Manufacturing method of bobbin type battery and bobbin type battery
A dual-base-material manufacturing method for bobbin-type batteries optimizes electrolyte permeation and molding density by varying binder content, enhancing discharge performance.
Patent Information
- Application Number
- JP2023077931
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
AI Technical Summary
Bobbin-type batteries face a challenge in simultaneously improving electrolyte permeation ease and molding density to enhance discharge performance, as increasing binder content enhances permeation but reduces density, while reducing binder content impedes permeation.
A manufacturing method involving two base materials with differing binder contents is used to form a positive electrode, where the first base material contains a higher binder amount than the second, allowing for a structured mixture that balances permeation and density by forming a cylindrical electrode within a case.
This method improves discharge performance by optimizing electrolyte permeation and molding density through a balanced binder distribution, resulting in enhanced battery capacity.
Smart Images

Figure 2024162434000001_ABST
Abstract
Description
[Technical field]
[0001] SUMMARY OF THE DISCLOSURE An embodiment of the present invention relates to a method for manufacturing a bobbin type battery and a bobbin type battery. [Background technology]
[0002] There is a bobbin type battery in which a cylindrical positive electrode is provided inside a cylindrical case with one end closed, a negative electrode and a separator are provided inside the positive electrode, and an electrolyte is poured inside the case. The positive electrode is made by molding a mixture containing manganese dioxide, a conductive material, and a binder. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-295307 A Summary of the Invention [Problem to be solved by the invention]
[0004] There is a demand for improved discharge performance in batteries, and this is also true for bobbin-type batteries. In bobbin-type batteries, the discharge performance can be improved by improving the ease of permeation of the electrolyte into the positive electrode and increasing the molding density. However, if the amount of binder contained in the positive electrode is large, the electrolyte will permeate more easily, but the molding density will decrease. Also, if the amount of binder contained in the positive electrode is small, the molding density will increase, but the electrolyte will not permeate easily. Thus, it has been difficult to improve discharge performance by improving the ease of permeation of the electrolyte and increasing the molding density at the same time.
[0005] The disclosed technique has been made in consideration of the above-mentioned points, and has an object to provide a manufacturing method for a bobbin type battery that can improve discharge performance. [Means for solving the problem]
[0006] A method for manufacturing a bobbin type battery according to one embodiment of the present disclosure includes the steps of: mixing and granulating a first base material containing manganese dioxide, a conductive material, and a binder to form a first mixture; mixing and granulating a second base material containing manganese dioxide, a conductive material, and a binder with the first mixture to form a second mixture; molding the second mixture into a cylindrical positive electrode and contacting the positive electrode with an inner surface of a cylindrical case having one end closed; injecting an electrolyte into the case; providing a cylindrical negative electrode and a separator inside the positive electrode; and closing and sealing the other end of the case, wherein the amount of binder contained in the first base material is greater than the amount of binder contained in the second base material. Effect of the Invention
[0007] According to one aspect of the method for producing a bobbin type battery disclosed in the present application, it is possible to improve the discharge performance. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram showing a cross-sectional structure of a bobbin type battery according to one embodiment. [Diagram 2] FIG. 2 is a flow chart showing the manufacturing procedure of the bobbin type battery. [Diagram 3] FIG. 3 is a flowchart illustrating the procedure for producing the positive electrode unit. [Figure 4] FIG. 4 is a flowchart showing the procedure for producing the negative electrode unit. [Diagram 5] FIG. 5 shows the results of a performance comparison experiment of bobbin type batteries. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the manufacturing method of the bobbin type battery and the bobbin type battery disclosed in the present application will be described in detail with reference to the drawings. Note that the battery disclosed in the present application is not limited to the following embodiments.
[0010] <Bobbin type battery configuration> 1 is a schematic diagram showing a cross-sectional structure of a bobbin type battery according to one embodiment. The bobbin type battery 100 shown in FIG. 1 has a case 101, a sealing plate 102, a terminal 103, a gasket 104, a washer 105, a positive electrode 106, a separator 107, a negative electrode 108, and a current collector 109.
[0011] Case 101 is a cylindrical metal container with one end (the lower end in FIG. 1) closed and the other end (the upper end in FIG. 1) open. Case 101 houses a positive electrode 106, a separator 107, a negative electrode 108, a current collector 109, and the like.
[0012] Sealing plate 102 is a lid shaped to fit the opening of case 101, and is laser welded to the opening at the other end of case 101 to seal case 101. As shown in Fig. 1, the outer periphery of sealing plate 102 rises along the inner periphery of case 101, and sealing plate 102 has a concave shape as a whole. A through hole through which terminal 103 is inserted is formed in the center of the concave shape of sealing plate 102, and the through hole is sealed by gasket 104.
[0013] Terminal 103 is inserted into a through hole formed in the center of sealing plate 102, with one end protruding to the outside of case 101 and the other end contacting current collector 109 inside case 101. Terminal 103 is electrically connected to negative electrode 108 via current collector 109. That is, terminal 103 functions as a negative electrode terminal.
[0014] Gasket 104 seals the through hole of sealing plate 102 through which terminal 103 is inserted. That is, gasket 104 is attached so as to sandwich sealing plate 102 from both sides around the through hole of sealing plate 102, and fills the gap between sealing plate 102 and terminal 103.
[0015] The washer 105 holds an end of the terminal 103 inside the case 101, and fixes the terminal 103. As shown in Fig. 1, the terminal 103 and the washer 105 sandwich the sealing plate 102 and the gasket 104, so that the terminal 103, the gasket 104, and the washer 105 are integrated with the sealing plate 102.
[0016] The positive electrode 106 is formed into a cylindrical shape that fits the inner circumferential surface of the case 101. The positive electrode 106 contains manganese dioxide, a conductive material, and a binder. The conductive material may be graphite, acetylene black, or the like. The binder may be made of a resin and may be elastic, and it is preferable to use granular PTFE (polytetrafluoroethylene), for example. The positive electrode 106 is disposed in contact with the inner circumferential surface of the case 101, so that the case 101 functions as a current collector for the positive electrode. The inside of the case 101 is filled with a volatile nonaqueous electrolyte (not shown), and this nonaqueous electrolyte permeates the positive electrode 106.
[0017] Separator 107 is a cylindrical material made of liquid-permeable and insulating material such as polypropylene, and is disposed inside the cylindrical shape of positive electrode 106. Since separator 107 is insulating, the inside of the cylindrical shape of separator 107 is insulated from positive electrode 106.
[0018] The negative electrode 108 contains a negative electrode active material such as lithium or zinc, and is formed into a cylindrical shape that fits the inner circumferential surface of the separator 107. As described above, the inside of the cylindrical shape of the separator 107 is insulated from the positive electrode 106, and therefore the negative electrode 108 is insulated from the positive electrode 106. However, since the separator 107 is liquid-permeable to allow the non-aqueous electrolyte to pass therethrough, ions such as lithium ions move from the negative electrode 108 to the positive electrode 106 through the separator 107.
[0019] The current collector 109 electrically connects the negative electrode 108 and the terminal 103. One end of the current collector 109 contacts the inside of the cylindrical shape of the negative electrode 108, and the other end contacts the terminal 103 below the sealing plate 102.
[0020] In the bobbin type battery 100, the case 101 and the positive electrode 106 constitute a positive electrode unit 111. The sealing plate 102, the terminal 103, the gasket 104, the washer 105, the separator 7, the negative electrode 108, and the current collector 109 constitute a negative electrode unit 112.
[0021] <Manufacturing method of bobbin type battery> Next, a description will be given of a manufacturing method for the bobbin type battery 100. Fig. 2 is a flow chart showing the manufacturing procedure for the bobbin type battery.
[0022] First, the positive electrode unit 111 is created (step S1). Next, the negative electrode unit 112 is created (step S2). Next, an electrolyte is poured into the positive electrode unit 111 (step S3). Next, the negative electrode unit 112 is inserted inside the positive electrode unit 111 (step S4). Next, the other end of the case 101 and the outer periphery of the sealing plate 102 are laser welded (step S5) to manufacture the bobbin type battery 100. Note that the order of step S1 for creating the positive electrode unit 111 and step S2 for creating the negative electrode unit 112 may be reversed, or they may be performed simultaneously.
[0023] Next, a detailed description will be given of a method for producing the positive electrode unit 111 in step S1 of the manufacturing procedure for the bobbin type battery 100. Fig. 3 is a flow chart illustrating the procedure for producing the positive electrode unit.
[0024] First, a first base material containing manganese dioxide, a conductive material, and a binder is mixed and granulated to form a first mixture (step S11). Here, the mixed first base material is compressed and solidified by a roller or the like, and the solidified first base material is crushed or granulated to form the first mixture.
[0025] Next, the second base material containing manganese dioxide, a conductive material, and a binder and the first mixture prepared in step S11 are mixed and granulated to prepare a second mixture (step S12). Here, the mixed first mixture and the second base material are compressed and solidified by a roller or the like, and the solidified first mixture and the second base material are crushed or otherwise granulated to prepare the second mixture.
[0026] Next, the second mixture is pressure-molded to form a cylindrical positive electrode 106 (step S13). Next, the positive electrode 106 is inserted inside the case 101, and pressure is applied to spread the positive electrode 106 in the outer circumferential direction, thereby bringing the outer circumferential surface of the positive electrode 106 into contact with the inner circumferential surface of the case 101 (step S14), thereby forming the positive electrode unit 111. Note that steps S13 and S14 may be performed together to mold the second mixture into a cylindrical shape inside the case 101.
[0027] Next, the method of producing the negative electrode unit 112 in step S2 of the manufacturing procedure of the bobbin type battery 100 will be described in detail. FIG. 4 is a flow chart showing the procedure of producing the negative electrode unit. First, the sealing plate 102 and the gasket 104 are sandwiched between the terminal 103 and the washer 105 (step S21). Next, one end of the current collector 109 is crimped to the negative electrode 108 containing lithium (step S22). Next, the other end of the current collector 109 is welded to the terminal 103 (step S23). Next, the separator 107 is wound around the negative electrode 108 (step S24) to produce the negative electrode unit 112.
[0028] <About the performance comparison experiment> In the process of producing the positive electrode 106 in steps S11 to S13, the ratio of the first mixture mixed with the second mixture was changed to perform a performance comparison experiment of the bobbin type battery 100. FIG. 5 is a diagram showing the results of the performance comparison experiment of the bobbin type battery. Various conditions in the performance comparison experiment are as follows. The outer diameter of the case 101 is 14 mm and the height is 25 mm. The height of the positive electrode 106 is 18.5 mm. The first base material contains 92 wt% manganese dioxide, 3 wt% graphite as a conductive material, and 5 wt% PTFE as a binder. The second base material contains 96 wt% manganese dioxide, 3 wt% graphite as a conductive material, and 1 wt% PTFE as a binder. In other words, the second base material contains less binder than the first base material.
[0029] In the performance comparison experiment, bobbin type batteries 100 having positive electrodes 106 made by varying the ratio of the first mixture mixed into the second base material when making the second mixture were prepared, and the 5.6 kΩ constant resistance discharge capacity of each bobbin type battery 100 was compared.
[0030] In Comparative Example 1, the mixing ratio of the first mixture is 0 wt%, and the second mixture does not contain the first mixture. As shown in Examples 1 to 4, the discharge capacity is lower than when the first mixture is mixed. This is considered to be because the amount of binder is insufficient due to the absence of the first mixture formed from the first base material, which increases the molding density of the positive electrode 106 and makes it difficult for the electrolyte to sufficiently permeate the positive electrode 106, resulting in a lower discharge capacity.
[0031] In Comparative Example 2, the mixing ratio of the first mixture is 80 wt%, and in Comparative Example 3, the mixing ratio of the first mixture is 100 wt%. In Comparative Example 2 and Comparative Example 3, the discharge capacity is lower than that of the positive electrode 106 of Comparative Example 1 formed only from the second mixture. This is thought to be because, by forming the positive electrode 106 only from the first mixture, the electrolyte can easily permeate, but the molding density of the positive electrode 106 is lower, resulting in a lower discharge capacity.
[0032] On the other hand, in the range shown in Example 1 to Example 4, that is, in the range of the mixing ratio of the first mixture from 3 wt% to 50 wt%, the discharge capacity is higher than that of Comparative Examples 1, 2, and 3. In the positive electrode 106 in which the mixing ratio of the first mixture is set to the range of 3 wt% to 50 wt%, the region (first region) in which the first mixture exists prevents the molding density from becoming too high, and the ease of permeation of the electrolyte is improved. In addition, the region (second region) formed of the second base material is intended to increase the molding density. In other words, the first region and the second region are intended to improve the ease of permeation of the electrolyte and to increase the molding density at the same time. As a result, the discharge capacity is improved in the positive electrode 106 in which the mixing ratio of the first mixture is set to the range of 3 wt% to 50 wt% (the ratio in the first region is set to the range of 3 wt% to 50 wt%). The first region can also be said to be the region formed of the first base material.
[0033] In addition, by mixing the first mixture and the second base material and then granulating them to form the second mixture, the particles that have aggregated due to mixing are in a uniform state in the second mixture.
[0034] Here, when positive electrodes are made by mixing granulated mixtures, the particles that have aggregated due to mixing are not aligned, resulting in variation in the amount sucked into the molding machine that forms the positive electrodes, and therefore variation in the mass and height of the positive electrodes.
[0035] On the other hand, in the positive electrode 106 made from the second mixture, the aggregated particles are arranged, so there is less variation in the amount sucked into the molding machine that forms the positive electrode, and there is less variation in the mass and height of the positive electrode. [Explanation of symbols]
[0036] 100 Bobbin type battery 101 cases 102 Sealing plate 103 Terminal 104 Gasket 105 Washer 106 Positive electrode 107 Separator 108 Negative electrode 109 Current collector 111 Positive electrode unit 112 Negative electrode unit
Claims
1. A step of mixing and granulating a first base material including manganese dioxide, a conductive material, and a binder to prepare a first mixture; A step of mixing and granulating a second base material containing manganese dioxide, a conductive material, and a binder with the first mixture to prepare a second mixture; a step of forming the second mixture into a cylindrical positive electrode and bringing the positive electrode into contact with an inner peripheral surface of a cylindrical case having one end closed; injecting an electrolyte into the inside of the case; providing a cylindrical negative electrode and a separator inside the positive electrode; and closing and sealing the other end of the case. A method for manufacturing a bobbin type battery, wherein the amount of binder contained in the first substrate is greater than the amount of binder contained in the second substrate.
2. 2. The method for producing a bobbin type battery according to claim 1, wherein the binder contained in the first base material and the second base material is polytetrafluoroethylene.
3. The method for producing a bobbin type battery according to claim 1 or 2, wherein the negative electrode contains lithium.
4. A cylindrical case and a positive electrode formed in a cylindrical shape and provided so as to be in contact with an inner surface of the case; a negative electrode provided inside the positive electrode; a separator provided between the positive electrode and the negative electrode; An electrolyte is poured inside the case, the positive electrode includes manganese dioxide, a conductive material, and a binder; the positive electrode has a first region and a second region having a smaller amount of binder than the first region, A bobbin type battery, wherein the first region occupies 3 to 50 wt % of the positive electrode.
5. 5. The bobbin type battery according to claim 4, wherein the binder contained in the first region and the second region is polytetrafluoroethylene.
6. 6. The bobbin type battery according to claim 4, wherein the negative electrode contains lithium.
Citation Information