Aluminum alloy for casting and aluminum alloy casting, and method for producing the same
A controlled alloy composition with Si, Ni, Cu, Fe, Mn, and P, and TiB2 enhances rigidity in aluminum alloys, achieving a Young's modulus of 100 GPa or more through gravity casting, addressing defects and cost issues in existing alloys.
Patent Information
- Application Number
- JP2023077686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Existing aluminum alloys struggle to achieve a Young's modulus of 100 GPa or more without particle dispersion, leading to defects and increased material costs due to the use of large amounts of Mg, Cr, V, and Mo, which also complicate casting methods like gravity casting.
A specific alloy composition with controlled amounts of Si, Ni, Cu, Fe, Mn, and P, along with regulated impurities, preferentially crystallizing compounds like Al-Fe-Mn-Si, Al-Ni, Al-Ni-Cu, and Al-Cu, and incorporating TiB2 to enhance rigidity, while using gravity casting to suppress coarse crystallization.
The solution results in a highly rigid aluminum alloy casting with a Young's modulus of 100 GPa or more, reducing costs and defects, and enabling efficient production without expensive equipment.
Smart Images

Figure 2024162309000002 
Figure 2024162309000003 
Figure 2024162309000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum alloy for casting, an aluminum alloy casting made of the aluminum alloy for casting, and a method for producing the same, and in particular to a high-rigidity aluminum alloy casting that can be suitably used for members that require high rigidity, such as ladder-type frames, perimeter-type frames and cases for various vehicles such as automobiles, and tables for machine tools. [Background technology]
[0002] Traditionally, cast iron has been used for components that require particularly high rigidity, such as automobile frames. However, in recent years, there has been a demand for lighter automobiles to conserve energy, and aluminum alloys have been attracting attention as a material that can meet this demand.
[0003] As an aluminum alloy material with high rigidity, a composite material with added ceramic particles is known. For example, Patent Document 1 (JP Patent Publication 6-212328A) proposes a highly heat-resistant, highly rigid, and low thermal expansion aluminum-based composite material, which is characterized in that, when the matrix is taken as 100% by weight, the matrix is an aluminum alloy containing, by weight %, 10-20% Ni, 8-25% Si, and at least 1.0-3.0% Mo, with the balance being Al, and when the entire composite material including the matrix is taken as 100% by weight, one or more types of nitride, boride, carbide, and oxide particles are dispersed in the matrix in an amount of more than 10% by weight and not more than 30% by weight in total, and which is manufactured by a powder metallurgy method.
[0004] In the high heat resistance, high rigidity and low thermal expansion aluminum-based composite material described in the above Patent Document 1, it is said that by adding borides, nitrides, carbides and oxides in specific amount ranges to a heat-resistant aluminum alloy matrix, it is possible to obtain excellent tensile strength at room temperature and at high temperatures, as well as reduce Young's modulus and thermal expansion coefficient.
[0005] Furthermore, the present inventors have proposed in Patent Document 2 (JP 2005-272868 A) "a casting aluminum alloy having excellent rigidity and a low linear expansion coefficient, characterized in that it contains 13 to 25 mass% Si, 2 to 8 mass% Cu, 0.5 to 3 mass% Fe, 0.3 to 3 mass% Mn, 0.001 to 0.02 mass% P, with the balance being Al and unavoidable impurities, and the total amount of Fe and Mn being 3.0 mass% or more."
[0006] In the aluminum alloy for casting described in Patent Document 2, fine crystallized particles of Al-Ni, Al-Ni-Cu, Al-Cu, Al-Fe-Si, Al-Fe-Mn, or Al-Si-Fe-Mn compounds can be dispersed during casting, and the required high rigidity and low linear expansion coefficient can be achieved. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 6-212328 [Patent Document 2] JP 2005-272868 A Summary of the Invention [Problem to be solved by the invention]
[0008] In recent years, aluminum alloy materials are required to have higher rigidity, specifically, a Young's modulus of 100 GPa or more. However, as in the high heat resistance, high rigidity, and low thermal expansion aluminum-based composite material described in the above Patent Document 1, although the rigidity of the aluminum alloy material can be increased by adding SiC particles or Al2O3 particles, the crystal matching between these particles and the aluminum phase is low, and defects occur at the interface between the aluminum phase and the particles, which is a problem.
[0009] In addition, in order to obtain a Young's modulus of 100 GPa or more without dispersing ceramic particles such as SiC particles or Al2O3 particles, as in the casting aluminum alloy described in Patent Document 2, it is necessary to add large amounts of Mg, Cr, V, Zr, and Mo, which inevitably increases the material cost. In addition, when these additive elements are added in large amounts, they form coarse crystals, making it difficult to use a casting method with a slow cooling rate such as gravity casting.
[0010] In view of the problems in the conventional techniques as described above, an object of the present invention is to provide an aluminum alloy that can provide a highly rigid and inexpensive aluminum alloy casting exhibiting a Young's modulus of 100 GPa or more without the dispersion of SiC particles or Al2O3 particles, even when using a casting method with a slow cooling rate such as gravity casting, an aluminum alloy casting made of said aluminum alloy, and a simple and efficient method for producing the same. [Means for solving the problem]
[0011] In order to achieve the above object, the inventors have conducted extensive research into the composition of aluminum alloys, and as a result, have discovered that in order to increase the rigidity of an aluminum alloy material, it is necessary to crystallize a large amount of a compound having a rigidity higher than aluminum, and that a specific compound is particularly effective in improving the rigidity of an aluminum alloy material, thereby arriving at the present invention.
[0012] That is, the present invention provides: Si: 16.0 to 20.0 wt%, Ni: 5.0-8.0wt%, Cu: 4.0-7.0wt%, Fe: 2.0-4.0 wt%, Mn: 1.0-3.0 wt%, P: 0.004 to 0.02 wt%, The balance is Al and unavoidable impurities. The inevitable impurities Mg, Cr, Zr, V and Mo are all restricted to 0.05 wt% or less. The present invention provides an aluminum alloy for casting, characterized by:
[0013] The aluminum alloy for casting according to the present invention has an alloy composition in which primary crystal Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds and Al-Cu compounds, which effectively improve the rigidity of the aluminum alloy material, are preferentially crystallized. These compounds contribute more to improving the rigidity of the aluminum alloy material than Mg-Si compounds and Al-Si-Fe-Mn-Cr compounds.
[0014] In addition, the amounts of Mg, Cr, V, Zr, and Mo, which reduce the amount of primary crystal Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds that effectively improve the rigidity of aluminum alloy materials, are strictly regulated (each to 0.05 wt% or less), making it possible to efficiently increase the rigidity of aluminum alloy castings.
[0015] The present invention also provides an aluminum alloy casting, which is made of the aluminum alloy for casting of the present invention and has a Young's modulus of 100 GPa or more.
[0016] In the aluminum alloy casting of the present invention, primary crystal Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds are preferentially crystallized in large amounts, and therefore the aluminum alloy casting has a high Young's modulus of 100 GPa or more. The Young's modulus of the aluminum alloy casting is preferably 110 GPa or more, more preferably 120 GPa or more, and most preferably 130 GPa or more.
[0017] In addition, the aluminum alloy casting of the present invention preferably contains 6.0 to 10.0 wt% TiB2. By containing 6.0 to 10.0 wt% TiB2, the Young's modulus of the aluminum alloy casting can be reliably improved. Unlike Al2O3 and SiC, TiB2 is also a crystallized phase of the aluminum alloy, and therefore has good wettability with aluminum and good crystal matching, thereby suppressing the formation of defects at the interface with the aluminum phase.
[0018] The present invention further provides a method for producing an aluminum alloy casting, which comprises casting a molten metal made of the aluminum alloy for casting of the present invention, and using gravity casting for the casting.
[0019] In the aluminum alloy for casting of the present invention, the amounts of Mg, Cr, V, Zr and Mo, which are likely to form coarse crystals, are strictly regulated (each is 0.05 wt% or less), so that even when gravity casting, which has a slow cooling rate, is used, the formation of coarse crystals that deteriorate the mechanical properties of the aluminum alloy casting is suppressed.
[0020] In addition, by controlling the content of each of the elements Mg, Cr, V, Zr and Mo to 0.05 wt% or less, it is possible to suppress the formation of compounds that contribute little to improving the rigidity of the aluminum alloy casting and promote the formation of compounds that contribute greatly to improving the rigidity, thereby making it possible to obtain an aluminum alloy casting having high rigidity with a Young's modulus of 100 GPa or more.
[0021] In addition, by using gravity casting or the like, it is possible to easily and efficiently obtain aluminum alloy castings having high rigidity while suppressing casting defects such as air entrapment. Furthermore, gravity casting does not require expensive equipment as in die casting, and the introduction cost of manufacturing equipment can be reduced.
[0022] Furthermore, in the manufacturing method of the aluminum alloy casting of the present invention, it is preferable to add Ti and B to the molten metal and crystallize TiB2. The method of adding Ti and B is not limited as long as it does not impair the effects of the present invention, and for example, it is sufficient to add Al-Ti and Al-B master alloys to the molten metal and adjust the amount added so that 6.0 to 10.0 wt% of TiB2 is formed. By crystallizing 6.0 to 10.0 wt% of TiB2, the Young's modulus of the aluminum alloy casting can be made 110 GPa or more. Effect of the Invention
[0023] According to the present invention, it is possible to provide an aluminum alloy that can produce a highly rigid and inexpensive aluminum alloy casting that exhibits a Young's modulus of 100 GPa or more without the dispersion of SiC particles or Al2O3 particles, even when using a casting method with a slow cooling rate such as gravity casting, an aluminum alloy casting made of the aluminum alloy, and a simple and efficient method for producing the same. [Brief description of the drawings]
[0024] [Figure 1] 1 shows the shape of a gravity casting die used in the examples. [Diagram 2] 1 shows the shape of a tensile test piece used in the examples. [Diagram 3] 1 shows the microstructure of the aluminum alloy casting 4. [Figure 4] 1 is a backscattered electron image of an example aluminum alloy casting 4. [Diagram 5] 1 shows the mapping results of B for the aluminum alloy casting 4. [Figure 6] 1 shows the results of mapping Ti in the example aluminum alloy casting 4. [Figure 7] 1 shows the Fe mapping results for the aluminum alloy casting 4. [Figure 8] 1 shows a mapping result of Ni in the aluminum alloy casting 4. [Figure 9] 1 shows the results of mapping Si in the example aluminum alloy casting 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The aluminum alloy for casting and the aluminum alloy casting, as well as the method for producing the same, according to the present invention will be described in detail below, but the present invention is not limited to these alone.
[0026] 1. Aluminum alloys for casting The aluminum alloy for casting according to the present invention is characterized in that its composition is optimized for the purpose of crystallizing a large amount of compounds effective in improving the rigidity of aluminum alloy castings. The compounds effective in improving the rigidity of aluminum alloy castings are Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds. As a result of the inventor's intensive research, it has become clear that these compounds contribute more to improving the rigidity of aluminum alloy castings than Mg-Si compounds and Al-Si-Fe-Mn-Cr compounds. Each component will be described in detail below.
[0027] (1) Essential additive elements Si: 16.0-20.0wt% Silicon crystallizes as primary silicon and Al-Fe-Mn-Si compounds, and has the effect of improving the rigidity of aluminum alloy castings. This effect is remarkable at 16.0wt% or more, but at more than 20.0wt%, the primary silicon crystals become coarse, and the machinability of the aluminum alloy castings is significantly reduced due to the coarse primary silicon crystals. Silicon also has the effect of lowering the linear expansion coefficient of the aluminum alloy castings and improving their wear resistance. The Si content is preferably 16.5-19.5wt%.
[0028] Ni: 5.0~8.0wt% Ni crystallizes as Al-Ni compounds, Al-Ni-Cu compounds, and Al-Ni-Fe compounds, and has the effect of improving the rigidity of aluminum alloy castings and reducing the linear expansion coefficient. This effect is remarkable at 5.0 wt% or more, but at more than 8.0 wt%, the crystallized particles become coarse and the elongation of the aluminum alloy castings decreases. From the viewpoint of improving Young's modulus, it is preferable to increase the Ni content as much as possible.
[0029] Cu: 4.0-7.0wt% Cu crystallizes as Al-Cu compounds and Al-Ni-Cu compounds, and contributes to improving the rigidity of aluminum alloy castings. This effect is significant at 4.0 wt% or more, but if the content exceeds 7.0 wt%, the crystallized particles become coarse and the elongation of the aluminum alloy casting decreases. In addition, if the content exceeds 7.0 wt%, the corrosion resistance of the aluminum alloy casting also decreases. From the viewpoint of improving Young's modulus, it is preferable to increase the Cu content as much as possible.
[0030] Fe: 2.0-4.0wt% Fe crystallizes as Al-Fe-Mn-Si compounds and Al-Ni-Fe compounds, and contributes to improving the rigidity of aluminum alloy castings. This effect is remarkable at 2.0wt% or more, but at more than 4.0wt%, the crystallized particles tend to become coarse, and the elongation of the aluminum alloy castings decreases. In addition, by adding 2.0 to 4.0wt% of Fe, it is possible to prevent seizure on the mold. From the viewpoint of improving Young's modulus, it is preferable to increase the Fe content as much as possible.
[0031] Mn: 1.0-3.0wt% Mn crystallizes as an Al-Fe-Mn-Si compound and contributes to improving the rigidity of aluminum alloy castings. This effect is significant at 1.0 wt% or more, but if it exceeds 3.0 wt%, the crystallized particles tend to become coarse, and the elongation of the aluminum alloy casting decreases. In addition, by adding 1.0 to 3.0 wt% of Mn, it is possible to prevent seizure on the mold. From the viewpoint of improving Young's modulus, it is preferable to increase the Mn content as much as possible.
[0032] P: 0.004 to 0.02 wt% P acts as a crystallization nucleus for primary Si crystals and contributes to the refinement of primary Si crystals. This effect is significant at 0.004wt% or more, but no improvement in this effect is observed even if the content of P exceeds 0.02wt%. The P content is preferably 0.007-0.015wt%.
[0033] (2) Inevitable impurities The aluminum alloy for casting according to the present invention is characterized in that the contents of Mg, Cr, Zr, V and Mo as inevitable impurities are restricted to 0.05 wt% or less.
[0034] Mg: 0.05wt% or less Mg dissolves in the matrix and contributes to improving the rigidity of aluminum alloy castings, but it crystallizes as Mg-Si compounds, which reduces the amount of primary crystallized Si, which contributes more to improving rigidity, so it is restricted to 0.05 wt% or less, and it is preferable to restrict Mg to 0.01 wt% or less.
[0035] Cr:0.05wt% or less Cr crystallizes as a Cr-Si compound. This compound does not contribute to improving rigidity with the usual amount of Cr added. On the other hand, the presence of Cr reduces the amount of primary crystallized Si, which contributes to improving the rigidity of aluminum alloy castings. In addition, when Ti and B are added to the molten metal to crystallize TiB2, the presence of Cr reduces the amount of TiB2 crystallized, which contributes to improving the rigidity of aluminum alloy castings. For these reasons, Cr is restricted to 0.05 wt% or less. It is preferable to restrict Cr to 0.01 wt% or less.
[0036] Zr: 0.05wt% or less Zr crystallizes as a Zr-Si compound. This compound does not contribute to improving the rigidity of aluminum alloy castings with the usual amount of Zr added. On the other hand, the presence of Zr reduces the amount of primary crystallized Si, which contributes to improving the rigidity of aluminum alloy castings. In addition, when Ti and B are added to the molten metal to crystallize TiB2, the presence of Zr reduces the amount of TiB2 crystallized, which contributes to improving the rigidity of aluminum alloy castings. For these reasons, Zr is restricted to 0.05 wt% or less. It is preferable to restrict Zr to 0.01 wt% or less.
[0037] V: 0.05wt% or less V crystallizes as a V-Si compound. This compound does not contribute to improving the rigidity of aluminum alloy castings with the usual V addition amount. On the other hand, the presence of V reduces the amount of primary crystallized Si, which contributes to improving the rigidity of aluminum alloy castings. In addition, when Ti and B are added to the molten metal to crystallize TiB2, the presence of V reduces the amount of TiB2 crystallized, which contributes to improving the rigidity of aluminum alloy castings. For these reasons, V is restricted to 0.05 wt% or less. It is preferable to restrict V to 0.01 wt% or less.
[0038] Mo: 0.05wt% or less Mo crystallizes as a Mo-Si compound. This compound does not contribute to improving rigidity with the usual amount of Mo added. On the other hand, the presence of Mo reduces the amount of primary crystallized Si, which contributes to improving the rigidity of aluminum alloy castings. In addition, when Ti and B are added to the molten metal to crystallize TiB2, the presence of Mo reduces the amount of TiB2 crystallized, which contributes to improving the rigidity of aluminum alloy castings. For these reasons, Mo is restricted to 0.05 wt% or less. It is preferable to restrict Mo to 0.01 wt% or less.
[0039] In addition, since recycled raw materials are often used for Al-Si based aluminum alloys for casting, the inclusion of unavoidable impurities is permitted within a range that does not impair the properties of the aluminum alloy casting of the present invention.
[0040] 2.Aluminum alloy castings The aluminum alloy casting of the present invention is a high-rigidity aluminum alloy casting made of the aluminum alloy for casting of the present invention, and is characterized in that the Young's modulus is 100 GPa or more, preferably 110 GPa or more, more preferably 120 GPa or more, and most preferably 130 GPa or more.
[0041] In the aluminum alloy casting of the present invention, crystallization of Mg-Si compounds, which contribute relatively little to improving rigidity, is suppressed, and primary Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds and Al-Cu compounds, which contribute relatively much to improving rigidity, are preferentially crystallized in large amounts.
[0042] Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds and Al-Cu compounds all have a Young's modulus of approximately 200 GPa or more, and by crystallizing them in an Al alloy, the Young's modulus of the Al alloy is improved in accordance with the rule of mixtures.
[0043] The shapes and sizes of primary crystal Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds are not particularly limited as long as they do not impair the effects of the present invention, but are preferably fine. More specifically, the particle size of primary crystal Si is preferably 100 μm or less. In addition, the particle size of Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds is preferably 100 μm or less.
[0044] The method for measuring the particle size of primary crystal Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known structure observation methods can be used, for example, optical microscope observation or SEM observation. More specifically, for example, the microstructure in the cross section of an aluminum alloy casting is observed, and 10 primary crystal Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds confirmed in the observation image are selected from the largest ones per unit area, and the average particle size of primary crystal Si and the average maximum length of Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds are calculated.
[0045] In addition, the aluminum alloy casting of the present invention preferably contains 6.0 to 10.0 wt% of TiB2. By making TiB2 6.0 wt% or more, the Young's modulus of the aluminum alloy casting can be efficiently improved, and by making TiB2 10.0 wt% or less, embrittlement and deterioration of workability of the aluminum alloy casting can be suppressed. Furthermore, if TiB2 exceeds 10.0 wt%, the viscosity of the molten metal increases, making casting difficult.
[0046] The shape and size of TiB2 are not particularly limited as long as they do not impair the effects of the present invention, but granular TiB2 having a particle size of 1 μm or less is preferable.
[0047] The method for producing the aluminum alloy casting of the present invention is not particularly limited as long as the effects of the present invention are not impaired, and a conventionally known die casting method or gravity casting method can be used. However, the aluminum alloy casting can be preferably obtained by the method for producing the aluminum alloy casting of the present invention.
[0048] 3. Manufacturing method of aluminum alloy castings The method for producing an aluminum alloy casting of the present invention is characterized by using the aluminum alloy for casting of the present invention and gravity casting.
[0049] In the aluminum alloy for casting of the present invention, the amounts of Mg, Cr, V, Zr and Mo, which are likely to form coarse crystals, are strictly regulated (each is 0.05 wt% or less), so that even when gravity casting, which has a slow cooling rate, is used, the formation of coarse crystals that deteriorate the mechanical properties of the aluminum alloy casting is suppressed.
[0050] In addition, by controlling the content of each of the elements Mg, Cr, V, Zr and Mo to 0.05 wt% or less, it is possible to suppress the formation of compounds that contribute little to improving the rigidity of the aluminum alloy casting and promote the formation of compounds that contribute greatly to improving the rigidity, thereby making it possible to obtain an aluminum alloy casting having high rigidity with a Young's modulus of 100 GPa or more.
[0051] In addition, by using gravity casting or the like, it is possible to easily and efficiently obtain aluminum alloy castings having high rigidity while suppressing casting defects such as air entrapment. Furthermore, gravity casting does not require expensive equipment as in die casting, and the introduction cost of manufacturing equipment can be reduced.
[0052] Furthermore, by dispersing 6.0-10.0 wt% of TiB2 in the molten metal of the aluminum alloy for casting of the present invention, the Young's modulus of the aluminum alloy casting can be made 110 GPa or more. Since the Young's modulus of the aluminum alloy casting basically increases with an increase in the amount of TiB2 added, if a higher Young's modulus is required, the amount added may be increased within the range of 6.0-10.0 wt%. TiB2 may be crystallized by adding Ti and B to the molten metal, or TiB2 particles may be added from the outside, or both may be performed.
[0053] Although the effect of adding TiB2 on improving the Young's modulus of aluminum alloy castings depends on the composition of the aluminum alloy and the shape and size of TiB2, 1.0 wt% of TiB2 can improve the Young's modulus of aluminum alloy castings by about 2 GPa. Here, the method of adding TiB2 particles to the molten metal is not particularly limited as long as it does not impair the effects of the present invention, and for example, a conventionally known molten metal stirring method can be used.
[0054] Furthermore, since the aluminum alloy for casting according to the present invention contains 0.004 to 0.02 wt % of P, the P acts as crystallization nuclei for primary Si crystals, making it possible to refine the primary Si crystals.
[0055] Other casting conditions are not particularly limited as long as they do not impair the effects of the present invention, and various conventionally known casting methods and casting conditions can be used.
[0056] Representative embodiments of the present invention have been described above, but the present invention is not limited to these, and various design modifications are possible, all of which are included in the technical scope of the present invention. EXAMPLES
[0057] Example The raw materials mixed to obtain the compositions shown in Examples 1 to 7 in Table 1 were inserted into a graphite crucible, and after melting in air at 1050°C, the temperature was lowered to 800°C, and a deslag treatment was performed at 800°C using a deslag flux. The inevitable impurities of Mg, Cr, Zr, V, and Mo were all 0.05wt% or less. Here, for Examples 3 to 7, a mother alloy of Al-35wt%Ti and Al-10wt%B was put into the molten aluminum and melted, and Ti and B were added in the amounts shown in Table 1 to crystallize TiB2. Next, for Examples 1, 2, and 4 to 6, gravity casting was performed using a mold shown in FIG. 1 to obtain the aluminum alloy castings 1, 2, 4 to 6 according to the present invention. For Examples 3 and 7, the alloys were melted in air at 1,050°C, then the temperature was lowered to 800°C, and a slag removal treatment was performed at 800°C using a slag removal flux to produce ingots, which were then remelted at 800°C and used for die casting. The die casting injection conditions were a low speed of 0.1 m / s, a high speed of 1.0 m / s, and a casting pressure of 70 MPa, and plate-shaped aluminum alloy castings 3 and 7 with dimensions of 180 mm x 150 mm x 6 mm were obtained.
[0058] [Table 1]
[0059] When gravity casting was used, test pieces with the shape and size shown in Figure 2 were cut out from a position 13 mm from the bottom of the mold and a tensile test was performed. When die casting was used, test pieces with the shape and size shown in Figure 2 were cut out from the die cast material and a tensile test was performed. Young's modulus was calculated from the slope of the elastic region of the load-displacement curve obtained in the tensile test. The obtained values are shown in Table 1.
[0060] A cube of 1 cm square was cut out from the obtained aluminum alloy casting, and the cross section was buffed to prepare a sample for microstructural observation. As a representative result of microstructural observation, the microstructure of the aluminum alloy casting 4 observed with an optical microscope is shown in Figure 3. From Figure 3, it can be seen that many compounds (Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds) are crystallized.
[0061] Next, the inclusions in the structure observation sample of the aluminum alloy casting 4 were analyzed by element mapping using an EPMA (EPMA-1610, Shimadzu Corporation, accelerating voltage 15 kV, probe current 100 mA, beam diameter φ1 μm). The backscattered electron image obtained is shown in Figure 4, the mapping of B in Figure 5, the mapping of Ti in Figure 6, the mapping of Fe in Figure 7, the mapping of Ni in Figure 8, and the mapping of Si in Figure 9. It can be seen that the area where B and Ti overlap is TiB2, and that fine TiB2 is uniformly dispersed.
[0062] Comparative Example Comparative aluminum alloy castings 1 to 8 were obtained in the same manner as in the examples, except that the compositions shown in Comparative Examples 1 to 8 in Table 1 were used. Comparative Example 6 contained 0.7 wt% V, and Comparative Example 7 contained 0.9 wt% Zr. Gravity casting was used in Comparative Examples 1, 2, 4, and 8, and die casting was used in Comparative Examples 3 and 5 to 7. In Comparative Examples 2 to 7, a mother alloy of Al-35 wt% Ti and Al-10 wt% B was poured into molten aluminum and melted, and Ti and B were added in the amounts shown in Table 1 to crystallize TiB2. Furthermore, a tensile test was performed in the same manner as in the examples, and the Young's modulus of each comparative aluminum alloy casting was obtained. The obtained values are shown in Table 1.
[0063] From Table 1, in all the examples (Example aluminum alloy castings 1 to 7), a high Young's modulus of 100 GPa or more is obtained. Comparing Example aluminum alloy casting 1, which does not crystallize TiB2, with Example aluminum alloy casting 2, a higher Young's modulus is obtained in Example aluminum alloy casting 1, which has a high content of each added element. In addition, it is found that the effect of the casting method on Young's modulus is small, and an aluminum alloy casting with a high Young's modulus can be obtained even by using gravity casting. In addition, the highest Young's modulus is obtained in Example aluminum alloy casting 6, which has a high content of each added element and a high amount of TiB2 crystallization, and reaches 131 GPa.
[0064] On the other hand, the Young's modulus of the comparative aluminum alloy casting 1, which has low contents of Si, Fe, and Mn and does not crystallize TiB2, is a low value of 95 GPa. Even when 5.3 wt% of TiB2 is crystallized, the Young's modulus of the comparative aluminum alloy casting 3 and the comparative aluminum alloy casting 4, which have low contents of Fe and Mn, does not reach 100 GPa. The Young's modulus of the comparative aluminum alloy casting 4 and the comparative aluminum alloy casting 5, which have an increased amount of TiB2 crystallization to 6.5 wt%, is 100 GPa or more, but since the amounts of Cu, Fe, and Mn added are small, it can be seen that the Young's modulus is lower than that of the practical aluminum alloy casting 4 and the practical aluminum alloy casting 7, which have the same amount of TiB2 crystallization.
[0065] The comparative aluminum alloy casting 6 has a composition based on the composition of the practical aluminum alloy casting 7, to which 0.7 wt% of V has been added. Furthermore, VB2 crystallizes in the comparative aluminum alloy casting 6, and the amount of TiB2 crystallized is smaller than that in the practical aluminum alloy casting 7. As a result, the Young's modulus of the comparative aluminum alloy casting 6 is 105 GPa, which is lower than that of the practical aluminum alloy casting 7, 110 GPa.
[0066] The comparative aluminum alloy casting 7 has a composition with 0.9 wt% Zr added to the composition of the practical aluminum alloy casting 7. Furthermore, ZrB2 crystallizes in the comparative aluminum alloy casting 7, and the amount of TiB2 crystallized is smaller than that of the practical aluminum alloy casting 7. As a result, the Young's modulus of the comparative aluminum alloy casting 7 is 108 GPa, which is lower than that of the practical aluminum alloy casting 7, 110 GPa.
[0067] Comparative aluminum alloy casting 8 has a composition based on that of Example aluminum alloy casting 2, to which 0.5 wt% of Mg has been added. The Young's modulus of Comparative aluminum alloy casting 8 is 99 GPa, which is lower than the 100 GPa of Example aluminum alloy casting 2. This result is due to the fact that the amount of compounds that contribute to improving the Young's modulus is reduced by the addition of Mg.
[0068] From the above results, it is found that by using an alloy composition in which primary crystal Si, Al-Fe-Mn-Si compounds, Al-Ni compounds, Al-Ni-Cu compounds, Al-Ni-Fe compounds, and Al-Cu compounds, which effectively improve the rigidity of aluminum alloy castings, are preferentially crystallized, it is possible to obtain highly rigid and inexpensive aluminum alloy castings that exhibit a Young's modulus of 100 GPa or more without the dispersion of SiC particles or Al2O3 particles, even with a casting method with a slow cooling rate such as gravity casting. It is also found that a higher Young's modulus can be obtained by the crystallization of TiB2.
Claims
1. Si: 16.0-20.0wt%, Ni: 5.0 to 8.0 wt%, Cu: 4.0 to 7.0 wt%, Fe: 2.0-4.0wt%, Mn: 1.0 to 3.0 wt%, P: 0.004 to 0.02 wt %, The balance is Al and unavoidable impurities, The inevitable impurities Mg, Cr, Zr, V and Mo are all restricted to 0.05 wt% or less. An aluminum alloy for casting, characterized by:
2. The aluminum alloy for casting according to claim 1, Young's modulus is 100 GPa or more; Aluminum alloy castings characterized by:
3. 6.0 to 10.0 wt% TiB 2 Including, The Young's modulus is 110 GPa or more; The aluminum alloy casting according to claim 2 .
4. A molten metal made of the aluminum alloy for casting according to claim 1 is cast, The casting is performed using gravity casting; A method for manufacturing an aluminum alloy casting, comprising the steps of:
5. Add Ti and B to the molten metal to obtain TiB 2 To crystallize out The method for producing an aluminum alloy casting according to claim 4, characterized in that
Citation Information
Patent Citations
Aluminum matrix composite material having high heat resistance, high rigidity, and low thermal expansion
JP1994212328A
Casting aluminum alloy with high rigidity / low linear expansion coefficient
JP2005272868A