufactured, for example, by winding a heat conductive part forming sheet (heat conductive part forming member) used for forming the heat conductive part 10, which has a joint forming composition applied to at least one surface thereof, around the peripheral surface of a winding roll, thereby forming an alternating layer structure of the heat conductive parts 10 and the joints 20.
[0027] In this specification, the stacking direction of the thermal conductive portion 10 and the joint portion 20 in the thermal conductor body 2 is defined as the stacking direction of the thermal conductor body 2, and the in-plane direction of the sheet for forming the thermal conductive portion is defined as the in-plane direction of the thermal conductive portion 10. For example, in the configuration shown in Fig. 2, the left-right direction is the stacking direction of the thermal conductor body 2, and the vertical depth direction is the in-plane direction of the thermal conductive portion 10.
[0028] In this specification, the extending direction of the heat conducting part 10 in the plane of the upper surface of the heat conductor body 2 is defined as the extending direction of the heat conducting part 10. For example, in the configuration shown in Fig. 2, the extending direction of the heat conducting part 10 is the depth direction in the plane of the upper surface of the heat conductor body 2.
[0029] With the above-mentioned configuration, the thermal conductor body 2 has anisotropic thermal conductivity. Since the thermal conductor body 2 has anisotropic thermal conductivity, the thermal conductor body 2 can transmit heat more efficiently in a predetermined direction. In addition, unintended heat conduction can be prevented.
[0030] In the thermal conductor body 2 having the configuration shown in Figure 2, it is preferable that the thermal conductivity in a pair of surfaces to which the first member 110 and the second member 120 are respectively joined in the thermal conductor 1, in other words, a first direction vertically connecting the top surface (first surface 23) and the bottom surface (second surface 24), is higher than the thermal conductivity in a specified in-plane direction of the pair of surfaces. This makes the above-mentioned effects more pronounced.
[0031] In this specification, "perpendicular" does not mean "perpendicular" in the strict mathematical sense, but allows for a slight deviation.
[0032] 2, which is the lamination direction of the heat conductive portion 10 and the bonding portion 20. In addition, the "predetermined direction in the in-plane direction of the pair of surfaces" is, for example, the X direction shown in FIG.
[0033] The thermal conductor body 2 also has anisotropic thermal conductivity on the upper surface (first surface 23). That is, in the upper surface (first surface 23) of the thermal conductor body 2, the thermal conductivity in the stacking direction of the thermal conductive portion 10 and the joint portion 20 is lower than the thermal conductivity in the extending direction of the thermal conductive portion 10. The same is true for the lower surface (second surface 24) of the thermal conductor body 2.
[0034] As described later, by controlling the extension direction of the heat conducting portions 10 and the joint portions 20 and the stacking direction of the heat conducting portions 10 and the joint portions 20 of the heat conductor body 2, it is possible to impart anisotropy to the thermal conductivity of the heat conductor body 2.
[0035] The shape of the thermal conductor body 2 is not particularly limited, but is preferably set appropriately according to the shapes of the members to be joined with the thermal conductor 1, in other words, the first member 110 and the second member 120. This makes the above-mentioned effects more pronounced.
[0036] The shape of the thermal conductor body 2 in plan view, or the cross-sectional shape of the thermal conductor body 2, may be, for example, a circle, an ellipse, a polygon, or a combination of these. The vertical cross-sectional shape of the thermal conductor body 2 may be, for example, a shape having a constant width in a first direction, or a shape having a portion whose width changes in the first direction.
[0037] When the thermal conductor body 2 has a polygonal shape, such as a rectangular cross-sectional shape, in a plan view, the length of the longest side of the rectangle is preferably 0.3 mm or more and 200 mm or less.
[0038] This ensures a sufficient bonding area between the thermal conductor 1 and the members (first member 110, second member 120) bonded to the thermal conductor 1, thereby making the aforementioned effects more pronounced.
[0039] Specifically, for example, the thermal conductor body 2 preferably has a rectangular shape larger than 5 mm×5 mm when viewed from above. This makes it possible to exhibit the above-mentioned effects more significantly.
[0040] The size of the thermal conductor body 2 may or may not be constant in the first direction. When the thermal conductor body 2 has a portion with a different size in the first direction, it is preferable that the value of one side of the thermal conductor body 2 at the portion where the length of one side is maximum is within the above range.
[0041] For example, in the illustrated configuration, the shape and size of the thermal conductor body 2 are constant in the first direction. Specifically, the thermal conductor body 2 is in the shape of a quadrangular prism. This allows the thermal conductivity of the thermal conductor body 2 in the first direction to be kept constant, and the above-mentioned effects are more prominently exhibited.
[0042] The length of the thermal conductor body 2 in its natural state in the first direction, ie, the length indicated by T in FIG. 2, is preferably 0.3 mm or more and 10 mm or less, and more preferably 0.3 mm or more and 3.0 mm or less.
[0043] This can provide particularly excellent substantial thermal conductivity between the thermal conductor 1 and a member joined to the thermal conductor 1. This can provide excellent heat dissipation properties, for example, when the member joined to the thermal conductor 1 is a heat generating body.
[0044] In the following description, the case where the thermal conductor body 2 has a rectangular prism shape will be mainly described. In addition, in the figures referred to in this specification, the interface between the heat conductive portion 10 and the joint portion 20 is clearly shown, but the interface between the heat conductive portion 10 and the joint portion 20 may be unclear, for example, because a part of the heat conductive portion 10 penetrates into the joint portion 20.
[0045] [1-1-1] Heat transfer part The plurality of heat conducting portions 10 are portions which mainly contribute to the thermal conductivity of the entire heat conductor body 2, particularly the thermal conductivity in the in-plane direction of the heat conducting portions 10.
[0046] It is preferable that at least a portion of the multiple heat conducting portions 10 are provided continuously inside the heat conductor body 2, particularly in a first direction perpendicularly connecting a pair of faces, and are exposed to two different faces of the heat conductor body 2, particularly two different faces where the heat conductor 1 is joined to other members.
[0047] This makes it possible to improve the substantial thermal conductivity in the first direction.
[0048] In particular, the thermal conductor body 2 of the illustrated configuration has at least one pair of parallel surfaces, and at least a portion of the multiple thermal conductive portions 10 are penetrating thermal conductive portions that are continuously provided inside the thermal conductor body 2 and exposed on two surfaces.
[0049] This allows for more optimal adhesion between the thermal conductor 1 and the member to be joined to the thermal conductor 1, and improves the actual thermal conductivity between the two parallel surfaces, in other words, between a pair of faces.
[0050] In this specification, "parallel" does not mean "parallel" in the strict mathematical sense, but allows for a slight deviation.
[0051] The thermal conductive portion 10 is not particularly limited as long as it has thermal conductivity. Examples of materials constituting the thermal conductive portion 10 include ceramic materials such as aluminum nitride, boron nitride, silicon nitride, silicon carbide, and alumina; carbon materials such as graphite and carbon fiber; and metal materials such as copper and aluminum. It is preferable for the thermal conductive portion 10 to contain a carbon material, and it is more preferable for the thermal conductive portion 10 to contain graphite.
[0052] This makes it possible to suppress the manufacturing cost of the thermal conductor 1 while improving the substantial thermal conductivity between the thermal conductor 1 and the member to be joined to the thermal conductor 1. Furthermore, since there is a space between the graphite particles in a part of the space, a solder layer 3 is formed in the space, and when the solder layer 3 is melted to bond the member to the thermal conductor body 2, the adhesion is improved via the solder layer 3. Furthermore, the anchor effect is more prominent due to the solder layer 3 penetrating into the voids 4 present in the joint 20.
[0053] [1-1-1-1] Carbon materials In particular, when the heat conductive part 10 is formed from a heat conductive part forming sheet containing a carbon material such as graphite or carbon fiber, the following effects can be obtained in addition to the effects described above. That is, the flexibility and flexibility of the heat conductor body 2 can be improved, and, for example, the restoring force when the heat conductor body 2 is bent, the cushioning properties due to internal voids, and the improvement of adhesion due to moderate deformation when the heat conductor 1 is joined to a member to be joined can be improved. In particular, such effects are more prominent when graphite is used as the carbon material.
[0054] As the graphite constituting the heat conductive portion 10, it is preferable to use flake graphite. By using flake graphite, the flake graphite can be preferably oriented in the in-plane direction of the heat conductive part 10 by a method to be described later, and the heat conductive part 10 can have particularly excellent thermal conductivity in the in-plane direction. In addition, by using flake graphite, voids 4 as described later can be preferably provided in portions of the heat conductive part 10 other than the hole portions 11 to be described later, particularly in portions near the center of the heat conductive part 10 in the thickness direction, which is the normal direction to the in-plane direction of the heat conductive part 10, and the effects to be described later can be obtained.
[0055] [1-1-1-2] Ceramic materials Furthermore, when the heat conducting portion 10 contains a ceramic material, the substantial thermal conductivity between the heat conductor 1 and the member joined to the heat conductor 1 can be improved while the dust generation of the heat conductor main body 2 can be reduced.
[0056] [1-1-1-3] Metal material Furthermore, when the heat conductive part 10 is formed from a heat conductive part forming sheet containing a metal material, the following effects can be obtained in addition to the effects described above. That is, the dust generation of the heat conductor body 2 can be reduced due to the strength of the bonding force inside the metal material. Furthermore, even if a relatively large load is applied to the heat conductor 1, irreversible deformation of the heat conductor 1, such as collapse of the heat conductor body 2 due to buckling, can be more effectively prevented.
[0057] Examples of the metal material constituting the heat conductive part 10 include various simple metals and alloys, and one or more selected from these may be used in combination. More specifically, examples of the metal material constituting the heat conductive part 10 include those containing one or more selected from the group consisting of Al, Cu, Ag, Au, Mg, and Zn, and preferably those containing Al. This can provide the heat conductive portion 10 with even better thermal conductivity.
[0058] An example of an alloy containing the metal elements constituting the above group is duralumin, which is an aluminum alloy containing Al, Cu, and Mg.
[0059] The heat conductive portion 10 is preferably made of substantially a single component. This can further improve the thermal conductivity of the thermal conductive portion 10. Generally, this is also advantageous in terms of reducing the manufacturing costs of the thermal conductor 1.
[0060] The phrase "consisting substantially of a single component" means that the ratio of the main component in the target area is 95% by weight or more, preferably 97% by weight or more, and more preferably 99% by weight or more.
[0061] However, if the thermally conductive portion 10 contains a gas such as air, the amount of said gas contained therein is to be ignored. Also, if the thermally conductive portion 10 contains a metal material, an oxide film of the metal constituting the thermally conductive portion 10, such as a passivation film, may be formed on the surface. Even when such an oxide film is formed, the thermally conductive portion 10 is treated as being "consisting substantially of a single component."
[0062] The thermal conductivity of the heat conductive portion 10 in an in-plane direction at 20° C. is preferably 7 W / (m·K) or more and 2500 W / (m·K) or less, and more preferably 20 W / (m·K) or more and 1800 W / (m·K) or less.
[0063] The thermal conductivity value can be determined by measurement using a non-steady hot wire method based on the laser flash method.
[0064] t in Figure 2 10 The thickness of the heat conductive portion 10 in the stacking direction indicated by is preferably 5 μm or more and 500 μm or less, more preferably 20 μm or more and 150 μm or less, and further preferably 40 μm or more and 120 μm or less.
[0065] This makes it possible to ensure that the proportion of the heat conducting portion 10 in the heat conductor body 2 is sufficiently high, while also making it easier to improve the flexibility of the heat conductor body 2 as a whole, thereby more reliably achieving the aforementioned effects more significantly.
[0066] Here, the thickness of the heat conductive portion 10 refers to the thickness at a portion where the hole portion 11 described below is not provided.
[0067] The thickness values shown in this specification may be calculated by taking the average value of thickness measurements at 10 points randomly selected for the target component.
[0068] As shown in FIG. 3, each of the heat conductive portions 10 constituting the heat conductor body 2 may be provided with a recess in the thickness direction.
[0069] This can improve the bonding strength between the heat conductive portion 10 and the bonding portion 20 .
[0070] In particular, in each heat conductive portion 10 shown in FIG. 3, the recess is a hole 11 penetrating the heat conductive portion 10 in the thickness direction. This makes the above-mentioned effects more pronounced.
[0071] In the following description, the case where the recess is a hole will be mainly described. The number of holes (recesses) 11 provided in each heat conductive portion 10 may be only one depending on the size of the heat conductive portion 10 in the in-plane direction, but is preferably multiple. This makes the above-mentioned effects even more pronounced.
[0072] When multiple holes 11 are provided in a single heat conductive portion 10, the distance between adjacent holes 11 in the in-plane direction of the heat conductive portion 10 is preferably 300 μm or more and 3000 μm or less, and more preferably 500 μm or more and 2000 μm or less. This makes the above-mentioned effects more pronounced.
[0073] In this specification, the "interval between holes 11" refers to the distance between the centers of adjacent holes 11.
[0074] In the configuration shown in FIG. 4, the multiple holes 11 provided in the single heat conductive portion 10 are arranged in a staggered pattern, but the arrangement pattern of the multiple holes 11 in the in-plane direction of the single heat conductive portion 10 is not limited to this and may be any pattern, for example, may be arranged randomly.
[0075] A flexible material 21 fills at least a part of the recess (hole) 11. In particular, since the recess is a hole and the flexible material 21 penetrates into the hole, the bond between the heat conducting portion 10 and the joint portion 20 can be made stronger, and the shape conformity to the surface shape of the member to be joined to the heat conductor 1, such as a heat generating member or a heat dissipating member, and the durability of the heat conductor 1 can be improved.
[0076] As shown in FIG. 5, when the heat conductive portion 10 is observed from the stacking direction with the joint portion 20, it is preferable that the plurality of heat conductive portions 10 have holes 11 that do not overlap each other.
[0077] When overlapping holes 11 exist in a plurality of heat conductive parts 10, the flexible material 21 of the joint part 20 that penetrates the overlapping holes 11 becomes pierced like a skewer that penetrates the plurality of heat conductive parts 10. In such a case, the flexible material 21 may slip through the hole 11, and the joint between the heat conductive parts 10 may become insufficient.
[0078] In contrast, when the heat conductive portions 10 are observed from the stacking direction with the joint portions 20, the presence of non-overlapping holes 11 in the multiple heat conductive portions 10 prevents the flexible material 21 of the joint portions 20 that has penetrated into the holes 11 from slipping through, making the joints between the heat conductive portions 10 stronger.
[0079] In FIG. 5, only the heat conductive portion 10 is shown, and the bonding portion 20 is omitted.
[0080] The shape of the hole 11 is not particularly limited, and examples of the shape of the hole 11 when the heat conductive part 10 is viewed in a plane and the cross-sectional shape of the hole 11 in the heat conductive part 10 include a circle, an ellipse, a polygon, etc. In addition, the vertical cross-sectional shape of the heat conductive part 10 may be, for example, a shape having a constant width in the depth direction of the hole 11, or a shape having a portion whose width changes in the depth direction of the hole 11.
[0081] When the shape of the hole 11 when the heat conductive portion 10 is viewed in a plane, that is, the cross-sectional shape of the hole 11 in the heat conductive portion 10 is circular, the diameter of the hole 11 is preferably 20 μm or more and 300 μm or less, and more preferably 30 μm or more and 200 μm or less. This makes the above-mentioned effects more pronounced.
[0082] The size (diameter) of the pores 11 may or may not be constant in the thickness direction of the thermally conductive section 10. When the thermally conductive section 10 has portions with different sizes (diameters) of the pores 11 in the thickness direction, it is preferable that the diameter value at the portion where the diameter of the pores 11 is maximum is within the above range.
[0083] The proportion of the heat conductive portion 10 in the heat conductor body 2 (the solid portion excluding the voids 4) is preferably 15 volume % or more and 80 volume % or less, and more preferably 20 volume % or more and 70 volume % or less. This makes the above-mentioned effects more pronounced.
[0084] The proportion of the thermal conductive portion 10 in the thermal conductor body 2 (but the solid portion excluding the void portion 4) is preferably 35% or more and 95% or less, and more preferably 45% or more and 87% or less, in terms of area ratio in the cross section in the stacking direction of the thermal conductor body 2. This makes the above-mentioned effects more pronounced.
[0085] Furthermore, for example, when the thermally conductive portion 10 contains a material with excellent electrical conductivity, the electrical conductivity of the thermal conductor 1 can be improved. Therefore, for example, when an electrode is to be drawn from an electronic component electrically via the thermal conductor 1, the electrode can be drawn more efficiently by using a relatively high proportion of the thermally conductive portion 10.
[0086] [1-1-2]Joint part The joint portion 20 is disposed between two adjacent heat conductive portions 10 to join the heat conductive portions 10 together, and includes a flexible material 21.
[0087] The inclusion of the flexible material 21 in the joint 20 improves the adhesion between the thermal conductor 1 and the member to be joined and the ability to follow the expansion and contraction of the member due to temperature changes. The thermal conductor body 2 also improves shape conformity to the surface shape of the member to be joined to the thermal conductor 1. The inclusion of the flexible material 21 in the joint 20 also makes it possible to suitably prevent the thermal conductor body 2 from being damaged when the thermal conductor body 2 is deformed.
[0088] [1-1-2-1] Flexible material The flexible material 21 constituting the joint 20 has flexibility and has the function of joining two adjacent heat conductive parts 10 together.
[0089] The compressive elastic modulus of flexible material 21 is preferably 0.5 MPa or more and 3.0 MPa or less, more preferably 0.8 MPa or more and 2.5 MPa or less, and even more preferably 0.9 MPa or more and 1.8 MPa or less.
[0090] The compressive elastic modulus value of the flexible material 21 can be determined by carrying out a measurement at 20° C. in accordance with JIS K7181.
[0091] More specifically, the compressive elastic modulus can be calculated from the slope of 10 to 20 N at a measurement speed of 20% compression / min using an autograph (manufactured by Shimadzu Corporation).
[0092] The flexible material 21 constituting the joint 20 may be, for example, a resin material.
[0093] Examples of the resin material that is the flexible material 21 include flexible epoxy resin, rubber-based resin, urethane-based resin, silicone-based resin, fluorine-based resin, acrylic-based resin, thermoplastic elastomer, etc., but it is preferable that the flexible material 21 includes a polyrotaxane 50 having a cyclic molecule 51, a first polymer 52 having a linear molecular structure and encapsulating the cyclic molecule 51 in a skewered shape, and blocking groups 53 provided near both ends of the first polymer 52, and a second polymer 60, as shown in Figure 6, and the polyrotaxane 50 and the second polymer 60 are bonded via the cyclic molecule 51.
[0094] This improves the adhesion between the thermal conductor 1 and the member to be joined, and the ability to follow the expansion and contraction of the member due to temperature changes. Also, the joining strength between the thermal conductive portion 10 and the joining portion 20 in the thermal conductor body 2 can be improved, and the durability of the thermal conductor body 2 can be improved. Also, the flexibility, heat resistance, etc. of the thermal conductor body 2 can be particularly improved.
[0095] In particular, when a stress in the direction of the arrow is applied to the cured product of the curable resin material as the flexible material 21 in the state shown in FIG. 6(A), the flexible material 21 can take the form shown in FIG. 6(B). That is, in the flexible material 21, the cyclic molecules 51 can move along the first polymer 52, that is, the first polymer 52 can move within the cyclic molecules 51, so that the stress of deformation can be efficiently absorbed in the flexible material 21. Therefore, even if a large external force such as a twisting force is applied, the joint 20 is effectively prevented from being destroyed, and the joint between the heat conductive parts 10 is effectively prevented from being destroyed. In addition, the adhesion between the heat conductor 1 and the member to be joined and the ability to follow the expansion and contraction of the member due to temperature changes are further improved.
[0096] The flexible material 21 including the polyrotaxane 50 and the second polymer 60 will be described in detail below.
[0097] The cyclic molecule 51 constituting the polyrotaxane 50 may be any molecule capable of moving along the first polymer 52, but is preferably a cyclodextrin molecule which may be substituted, and it is particularly preferable that the cyclodextrin molecule is selected from the group consisting of α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, and derivatives thereof.
[0098] At least a portion of the cyclic molecules 51 in the polyrotaxane 50 is bonded to at least a portion of the second polymer 60 as described above.
[0099] Examples of the functional group (functional group bonded to the second polymer 60) possessed by the cyclic molecule 51 include, for example, an -OH group, an -NH2 group, an -COOH group, an epoxy group, a vinyl group, a thiol group, and a photocrosslinking group. Examples of the photocrosslinking group include cinnamic acid, coumarin, chalcone, anthracene, styrylpyridine, styrylpyridinium salt, and styrylquinolium salt.
[0100] When the maximum amount of cyclic molecules 51 included when the cyclic molecules 51 are included in the first polymer 52 in a skewered manner is taken as 1, the amount of the cyclic molecules 51 included in the first polymer 52 in a skewered manner is preferably 0.001 to 0.6, more preferably 0.05 to 0.4. Two or more different types of cyclic molecules 51 may be used.
[0101] Examples of the first polymer 52 constituting the polyrotaxane 50 include cellulose-based resins such as polyvinyl alcohol, polyvinylpyrrolidone, poly(meth)acrylic acid, carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; polyacrylamide, polyethylene oxide, polyethylene glycol, polypropylene glycol, polyvinyl acetal-based resins, polyvinyl methyl ether, polyamine, polyethyleneimine, casein, gelatin, starch, and / or copolymers thereof; polyolefin-based resins such as polyethylene, polypropylene, and copolymer resins with other olefin-based monomers; polyester resins; polyvinyl chloride resins; polystyrene-based resins such as polystyrene and acrylonitrile-styrene copolymer resins; polymethyl methacrylate resins; Examples of the polyimide resin include acrylic resins such as acrylates, (meth)acrylic acid ester copolymers, acrylonitrile-methyl acrylate copolymer resins, polycarbonate resins, polyurethane resins, vinyl chloride-vinyl acetate copolymer resins, polyvinyl butyral resins, and derivatives or modified products thereof, polyisobutylene, polytetrahydrofuran, polyaniline, acrylonitrile-butadiene-styrene copolymers, polyamides such as nylon, polyimides, polyisoprene, polybutadiene, and other polysiloxanes, polydimethylsiloxane, and other polysulfones, polyimines, polyacetic anhydrides, polyureas, polysulfides, polyphosphazenes, polyketones, polyphenylenes, polyhaloolefins, and derivatives thereof, and polyethylene glycol is particularly preferred.
[0102] The weight average molecular weight of the first polymer 52 is preferably at least 10,000, and more preferably at least 35,000. Two or more different types of first polymers 52 may be used.
[0103] A preferred combination of the cyclic molecule 51 and the first polymer 52 is one in which the cyclic molecule 51 is an optionally substituted α-cyclodextrin, and the first polymer 52 is polyethylene glycol.
[0104] The blocking group 53 constituting the polyrotaxane 50 is not particularly limited as long as it is a group having the function of preventing the cyclic molecule 51 from detaching from the first polymer 52, and examples thereof include dinitrophenyl groups, cyclodextrins, adamantane groups, trityl groups, fluoresceins, pyrenes, substituted benzenes, optionally substituted polynuclear aromatics, steroids, and the like.
[0105] Substituents constituting the substituted benzenes and substituted polynuclear aromatics include alkyl, alkyloxy, hydroxy, halogen, cyano, sulfonyl, carboxyl, amino, phenyl, etc. One or more substituents may be present. Two or more different blocking groups 53 may be used.
[0106] In the flexible material 21, at least a portion of the polyrotaxane 50 is bonded to the second polymer 60 via the cyclic molecule 51, but the flexible material 21 may contain polyrotaxane 50 that is not bonded to the second polymer 60, or the polyrotaxanes 50 may be bonded to each other.
[0107] The second polymer 60 is bonded to the polyrotaxane 50 via the cyclic molecule 51. Examples of the functional group that the second polymer 60 has and that bonds to the cyclic molecule 51 include an -OH group, an -NH2 group, an -COOH group, an epoxy group, a vinyl group, a thiol group, and a photocrosslinking group. Examples of the photocrosslinking group include cinnamic acid, coumarin, chalcone, anthracene, styrylpyridine, styrylpyridinium salt, and styrylquinolium salt.
[0108] Examples of the second polymer 60 include cellulose-based resins such as polyvinyl alcohol, polyvinylpyrrolidone, poly(meth)acrylic acid, carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; polyacrylamide, polyethylene oxide, polyethylene glycol, polypropylene glycol, polyvinyl acetal-based resins, polyvinyl methyl ether, polyamine, polyethyleneimine, casein, gelatin, starch, and / or copolymers thereof; polyolefin-based resins such as polyethylene, polypropylene, and copolymer resins with other olefin-based monomers; polyester resins, polyvinyl chloride resins, polystyrene-based resins such as polystyrene and acrylonitrile-styrene copolymer resins; polymethyl methacrylate, Examples of the resin include those having a skeleton of various resins such as acrylic resins such as (meth)acrylic acid ester copolymers and acrylonitrile-methyl acrylate copolymer resins, polycarbonate resins, polyurethane resins, vinyl chloride-vinyl acetate copolymer resins, polyvinyl butyral resins, and derivatives or modified products thereof, polyisobutylene, polytetrahydrofuran, polyaniline, acrylonitrile-butadiene-styrene copolymers, polyamides such as nylon, polyimides, polyisoprene, polybutadiene, polysiloxanes such as polydimethylsiloxane, polysulfones, polyimines, polyacetic anhydrides, polyureas, polysulfides, polyphosphazenes, polyketones, polyphenylenes, and polyhaloolefins, and having the functional groups described above.
[0109] The second polymer 60 and the cyclic molecule 51 may be chemically bonded to each other by a crosslinking agent.
[0110] The molecular weight of the crosslinking agent is preferably less than 2000, and more preferably less than 400.
[0111] Examples of the crosslinking agent include cyanuric chloride, trimesoyl chloride, terephthaloyl chloride, epichlorohydrin, dibromobenzene, glutaraldehyde, phenylene diisocyanate, trilein diisocyanate, divinyl sulfone, 1,1'-carbonyldiimidazole, alkoxysilanes, etc. Two or more different crosslinking agents may be used.
[0112] The second polymer 60 may be a homopolymer or a copolymer. In the flexible material 21, at least a part of the second polymer 60 is bonded to the polyrotaxane 50 via the cyclic molecule 51, but the flexible material 21 may contain a second polymer 60 that is not bonded to the polyrotaxane 50, or the second polymers 60 may be bonded to each other. Two or more different types of second polymers 60 may be used.
[0113] The ratio of the content of the polyrotaxane 50 to the content of the second polymer 60 in the flexible material 21 is preferably 1 / 1000 or more in terms of weight ratio.
[0114] The content of the flexible material 21 (particularly the above-mentioned resin material) in the joint 20 is preferably 5 volume % or more and 90 volume % or less, and more preferably 25 volume % or more and 75 volume % or less.
[0115] This improves the bonding strength of the heat conductive section 10 by the joint 20, and when the joint 20 contains the resin fibers 22, the content of the resin fibers 22 in the joint 20 can be sufficiently ensured, and the effect of including the resin fibers 22 can be fully exerted.
[0116] [1-1-2-2] Resin fiber The joint 20 may include resin fibers 22 in addition to the flexible material 21 as described above.
[0117] This effectively prevents the thermal conductor 1 from sagging and deforming even when the thermal conductor 1 is used for a long period of time, and effectively prevents problems such as a decrease in adhesion between the thermal conductor 1 and the member to which it is joined, resulting in increased thermal resistance and electrical resistance.
[0118] The thickness of the resin fibers 22 contained in the joint 20 is preferably 1.0 μm or more and 30 μm or less, more preferably 2.0 μm or more and 25 μm or less, even more preferably 3.0 μm or more and 20 μm or less, and most preferably 4.0 μm or more and 15 μm or less. This makes the above-mentioned effects more pronounced.
[0119] The resin fibers 22 may be any fiber that mainly contains a resin material. Examples of the resin material constituting the resin fibers 22 include polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyamides, ethylene vinyl acetate resins, polyvinyl alcohol, etc., but it is preferable that the resin fibers 22 are made of polyester, and it is more preferable that the resin fibers 22 are made of polyethylene terephthalate.
[0120] This makes it possible to improve the strength of the resin fibers 22 themselves, and to more effectively exert the effect of including the resin fibers 22 in the joint 20 as described above. It also makes it possible to improve the adhesion between the resin fibers 22 and the resin material as the flexible material 21, thereby improving the durability and reliability of the thermal conductor 1.
[0121] It is sufficient that at least one resin fiber 22 is contained in the joint 20, but it is preferable that a plurality of resin fibers 22 are contained. This makes the above-mentioned effects more pronounced.
[0122] Furthermore, each resin fiber 22 may be contained in an independent state in the joint 20, or a plurality of resin fibers 22 may be contained in an entangled state. More specifically, the resin fibers 22 may be, for example, made of a woven fabric or a nonwoven fabric.
[0123] In particular, since the resin fibers 22 are contained in the joint 20 as a nonwoven fabric, the resin fibers 22 can be distributed more uniformly in the joint 20, and unintended compositional variations can be effectively suppressed, so that the above-mentioned effects are more significantly exhibited.
[0124] The content of the resin fibers 22 in the joint 20 is preferably 2 volume % or more and 70 volume % or less, more preferably 4 volume % or more and 50 volume % or less, and even more preferably 6 volume % or more and 30 volume % or less.
[0125] This makes it possible to more significantly exert the effect of including the resin fibers 22 described above, while ensuring a sufficient content of the flexible material 21 in the joint 20, thereby making the joining strength of the heat conductive part 10 by the joint 20 sufficiently excellent.
[0126] When the content of the flexible material 21 in the joint 20 is X1 [volume %] and the content of the resin fiber 22 in the joint 20 is X2 [volume %], it is preferable to satisfy the relationship of 0.04≦X2 / X1≦10.0, it is more preferable to satisfy the relationship of 0.07≦X2 / X1≦5.0, and it is even more preferable to satisfy the relationship of 0.10≦X2 / X1≦1.5. This makes the above-mentioned effects more pronounced.
[0127] [1-1-2-3] Metal particles In addition to the flexible material 21 and the resin fibers 22, the joint 20 may contain metal particles (not shown).
[0128] As mentioned above, the part that mainly contributes to the thermal conductivity in the in-plane direction of the thermal conductor body 2 is the thermal conductive portion 10. However, since metal particles generally have a higher thermal conductivity than the flexible material 21 that constitutes the joint 20, the inclusion of metal particles in the joint 20 can improve the thermal conductivity of the joint 20, thereby enabling the thermal conductivity of the thermal conductor body 2 as a whole to be further improved.
[0129] In particular, when adjacent heat conductive sections 10 are connected by one or more metal particles contained in the joint 20, the metal particles act as a "thermal path" that thermally connects the heat conductive sections 10, thereby further improving the overall thermal conductivity of the heat conductor body 2.
[0130] Furthermore, by including metal particles made of a metal material having electromagnetic shielding properties, an electromagnetic shielding function can be imparted to the thermal conductor 1. In particular, it is possible to suitably impart a shielding function against high-frequency electromagnetic waves such as those used in fifth-generation mobile communications.
[0131] The metal particles preferably contain one or more types selected from the group consisting of Fe, Ag, Pt, Cu, Sn, Al and Ni, and iron particles are more preferred.
[0132] The average particle size of the metal particles is not particularly limited, but is preferably from 0.01 μm to 10 μm, and more preferably from 0.1 μm to 3.0 μm.
[0133] In this specification, the average particle size refers to the particle size at which the cumulative 50% from the small diameter side is measured in a weight-based particle size distribution measured by a laser diffraction particle size distribution analyzer.
[0134] The content of metal particles in the joint 20 is preferably 1 volume % or more and 50 volume % or less, and more preferably 10 volume % or more and 30 volume % or less.
[0135] [1-1-2-4] Ceramic particles In addition to the above materials, the joint 20 may contain ceramic particles (not shown).
[0136] This makes it possible to stabilize and uniform the structure of the joint 20, and also stabilize the ratio and size of voids in the joint 20. As a result, it is possible to more effectively prevent unintended variations in the characteristics of each portion of the thermal conductor body 2.
[0137] The ceramic particles can be made of various ceramics, but when ceramic materials such as nitride-based ceramics such as aluminum nitride, boron nitride, and silicon nitride, carbide-based ceramics such as silicon carbide, and oxide-based ceramics such as alumina are used, the thermal conductivity of the thermal conductor body 2 as a whole can be further improved. In particular, when adjacent thermal conductive parts 10 are connected by one or more ceramic particles contained in the joint 20, the ceramic particles become a "thermal path" that thermally connects the thermal conductive parts 10, and the thermal conductivity of the thermal conductor body 2 as a whole can be further improved.
[0138] When the joint 20 contains the above-mentioned metal particles in addition to the ceramic particles, the heat path may be formed by the ceramic particles and the metal particles.
[0139] The ceramic particles may be made of silica, which can reduce the production cost of the thermal conductor 1 and can provide the effects of stabilizing and homogenizing the structure of the bonding portion 20 described above.
[0140] The average particle size of the ceramic particles is not particularly limited, but is preferably from 5 μm to 200 μm, and more preferably from 20 μm to 70 μm.
[0141] The content of the ceramic particles in the joint 20 is preferably 1 volume % or more and 50 volume % or less, and more preferably 10 volume % or more and 30 volume % or less.
[0142] This makes it possible to achieve a good balance between the effect of containing the flexible material 21 and the effect of containing the ceramic particles.
[0143] [1-1-2-5] Other ingredients The joint 20 may contain components other than those mentioned above.
[0144] Examples of such components include plasticizers, colorants, antioxidants, ultraviolet absorbers, light stabilizers, softeners, modifiers, rust inhibitors, fillers, electromagnetic wave absorbing materials such as ferrite, surface lubricants, corrosion inhibitors, heat stabilizers, lubricants, primers, antistatic agents, polymerization inhibitors, crosslinking agents, catalysts, leveling agents, thickeners, dispersants, antioxidants, flame retardants, and hydrolysis inhibitors.
[0145] However, the content of these components in the joint 20 is preferably 5% by weight or less, and more preferably 1% by weight or less.
[0146] In Figure 2, t 20 The thickness of the joint 20 in the stacking direction of the heat conductive portion 10 and the joint 20 indicated by is preferably 0.1 μm or more and 1000 μm or less, and more preferably 5.0 μm or more and 100 μm or less. This makes the above-mentioned effects more pronounced.
[0147] Here, the thickness of the joint 20 refers to the thickness at a portion of the heat conductive part 10 in contact therewith where no hole 11 is provided.
[0148] The proportion of the joints 20 in the thermal conductor body 2 (the solid portion excluding the voids 4) is preferably 15% by volume or more and 70% by volume or less, more preferably 16% by volume or more and 60% by volume or less, and even more preferably 18% by volume or more and 50% by volume or less. This makes the above-mentioned effects more pronounced.
[0149] [1-1-3]Void part The thermal conductor body 2 has, in addition to the thermally conductive portions 10 and the joint portions 20, void portions 4 where the thermally conductive portions 10 and the joint portions 20 are not present.
[0150] The void portion 4 is a portion of the thermal conductor body 2 where the thermal conductive portion 10 and the joint portion 20 are not present. The void portion 4 usually contains air or a gas such as a gas generated when the curable resin material used to form the flexible material 21 constituting the joint portion 20 is cured.
[0151] By having such a void 4, the void 4 acts as a cushion, and the deformation of the thermal conductor body 2 caused by thermal stress due to the difference in thermal conductivity between the members bonded to both sides of the thermal conductor 1 can be efficiently absorbed by the void 4, and excessive deformation of the thermal conductor 1 as a whole can be effectively suppressed. In addition, it is possible to impart suitable flexibility to the thermal conductor body 2, and the adhesion between the member bonded to the thermal conductor 1 and the thermal conductor 1 can be improved, and the adhesion, substantial thermal conductivity, and electrical conductivity between the member and the thermal conductor 1 can be improved. In particular, the joint 20 contains the above-mentioned resin fiber 22 together with the flexible material 21 functioning as a binder, and thus the relatively small void 4 can be formed in a dispersed manner. This makes it possible to improve the adhesion between the thermal conductive portion 10 and the joint 20, and to improve the durability and reliability of the thermal conductor 1. In addition, the reliability of the joint between the thermal conductor 1 and the member can be improved.
[0152] The gap 4 usually contains air or a gas such as a gas generated when the curable resin material used to form the flexible material 21 is cured.
[0153] In the thermal conductor body 2 , the gap 4 is provided at least in a portion adjacent to the joint 20 .
[0154] The proportion of voids 4 in the thermal conductor body 2 (proportion in the natural state; the same applies below) is preferably 5 volume % or more and 65 volume % or less, more preferably 5 volume % or more and 50 volume % or less, even more preferably 6 volume % or more and 40 volume % or less, and most preferably 7 volume % or more and 32 volume % or less. This makes the above-mentioned effects more pronounced.
[0155] When the proportion of the thermal conductive section 10 in the thermal conductor body 2 is VC [volume %], the proportion of the joint section 20 in the thermal conductor body 2 is VJ [volume %], and the proportion of the void section 4 in the thermal conductor body 2 is VV [volume %], it is preferable to satisfy the relationship of 25≦[(VJ+VV) / (VC+VJ+VV)]×100≦90, it is more preferable to satisfy the relationship of 25≦[(VJ+VV) / (VC+VJ+VV)]×100≦70, it is even more preferable to satisfy the relationship of 31≦[(VJ+VV) / (VC+VJ+VV)]×100≦65, and it is most preferable to satisfy the relationship of 37≦[(VJ+VV) / (VC+VJ+VV)]×100≦62. This makes the above-mentioned effects more pronounced.
[0156] The density of the thermal conductor body 2 in its natural state is 0.6 g / cm 3 More than 2.5g / cm 3 It is preferable that the concentration is 0.9 g / cm or less. 3 More than 2.0g / cm 3 It is more preferable that:
[0157] By using the above-mentioned materials for forming the heat conductive portions 10 and the joint portions 20 in the heat conductor body 2, the overall density can be reduced.
[0158] This makes it possible to make the thermal conductor 1 particularly lightweight. When an electronic device having the thermal conductor 1 is mounted in an electronic device or the like, it does not prevent the weight of the electronic device or the like from being reduced. In other words, the electronic device or the like can be made even lighter.
[0159] [1-2] Manufacturing method of the thermal conductor body Next, a method for manufacturing the thermal conductor body will be described.
[0160] That is, the thermal conductor body 2 can be suitably manufactured, for example, by winding a thermal conductive part forming sheet (thermal conductive part forming member) used for forming the thermal conductive part 10, having a joint forming composition used for forming the joint 20 applied to at least one surface thereof, around the peripheral surface of a winding roll, thereby forming the thermal conductive parts 10 and the joints 20 in an alternating layered manner.
[0161] More specifically, the manufacturing method of the thermal conductor body 2 includes a winding step of winding a thermal conductive part forming sheet used for forming the thermal conductive part 10, to which a composition for forming a joint, which is a composition containing a curable resin material, is applied and in which a recess (hole) 11 is formed, around the peripheral surface of a winding roll to obtain a cylindrical wound body, a cutting step of cutting open the wound body in a direction non-perpendicular to the axial direction of the roll to obtain a cut body, and a hardening step of hardening the curable resin material contained in the cut body to form the joint 20.
[0162] By winding the heat conductive part forming sheet to which the joint forming composition is applied on the circumferential surface of a winding roll, the heat conductor body 2 can be produced more efficiently than, for example, when a sheet-like raw material is used. In addition, by curing the curable resin material after cutting the wound body, the wound body can be cut in a softer state than the joint 20 including the flexible material 21. For this reason, it is possible to suitably correct the distortion caused by the winding, and when making a cut body with a higher flatness than the wound body, it is possible to effectively prevent peeling or a decrease in adhesion between the heat conductive part forming sheet, which is the part corresponding to the heat conductive part 10, and the joint forming composition, which is the part corresponding to the joint 20. As a result, the finally obtained heat conductor body 2 can be one in which the distortion is suitably removed, and peeling or a decrease in adhesion between the heat conductive part 10 and the joint 20, destruction of the joint 20, destruction of the joint between the heat conductive parts 10, etc. are effectively prevented, and the heat conductive part 10 and the joint 20 are firmly adhered to each other.
[0163] When the thermal conductor body 2 to be manufactured is in a sheet shape, after the above-mentioned curing step, a cutting step is performed in which the thermal conductor body 2 is cut into a sheet shape in which the thermal conductive portions 10 and the bonding portions 20 are exposed on both sides.
[0164] In this way, for example, a sheet-like thermal conductor body 2 having a desired thickness can be obtained.
[0165] In addition, the manufacturing method of the thermal conductor body 2 may include, for example, a joint forming composition application process, prior to the winding process, in which a joint forming composition is applied to a thermal conductive part forming sheet having a recess (hole) 11 provided therein.
[0166] In the above explanation, the heat conductor body 2 is manufactured by rolling a heat conduction part forming sheet to which a joint formation composition has been applied to form a roll and then cutting the roll. However, the heat conductor body 2 may also be manufactured by stacking, for example, sheets of heat conduction part forming members to which a joint formation composition has been applied to form a laminate.
[0167] [1-3] Other examples of thermal conductor body configurations Next, other configuration examples of the thermal conductor body will be described.
[0168] Fig. 7 is a perspective view showing a schematic diagram of another example of the thermal conductor body. Fig. 8 is a longitudinal cross-sectional view of the thermal conductor body shown in Fig. 7, Fig. 8(a) is a cross-sectional view taken along line CC', and Fig. 8(b) is a cross-sectional view taken along line D-D'.
[0169] In the thermal conductor body 2 shown in Figs. 7 and 8, a plurality of thermal conductive portions 10 are provided in an island shape when viewed in a plan view from the second direction.
[0170] This makes it possible to reduce the variation in thermal conductivity at each part within the surface of the thermal conductor body 2 (in the direction of the xy plane shown in Figure 7) while also making it easier to improve the flexibility of the thermal conductor body 2 as a whole, thereby making it possible to more significantly exert the effects of the present invention described above.
[0171] In this specification, the term "island-like" refers to a state in which a plurality of heat conductive parts 10 are not continuous but are scattered in the joint 20. In other words, each heat conductive part 10 is independent of other heat conductive parts 10 in both the x direction and the y direction.
[0172] 7, the heat conducting body 2 has a plurality of heat conducting parts 10 arranged in a staggered manner when viewed from the second direction. In other words, a first row 10a in which the heat conducting parts 10 are arranged in the y direction and a second row 10b are arranged alternately in the x direction such that the heat conducting parts 10 are staggered. This makes it possible to more significantly exhibit the above-mentioned effects.
[0173] It is preferable that the thermally conductive portions 10 in the first row 10a and the thermally conductive portions 10 in the second row 10b at least partially overlap with each other in the x-direction. This makes it possible to exhibit the above-mentioned effects more significantly.
[0174] w in Figure 7 when viewed from the second direction 10 The width of the thermally conductive portion 10 indicated by is preferably 1 mm or more and 30 mm or less, more preferably 5 mm or more and 20 mm or less, and further preferably 7 mm or more and 15 mm or less.
[0175] This makes it possible to ensure that the proportion of the heat conducting portion 10 in the heat conductor body 2 is sufficiently high, while also making it easier to improve the flexibility of the heat conductor body 2 as a whole, thereby more reliably achieving the aforementioned effects more significantly.
[0176] When the thermal conductor body 2 is viewed from a second direction in plan view, the thermal conductor body 2 is 10 The distance between adjacent thermally conductive portions 10 indicated by is preferably 1 μm or more and 2000 μm or less, more preferably 2 μm or more and 1500 μm or less, and even more preferably 3 μm or more and 1000 μm or less.
[0177] This makes it possible to ensure that the proportion of the thermal conductive portion 10 in the thermal conductor body 2 is sufficiently high, while also making it easier to provide the thermal conductor body 2 as a whole with better flexibility, thereby making it possible to more significantly exert the aforementioned effects.
[0178] In this specification, the "distance between adjacent heat conductive parts 10" refers to the gap as the shortest distance between adjacent heat conductive parts 10.
[0179] 7 shows a case where the plurality of heat conductive parts 10 are arranged in a staggered manner, the plurality of heat conductive parts 10 may be arranged in a manner other than a staggered manner. The plurality of heat conductive parts 10 may be arranged regularly or randomly.
[0180] As shown in FIG. 8, the inclination direction of the heat conducting portions 10 (through heat conducting portions 10c) with respect to the normal direction V1 of the surface is opposite between the first row 10a and the second row 10b of the heat conducting portions 10.
[0181] The inclination direction of the through-hole heat conductive portions 10c in the first row 10a with respect to the normal direction V1 of the surface is defined as a positive (+) direction, and the inclination direction of the through-hole heat conductive portions 10c in the second row 10b with respect to the normal direction of the surface is defined as a negative (-) direction.
[0182] That is, the through-hole heat conductive portion 10c in the first row 10a is inclined at an angle θ1 in the positive direction with respect to the normal direction V1 of the surface, and the through-hole heat conductive portion 10c in the second row 10b is inclined at an angle θ2 in the negative direction with respect to the normal direction V1 of the surface.
[0183] In this way, by providing the through-hole heat conducting portions 10c inclined in different directions, in particular by providing the through-hole heat conducting portions 10c inclined in a positive direction with respect to the surface normal direction V1 as well as the through-hole heat conducting portions 10c inclined in a negative direction with respect to the surface normal direction V1, even when a relatively large load is applied to the heat conductor 1, irreversible deformation of the heat conductor 1, such as the collapse of the heat conductor body 2 due to buckling, can be more effectively suppressed, and the durability of the heat conductor 1 can be further improved.
[0184] In particular, by alternately arranging the through-hole heat conductive portions 10c inclined in a positive direction with respect to the normal direction V1 of the surface and the through-hole heat conductive portions 10c inclined in a negative direction with respect to the normal direction V1 of the surface, the aforementioned effect can be more significantly exerted.
[0185] As shown in FIG. 8, the normal direction V1 of the surface and the extending direction e of the penetrating heat conductive portion 10c are 10 The absolute values of the angles θ1, θ2 formed by these are preferably 3° or more and 45° or less, more preferably 5° or more and 40° or less, and even more preferably 8° or more and 35° or less. This makes it possible to more significantly exhibit the above-mentioned effects.
[0186] Although the angles θ1 and θ2 may have different sizes, it is preferable that they are the same.
[0187] In addition, the angles are not exact numerical values in the mathematical sense, but may include normal errors in the technical field of the present invention. For example, a difference of less than 1° is interpreted as the same angle as the error.
[0188] The inclination direction of the heat conductive portion 10 is not particularly limited, but when the heat conductive portion 10 (heat conductive portion forming member) is strip-shaped, it is preferable that the surface direction of the heat conductive portion 10 is inclined with respect to the normal direction V1 of the surface.
[0189] As a result, even if a relatively large load is applied to the thermal conductor 1, irreversible deformation of the thermal conductor 1, such as the collapse of the thermal conductor body 2 due to buckling, can be more effectively suppressed, and the durability of the thermal conductor 1 can be further improved.
[0190] [1-4] Solder layer The solder layer 3 is disposed so as to cover at least a portion of the outer surface of the thermal conductor body 2 .
[0191] In particular, the solder layer 3 is arranged so as to cover, for example, at least a portion of two faces aligned in the thickness direction of the thermal conductor body 2, in other words, a pair of opposing faces, on the outer surface of the thermal conductor body 2 to which the first member 110 and the second member 120 are joined.
[0192] This makes it possible to achieve excellent adhesion between the thermal conductor 1 and the first member 110 and second member 120, which are joined to the thermal conductor 1 by heating the solder above its melting point between a pair of opposing surfaces, and enables efficient transfer of heat between the thermal conductor 1 and the first member 110 and second member 120.
[0193] In the cross-sectional view shown in FIG. 1, the solder layers 3 are disposed on a pair of opposing outer surfaces of the thermal conductor body 2, in other words, on the top and bottom surfaces.
[0194] In the cross-sectional view shown in FIG. 1, the solder layer 3 is disposed so as to cover the entire top and bottom surfaces of the thermal conductor body 2. In FIG.
[0195] The melting point of the solder constituting the solder layer 3 is preferably less than 300°C, more preferably 110°C or higher and lower than 200°C, and even more preferably 110°C or higher and lower than 160°C.
[0196] This can improve the bonding strength between the thermal conductor 1 and the member to be bonded to the thermal conductor 1, and can more effectively prevent damage to the thermal conductor body 2 and the member when bonding the thermal conductor 1 to the member. In addition, the energy required to bond the thermal conductor 1 to the member can be made relatively low, which is also preferable from the viewpoint of energy saving.
[0197] The melting point of the solder can be determined by measurement in accordance with JIS Z3198-1:2014.
[0198] The solder constituting the solder layer 3 may be any solder containing an alloy material including lead (Pb) or tin (Sn), but from the viewpoint of preventing environmental pollution, it is preferable that the solder be lead-free solder.
[0199] In addition, JIS Z3282:2017 (Solder - Chemical composition and shape) specifies that lead-free solder has a lead content of 0.10 mass% or less.
[0200] Lead-free solder is an alloy material that contains tin (Sn) and at least one element selected from the group consisting of silver (Ag), antimony (Sb), bismuth (Bi), copper (Cu), indium (In), zinc (Zn), nickel (Ni), germanium (Ge), phosphorus (P), and gallium (Ga).
[0201] In particular, the solder constituting the solder layer 3 is preferably an alloy material containing tin (Sn) and at least one selected from the group consisting of silver (Ag), bismuth (Bi), copper (Cu) and zinc (Zn), and more preferably an alloy material containing tin (Sn) and indium (In).
[0202] This provides the solder layer 3 with a particularly excellent balance of thermal conductivity, bondability, and stress relaxation properties, and the aforementioned effects of the present invention are prominently exhibited.
[0203] Indium (In) is the softest of the metal elements that can be practically used, and due to its softness, it has an extremely excellent stress relaxation property. This allows it to fully absorb thermal stress and the like, and significantly improves the reliability of the bonded body 100. Furthermore, In has a melting point of 156°C and melts at a relatively low temperature, so that the melting point of the solder can be made relatively low.
[0204] When the solder contains In, the In content in the solder is preferably 60 mass % or less, and more preferably 10 mass % or less. This makes the above-mentioned effects more pronounced.
[0205] Tin (Sn) is generally a soft metal, but it is harder than In. Therefore, by adding Sn to solder, the hardness of the solder can be adjusted and its workability can be improved.
[0206] Bismuth (Bi) is an element that can lower the melting point of solder and is also correlated with the hardness and heat cycle resistance of solder. In addition, the addition of Bi can adjust the electrical conductivity of solder.
[0207] When the solder contains Bi, the Bi content in the solder is preferably 60 mass % or less, and more preferably 10 mass % or less. This makes the above-mentioned effects more pronounced.
[0208] When the solder contains silver (Ag), the wettability and processability of the solder can be improved.
[0209] When the solder contains Ag, the Ag content in the solder is preferably 0.01% by mass or more and 21.0% by mass or less. This makes the above-mentioned effects more pronounced.
[0210] When the solder contains copper (Cu), the stress relaxation properties of the solder layer 3 can be improved.
[0211] When the solder contains Cu, the Cu content in the solder is preferably 0.01 mass % or more and 0.90 mass % or less. This makes the above-mentioned effects more pronounced.
[0212] When solder contains zinc (Zn), the wettability and softness (workability) of the solder can be improved.
[0213] When the solder contains Zn, the Zn content in the solder is preferably 0.01% by mass or more and 3.0% by mass or less. This makes the above-mentioned effects more pronounced.
[0214] When the solder contains phosphorus (P), oxidation of the solder surface can be suppressed, and the bondability, reliability, and the like of the solder layer 3 can be improved.
[0215] When the solder contains P, the P content in the solder is preferably 0.0005% by mass or more and 0.500% by mass or less. This makes the above-mentioned effects more pronounced.
[0216] Specific examples of the above solder include Sn-58Bi eutectic solder (melting point 138° C.) and Sn-52In alloy solder (melting point 118° C.).
[0217] The thickness of the solder layer 3 is preferably 0.1 μm or more and 500 μm or less, more preferably 0.5 μm or more and 400 μm or less, and further preferably 1.0 μm or more and 300 μm or less. This makes the above-mentioned effects more pronounced.
[0218] Here, the thickness of the solder layer 3 can be measured from a cross-sectional image of the thermal conductor 1 taken using an electron microscope.
[0219] Furthermore, as described below, when a portion of the solder layer 3 penetrates into the thermal conductor body 2, the thickness of the solder layer 3 is the sum of the thickness T1 of the portion that penetrates into the thermal conductor body 2 and the thickness T2 of the portion that does not penetrate into the thermal conductor body 2.
[0220] The thickness of the solder layer 3 is the thickness at the portion of the solder layer 3 where it is at its maximum thickness. It is preferable that a portion of the solder layer 3 penetrates into the thermal conductor body 2 .
[0221] This provides an anchor effect, which improves the adhesion between the thermal conductor body 2 and the solder layer 3, and the above-mentioned effect can be more significantly achieved. In addition, the solder layer 3 is preferably prevented from peeling off from the thermal conductor body 2 due to deformation of the thermal conductor 1, and the durability of the thermal conductor 1 can be improved. Such an anchor effect is more significantly achieved when the thermal conductive part 10 contains graphite that is not easily wetted by molten metal as described above. By contacting the thermal conductor body 2 with a molten solder having fluidity and then cooling and solidifying it, a state in which a part of the solder layer 3 penetrates into the thermal conductor body 2 can be preferably formed.
[0222] Here, "a part of the solder layer 3 penetrates into the inside of the thermal conductor body 2" means that a part of the solder layer 3 penetrates into the unevenness on the surface of the thermal conductor body 2 and at least a part of the gaps of the thermal conductive parts 10 and the joint parts 20 exposed on the surface of the thermal conductor body 2. In contrast, a state in which the solder layer 3 does not penetrate into the inside of the thermal conductor body 2 means that the solder layer 3 does not penetrate into any of the unevenness on the surface of the thermal conductor body 2 and the gaps of the thermal conductive parts 10 and the joint parts 20 exposed on the surface of the thermal conductor body 2.
[0223] FIG. 9 is an electron microscope photograph showing a thermal conductor with a portion of the solder layer penetrating into the thermal conductor body.
[0224] When the thickness of the portion of the solder layer 3 that penetrates into the thermal conductor body 2 is T1 [μm] and the thickness of the portion that does not penetrate into the thermal conductor body 2 is T2 [μm], it is preferable for the relationship to satisfy 0.005≦T1 / T2≦500, it is more preferable for the relationship to satisfy 0.05≦T1 / T2≦60, and it is even more preferable for the relationship to satisfy 0.5≦T1 / T2≦10.
[0225] As a result, the anchor effect can be achieved to a high degree to improve adhesion between the thermal conductor body 2 and the solder layer 3, while at the same time improving adhesion between the thermal conductor 1 and the member joined to the thermal conductor 1, thereby making it possible to more significantly exert the effects of the present invention described above.
[0226] Here, the "portion of the solder layer 3 that does not penetrate into the interior of the thermal conductor body 2" refers to the portion of the solder layer 3 other than the portion that penetrates into the interior of the thermal conductor body 2, and refers to the portion that is exposed from the surface of the thermal conductor body 2.
[0227] The thickness T1 of the portion of the solder layer 3 that penetrates into the thermal conductor body 2 is preferably 10 μm or more and 500 μm or less, more preferably 15 μm or more and 300 μm or less, and even more preferably 20 μm or more and 100 μm or less.
[0228] This provides an anchor effect that further improves the adhesion between the thermal conductor body 2 and the solder layer 3, thereby making the above-mentioned effects even more pronounced.
[0229] The thickness T2 of the portion of the solder layer 3 that does not penetrate into the inside of the thermal conductor body 2 is preferably 1 μm or more and 2000 μm or less, more preferably 5 μm or more and 1000 μm or less, and even more preferably 10 μm or more and 300 μm or less.
[0230] This allows the thermal conductor 1 and the member joined to the thermal conductor 1 to be more appropriately adhered to each other, and the above-mentioned effects are more significantly exhibited.
[0231] The solder layer 3 may be formed, for example, by printing a solder paste on one surface (first surface 23) and the other surface (second surface 24) of the thermal conductor body 2, or the like.
[0232] At this time, for example, if part of the solder paste penetrates into the unevenness on the surface of the thermal conductor body 2, or into the gaps of the thermal conductive sections 10 and joint sections 20 exposed on the surface of the thermal conductor body 2, the formed solder layer 3 will have a part of it penetrating inside the thermal conductor body 2.
[0233] In addition, when the member to be joined to the thermal conductor 1 and the thermal conductor 1 are not joined via the solder layer 3, a portion of the solder layer 3 does not penetrate into the interior of the thermal conductor main body 2. However, when the member to be joined to the thermal conductor 1 and the thermal conductor 1 are joined via the solder layer 3, a portion of the solder layer 3 may penetrate into the interior of the thermal conductor main body 2.
[0234] When joining the member to be joined to the thermal conductor 1 and the thermal conductor 1 via the solder layer 3, as described below, the member to be joined to the thermal conductor 1 and the thermal conductor 1 may be heated in a state of being superimposed on each other, and may be pressed in the thickness direction of the thermal conductor 1. The pressing at this time may cause the layer of the thermal conductive portion 10 and the joint portion 20 constituting the thermal conductor body 2 to collapse, and part of the molten solder may penetrate into the collapsed layer. In such a case, the solder will subsequently solidify, and part of the solder layer 3 will have penetrated into the inside of the thermal conductor body 2.
[0235] In addition, the thermal conductor of the present invention may have a plurality of thermal conductor bodies disposed between the solder layer on the side bonded to the first member and the solder layer on the side bonded to the second member. In such a case, the thermal conductor bodies disposed between the two solder layers may have the same or different extension directions of the thermal conductive portion and the joint portion. Also, a solder layer may be provided between the adjacent thermal conductor bodies.
[0236] [2] Zygote Next, the bonded body of the present invention will be described. FIG. 10 is a cross-sectional view that illustrates an example of the bonded body of the present invention.
[0237] The joint of the present invention comprises a heat conductor body having a plurality of heat conductive portions and a joint including a flexible material that joins the plurality of heat conductive portions, and a first member joined to the heat conductor body via a solder layer on one of two surfaces (a first surface and a second surface) that are aligned in the thickness direction of the heat conductor body.
[0238] The bonded body of the present invention can be manufactured, for example, by heating the heat conductor body and the first member with molten solder placed between them. In this case, the bonded body obtained has the heat conductor and the first member bonded thereto. The second member described below can be bonded in the same manner.
[0239] The thermal conductor of the present invention described above can be suitably used to manufacture the bonded body of the present invention. In such a case, the bonded body can be obtained by heating the thermal conductor of the present invention in a state where the first member is in contact with the thermal conductor of the present invention. The bonding of the second member described below can be performed in the same manner.
[0240] In particular, the joint body 100 shown in FIG. 10 further includes a second member 120 joined to the thermal conductor body 2 via a solder layer 3 on the other surface, that is, the second surface 24, opposite the one surface, that is, the first surface 23.
[0241] In the following explanation, the joint 100 is manufactured using the thermal conductor 1 of the present invention described above, and the explanation will be focused on the case where the joint 100 has a first member 110 joined to one surface (first surface 23) of the thermal conductor 1 via a solder layer 3, and a second member 120 joined to the other surface (second surface 24) via a solder layer 3.
[0242] In such a bonded body 100, the heat conductor 1 has the bonded portion 20 including a flexible material and the solder layer 3 having ductility and flexibility, so that the heat conductor 1 has flexibility as a whole and has excellent adhesion to the bonded first member 110 and second member 120 and excellent followability to expansion and contraction of the first member 110 and second member 120 due to temperature changes. In other words, the heat conductor 1 itself can deform to absorb and relieve thermal stress generated by the difference in thermal expansion coefficient between the first member 110 and the second member 120, which are bonded to both sides of the heat conductor 1 via the solder layer 3. In other words, the heat conductor 1 functions as a buffer material that exerts a buffering effect.
[0243] This makes it possible to prevent separation at the bonding interfaces between the thermal conductor 1 and the first and second members 110 and 120, and to maintain sufficient adhesion.
[0244] Furthermore, since the thermal conductor 1 is flexible, the adhesion between the thermal conductor 1 and the first member 110 and the second member 120 joined to the thermal conductor 1 can be excellent, and the substantial thermal conductivity between the thermal conductor 1 and the first member 110 and the second member 120 can be excellent.
[0245] Furthermore, since the thermal conductor 1 is not only in contact with the first member 110 and the second member 120 but is also bonded thereto, good adhesion can be ensured without applying surface pressure, and the substantial thermal conductivity between the first member 110 and the second member 120 and the thermal conductor 1 can be made more excellent. Moreover, even if at least one of the first member 110 and the second member 120 is a member to which it is difficult to apply surface pressure, the above-mentioned effects can be obtained.
[0246] As described in the above [1-4], in the bonded body 100 as well, it is preferable that a part of the solder layer 3 penetrates into the thermal conductor body 2 .
[0247] This provides an anchor effect that improves adhesion between the thermal conductor body 2 and the solder layer 3, thereby enabling the above-mentioned effects to be exhibited more significantly. Also, the solder layer 3 is preferably prevented from peeling off from the thermal conductor body 2 due to deformation of the thermal conductor 1, thereby improving the durability of the joined body 100. Such an anchor effect is exhibited more significantly when the thermal conductive part 10 contains graphite that is difficult to wet with molten metal as described above.
[0248] In the bonded body 100, when the thickness of the portion of the solder layer 3 that penetrates into the thermal conductor body 2 is T3 [μm] and the thickness of the portion that does not penetrate into the thermal conductor body 2 is T4 [μm], it is preferable that the bonded body 100 satisfies the relationship 0.05≦T3 / T4≦10,000, it is more preferable that the bonded body 100 satisfies the relationship 0.5≦T3 / T4≦600, and it is even more preferable that the bonded body 100 satisfies the relationship 5≦T3 / T4≦100.
[0249] As a result, the anchor effect makes it possible to achieve a higher level of adhesion between the thermal conductor body 2 and the solder layer 3, and between the thermal conductor 1 and the members joined to the thermal conductor 1 (first member 110, second member 120), thereby making the above-mentioned effects more pronounced.
[0250] In the bonded body 100, the thickness T3 of the portion of the solder layer 3 that penetrates into the thermal conductor body 2 is preferably 10 μm or more and 1000 μm or less, more preferably 15 μm or more and 600 μm or less, and even more preferably 20 μm or more and 200 μm or less.
[0251] This provides an anchor effect that further improves the adhesion between the thermal conductor body 2 and the solder layer 3, thereby making the above-mentioned effects even more pronounced.
[0252] In the bonded body 100, the thickness T4 of the portion of the solder layer 3 that does not penetrate into the thermal conductor body 2 is preferably 0.1 μm or more and 200 μm or less, more preferably 0.5 μm or more and 100 μm or less, and even more preferably 1 μm or more and 50 μm or less.
[0253] This allows the thermal conductor 1 and the members (first member 110, second member 120) joined to the thermal conductor 1 to be more appropriately adhered to each other, and the above-mentioned effects are more significantly exhibited.
[0254] When at least one of the first member 110 and the second member 120 is made of a non-metallic material, it is preferable that a metal film (metallized film) (not shown) is disposed at the portion of the member to be joined to the thermal conductor 1. This allows for more suitable joining to the thermal conductor 1 via the solder layer 3, and the above-mentioned effects are more prominently exhibited.
[0255] The material constituting the metallic film is not particularly limited as long as it is a metallic material, and examples thereof include materials containing gold, silver, nickel, copper, zinc, tin, and the like.
[0256] Furthermore, the thickness of the metal film is not particularly limited, but is preferably 0.01 μm to 100 μm, more preferably 0.1 μm to 20 μm, and even more preferably 1 μm to 15 μm.
[0257] The thermal conductor 1 is joined to the first member 110 and the second member 120 via the solder layer 3 by soldering.
[0258] Soldering is a welding method in which solder with a lower melting point than the materials (base materials) to be joined is melted and used as a kind of adhesive.
[0259] The first member 110 and the thermal conductor 1, and the thermal conductor 1 and the second member 120 can be joined by heating the first member 110, the thermal conductor 1, and the second member 120 in a state where they are superimposed on each other. As a result, the solder layer 3 melted by heating becomes in a state where it can be physically joined to the members. Then, as the solder solidifies, the thermal conductor 1 and the members are joined via the solder layer 3.
[0260] In particular, when the component has the metal film, the solder layer 3 melted by heating is in a state in which it can be physically bonded to the metal film provided on the component. Then, as the solder solidifies, the thermal conductor 1 and the metal film provided on the component are bonded via the solder layer 3.
[0261] The heating temperature during soldering is preferably 80°C or higher and 300°C or lower, more preferably 100°C or higher and 280°C or lower, and even more preferably 150°C or higher and 250°C or lower.
[0262] This makes it possible to more suitably join the first member 110 and the second member 120 to the thermal conductor 1. Furthermore, when joining the first member 110 and the second member 120 to the thermal conductor 1, it is possible to prevent damage to the thermal conductor body 2, the first member 110 or the second member 120.
[0263] Furthermore, during heating, the first member 110, the thermal conductor 1, and the second member 120 may be pressed in the thickness direction of the thermal conductor 1 while being superimposed.
[0264] The pressure at this time is preferably 0.05 MPa or more and 4.0 MPa or less, more preferably 0.1 MPa or more and 2.0 MPa or less, and even more preferably 0.5 MPa or more and 1.0 MPa or less.
[0265] This allows the first member 110 and the second member 120 to be joined to the thermal conductor 1 more suitably.
[0266] The treatment time for bonding by heating and pressing is preferably from 1 to 60 minutes, more preferably from 1 to 30 minutes, and even more preferably from 1 to 10 minutes.
[0267] Furthermore, since the thermal conductor 1 is not simply in contact with the first member 110 and the second member 120 but is joined via the solder layer 3, good adhesion can be ensured without applying surface pressure, and substantial thermal conductivity between the first member 110 and the second member 120 and the thermal conductor 1 can be improved. Furthermore, even if at least one of the first member 110 and the second member 120 is a member to which it is difficult to apply surface pressure, the thermal conductor 1 can be applied.
[0268] The combination of the first member 110 and the second member 120 is not particularly limited, and they may be made of the same material, but it is preferable that they are made of different materials. This makes it possible to more significantly exhibit the effects of the present invention described above.
[0269] It is preferable that one of the pair of surfaces (first surface 23 of heat conductor body 2) of the heat conductor 1 is joined to a member containing a metal material, and the other surface (second surface 24 of heat conductor body 2) is joined to a member containing a ceramic material. In other words, in Fig. 10, it is preferable that one of the first member 110 and the second member 120 contains a metal material, and the other member contains a ceramic material.
[0270] Generally, the thermal expansion coefficient of metal materials is relatively large and that of ceramic materials is relatively small, so the difference between these thermal expansion coefficients is large. Therefore, by joining the thermal conductor 1 to a member containing a metal material on one side (the first surface 23 of the thermal conductor body 2) and joining to a member containing a ceramic material on the other side (the second surface 24 of the thermal conductor body 2), the above-mentioned effects of the present invention can be more significantly exhibited.
[0271] The metal material is not particularly limited, and various elemental metals and various alloys can be used. More specifically, examples include copper, copper alloys, aluminum, and aluminum alloys, with copper being preferred among them. This allows the above-mentioned effects of the present invention to be more pronounced.
[0272] The ceramic material is not particularly limited, and various oxide-based ceramics, various carbide-based ceramics, various nitride-based ceramics, and composites of two or more selected from these can be used. Among them, at least one selected from the group consisting of aluminum nitride, boron nitride, silicon nitride, gallium nitride, aluminum oxide, zirconium oxide, silicon carbide, silicon, and gallium arsenide is preferable. This allows the above-mentioned effects of the present invention to be more pronounced.
[0273] The absolute value of the difference between the average linear expansion coefficients of the first member 110 and the second member 120 at 40 to 100° C. is 2.0×10 -6 / K or more 40.0×10 -6 / K or less, and 3.0×10 -6 / K or more 30.0×10 -6 / K or less is more preferable, and 4.0×10 -6 / K or more 20.0×10 -6 It is more preferable that the value is equal to or less than 1 / K.
[0274] As a result, the thermal stress generated by the difference in thermal expansion coefficient between the first member 110 and the second member 120 can be more effectively absorbed and alleviated by the deformation of the thermal conductor 1 itself, and the effects of the present invention are more pronounced.
[0275] FIG. 11 is an electron microscope photograph showing a joint in which a portion of the solder layer penetrates into the thermal conductor body.
[0276] At least one of the first member 110 and the second member 120 joined to the thermal conductor 1 may be another thermal conductor body 2 or thermal conductor 1 .
[0277] Fig. 12 is a perspective view showing a schematic diagram of another example of the joined body of the present invention, in which one of a first member and a second member joined to a thermal conductor is a main body of another thermal conductor.
[0278] When the thermal conductor body 2 has anisotropic thermal conductivity in the plane, the joint body 100 shown in FIG. 12 has a two-stage structure in which a thermal conductor 1 having a thermal conductor body 2 with high thermal conductivity in the X direction in the plane and a thermal conductor body 2 with high thermal conductivity in the Y direction in the plane are joined via a solder layer 3.
[0279] In this way, by stacking a plurality of heat conductor bodies 2 so that the extending directions of the heat conductive parts 10 are different, it is possible to obtain excellent heat conductivity in different directions in the XY plane, in addition to the first direction perpendicularly connecting the pair of faces, particularly in the illustrated configuration, in both the X direction and the Y direction. In other words, heat can be dissipated by conducting heat three-dimensionally. In addition, by stacking a plurality of heat conductor bodies 2 so that the extending directions of the heat conductive parts 10 are different, it becomes easier to design a space that is difficult to conduct heat, and electronic components that are sensitive to heat can be more suitably protected.
[0280] A method for stacking heat conductor bodies 2 having different thermal conductivities in a plane can be, for example, a method of stacking a heat conductor 1 arranged so that the extension direction of the heat conductive portion 10 in the heat conductor body 2 is the X direction in the plane, and a heat conductor body 2 arranged so that the extension direction of the heat conductive portion 10 is the Y direction in the plane.
[0281] By joining adjacent thermal conductor bodies 2 in the stacking direction via a solder layer 3, the interfacial thermal resistance between adjacent thermal conductor bodies 2 can be reduced, thereby further increasing the actual thermal conductivity.
[0282] Furthermore, good adhesion can be ensured between adjacent thermal conductor bodies 2 without applying surface pressure, and the bonded body 100 can be constructed even if it is difficult to apply surface pressure to at least one of the adjacent thermal conductor bodies 2.
[0283] 12, the case where the first member (the member arranged on the upper surface side of the thermal conductor 1) is another thermal conductor body 2 has been described, but the first member may be another thermal conductor 1. In other words, the bonded body 100 may have a configuration in which a plurality of thermal conductors 1 are stacked.
[0284] [3]Electronic equipment The thermal conductor and bonded body of the present invention described above can also be applied to an electronic device. Such an electronic device has, for example, an electronic component and the thermal conductor of the present invention as a heat transfer member.
[0285] FIG. 13 is a cross-sectional view showing a schematic configuration example of an electronic device to which the thermal conductor and bonded body of the present invention are applied.
[0286] The electronic device 200 shown in FIG. 13 has an electronic component 210, a heat dissipation substrate 220, and an insulating member 230 arranged between the electronic component 210 and the heat dissipation substrate 220, and the thermal conductor 1 described above is arranged between the heat dissipation substrate 220 and the insulating member 230, and is joined to the heat dissipation substrate 220 and the insulating member 230 via solder layers 3 on both sides of a pair of opposing surfaces.
[0287] The thermal conductor 1 can be, for example, in contact with a high-temperature member on one side and in contact with a heat-dissipating member on the other side, and can be used as a heat transfer member that transfers heat from the high-temperature member to the heat-dissipating member and dissipates the heat efficiently from the heat-dissipating member, or as a heat transfer member that contacts a heating object to be heated and a high-temperature member that is at a higher temperature than the heating object and transfers thermal energy from the high-temperature member to the heating object and efficiently heats the heating object, etc.
[0288] 13, one surface of the thermal conductor 1 is joined to an insulating member 230, which is a high-temperature member, via a solder layer 3, and the other surface is joined to a heat dissipation substrate 220, which is a heat dissipation member. The insulating member 230 is joined to an electronic component 210 on the surface opposite to the surface joined to the thermal conductor 1.
[0289] In such an electronic device 200, heat generated from the electronic component 210 is conducted to the heat dissipation substrate 220 via the insulating member 230 and the thermal conductor 1, and is dissipated via the heat dissipation substrate 220.
[0290] In particular, in the electronic device 200, the thermal conductor 1 has flexibility as a whole. In other words, the thermal conductor 1 itself deforms to absorb and alleviate the thermal stress caused by the difference in thermal expansion coefficient between the material constituting the insulating member 230 and the material constituting the heat dissipation board 220, which are bonded to both sides of the thermal conductor 1 via the solder layer 3.
[0291] This makes it possible to prevent peeling at the bonding interfaces between the thermal conductor 1 and the insulating member 230 and between the thermal conductor 1 and the heat dissipation substrate 220, and to maintain sufficient adhesion.
[0292] Furthermore, since the thermal conductor 1 has flexibility, the adhesion between the insulating member 230 and the heat dissipation substrate 220 and the thermal conductor 1 can be excellent, and the substantial thermal conductivity between the insulating member 230 and the heat dissipation substrate 220 and the thermal conductor 1 can be excellent.
[0293] Furthermore, the thermal conductor 1, the insulating member 230, and the heat dissipation substrate 220 are not simply in contact with each other but are bonded together, thereby making it possible to achieve better adhesion.
[0294] Such an electronic device 200 is provided with a thermal conductor 1 having excellent substantial thermal conductivity, and therefore can more efficiently dissipate heat from the electronic component 210, which is a heat-generating body, and can more effectively reduce the risk of shortened life span of the device or system, malfunction, etc.
[0295] [3-1] Electronic components Examples of electronic components 210 include various electronic components, and more specifically, examples of electronic components include a computer's central processing unit (CPU), a graphics processing unit (GPU), a power semiconductor element (power device), an FPGA, an ASIC, a smartphone's SoC, a DSP or microcontroller of an embedded device, and semiconductor elements such as transistors. The electronic component 210 is, for example, a high-temperature component that becomes hotter than the surrounding atmosphere.
[0296] The maximum surface temperature of the high temperature member is preferably 40°C or higher and 250°C or lower, more preferably 50°C or higher and 200°C or lower, and even more preferably 60°C or higher and 180°C or lower.
[0297] When the thermal conductor 1 is applied to such high-temperature members, it can conduct and dissipate heat more effectively, and the effects of the present invention are more pronounced.
[0298] Among the electronic components described above, when a power semiconductor element is used, the amount of heat generated tends to be particularly large. In other words, the thermal stress generated due to the difference in thermal expansion coefficient between the material constituting the insulating member 230, which becomes hot due to heat transfer from the electronic component 210, and the material constituting the heat dissipation substrate 220 tends to be large. Therefore, by applying a power semiconductor element as the electronic component 210 and arranging the thermal conductor 1 between the electronic component 210 and the heat dissipation substrate 220, the effect of the present invention as described above can be made even more remarkable.
[0299] The electronic component 210 is joined to the insulating member 230 via solder 250 . This can improve the bonding strength between the insulating member 230 and the electronic component 210, and can more reliably prevent damage to the electronic component 210 when the electronic component 210 is fixed. Also, the productivity of the electronic device 200 can be improved.
[0300] It is preferable that electronic component 210 has metal film 211 at a portion where insulating member 230 is to be joined. This allows for suitable bonding to the insulating member 230 via the solder 250 .
[0301] The material constituting the metallic film 211 is not particularly limited as long as it is a metallic material, and examples thereof include materials containing gold, silver, nickel, copper, zinc, tin, and the like.
[0302] Furthermore, the thickness of the metal film 211 is not particularly limited, but is preferably 0.1 μm to 100 μm, more preferably 0.2 μm to 50 μm, and even more preferably 0.3 μm to 20 μm. This makes it possible to make the above-mentioned effects more pronounced.
[0303] In the following description, the electronic device 200 including a power semiconductor element as the electronic component 210 will be mainly described.
[0304] [3-1-1] Power semiconductor devices A power semiconductor element is a semiconductor element (power device) for power control. Examples of such power semiconductor elements include rectifier diodes, power transistors (power MOSFETs, insulated gate bipolar transistors (IGBTs)), thyristors, gate turn-off thyristors (GTOs), and triacs.
[0305] In such power semiconductor devices, a large current flows, and therefore the amount of heat generated is particularly large, which means that the above-mentioned problems caused by the difference in thermal expansion coefficient become more pronounced.
[0306] When the thermal conductor 1 is applied to such a power semiconductor element, the above-described effects of the present invention are particularly pronounced.
[0307] 13, when an electronic device 200 has an insulating member 230 disposed between an electronic component 210 and a heat dissipation substrate 220, a vertical element such as a vertical IGBT, a vertical MOSFET, or a vertical diode, among the above-mentioned power semiconductor elements, can be used as the electronic component 210. In an electronic device including a vertical element, a voltage is applied to the vertical element by electrodes provided on both the upper and lower surfaces of the semiconductor substrate to turn it on.
[0308] Note that a vertical element refers to an element having a structure in which a current flows from one surface to the other surface of a semiconductor substrate when the element is turned on.
[0309] In such a vertical element, the current flows uniformly throughout the element, making it suitable for use in large current applications. In addition, the vertical element generates a large amount of heat due to the large current flowing through it. In other words, the problems caused by the difference in thermal expansion coefficients described above become more pronounced.
[0310] When the thermal conductor 1 is applied to such a vertical power semiconductor element, the above-mentioned effects of the present invention are particularly pronounced.
[0311] [3-2] Insulating materials The insulating member 230 is a member that is mainly made of an insulating material, and has a function of insulating the heat dissipation substrate 220 and the electronic component 210 from each other.
[0312] By providing such an insulating member 230, problems such as short circuits in electronic circuits can be effectively prevented.
[0313] There are no particular limitations on the insulating member 230 as long as it is made of a material having insulating properties, but it is preferable that it is made of a material containing a ceramic material.
[0314] This makes it possible to more reliably insulate the heat dissipation substrate 220 from the electronic component 210 .
[0315] The ceramic material constituting the insulating member 230 is not particularly limited, but is preferably at least one selected from the group consisting of aluminum nitride, boron nitride, silicon nitride, aluminum oxide, and zirconium oxide.
[0316] This makes it possible to more reliably insulate the heat dissipation substrate 220 from the electronic component 210, and since these ceramic materials themselves have relatively high thermal conductivity, the overall thermal conductivity can be improved.
[0317] An example of a ceramic material containing multiple components included in the above group is zirconia-reinforced alumina.
[0318] The thickness of the insulating member 230 is not particularly limited, but is preferably 0.10 mm or more and 2.0 mm or less, more preferably 0.15 mm or more and 1.5 mm or less, and even more preferably 0.20 mm or more and 1.0 mm or less.
[0319] This allows the heat from the electronic component 210 to be more effectively conducted to the heat dissipation board 220 via the thermal conductor 1 while improving the mechanical strength and insulating properties.
[0320] In the illustrated configuration, an insulating member 230 is divided into a plurality of divided bodies 231, and gaps 232 are provided between each of the divided bodies 231.
[0321] As a result, even if insulating member 230 expands due to heat from electronic component 210, the amount of thermal expansion can be absorbed by gap 232, and insulating member 230 can be suitably prevented from cracking or deforming due to heat.
[0322] The insulating member 230 is not limited to the configuration shown in the figure, and may be configured as a single plate-like body.
[0323] The insulating member 230 preferably has a metal film 233 at a portion where the insulating member 230 is joined to the thermal conductor 1 .
[0324] As a result, even if the portion of the insulating member 230 to be joined to the thermal conductor 1 is made of a material containing a ceramic material, the insulating member 230 can be suitably joined to the thermal conductor 1 by the solder layer 3 .
[0325] It is preferable that the insulating member 230 has a metallic film 233 at a portion where the electronic component 210 is to be joined.
[0326] As a result, even if the portion of the insulating member 230 to be joined to the electronic component 210 is made of a material containing a ceramic material, it can be suitably joined to the thermal conductor 1 by the solder 250.
[0327] It is preferable that the metallic film 233 is selectively formed on the surface of the insulating member 230 that is to be joined to the electronic component 210 (the upper surface in the illustrated configuration) and on the surface that is to be joined to the thermal conductor 1 (the lower surface in the illustrated configuration), and not formed on the side surfaces.
[0328] This makes it possible to reliably insulate the heat dissipation substrate 220 from the electronic component 210 and to more suitably obtain the above-mentioned effects.
[0329] [3-3] Heat dissipation board The heat dissipation substrate 220 is a substrate including a metal material.
[0330] When electronic component 210 is mounted on one surface side of heat dissipation substrate 220, heat generated from electronic component 210 is dissipated to the outside. In particular, in the configuration shown in Fig. 13, heat generated from electronic component 210 is dissipated to the outside from heat dissipation substrate 220 via insulating member 230 and thermal conductor 1.
[0331] Examples of metal materials that can be used to form the heat dissipation substrate 220 include copper, copper alloys, aluminum, and aluminum alloys.
[0332] Of these, it is preferable that the heat dissipation substrate 220 contains copper, which allows the heat from the electronic components 210 to be dissipated more efficiently.
[0333] The thickness of the heat dissipation substrate 220 is not particularly limited, but is preferably 0.1 mm or more and 20.0 mm or less, and more preferably 0.5 mm or more and 5.0 mm or less.
[0334] This can improve the heat dissipation properties of the heat dissipation board 220, and can also reduce the overall thickness of the electronic device 200 and improve the workability of the heat dissipation board 220 in contour processing, cutting, and the like.
[0335] The heat dissipation substrate 220 is bonded to the other surface side of the thermal conductor 1 via a solder layer 3 . This can improve the bonding strength between the heat dissipation board 220 and the thermal conductor 1. Also, the productivity of the electronic device 200 can be improved.
[0336] Furthermore, a cooling unit (not shown) may be attached to the surface of heat dissipation substrate 220 opposite to the surface on which electronic components 210 and insulating member 230 are mounted.
[0337] The cooling unit is a member for dissipating heat from the electronic component 210. Examples of such a cooling unit include a vapor chamber, a heat dissipation fin, a Peltier element, an air-cooled unit, and a water-cooled unit. This allows the heat from the electronic component 210 to be dissipated more efficiently.
[0338] As described above, the thermal conductor 1 is made of a material having excellent thermal conductivity, and is also excellent in flexibility and shape compatibility with the surfaces of the members to be joined. Therefore, even if the surfaces of the members to be joined have relatively large irregularities, the thermal conductor 1 can be suitably attached to these members. Therefore, the interface thermal resistance can be kept low, and the substantial thermal conductivity from the electronic component 210, which is a high-temperature member, to the heat dissipation board 220, which is a heat dissipation member, via the insulating member 230 and the thermal conductor 1 can be excellent.
[0339] This allows the heat from the electronic component 210, specifically the power semiconductor element, to be effectively dissipated, suppressing the occurrence of problems such as breakdown or malfunction of the power semiconductor element due to heat, and lengthening the product life of the power semiconductor element.
[0340] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these.
[0341] For example, in the above-mentioned embodiment, the bonded body of the present invention is typically described as a heat conductor having members bonded to both sides thereof, but it is sufficient that a member is bonded to at least one side thereof, and it is not necessary that a member is bonded to the other side thereof. Even in such a configuration, since a solder layer is also provided on the other side thereof, another member can be bonded to the other side thereof when necessary, and the same effect as described above can be obtained.
[0342] In addition, the above explanation has focused on the case where the heat conducting parts and joints that make up the heat conductor body are planar, but at least a portion of the heat conducting parts and joints that make up the heat conductor body may be non-planar, for example, curved or bent.
[0343] In addition, in the above explanation, a case where a hole is provided in each heat conducting portion constituting the heat conductor body is described as a representative example, but some of the multiple heat conducting portions constituting the heat conductor body may not need to have a hole.
[0344] Further, the heat conductive portion may be provided with a recess that does not penetrate the heat conductive portion in the thickness direction, i.e., a bottomed recess, instead of or in addition to the above-mentioned hole. Further, the heat conductive portion may not be provided with a recess.
[0345] Furthermore, the heat conductor body may have a configuration other than the heat conductive portion, joint portion, and gap portion described above.
[0346] The thermal conductor body and the bonded body are not limited to those manufactured by the above-mentioned methods. For example, the manufacturing method of the thermal conductor body or the manufacturing method of the bonded body may further include other steps (pre-treatment step, intermediate treatment step, post-treatment step, etc.) in addition to the above-mentioned steps. EXAMPLES
[0347] The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited to these. Treatments for which no temperature conditions were specified were carried out at 20°C.
[0348] [4] Manufacturing of thermal conductors The thermal conductors of the examples and comparative examples were produced as follows. Example 1 First, a sheet for forming a heat conductive portion, a nonwoven fabric composed of resin fibers, and a composition for forming a joint portion were prepared.
[0349] As the sheet for forming the thermally conductive portion, a commercially available graphite sheet material having holes formed therein was prepared.
[0350] The graphite sheet material used in this example had a thickness of 80 μm, and the flake graphite was oriented along the thickness direction of the graphite sheet material. In addition, near the surface of the graphite sheet material, the flake graphite was densely packed, and near the center of the graphite sheet material in the thickness direction, there were relatively many voids. In addition, there were no voids that penetrated the graphite sheet material in the thickness direction. In addition, the density of the graphite sheet material was 1.5 g / cm 3 In addition, the thermal conductivity of the graphite sheet in the in-plane direction at 20°C, measured by the transient hot wire method in accordance with JIS R 2616-2000, was 450 W / (m K).
[0351] The formation of holes in the graphite sheet material was carried out as follows. That is, a roll body on which a plurality of protrusions corresponding to the holes were formed in a staggered arrangement was pressed against the surface of the graphite sheet material to form a plurality of holes in the graphite sheet material. The holes thus formed were circular with a diameter of 200 μm and penetrated the graphite sheet material in the thickness direction. The center-to-center distance between adjacent holes was 700 μm.
[0352] In addition, a nonwoven fabric made of polyethylene terephthalate fiber as a resin fiber has a polyethylene terephthalate fiber thickness of 7 μm, a thickness of 20 μm, and a basis weight of 12 g / cm. 2 We have prepared a product that meets the following conditions.
[0353] In this example, the joint forming composition was made of CELEM ELASTOMER, a solvent-free, one-liquid type elastomer material.
[0354] The SERM Elastomer used in this example as the composition for forming a joint contains a cyclic molecule, a first polymer which has a linear molecular structure and encapsulates the cyclic molecule in a skewered manner, a polyrotaxane having blocking groups provided near both ends of the first polymer, and a second polymer, with the polyrotaxane and the second polymer bonded via the cyclic molecule, and becomes a flexible material when cured.
[0355] Next, the composition for forming a joint was applied to one side of the sheet for forming a heat conductive part using a kiss coater, and then the sheet for forming a heat conductive part to which the composition for forming a joint was applied was overlapped with a resin fiber sheet (nonwoven fabric) and wound up on a winding roll having a diameter of 20 cm at a speed of 2 m / min to obtain a rolled body.
[0356] When the joint forming composition was applied to the heat conductive part forming sheet, the joint forming composition penetrated into the inside of the holes and also penetrated through the holes into the voids provided near the center of the heat conductive part forming sheet in the thickness direction.
[0357] Furthermore, in the thermal conductor body obtained in this example, when observed from the lamination direction of the thermal conductive portions and the joint portions, the holes in the multiple thermal conductive portions were present so as not to overlap each other.
[0358] Next, the wound body was cut open by making an incision parallel to the axial direction of the winding roll using a cutter, and the wound body was removed from the winding roll to obtain a cut body. The obtained cut body was curved in its natural state, but the curvature of the inner peripheral surface of the cut body, i.e., the surface that had been in contact with the winding roll, was smaller than that when in contact with the winding roll, and the cut body was flatter than the wound body.
[0359] Next, the resulting cut body was sandwiched between two flat plates and pressed at 20 MPa such that the entire area corresponding to the outer circumferential surface of the wound body was in contact with one flat plate, and the entire area corresponding to the inner circumferential surface of the wound body was in contact with the other flat plate.
[0360] Next, in this state, while the cut body was pressed, a heat treatment was performed at 170°C for 10 hours to harden the curable resin material constituting the joint forming composition, thereby obtaining a thermal conductor body. Even after the thermal conductor body obtained in this way was released from the pressurized state, both of the two surfaces that had been in contact with the flat plate were flat and parallel to each other.
[0361] Next, the thermal conductor body was cut along the lamination direction to a thickness T of 0.5 mm, and then cut into a 4.0 cm square to obtain a sheet-like thermal conductor body of 4.0 cm x 4.0 cm x 0.5 mm.
[0362] The sheet-like thermal conductor body thus obtained had a plurality of thermally conductive parts and joints arranged alternately, with the thermally conductive parts and joints exposed on both main surfaces (see FIG. 2). The thermally conductive parts were made of flake-like graphite, and the joints were made of a flexible resin material. In the thermally conductive parts, the graphite was oriented so that its thickness direction was aligned with the thickness direction of the thermally conductive parts.
[0363] In the thermal conductor, the thickness of the thermal conductive portion obtained by the thermal conductive portion forming sheet was 80 μm, and the thickness of the joint portion made of the resin material was 40 μm. The surface roughness Ra of both main surfaces of the thermal conductor was 5.5 μm. The joint portion contained polyethylene terephthalate fibers as resin fibers together with the cured product of the curable resin material.
[0364] The compressive modulus of the flexible material constituting the thermal conductor body, i.e., the flexible material obtained by curing the above-mentioned joint forming composition (Cerm Elastomer), was measured at 20°C according to JIS K7181 and found to be 1.0-2.0 MPa. The compressive modulus was measured using an Autograph AGS-X (Shimadzu Corporation) at a measurement speed of 20% compression / min, and the compressive modulus was calculated from the slope of 10-20N.
[0365] Then, solder layers were formed on both main surfaces (4.0 cm x 4.0 cm surfaces) of the sheet-like thermal conductor body obtained as described above, as follows. That is, first, solder paste was printed on both main surfaces of the sheet-like thermal conductor body. Next, the thermal conductor body on which the solder paste was printed was sandwiched between two surface-treated metal plates, and heated and pressed at 0.1 MPa. Then, the metal plates were peeled off to obtain a thermal conductor having solder layers on both main surfaces of the thermal conductor body. The solder layer formed as described above was composed of 50% tin (melting point: 215°C), and the thickness of the solder layer was 100 μm. Also, it was confirmed by observation with an electron microscope that a part of the solder layer penetrated into the thermal conductor body. In addition, when the thickness of the part of the solder layer that penetrates into the thermal conductor body is T1 [μm] and the thickness of the part that does not penetrate into the thermal conductor body is T2 [μm], the value of T1 / T2 was 5.1.
[0366] Comparative Example 1 A sheet-shaped thermal conductor body measuring 4.0 cm×4.0 cm×0.5 mm was manufactured in the same manner as described in Example 1, and a solder layer was not formed on the sheet-shaped thermal conductor body, which was used as it was. In other words, the thermal conductor of this comparative example does not have a solder layer.
[0367] [5] Manufacturing of the joint The thermal conductor of Example 1 was sandwiched between two copper plates, and a pressure of 0.1 MPa was applied in the lamination direction, and a heat treatment was performed for 180 seconds to obtain a joint in which the copper plates were joined to both sides of the thermal conductor. In the joint obtained in this way, the thickness of the part of the solder layer that penetrated into the thermal conductor body was T3 [μm], and the thickness of the part that did not penetrate into the thermal conductor body was T4 [μm], and the value of T3 / T4 was 5.1.
[0368] [6] Evaluation The following items were evaluated: [6-1] Evaluation of actual thermal conductivity First, the bonded body according to Example 1 produced in [5] above was placed on a hot plate placed at room temperature, and heated by setting the hot plate to a temperature of 140°C. The surface temperature of the hot plate and the outer surface temperature of the bonded body (the temperature of the surface opposite to the surface in contact with the hot plate) were measured using a thermocouple, and the bonded body was left until both temperatures reached a steady state. Thereafter, the bonded body was heated while placed on the hot plate for another 2 minutes, and the temperature was measured to confirm that the temperature was stable. The temperatures at this point were taken as the steady surface temperature of the hot plate and the steady outer surface temperature of the bonded body.
[0369] Thereafter, heating was performed in the same manner as above, except that a copper plate, a thermal conductor according to Comparative Example 1, and a laminate in which copper plates were stacked (the copper plate and the thermal conductor were not joined) were used instead of the bonded body according to Example 1. The surface temperature of the hot plate and the outer surface temperature of the laminate (the temperature of the outer surface of the copper plate opposite to the surface in contact with the hot plate) were measured, and the laminate was left to stand until both temperatures reached a steady state. Thereafter, the laminate was heated while placed on the hot plate for another 2 minutes, the temperature was measured, and it was confirmed that the temperature was stable. The temperatures at this point were taken as the steady surface temperature of the hot plate and the steady outer surface temperature of the laminate.
[0370] As a result of the above measurement, in the laminate according to Comparative Example 1, the difference between the steady-state surface temperature of the hot plate and the steady-state outer surface temperature of the laminate was 6.4°C, whereas in the bonded body according to Example 1, the difference between the steady-state surface temperature of the hot plate and the steady-state outer surface temperature of the bonded body was 2.0°C, and it was found that the present invention has a significantly improved substantial thermal conductivity.
[0371] [6-2] Adhesion between the thermal conductor body and the solder layer A copper strand (wire rod) was soldered to the exposed surface of the copper plate opposite to the solder layer joined to one of the solder layers of the thermal conductor obtained in Example 1.
[0372] The thermal conductor to which the wire was joined was then fixed, and the wire was chucked with a tensile testing machine and pulled at a speed of 40 mm / min until it broke, to determine the tensile strength as an index of adhesion between the thermal conductor body and the solder layer.
[0373] The required tensile strength was a high value of 18N, confirming that the thermal conductor and the solder layer were in extremely close contact with each other. [Explanation of symbols]
[0374] 1: Thermal conductor 2: Thermal conductor body 3: Solder layer 4 :Void part 10: Heat conducting part 10a: First row 10b: Second column 10c: Heat conducting through-hole 11: Hole (recess) 20: Joint 21: Flexible material 22: Resin fiber 23: 1st page 24:Second side 50: Polyrotaxane 51: Cyclic molecules 52: First polymer 53: Blocking group 60: Second polymer 100:zygote 110: First member 120: Second member 200:Electronic equipment 210: Electronic parts 211: Metallic membrane 220: Heat dissipation board 230: Insulating materials 231: Divided body 232: Gap 233: Metallic membrane 250: Solder e 10 :Extending direction g 10 :interval T: Thickness T1: Thickness T2: Length T3: Thickness T4: Length t 10 :Thickness t 20 :Thickness V1: Normal direction w 10 :width θ1: angle θ2: angle
Claims
1. A thermal conductor comprising a thermal conductor body having a plurality of thermal conductive portions and a joint portion including a flexible material that joins the plurality of thermal conductive portions, a solder layer covering at least a portion of an outer surface of the thermal conductor body; A thermal conductor having two surfaces aligned in the thickness direction of the thermal conductor body, one of which is joined to a first member via the solder layer and the other of which is joined to a second member via the solder layer.
2. At least a portion of the solder layer penetrates into the thermal conductor body; 2. The thermal conductor according to claim 1, wherein the thickness of the solder layer that penetrates into the thermal conductor body is T1 [μm] and the thickness of the solder layer that does not penetrate into the thermal conductor body is T2 [μm], and the relationship T1 / T2 is satisfied: 0.005≦T1 / T2≦500.
3. 2. The thermal conductor according to claim 1, wherein the melting point of the solder constituting the solder layer is less than 300°C.
4. 4. The thermal conductor according to claim 3, wherein the solder layer contains tin (Sn) and at least one selected from the group consisting of silver (Ag), bismuth (Bi), copper (Cu) and zinc (Zn).
5. 2. The thermal conductor according to claim 1, wherein the thickness of the solder layer is 0.1 μm or more and 500 μm or less.
6. The thermal conductor according to claim 1 , wherein the thermal conductor body has anisotropic thermal conductivity.
7. The thermal conductor of claim 6, wherein the thermal conductivity of the thermal conductor body in a first direction perpendicularly connecting the pair of surfaces is higher than the thermal conductivity in a specified in-plane direction of at least one of the pair of surfaces.
8. The thermal conductor of claim 1 , wherein the thermally conductive portion comprises graphite.
9. A heat conductor body having a plurality of heat conductive portions and a joint portion including a flexible material that joins the plurality of heat conductive portions; a first member joined to the heat conductor body via a solder layer on one of two surfaces aligned in the thickness direction of the heat conductor body.
10. The joint body according to claim 9 , further comprising a second member joined to the heat conductor body via a solder layer on the other surface opposite to the one surface.
Citation Information
Patent Citations
Semiconductor device
JP2016072281A
Cited By
Heat conducting sheet
WO2026160140A1