Polar group-containing olefin copolymer, and method for producing the same
A novel polar group-containing olefin copolymer with a norbornene structural unit and metal carboxylate addresses the copolymerization challenges of α-olefins, offering improved adhesion and compatibility in multilayer films by enhancing glass transition temperatures.
Patent Information
- Application Number
- JP2023077656
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Existing olefin polymers, such as those based on α-olefins like propylene, face challenges in copolymerization with acrylic esters and acrylic acid, making it difficult to produce ionomers with sufficient adhesion and compatibility for multilayer films.
A novel polar group-containing olefin copolymer is developed, incorporating a norbornene structural unit with a metal carboxylate, produced through copolymerization with α-olefins using a transition metal catalyst, followed by conversion of alkoxycarbonyl groups to carboxyl groups and then to metal-containing carboxylates.
The resulting ionomer exhibits improved functionality with higher glass transition temperatures, enhancing adhesion and compatibility in multilayer films beyond traditional ethylene-based ionomers, particularly suitable for polypropylene-based films.
Smart Images

Figure 2024162290000016 
Figure 2024162290000017 
Figure 2024162290000018
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel polar group-containing olefin copolymer and a production method thereof, and more particularly to a novel polar group-containing olefin copolymer containing a norbornene structural unit having a metal carboxylate, and a production method thereof. [Background technology]
[0002] Among resin materials, olefin polymers such as ethylene polymers and propylene polymers are excellent in various properties such as physical properties and moldability, and are also highly economical and environmentally friendly, etc. Therefore, olefin polymers are very widely used and important industrial materials. However, since olefin polymers do not have polar groups, it has been difficult to apply them to applications requiring physical properties such as adhesion to other materials, printability, or compatibility with fillers. Therefore, in recent years, there has been an increasing need for polar group-containing olefin copolymers in which polar groups have been introduced into polyolefins, and various examples of such copolymers have been reported.
[0003] As one type of polar group-containing olefin copolymer, metal ion-containing polyolefins (ionomers) are known that utilize the cohesive force of metal ions to enhance the functionality of olefin polymers. Ionomers that use polyethylene as a base polymer are industrially produced. In recent years, particularly, starting from the development of copolymerization of ethylene and polar monomers by catalytic polymerization, linear polyethylene-based ionomers that apply this method have been developed (e.g., Patent Documents 1 and 2).
[0004] The main application of ionomers with polyethylene as the base polymer is as a multilayer film material. However, polyethylene-based ionomers have the problem that unless the adjacent layers are ethylene-based polymers, the layers do not have sufficient affinity with each other and are prone to peeling. For example, to use in olefin-based multilayer films based on α-olefins other than ethylene, such as propylene-based ionomers, olefin-based ionomers based on α-olefins other than ethylene, such as propylene-based ionomers, are desirable. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-112623 A [Patent Document 2] JP 2020-117712 A Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, in order to improve the performance of olefin-based polymers based on α-olefins other than ethylene, ionomers based on α-olefins other than ethylene are desired. However, it is difficult to copolymerize α-olefins other than ethylene such as propylene with acrylic acid esters or acrylic acid. Therefore, it is difficult to obtain an ionomer from α-olefins other than ethylene such as propylene by converting the ester group or carboxy group of a copolymer with acrylic acid esters or acrylic acid to a carboxylate, as with ethylene. Therefore, it has been difficult to produce ionomers based on α-olefins other than ethylene, such as ionomers based on polypropylene as a base polymer.
[0007] In view of the above-mentioned problems in the conventional art, an object of the present invention is to provide a novel polar-group-containing olefin copolymer containing a norbornene structural unit having a metal carboxylate, which is a novel ionomer, in order to enhance the functionality of an olefin polymer based on an α-olefin other than ethylene, and a method for producing the same. [Means for solving the problem]
[0008] The present invention relates to the following [1] to [6]. [1] A structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms; and a structural unit (B) represented by the following general formula (I): The polar group-containing olefin copolymer is characterized in that at least a part of the structural unit (B) is represented by the following general formula (I), in which M is a metal ion:
[0009] [ka] (In general formula (I), R 1 is a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms, n is an integer of 0 to 3, and M is a hydrogen atom or a metal ion.
[0010] [2] The polar group-containing olefin copolymer according to [1] above, characterized in that in the general formula (I), the n is 0. [3] The polar group-containing olefin copolymer according to [1] or [2], wherein the metal ion in M is at least one selected from the group consisting of a lithium ion, a sodium ion, a potassium ion, a calcium ion, a magnesium ion, an aluminum ion, and a zinc ion. [4] The polar-group-containing olefin copolymer according to any one of the above [1] to [3], wherein the structural unit (A) is a structural unit derived from propylene.
[0011] [5] A method for producing the polar group-containing olefin copolymer according to any one of the above [1] to [4], comprising the steps of: A method for producing a polar group-containing olefin copolymer, comprising the steps of: copolymerizing at least one olefin having 3 to 20 carbon atoms with at least one norbornene having an alkoxycarbonyl group in the presence of a transition metal catalyst of Groups 4 to 10 of the periodic table; obtaining a carboxy group-containing copolymer by converting the alkoxycarbonyl groups of the obtained copolymer to carboxy groups; and reacting the carboxy group-containing copolymer with a metal ion to convert at least a portion of the carboxy groups into a metal-containing carboxylate. [6] The method for producing a polar group-containing olefin copolymer according to [5] above, wherein the transition metal catalyst is a transition metal catalyst in which a chelating phosphine compound is coordinated to nickel or palladium metal. Effect of the Invention
[0012] According to the present invention, it is possible to provide a novel polar group-containing olefin copolymer containing a norbornene structural unit having a metal carboxylate, which is a novel ionomer, for improving the functionality of an olefin polymer based on an α-olefin other than ethylene, and a production method thereof. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 shows the 13C NMR spectrum of the polar group-containing olefin copolymer e1 of Example 1. [Diagram 2] FIG. 2 shows an expanded view of the chemical shifts 42 ppm-12 ppm of the 13C NMR spectrum of FIG. [Diagram 3] FIG. 3 shows an enlarged view of the chemical shifts 79.9 ppm-78.8 ppm of the 13C NMR spectrum of FIG. [Figure 4] FIG. 4 shows an expanded view of the chemical shifts 18.5 ppm-22.0 ppmppm of the 13C NMR spectrum of FIG. [Diagram 5]FIG. 5 shows the FTIR spectrum of the polar group-containing olefin copolymer h1 of Example 1. [Figure 6] FIG. 6 shows the FTIR spectrum of the polar group-containing olefin copolymer (ionomer) 1 of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The polar group-containing olefin copolymer of the present invention will be described in detail below for each item. In this specification, the term "(meth)acrylic" refers to both acrylic and methacrylic. In addition, in this specification, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower and upper limits. In addition, in this specification, the upper and lower limits indicating a numerical range can adopt any combination.
[0015] 1. Polar group-containing olefin copolymer The polar group-containing olefin copolymer of the present invention comprises a structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms, and a structural unit (B) represented by the following general formula (I): At least a part of the structural unit (B) is characterized in that M in the following general formula (I) is a metal ion.
[0016] [ka] (In general formula (I), R 1 is a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms, n is an integer of 0 to 3, and M is a hydrogen atom or a metal ion.
[0017] The polar group-containing olefin copolymer of the present invention is a novel polar group-containing olefin copolymer containing a norbornene structural unit having a metal carboxylate, and is a novel ionomer, which contributes to improving the functionality of olefin polymers based on α-olefins other than ethylene.
[0018] As mentioned above, it is difficult to copolymerize α-olefins other than ethylene such as propylene with acrylic acid esters or acrylic acid. Therefore, it is difficult to obtain an ionomer from a copolymer of α-olefins other than ethylene such as propylene with acrylic acid esters or acrylic acid, as with ethylene. Therefore, it has been difficult to produce ionomers based on α-olefins other than ethylene, such as ionomers based on polypropylene as a base polymer. In contrast, in the present invention, an alkoxycarbonyl group-containing norbornene compound is used as a comonomer and copolymerized with an α-olefin other than ethylene, such as propylene, to obtain a copolymer in which an alkoxycarbonyl group has been introduced into polypropylene or the like. By converting the alkoxycarbonyl group contained in the copolymer to a metal-containing carboxylate, an ionomer based on an α-olefin other than ethylene, such as an ionomer having polypropylene as the base polymer, can be produced. The novel ionomer of the present invention has a metal-containing carboxylate in the structural unit derived from norbornene, and therefore, in an olefin-based polymer based on an α-olefin other than ethylene, the content of the metal-containing carboxylate can be easily increased. The novel ionomer of the present invention is capable of having a higher glass transition temperature (Tg) than conventional ionomers based on polyethylene as a base polymer, and by containing norbornene-derived structural units, the thermal properties of the ionomer can be controlled by adjusting the content thereof. In addition, the novel ionomer of the present invention can be suitably used in polyolefin multi-layer films based on α-olefins other than ethylene, such as polypropylene-based films. In addition to the applications that have been used for conventional ethylene-based ionomers, the range of applications can be further expanded by taking advantage of the characteristics of the ionomer, due to its higher glass transition temperature.
[0019] (1) Structural unit (A) The structural unit (A) is a structural unit derived from at least one olefin having 3 to 20 carbon atoms. The monomer (A) used in the present invention from which the structural unit (A) is derived is at least one olefin having 3 to 20 carbon atoms. The olefin having 3 to 20 carbon atoms may be a chain olefin or a cyclic olefin, and examples thereof include at least one selected from the group consisting of α-olefins having 3 to 20 carbon atoms and cyclic olefins having 4 to 20 carbon atoms. The α-olefin having 3 to 20 carbon atoms used in the present invention is an α-olefin having 3 to 20 carbon atoms represented by the structural formula: CH2=CHR (wherein R is a hydrocarbon group having 1 to 18 carbon atoms, which may have a linear structure or may be branched), and more preferably an α-olefin having 3 to 12 carbon atoms. Examples of the cyclic olefin having 4 to 20 carbon atoms include cyclobutene, cyclopentene, cyclohexene, and norbornene.
[0020] Specific examples of the monomer (A) include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, 4-methyl-1-pentene, and norbornene, etc. From the viewpoint of the production efficiency of the polymer, the monomer (A) is preferably one or more selected from the group consisting of propylene, 1-butene, and norbornene, and more preferably propylene. The structural unit (A) may be of one type alone or of two or more types.
[0021] Combinations of the two types include structural units derived from propylene-1-butene, propylene-1-hexene, propylene-1-octene, propylene-norbornene, and the like. Examples of combinations of the three types include structural units derived from propylene-1-butene-1-hexene and propylene-1-butene-1-octene.
[0022] In the present invention, the monomer (A) used in the structural unit (A) preferably contains propylene as an essential component and may further contain one or more α-olefins having 4 to 20 carbon atoms, if necessary. The amount of propylene in the monomer (A) may be 65 to 100 mol %, 80 to 100 mol %, 90 to 100 mol %, or 100 mol %, relative to 100 mol % of the entire monomer (A).
[0023] (2) Structural unit (B) The structural unit (B) is a structural unit represented by the following general formula (I), and in at least a part of the structural unit (B), M in the following general formula (I) is a metal ion.
[0024] [ka] (In general formula (I), R 1 is a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms, n is an integer of 0 to 3, and M is a hydrogen atom or a metal ion.
[0025] In general formula (I), R 1 Examples of the hydrocarbon group having 1 to 4 carbon atoms in the formula (1) include linear, branched, and cyclic saturated or unsaturated aliphatic hydrocarbon groups. Examples of the hydrocarbon group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, an ethenyl group, a propenyl group, a butenyl group, a cyclopropyl group, and a cyclobutyl group. In general formula (I), R 1 may be a hydrogen atom, a methyl group, or an ethyl group, or may be a hydrogen atom or a methyl group, or may be a hydrogen atom, from the standpoint of ease of synthesis or procurement.
[0026] In general formula (I), n represents the number of methylene groups. When n is 0, it represents a structure in which CO2M is bonded directly to the norbornene skeleton without a methylene group, and when n is 3, it represents a structure in which CO2M is bonded to the norbornene skeleton via a trimethylene group (-CH2CH2CH2-). In general formula (I), n is an integer of 0 to 3, but may be an integer of 0 to 2, or an integer of 0 to 1, and may be 0 from the viewpoint of ease of synthesis or procurement.
[0027] In the general formula (I), M is a hydrogen atom or a metal ion, and in at least a part of the structural units (B), M is a metal ion. That is, the polar group-containing olefin copolymer of the present invention necessarily contains a metal ion.
[0028] In the general formula (I), the metal ion in M is not particularly limited and may include metal ions used in conventionally known ethylene-based ionomers. Among them, the metal ion in M may be at least one metal ion selected from the group consisting of Groups 1, 2, 12, and 13 of the periodic table, and may be at least one metal ion selected from the group consisting of lithium ion, sodium ion, potassium ion, rubidium ion, cesium ion, calcium ion, magnesium ion, strontium ion, barium ion, aluminum ion, and zinc ion, and is preferably at least one metal ion selected from the group consisting of lithium ion, sodium ion, potassium ion, calcium ion, magnesium ion, aluminum ion, and zinc ion. In the general formula (I), M can contain one or a mixture of two or more of these metal ions. When M is a divalent or higher metal ion, the counter anion may be a carboxylate of the copolymer or another anion.
[0029] M in the general formula (I) is a hydrogen atom or a metal ion, and necessarily contains a metal ion as a part thereof, but all of M does not have to be a metal ion. The content of the metal ion can be appropriately selected according to the application of the polar group-containing olefin copolymer of the present invention. The content of the metal ion, i.e., the proportion of M in the general formula (I) that is a metal ion (neutralization degree), may be 5 mol% or more, 10 mol% or more, or 20 mol% or more, and the upper limit may be 100 mol%, but may be 90 mol% or less, or 80 mol% or less, based on 100 mol% of the entire structural unit (B). In the polar group-containing olefin copolymer of the present invention, the proportion of metal ions in M in the general formula (I) (degree of neutralization) can be determined by Fourier transform infrared spectroscopy (FTIR). -1 ~1705cm -1 When M is a metal ion, the C=O stretching vibration peak is at 1550 cm -1 ~1600cm -1 The ratio of the absorbance intensities of these two compounds can be used to determine the proportion of metal ions in M (degree of neutralization). Specifically, the degree of neutralization can be measured by the method described in the Examples below.
[0030] (3) Other structural units (C) The polar group-containing olefin copolymer of the present invention may further contain other structural units (C) different from the structural units (A) and (B). The other structural units (C) may be, for example, structural units derived from monomer (C) that are copolymerizable with monomer (A) in the presence of a transition metal catalyst of Groups 4 to 10 of the periodic table described below. Examples of such structural units derived from monomer (C) include structural units represented by the following general formula (I'), 3-butenyl acetate, 3-cyanopropene, 3-chloropropene, 3-(methylthio)-1-propene, 3-(methylsulfinyl)-1-propene, 3-(methylsulfonyl)-1-propene, 2-propene-1-methyl sulfonate, 2-propenylphosphonic acid dimethyl, 5-methoxycarbonyl-2-norbornene, 2-norbornene-5-methanol, 9-epoxy-1-decene, vinylene carbonate, undecenoic acid ester, and undecenol. The polar group-containing olefin copolymer of the present invention does not need to contain structural units derived from ethylene.
[0031] [ka] (In general formula (I'), R 1 , n, and R 2 is the same as in general formula (1) described later.)
[0032] (4) Polar group-containing olefin copolymer The polar-group-containing olefin copolymer of the present invention contains a structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms, and a structural unit (B) represented by the above general formula (I). The polar-group-containing olefin copolymer of the present invention must contain at least one type of structural unit (A) and at least one type of structural unit (B), and must contain structural units derived from a total of two or more types of monomers.
[0033] In the present invention, the content of the structural unit (A) in the polar group-containing olefin copolymer may be appropriately selected according to the desired physical properties. The content of the structural unit (A) in the polar group-containing olefin copolymer may be, for example, 85.0 mol% or more, 90.0 mol% or more, preferably 93.0 mol% or more, 95.0 mol% or more, or 96.0 mol% or more, based on 100 mol% of the total structural units. On the other hand, the upper limit may be 99.99 mol% or less, 99.9 mol% or less, 99.0 mol% or less, or 98.0 mol% or less.
[0034] The content of the structural unit (B) in the polar group-containing olefin copolymer may be appropriately selected according to the average molecular weight and the desired physical properties. The content of the structural unit (B) in the polar group-containing olefin copolymer may be, for example, 0.01 mol% or more, 0.1 mol% or more, 1.0 mol% or more, or 2.0 mol% or more, based on 100 mol% of the total structural units. On the other hand, the upper limit may be 6.0 mol% or less, preferably 5.0 mol% or less, or 4.0 mol% or less.
[0035] The polar group-containing olefin copolymer of the present invention may further contain at least one other structural unit (C). When the polar group-containing olefin copolymer of the present invention contains other structural units (C), the upper limit of the total content of the other structural units (C) in the polar group-containing olefin copolymer may be 10 mol% or less, preferably 6 mol% or less, more preferably 2 mol% or less, based on 100 mol% of the total structural units. The polar group-containing olefin copolymer of the present invention may have a total content of other structural units (C) of 0 mol%. That is, the total content of the structural units (A) and (B) in the polar group-containing olefin copolymer may be 90 mol% or more, 94 mol% or more, 98 mol% or more, or 100 mol% based on 100 mol% of the total structural units.
[0036] A structure derived from one molecule of each monomer is defined as one structural unit in the polar group-containing olefin copolymer. The amount of structural units is the ratio of each structural unit expressed in mol % when the total structural units in the polar group-containing olefin copolymer is taken as 100 mol %.
[0037] The polar group-containing olefin copolymer of the present invention may be a random copolymer, block copolymer, graft copolymer, etc., of the structural unit (A), the structural unit (B), and other structural units contained as necessary. Among these, a random copolymer that can contain a large amount of the structural unit (B) may be used.
[0038] The amount of structural units can be controlled by the following method. 1) Selection of catalyst 2) The amount of monomer that derives each structural unit added during polymerization 3) Polymerization pressure 4) Polymerization temperature As a specific means for increasing the amount of the structural unit (B) in the copolymer, it is effective to increase the amount of the monomer (B) added during polymerization, decrease the amount of the monomer (A), increase the polymerization temperature, etc. For example, it is required to adjust these factors and control them to the desired copolymer region.
[0039] The amount of structural units in the polar group-containing olefin copolymer of the present invention is 1 H-NMR spectrum and 13 The C-NMR spectrum can be measured by the method described in the Examples below.
[0040] The weight average molecular weight (Mw) of the polar group-containing olefin copolymer in the present invention is usually in the range of 1,000 to 2,000,000, preferably 2,000 to 1,500,000, more preferably 3,000 to 1,000,000, more preferably 4,000 to 800,000, and even more preferably 5,000 to 800,000. When Mw is 1,000 or more, physical properties such as mechanical strength and impact resistance tend to be sufficient, and when Mw is 2,000,000 or less, it is easy to prevent molding processing from becoming difficult.
[0041] The number average molecular weight (Mn) of the polar group-containing olefin copolymer of the present invention is usually in the range of 1,000 to 1,000,000, preferably 1,000 to 750,000, more preferably 1,500 to 500,000, more preferably 2,000 to 400,000, and even more preferably 2,500 to 400,000. When Mn is 500 or more, physical properties such as mechanical strength and impact resistance tend to be sufficient, and when Mn is 1,000,000 or less, it is easy to prevent molding processing from becoming difficult.
[0042] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the polar group-containing olefin copolymer of the present invention may be in the range of 1.5 to 5.0, preferably 2.0 to 4.0, and more preferably 2.2 to 3.5. When Mw / Mn is 1.5 or more, various processability tends to be sufficient, and when it is 5.0 or less, mechanical properties tend to be good.
[0043] In the present invention, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are determined by gel permeation chromatography (GPC). In the present invention, the GPC can be measured by the method described in the Examples below.
[0044] The glass transition temperature (Tg) of the polar group-containing olefin copolymer of the present invention may be in the range of −20° C. to 30° C., or may be in the range of −10° C. to 20° C. The glass transition temperature (Tg) of the polar group-containing olefin copolymer of the present invention can be appropriately adjusted by the type of monomer of the olefin copolymer and the selection and content of the norbornene compound. The glass transition temperature (Tg) in the present invention is the midpoint glass transition temperature measured by differential scanning calorimetry (DSC) in accordance with JIS K7121-2012. In the present invention, the glass transition temperature (Tg) can be measured by the method described in the Examples below.
[0045] 2. Method for producing polar group-containing olefin copolymer The method for producing the polar group-containing olefin copolymer of the present invention is a method for producing the polar group-containing olefin copolymer of the present invention, and is characterized by comprising the steps of: copolymerizing at least one olefin having 3 to 20 carbon atoms with at least one norbornene having an alkoxycarbonyl group in the presence of a transition metal catalyst of Groups 4 to 10 of the periodic table; obtaining a carboxy group-containing copolymer by converting the alkoxycarbonyl groups of the obtained copolymer to carboxy groups; and reacting the carboxy group-containing copolymer with a metal ion to convert at least a portion of the carboxy groups into a metal-containing carboxylate.
[0046] (1) Copolymerization process The method for producing a polar group-containing olefin copolymer of the present invention first includes a step of copolymerizing at least one olefin having 3 to 20 carbon atoms with at least one norbornene having an alkoxycarbonyl group in the presence of a transition metal catalyst of Groups 4 to 10 of the periodic table.
[0047] (1-1) Catalyst The polar group-containing olefin copolymer of the present invention may be polymerized in the presence of a catalyst containing a transition metal catalyst of Groups 4 to 10 of the periodic table. In this case, it is easy to produce a copolymer containing the structural unit (A) and the structural unit (Bp) derived from at least one type of norbornene having an alkoxycarbonyl group. The structural unit (Bp) derived from at least one type of norbornene having an alkoxycarbonyl group can be a structural unit of a precursor of the structural unit (B).
[0048] The catalyst containing a transition metal catalyst of Groups 4 to 10 of the periodic table is not particularly limited as long as it is capable of polymerizing at least one olefin having 3 to 20 carbon atoms, which derives the structural unit (A), and at least one norbornene having an alkoxycarbonyl group. The transition metal catalyst may be, for example, a transition metal compound of Groups 5 to 10 of the periodic table, and further includes a transition metal compound of Groups 5 to 10 of the periodic table having a chelating ligand.
[0049] Specific examples of preferred transition metals include titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, iron, platinum, ruthenium, cobalt, rhodium, nickel, and palladium. Among these, preferred are transition metals of Groups 8 to 10, and more preferred are transition metals of Group 10. Examples of the transition metals of Group 10 include nickel, palladium, and platinum. Particularly preferred are nickel (Ni) and palladium (Pd). These transition metals may be used alone or in combination.
[0050] Chelating ligands have at least two atoms selected from the group consisting of P, N, O, C, and S, and include ligands that are bidentate or multidentate, and are electronically neutral or anionic. Exemplary structures are given in the review by Brookhart et al. (Chem. Rev., 2000, 100, 1169). Preferably, the bidentate anionic P, O ligand includes, for example, phosphorus sulfonate, phosphorus carboxylate, phosphorus phenoxide, phosphorus alkoxide, and phosphorus enolate. Also, the bidentate anionic N, O ligand includes, for example, salicylaldiminate and pyridine carboxylate. And, the bidentate anionic C, O ligand includes, for example, carbene phenoxide, carbene alkoxide, and carbene carboxylate. Other examples include diimine ligand, diphenoxide ligand, and diamide ligand.
[0051] From the viewpoints of the production efficiency of the polymer, the molecular weight of the polymer, and copolymerizability with at least one of the monomer (A) and norbornene having an alkoxycarbonyl group, the catalyst containing a transition metal is preferably a catalyst containing a late transition metal selected from the group consisting of transition metals of Groups 8 to 10. Among them, a catalyst containing a transition metal of Group 10 is preferable. Furthermore, a catalyst containing a transition metal of Group 10 is preferable, and has a chelating ligand containing one or more phosphorus atoms or oxygen atoms as a coordination point to the transition metal of Group 10.
[0052] From the viewpoints of the production efficiency of the polymer, the molecular weight of the polymer, and copolymerizability with at least one of the monomer (A) and norbornene having an alkoxycarbonyl group, the catalyst containing a transition metal may be at least one selected from the group consisting of compounds represented by the following general formula (101): Also, the transition metal catalyst may be a transition metal catalyst in which a chelating phosphine compound or a chelating carbene compound is coordinated to nickel or palladium metal.
[0053] [ka] (In general formula (101), M represents a Group 10 transition metal. Q represents a divalent group shown in "[ ]" of A[-S(=O)2-O-]M, A[-C(=O)-O-]M, A[-O-]M, A[-P(=O)(R)-O-]M, or A[-S-]M, and R represents a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent (however, A and M on both sides are written to indicate the bonding direction of the group). A is a divalent hydrocarbon group having 1 to 30 carbon atoms which links Q and the phosphorus atom and may have a substituent. L represents a zero-valent ligand which can be removed from the metal. R 11 R represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. 12 and R 13 R each independently represents a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. 11 and L may form a ring, R 12 and R 13 may form a ring, R 12 or R 13 may be bonded to A to form a ring.
[0054] In the general formula (101), M represents a Group 10 transition metal, and among these, Ni or Pd is preferable, and among these, Pd is preferable from the viewpoint of production efficiency of the copolymerization of the present invention. Q represents a divalent group represented by -S(=O)2-O-, -C(=O)-O-, -O-, -P(=O)(R)-O-, or -S-, and is a moiety that coordinates one electron to M. The left side of each of the groups is bonded to A, and the right side is bonded to M. Among these, in terms of catalytic activity, Q is particularly preferably -S(=O)2-O-. R represents a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent, and R 11 The substituent may be the same as the hydrocarbon group having 1 to 30 carbon atoms in the above formula (1).
[0055] A is a divalent hydrocarbon group having 1 to 30 carbon atoms that links Q to the phosphorus atom, and the hydrocarbon group may have a substituent. The divalent hydrocarbon group having 1 to 30 carbon atoms is preferably a divalent hydrocarbon group having 1 to 12 carbon atoms, more preferably an alkylene group or an arylene group, and particularly preferably an arylene group.
[0056] Examples of the substituent of the hydrocarbon group in A include a halogen atom, -OR α , -CO2R α , -CO2M', -CON(R β )2, -COR α , -SR α , -SO2R α , -SOR α , -OSO2R α , -PO(OR α ) 2-y (R β ) y , -CN, -NHR α , -N(R α )2, -Si(OR β ) 3-x (R β ) x , -OSi(OR β ) 3-x (R β ) x , -NO2, -SO3M', -PO3M'2, -P(O)(OR α ) 2M′, or an epoxy-containing group, etc. (wherein R β represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, R α represents a hydrocarbon group having 1 to 20 carbon atoms, M' represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium, x represents an integer of 0 to 3, and y represents an integer of 0 to 2). The hydrocarbon group having 1 to 20 carbon atoms is R 11 Examples of the hydrocarbon groups having 1 to 30 carbon atoms which may have a substituent in the above formula include the same hydrocarbon groups having 1 to 20 carbon atoms.
[0057] Examples of the divalent hydrocarbon group having 1 to 30 carbon atoms represented by A include the following formulae (a-1) to (a-7). In the following formulae, R 101R are each independently a hydrogen atom, a hydrocarbon group having 1 to 30 carbon atoms, or a substituent. 101 The hydrocarbon group having 1 to 30 carbon atoms is R 11 Examples of the hydrocarbon group having 1 to 30 carbon atoms, which may have a substituent, are the same as those in the above-mentioned formula (1). Of the hydrocarbon groups having 1 to 30 carbon atoms, hydrocarbon groups having 1 to 20 carbon atoms are preferred, and hydrocarbon groups having 1 to 10 carbon atoms are more preferred. The divalent hydrocarbon group having 1 to 30 carbon atoms for A may be, among others, the following formula (a-7) in terms of catalytic activity.
[0058] [ka]
[0059] L represents a zero-valent ligand that can be removed from the metal. L is preferably a compound having an electron donating group and capable of stabilizing the metal complex by coordinating with the transition metal M. L may be a hydrocarbon compound having 1 to 20 carbon atoms and containing at least one atom selected from the group consisting of oxygen atom, nitrogen atom, and sulfur atom as an atom capable of coordinating with the transition metal, or a hydrocarbon compound having a carbon-carbon unsaturated bond capable of coordinating with the transition metal and optionally containing a heteroatom. L preferably has 1 to 16 carbon atoms, more preferably 1 to 10 carbon atoms.
[0060] Preferred examples of L include pyridines, piperidines, alkyl ethers, aryl ethers, alkylaryl ethers, cyclic ethers, alkylnitrile derivatives, arylnitrile derivatives, alcohols, amides, aliphatic esters, aromatic esters, amines, and cyclic unsaturated hydrocarbons.
[0061] An example of L having a sulfur atom is dimethyl sulfoxide (DMSO). Examples of L having a nitrogen atom include trialkylamines in which the alkyl group has 1 to 10 carbon atoms, dialkylamines in which the alkyl group has 1 to 10 carbon atoms, pyridine, 2,6-dimethylpyridine (also known as 2,6-lutidine), aniline, 2,6-dimethylaniline, 2,6-di-propylaniline, N,N,N',N'-tetramethylethylenediamine (TMEDA), 4-(N,N-dimethylamino)pyridine (DMAP), acetonitrile, benzonitrile, quinoline, and 2-methylquinoline. Examples of L having an oxygen atom include diethyl ether, tetrahydrofuran, and 1,2-dimethoxyethane. From the viewpoints of the stability and catalytic activity of the complex, L is preferably dimethyl sulfoxide (DMSO), pyridine, 2,6-dimethylpyridine (also known as 2,6-lutidine), or N,N,N',N'-tetramethylethylenediamine (TMEDA), and more preferably dimethyl sulfoxide (DMSO) or 2,6-dimethylpyridine (also known as 2,6-lutidine).
[0062] R 11 represents a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. R 11 Examples of the halogen atom in include a fluorine atom, a chlorine atom, and a bromine atom.
[0063] R 11 Examples of the hydrocarbon group in the optionally substituted hydrocarbon group having 1 to 30 carbon atoms include linear, branched and cyclic saturated or unsaturated aliphatic hydrocarbon groups, aromatic hydrocarbon groups, and combinations thereof. Examples of the hydrocarbon group having 1 to 30 carbon atoms include a methyl group, an ethyl group, a 1-propyl group, a 1-butyl group, a 1-pentyl group, a 1-hexyl group, a 1-heptyl group, a 1-octyl group, a 1-nonyl group, a 1-decyl group, a t-butyl group, a tricyclohexylmethyl group, a 1,1-dimethyl-2-phenylethyl group, an i-propyl group, a 1-dimethylpropyl group, a 1,1,2-trimethylpropyl group, a 1,1-diethylpropyl group, a 1-phenyl-2-propyl group, an i-butyl group, a 1,1-dimethylbutyl group, a 2-pentyl group, a 3-pentyl group, a 2-hexyl group, a 3-hexyl group, a 2-ethylhexyl group, a 2-heptyl group, a 3-heptyl group, a 4-heptyl group, a 2-propylheptyl group, a Examples of such alkyl groups include aryl, 2-octyl, 3-nonyl, cyclopropyl, cyclobutyl, cyclopentyl, methylcyclopentyl, cyclohexyl, methylcyclohexyl, cycloheptyl, cyclooctyl, cyclododecyl, 1-adamantyl, 2-adamantyl, exo-norbornyl, endo-norbornyl, 2-bicyclo[2.2.2]octyl, decahydronaphthyl, menthyl (2-i-propyl-5-methylcyclohexyl), neomenthyl, neopentyl, 5-decyl, phenyl, naphthyl, anthracenyl, fluorenyl, tolyl, xylyl, benzyl, and p-ethylphenyl. R 11 The substituent in the optionally substituted hydrocarbon group having 1 to 30 carbon atoms in the above may be the same as the substituent in the hydrocarbon group in the above A.
[0064] R 11 is preferably a hydrocarbon group having 1 to 20 carbon atoms, a halogen-substituted hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group having 1 to 20 carbon atoms substituted with an alkoxy group or an aryloxy group.
[0065] The polymerization reaction in the present invention is carried out by reacting M and R 11 It is believed that the reaction is initiated by the insertion of the above-mentioned olefin such as propylene or a copolymerizable monomer thereof into the bond of R 11If the number of carbon atoms in R is too large, the initiation reaction tends to be inhibited. 11 The group preferably has 1 to 16 carbon atoms, excluding the carbon atoms contained in the substituent, and more preferably has 1 to 10 carbon atoms. R 11 Specifically, more preferably, the aryl group is an alkyl group having 1 to 3 carbon atoms, a benzyl group, a trifluoromethyl group, a pentafluorophenyl group, a 1-(methoxymethyl)ethyl group, a 1-(ethoxymethyl)ethyl group, a 1-(phenoxymethyl)ethyl group, or a 1-(2,6-dimethylphenoxymethyl)ethyl group, and even more preferably, a methyl group or a benzyl group. In addition, R 11 and L may form a ring. An example of such a ring is a cyclooct-1-enyl group, which is also a preferred embodiment of the present invention.
[0066] R 12 and R 13 each independently represents a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. R 12 and R 13 The hydrocarbon group having 1 to 30 carbon atoms which may have a substituent in R 11 The same can be mentioned.
[0067] R 12 and R 13 is in the vicinity of the transition metal M and exerts steric and / or electronic interactions with the transition metal M. In order to exert such effects, R 12 and R 13 The bulkier the better. 12 and R 13 The preferred carbon number is 3 to 30, and even more preferably 6 to 20.
[0068] R 12 and R 13 are preferably an optionally substituted alkyl group having 3 to 10 carbon atoms, or an optionally substituted cycloalkyl group having 6 to 20 carbon atoms. R 12and R 13 In the above formula, the alkyl group having 3 to 10 carbon atoms is preferably an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group or a t-butyl group.
[0069] R 12 and R 13 Examples of the cycloalkyl group having 6 to 20 carbon atoms which may have a substituent include a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, an adamantyl group, and the like which may have a substituent and which may be substituted with a linear or branched alkyl group having 3 to 10 carbon atoms. Also, it may be, for example, a cycloalkyl group described in paragraphs
[0104] to
[0113] of JP2018-141138A (X in paragraphs
[0104] to
[0113] of JP2018-141138A indicates the bonding position of P (phosphorus atom) in general formula (101) of the present invention).
[0070] R 12 and R 13 Among these, from the viewpoint of controlling the molecular weight of the polymer and the copolymerizability with the polar monomer, it is more preferable that is a cyclohexyl group substituted with a linear or branched alkyl group having 3 to 10 carbon atoms, or an adamantyl group, and among these, it is preferable that is a 2-i-propyl-5-methylcyclohexyl group (menthyl group) or an adamantyl group.
[0071] R 12 and R 13 may be bonded to A to form a ring structure. Specific examples include structures described in paragraphs 0120 to 0121 of JP 2018-141138 A (examples here include the substituent R 12 and A are bonded to form a ring structure, P and Q are the same as those in the general formula (101) of the present invention, and R 17 is R in the general formula (101) of the present invention. 13 is synonymous with R 104 is R in the general formula (101) of the present invention. 101 (Same meaning as above.)
[0072] Among the compounds represented by the general formula (101) of the present invention, a compound represented by the following general formula (102) is preferred from the viewpoint of production efficiency of the copolymer.
[0073] [ka] (In general formula (102), M, L, R 11 , R 12 and R 13 are the same as those in the general formula (101), and R 111 , R 112 , R 113 and R 114 are each independently a hydrogen atom, a hydrocarbon group having 1 to 30 carbon atoms, or a substituent.
[0074] In general formula (102), R 111 , R 112 , R 113 and R 114 The hydrocarbon group and the substituent having 1 to 30 carbon atoms in R 11 and A may be similar to those described above. R 111 , R 112 , R 113 and R 114 may all be hydrogen atoms. R 111 The bulkier the polymer, the higher the molecular weight of the polymer. 111 may be appropriately selected from the substituents such as a t-butyl group, a trimethylsilyl group, a phenyl group, a 9-anthracenyl group, a 4-t-butylphenyl group, a 2,4-di-t-butylphenyl group, a pentafluorophenyl group, and the like.
[0075] The transition metal complex used in the present invention can be prepared by a conventionally known method. The compound represented by the general formula (101) can be produced, for example, by referring to JP-A-2018-141138. The transition metal-containing catalyst used in the present invention contains the above-mentioned transition metal complex as a main catalyst component, and may be used in combination with an activator, a carrier, etc. Examples of the activator include alkylalumoxanes and boron-containing compounds, which are cocatalysts used in metallocene catalysts.
[0076] As the carrier, any carrier can be used as long as it does not interfere with the gist of the present invention. In general, inorganic oxides and polymer carriers are preferably used as the carrier. Specific examples of the carrier include SiO2, Al2O3, MgO, ZrO2, TiO2, B2O3, CaO, ZnO, BaO, ThO2, and mixtures thereof. Mixed oxides such as SiO2-Al2O3, SiO2-V2O5, SiO2-TiO2, SiO2-MgO, and SiO2-Cr2O3 can also be used. Inorganic silicates, polyethylene carriers, polypropylene carriers, polystyrene carriers, polyacrylic acid carriers, polymethacrylic acid carriers, polyacrylic acid ester carriers, polyester carriers, polyamide carriers, and polyimide carriers can also be used. There are no particular limitations on the particle size, particle size distribution, pore volume, specific surface area, and the like of these carriers, and any one can be used.
[0077] (1-2) Monomer In the production method of the present invention, at least the following monomer (A) which derives the structural unit (A) and the following monomer (Bp) which derives the structural unit (Bp), which is a precursor of the structural unit (B), are copolymerized. If necessary, other monomers may be further included and copolymerized. Monomer (A): At least one olefin having 3 to 20 carbon atoms Monomer (Bp): At least one norbornene having an alkoxycarbonyl group
[0078] As the at least one monomer (A) of an olefin having 3 to 20 carbon atoms, the same monomer (A) as explained in the structural unit (A) can be used.
[0079] At least one of the norbornene monomers (Bp) having an alkoxycarbonyl group may be a monomer represented by the following general formula (1).
[0080] [ka] (In general formula (1), R 1 is a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms, n is an integer of 0 to 3, and R 2 is a hydrocarbon group having 1 to 7 carbon atoms.
[0081] In general formula (1), R 1 and n are each R 1 and n may be the same as n. In general formula (1), R 2 is a hydrocarbon group having 1 to 7 carbon atoms. R 2 Examples of the hydrocarbon group in include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an i-propyl group, an i-butyl group, an s-butyl group, a t-butyl group, a 1-dimethylpropyl group, a 1,1,2-trimethylpropyl group, a 1,1-dimethylbutyl group, a cyclopentyl group, a cyclohexyl group, a 2-propenyl group, a 2-butenyl group, a phenyl group, and a benzyl group. R 2 As the hydrocarbon group in R, from the viewpoint of being easily deprotected by an acid to convert the alkoxycarbonyl group into a carboxy group, preferred are an i-propyl group, an i-butyl group, an s-butyl group, a t-butyl group, a 1,1-dimethylbutyl group, and the like, and a t-butyl group is more preferred. 2 As the hydrocarbon group in R, a benzyl group is preferred because it is easily deprotected by catalytic hydrogenation. 2 As the hydrocarbon group in the formula (I), a 2-propenyl group and a 2-butenyl group are preferred since they are easily deprotected via a π-allyl intermediate.
[0082] Examples of the monomer (Bp) used in the present invention include, but are not limited to, the following structures. In addition, in the examples of the following structural formulas, differences such as exo / endo / cis / trans are not considered, and any structure is acceptable.
[0083] [ka]
[0084] The monomer (Bp) can be synthesized by a method known in the art, or a commercially available product can be used. A particularly representative and common synthesis method is the Diels-Alder reaction of dicyclopentadiene with an olefin. In this case, the olefin is represented by the general formula: 1 -CH=CH-(CH2) n -CO2R 2 (In the formula, R 1 , n, and R 2 is the same as the general formula (1). By using the above, any of the above-listed monomers (Bp) can be synthesized.
[0085] As the monomer (C) from which the other structural unit (C) is derived, a monomer that is copolymerizable with the monomer (A) in the presence of the transition metal catalyst of Groups 4 to 10 of the periodic table can be used, and the same monomer (C) as that described for the structural unit (C) can be used.
[0086] (1-3) Polymerization method: The polymerization method in the production method of the polar group-containing olefin copolymer of the present invention is not limited. Solution polymerization in which all the produced polymer is dissolved in the medium, slurry polymerization in which at least a part of the produced polymer becomes a slurry in the medium, or bulk polymerization in which the liquefied monomer itself is used as the medium, can be used. The polymerization method may be any of batch polymerization, semi-batch polymerization, and continuous polymerization. For specific manufacturing processes and conditions, reference can be made to, for example, JP-A-2010-260913 and JP-A-2010-202647.
[0087] The unreacted monomers and the medium may be separated from the produced polymer and recycled for use. When recycling, these monomers and the medium may be purified and reused, or may be reused without purification. A conventionally known method can be used to separate the produced polymer from the unreacted monomers and the medium. For example, methods such as filtration, centrifugation, solvent extraction, and reprecipitation using a poor solvent can be used.
[0088] There are no particular limitations on the polymerization temperature, polymerization pressure and polymerization time, but they can usually be optimally set within the following ranges, taking into consideration productivity and process capacity. That is, the polymerization temperature is usually -20°C to 290°C, preferably 0°C to 250°C, more preferably 0°C to 200°C, further preferably 10°C to 150°C, and particularly preferably 20°C to 100°C. The polymerization pressure is 0.1 MPa to 100 MPa, preferably 0.3 MPa to 90 MPa, more preferably 0.5 MPa to 80 MPa, further preferably 1.0 MPa to 70 MPa, and particularly preferably 1.3 MPa to 60 MPa. The polymerization time can be selected from the range of 0.1 minute to 50 hours, preferably 0.5 minutes to 40 hours, and further preferably 1 minute to 30 hours. In the present invention, the polymerization is generally carried out under an inert gas atmosphere, for example, a nitrogen or argon atmosphere, and preferably a nitrogen atmosphere.
[0089] There is no particular restriction on the supply of catalyst and monomer to the polymerization reactor, and various supply methods can be used depending on the purpose. For example, in the case of batch polymerization, a method can be used in which a predetermined amount of monomer is supplied to the polymerization reactor in advance and a catalyst is supplied thereto. In this case, additional monomer or additional catalyst may be supplied to the polymerization reactor. In addition, in the case of continuous polymerization, a method can be used in which a predetermined amount of monomer and catalyst are supplied to the polymerization reactor continuously or intermittently to perform the polymerization reaction continuously.
[0090] The composition of the copolymer can be controlled, for example, by the following methods. 1) Changing the monomer supply ratio 2) Utilizing the difference in monomer reactivity ratio due to the difference in catalyst structure 3) Utilizing the polymerization temperature dependence of monomer reactivity ratio
[0091] For controlling the molecular weight of the copolymer, a conventionally known method can be used, for example, the following method. 1) Control of polymerization temperature 2) Control of monomer concentration 3) Control of ligand structure in transition metal complexes 4) Use of known chain transfer agents such as hydrogen
[0092] In this manner, a copolymer containing a structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms and a structural unit (Bp) derived from at least one norbornene having an alkoxycarbonyl group can be obtained. The copolymer having an alkoxycarbonyl group functions as a precursor copolymer to be subjected to a step of converting the alkoxycarbonyl group to a carboxy group, which will be described later. The copolymer may be a copolymer containing a structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms and a structural unit (Bp) represented by the following general formula (I').
[0093] [ka] (In general formula (I'), R 1 , n, and R 2 is the same as in the general formula (1).
[0094] (2) A step of converting an alkoxycarbonyl group into a carboxy group (deprotection step) In this step, the alkoxycarbonyl group of the copolymer obtained in the previous step, which contains the structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms and the structural unit (Bp) derived from at least one norbornene having an alkoxycarbonyl group, is converted to a carboxy group (deprotected), thereby obtaining a carboxy group-containing copolymer.
[0095] The method for converting the alkoxycarbonyl group of the copolymer containing the structural unit (A) and the structural unit (Bp) derived from at least one kind of norbornene having an alkoxycarbonyl group to a carboxy group includes acid decomposition, hydrolysis, hydrogenation, etc. From the viewpoint of simplicity, the method for converting the alkoxycarbonyl group to a carboxy group may be acid decomposition. The reaction conditions for converting an alkoxycarbonyl group into a carboxy group are not particularly limited, and the reaction can be carried out by a conventionally known method. When converting an alkoxycarbonyl group into a carboxyl group, an acid catalyst is used in the acid decomposition. In the hydrolysis, a conventionally known acid catalyst or base catalyst may be used as an additive to promote the reaction. The acid catalyst is not particularly limited, but for example, solid acids such as montmorillonite, inorganic acids such as hydrochloric acid, nitric acid, and sulfuric acid, and organic acids such as formic acid, acetic acid, benzoic acid, citric acid, paratoluenesulfonic acid, trifluoroacetic acid, and trifluoromethanesulfonic acid can be appropriately used. The base catalyst is not particularly limited, but for example, hydroxides of alkali metals or alkaline earth metals such as sodium hydroxide, potassium hydroxide, and lithium hydroxide, and carbonates of alkali metals or alkaline earth metals such as sodium hydrogencarbonate and sodium carbonate can be appropriately used. As the acid catalyst, in terms of the reaction promoting effect, the frequency of protonating and deprotecting the alkoxycarbonyl group, and the ease of adjusting the degree of neutralization, strong acids such as trifluoroacetic acid, paratoluenesulfonic acid, sulfuric acid, and hydrochloric acid are preferred, and trifluoroacetic acid and paratoluenesulfonic acid are more preferred. From the viewpoint of efficiency, the hydrogenation is preferably carried out under reducing conditions using a metal catalyst, and as the metal catalyst, a palladium carbon catalyst is preferred from the viewpoints of efficiency and availability.
[0096] The carboxyl group-containing copolymer obtained through the deprotection step is a copolymer containing a structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms and a structural unit (B') derived from at least one norbornene having a carboxyl group.
[0097] (3) A step of converting the carboxyl group into a metal-containing carboxylate (neutralization step) In this step, the carboxy group-containing copolymer obtained in the previous step is reacted with a metal ion to convert at least a part of the carboxy groups into a metal-containing carboxylate. All of the carboxy groups of the carboxy group-containing copolymer obtained in the above step may be converted into a metal-containing carboxylate, or only a portion of them may be converted into a metal-containing carboxylate. The proportion of metal ions converted to metal-containing carboxylate (degree of neutralization) can be appropriately selected depending on the application of the polar group-containing olefin copolymer to be produced, and may be the same as the proportion of metal ions in M in general formula (I) described in the polar group-containing olefin copolymer.
[0098] The conditions of the neutralization reaction in which the carboxyl group-containing copolymer obtained in the above step is reacted with a metal ion are not particularly limited, and the neutralization reaction can be carried out by a conventionally known method. For example, the carboxyl group-containing copolymer is dissolved in a solvent to obtain a solution, and a compound containing a metal ion is added to the solution, mixed, and appropriately heated as necessary, thereby allowing the carboxyl group to react with the metal ion.
[0099] The metal ion may be the same as the metal ion explained in relation to M in the general formula (I) explained in the polar group-containing olefin copolymer. The compound containing a metal ion used in the neutralization reaction is not particularly limited as long as it contains the above-mentioned metal ion, and examples thereof include metal hydroxides such as lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, zinc hydroxide, etc., metal carbonates such as sodium bicarbonate, sodium carbonate, lithium carbonate, zinc carbonate, etc., and metal oxides such as sodium oxide, potassium oxide, lithium oxide, zinc oxide, etc. These compounds are easy to use because counter ions of the metal ions are unlikely to remain in the ionomer. The amount of the compound containing a metal ion used in the neutralization reaction to be added during the reaction is appropriately adjusted according to the ratio of the compound converted into a metal-containing carboxylate (degree of neutralization).
[0100] As the solvent used in the neutralization reaction, it is necessary to select a solvent in which the carboxyl group-containing copolymer dissolves and in which metal ions can exist, and a mixed solvent may be used. For example, a mixed solvent of a good solvent for the carboxyl group-containing copolymer and a polar solvent in which metal ions can dissolve while being compatible with the good solvent may be used. Examples of the good solvent for the carboxyl group-containing copolymer include high-boiling hydrocarbon solvents having a boiling point (at 1 atmosphere) of 110°C or higher, such as toluene, xylene, and decalin. Examples of the polar solvent in which metal ions can dissolve while being compatible with the good solvent include butanol, hexanol, octanol, methyl ethyl ketone, and methyl butyl ketone. The ratio in the mixed solvent may be appropriately selected, and for example, the polar solvent in which metal ions can dissolve may be 3mL to 30mL per 100mL of the good solvent for the carboxyl group-containing copolymer. The good solvent for the carboxyl group-containing copolymer may be a solvent in which 5% by mass or more of the carboxyl group-containing copolymer can be dissolved. The temperature during the neutralization reaction may be 80°C to 140°C, or 90°C to 130°C. The reaction time for the neutralization reaction may be appropriately selected and is not particularly limited, but may be within a range of 30 minutes to 30 hours, and may be 12 hours to 24 hours.
[0101] In the method for producing a polar group-containing olefin copolymer of the present invention, the step (3) of converting a carboxy group into a metal-containing carboxylate (neutralization step) may be carried out after the step (2) of obtaining a carboxy group-containing copolymer (deprotection step), or the step (3) of converting a carboxy group into a metal-containing carboxylate (neutralization step) may be carried out while the step (2) of obtaining a carboxy group-containing copolymer (deprotection step) is being carried out. That is, a step of converting at least a part of the carboxy group into a metal-containing carboxylate by reacting with a metal ion may be carried out while converting the alkoxycarbonyl group of a copolymer containing the structural unit (A) and the structural unit (Bp) derived from at least one kind of norbornene having an alkoxycarbonyl group into a carboxy group. EXAMPLES
[0102] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples as long as they do not deviate from the gist of the invention. The physical properties of the polar group-containing olefin copolymer and the like were measured by the following methods.
[0103] [Structure of polar group-containing olefin copolymer] The structure of the polar group-containing olefin copolymer was prepared using Ascend 500 manufactured by BRUKER Co., Ltd. or AVANCE 400 manufactured by BRUKER Co., Ltd. 1 H-NMR and 13 This was determined by C-NMR analysis. The solvent used for NMR measurements was 1,1,2,2-tetrachloroethane-d2. 1 The polymer concentration measured by H-NMR was 5% by mass. 13 The polymer concentration for C-NMR was 15% by mass. NMR measurements were performed at 120°C. Alternatively, some of the NMR measurements were performed at 120°C by dissolving about 150 mg of a polar group-containing olefin copolymer in 2.4 mL of a mixed solvent of 1,2-dichlorobenzene:bromobenzene-d5 = 1:2 under heating to prepare a homogeneous solution. 1 H-NMR measurement was carried out under the following conditions, and quantitative analysis was performed. Pulse: 50 microsecond 30° pulse Spectral width: 10kHz Relaxation time: 5 seconds Capture time: 3.2 seconds FID integration count: 128 times 13 C-NMR measurements were performed using chromium(III) acetylacetonate as a relaxation reagent under the following conditions using the inverse gated decoupling method, and quantitative analysis was performed. Pulse: 15.8 microsecond 90° pulse Spectral width: 25kHz Relaxation time: 50 seconds Capture time: 1.5 seconds FID accumulation count: 1,024
[0104] [Content of structural unit (Bp) and structural unit (B) in polar group-containing olefin copolymer] The content of structural units (Bp) is: 13 C-NMR was used as follows. As an example, the polar group-containing olefin copolymer e1 of Example 1 13 The C-NMR spectrum is shown in Figure 1. Figure 2 is an enlarged view of the chemical shifts 42 ppm-12 ppm in Figure 1, Figure 3 is an enlarged view of the chemical shifts 79.9 ppm-78.8 ppm in Figure 1, and Figure 4 is an enlarged view of the chemical shifts 18.5 ppm-22.0 ppm in Figure 1. The specific isolated peak at chemical shift 173 ppm-175 ppm (position I) in Figure 1 corresponds to 1C of the alkoxycarbonyl group derived from the structural unit (Bp), and its peak area was designated as IB. The peak area of 3C derived from the structural unit (A) at chemical shift 10 ppm-50 ppm was designated as IA. The ratio of the structural unit (Bp) to the total monomer units was calculated as IB / (IA / 3+IB). The content of the structural unit (B) was kept the same, assuming that the content of the structural unit (Bp) would not change in the subsequent deprotection and neutralization steps.
[0105] [Number average molecular weight and weight average molecular weight] The number average molecular weight (Mn) and weight average molecular weight (Mw) were calculated under the following conditions by size exclusion chromatography using polystyrene as a molecular weight standard. Equipment: Tosoh Corporation high-temperature GPC equipment HLC-8321GPC / HT Column: Tosoh Corporation, TSKgel GMHHR-H(S)HT column (7.8 mm I.D. x 30 cm, two columns in series) Solvent: 1,2-dichlorobenzene Temperature: 145℃ or Equipment: High temperature GPC equipment manufactured by Waters Co., Ltd., ALC / GPC 150C Column: Showa Denko AT-806MS column (8.0 mm I.D. x 25 cm, 3 columns in series) Solvent: 1,2-dichlorobenzene Temperature: 140℃
[0106] [Measurement of glass transition temperature (Tg)] In accordance with JIS K7121-2012, a DSC (TA2000 model manufactured by DuPont) was used to record the glass transition temperature after one temperature increase / decrease from 20°C to 200°C at 10°C / min, followed by a second temperature increase / decrease from 20°C to 200°C at 10°C / min. The glass transition temperature (Tg) was determined as the temperature at the point where a straight line equidistant in the vertical direction from the straight line extending each baseline intersects with the curve of the stepwise change in the glass transition.
[0107] [Change from carboxylic acid structure to ionomer structure, degree of neutralization by IR spectrum analysis] The copolymer was coated onto a KBr disk and analyzed by Fourier transform infrared spectroscopy in transmitted light mode to obtain the infrared absorption spectrum of the copolymer, with the vertical axis of the output being the transmittance (%T). Product name: FT / IR-6100 manufactured by JASCO Corporation Measurement method: transmission method Detector: TGS Accumulation count: Auto (16 to 64 times) Resolution: 4.0cm -1 Measurement wavelength: 5000cm-1 ~500cm -1 The degree of neutralization can be measured by the C=O stretching vibration peak (1695 cm) when M is a hydrogen atom in the IR spectrum. -1 ~1705cm -1 ) and the C=O stretching vibration peak when M is a metal ion (sodium ion: 1550 cm -1 ~1600cm -1 The absorbance intensity of the peak (peak in the range of 100 to 150 nm) was calculated as follows: Degree of neutralization = absorbance intensity of the C=O stretching vibration peak when M is a metal ion / (absorbance intensity of the C=O stretching vibration peak when M is a metal ion + absorbance intensity of the C=O stretching vibration peak when M is a hydrogen atom) x 100 (%) More specifically, in the IR spectrum, the difference spectrum between the background measurement and the sample measurement was used, and the 1695 cm -1 ~1705cm -1 The absorbance intensity %T at the peak top position in the range of W and 1550 cm -1 ~1600cm -1 The degree of neutralization was defined as V / (W+V)×100(%), where V is the absorbance intensity %T at the peak top position in the range of 0.01 to 0.15.
[0108] [Synthesis of transition metal complexes] (Synthesis Example 1) A transition metal complex (A) represented by the following chemical formula (A), in which R is menthyl (2-i-propyl-5-methylcyclohexyl) and Lut is 2,6-dimethylpyridine, was synthesized as described in JP 2017-031300 A. In this specification, Me represents methyl.
[0109] [ka]
[0110] Example 1 (1) Preparation of a copolymer containing a structural unit (A) and a structural unit (Bp) derived from at least one type of norbornene having an alkoxycarbonyl group In a 50 mL autoclave, in a nitrogen atmosphere, a transition metal complex (A) (14 mg, 0.020 mmol) as a catalyst, toluene (6.7 mL) as a solvent, and 5-tertiary butoxycarbonyl-2-norbornene (2 mL, 9.8 mmol) as a monomer (Bp) were sequentially added. The autoclave was pressurized with propylene (monomer (A)) (6 g) and stirred at a reaction temperature of 50 ° C for 18 hours. The autoclave was returned to room temperature, and methanol (200 mL) was added. The precipitated solid was collected by filtration, washed three times with methanol (200 mL), and dried under reduced pressure at 120 ° C for 8 hours. The amount of the obtained polar group-containing olefin copolymer e1 was 940 mg. The results of various analyses of the polar group-containing olefin copolymer e1 are shown in Table 1.
[0111] (2) Preparation of carboxyl group-containing copolymer In a 50 mL autoclave, in a nitrogen atmosphere, the polar group-containing olefin copolymer e1 (228 mg) obtained in (1), toluene (18 mL) as a solvent, and trifluoroacetic acid (2.9 mL) as an acid catalyst were sequentially added. The autoclave was stirred at 100°C for 18 hours. The autoclave was returned to room temperature, and methanol (54 mL) was added thereto to obtain only the polar group-containing olefin copolymer h1. The obtained polar group-containing olefin copolymer h1 was dried under reduced pressure at 120°C for 10 hours. The obtained polar group-containing olefin copolymer h1 was 117 mg. The results of various analyses of the polar group-containing olefin copolymer h1 are shown in Table 2. The progress of the reaction of converting the tertiary butoxycarbonyl group to a carboxyl group is as follows: 13 In the C-NMR spectrum, the complete disappearance of the signal derived from the tertiary butyl group and the downfield shift of the signal derived from the carbonyl carbon were confirmed. In addition, FTIR measurement revealed the presence of a peak at 1703 cm derived from a carboxylic acid. -1 was observed, and from the wavenumber it was identified as a dimer of carboxylic acid.
[0112] (3) Production of copolymers (ionomers) containing metal-containing carboxylates In a 50 mL autoclave, in a nitrogen atmosphere, the polar group-containing olefin copolymer h1 (21 mg) obtained in (2) above, 20 mL of toluene as a solvent, 2 mL of butanol, and an aqueous sodium hydroxide solution (0.5 N, 3 mL) as a neutralizing agent were sequentially added. The autoclave was stirred at 100°C for 22 hours. The autoclave was returned to room temperature, and volatile components were removed under reduced pressure. The obtained polar group-containing olefin copolymer (ionomer) 1 was washed with pure water and dried under reduced pressure at 100°C for 10 hours. The obtained polar group-containing olefin copolymer (ionomer) 1 was 18 mg. The results of various analyses of the polar group-containing olefin copolymer (ionomer) 1 are shown in Table 2. Figure 5 shows the FTIR spectrum of the polar group-containing olefin copolymer h1, and Figure 6 shows the FTIR spectrum of the polar group-containing olefin copolymer (ionomer) 1. FTIR of polar group-containing olefin copolymer (ionomer) 1 shows a C=O stretching vibration peak at 1703 cm when M is a hydrogen atom. -1 is not observed, and the C=O stretching vibration peak is 1563 cm when M is a metal ion. -1 Since only M was observed, the proportion of metal ions in M (degree of neutralization) was calculated to be 100% based on the ratio of their absorbance intensities.
[0113] (Reference example 2) (1) Preparation of a copolymer containing a structural unit (A) and a structural unit (Bp) derived from at least one type of norbornene having an alkoxycarbonyl group The same procedure as in Example 1(1) was repeated except that the monomer (Bp) was changed to 5-tert-butoxycarbonyl-2-norbornene (4 mL, 19.6 mmol). The amount of the polar group-containing olefin copolymer e2 thus obtained was 700 mg. The results of various analyses of the polar group-containing olefin copolymer e2 are shown in Table 1.
[0114] (2) Preparation of carboxyl group-containing copolymer The procedure was carried out in the same manner as in Example 1(2), except that the polar group-containing olefin copolymer e2 obtained in the above (2) was used. The amount of the polar group-containing olefin copolymer h2 obtained was 53 mg. The results of various analyses of the polar group-containing olefin copolymer h2 are shown in Table 2.
[0115] (Reference example 3) (1) Preparation of a copolymer containing a structural unit (A) and a structural unit (Bp) derived from at least one type of norbornene having an alkoxycarbonyl group The same procedure as in Example 1(1) was repeated except that the monomer (B) was changed to 5-tert-butoxycarbonyl-2-norbornene (6 mL, 29.5 mmol). The amount of the polar group-containing olefin copolymer e3 thus obtained was 300 mg. The results of various analyses of the polar group-containing olefin copolymer e3 are shown in Table 1.
[0116] (2) Preparation of carboxyl group-containing copolymer The procedure was carried out in the same manner as in Example 1(2), except that the polar group-containing olefin copolymer e3 obtained in (2) above was used. The amount of the polar group-containing olefin copolymer h3 obtained was 39 mg. The results of various analyses of the polar group-containing olefin copolymer h3 are shown in Table 2.
[0117] [Table 1]
[0118] [Table 2]
[0119] As shown in Example 1, according to the present invention, in order to enhance the performance of an olefin-based polymer based on an α-olefin other than ethylene, a novel polar group-containing olefin copolymer containing a norbornene structural unit having a metal carboxylate, which is a novel ionomer, and a production method thereof can be provided. By using the copolymers h2 and h3 shown in Reference Examples 2 and 3, ionomers can be produced in the same manner as in the ionomer 1 of Example 1. In addition, a comparison of the glass transition temperature (Tg) of the copolymer h1 with that of the copolymer h2 and the copolymer h3 reveals that the glass transition temperature can be adjusted by the amount of structural units derived from norbornene. [Industrial Applicability]
[0120] The polar group-containing olefin copolymer of the present invention is a novel polar group-containing olefin copolymer containing a norbornene structural unit having a metal carboxylate, and is a novel ionomer, which contributes to improving the functionality of olefin polymers based on α-olefins other than ethylene. The novel ionomer of the present invention is capable of having a higher glass transition temperature (Tg) than conventional ionomers based on polyethylene as a base polymer, and by containing norbornene-derived structural units, the thermal properties of the ionomer can be controlled by adjusting the content thereof. In addition, the novel ionomer of the present invention can be suitably used in polyolefin multi-layer films based on α-olefins other than ethylene, such as polypropylene-based films. In addition to the applications that have been used for conventional ethylene-based ionomers, the range of applications can be further expanded by taking advantage of the characteristics of the ionomer, due to its higher glass transition temperature.
Claims
1. A structural unit (A) derived from at least one olefin having 3 to 20 carbon atoms; and a structural unit (B) represented by the following general formula (I): At least a part of the structural unit (B) is represented by the following general formula (I), in which M is a metal ion: 【Chemistry 1】 (In general formula (I), R 1 is a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms, n is an integer of 0 to 3, and M is a hydrogen atom or a metal ion.
2. 2. The polar group-containing olefin copolymer according to claim 1, wherein in the general formula (I), n is 0.
3. 3. The polar group-containing olefin copolymer according to claim 1, wherein the metal ion in M is at least one selected from the group consisting of a lithium ion, a sodium ion, a potassium ion, a calcium ion, a magnesium ion, an aluminum ion, and a zinc ion.
4. 3. The polar group-containing olefin copolymer according to claim 1, wherein the structural unit (A) is a structural unit derived from propylene.
5. A method for producing the polar group-containing olefin copolymer according to claim 1 or 2, comprising the steps of: A method for producing a polar group-containing olefin copolymer, comprising the steps of: copolymerizing at least one olefin having 3 to 20 carbon atoms with at least one norbornene having an alkoxycarbonyl group in the presence of a transition metal catalyst of Groups 4 to 10 of the periodic table; obtaining a carboxy group-containing copolymer by converting the alkoxycarbonyl groups of the obtained copolymer to carboxy groups; and reacting the carboxy group-containing copolymer with a metal ion to convert at least a portion of the carboxy groups into a metal-containing carboxylate.
6. 6. The method for producing a polar group-containing olefin copolymer according to claim 5, wherein the transition metal catalyst is a transition metal catalyst in which a chelating phosphine compound is coordinated to nickel or palladium metal.
Citation Information
Patent Citations
Multinary polar group-containing olefin copolymer
JP2019112623A
Polar group-containing olefin copolymer
JP2020117712A