Aqueous resin composition for heat-resistant layer of lithium ion secondary battery separator

An aqueous resin composition with specific acrylic polymers and a controlled polymerization initiator forms a heat-resistant layer, addressing thermal shrinkage and rupture issues in lithium ion secondary battery separators, enhancing safety.

JP2024162708APending Publication Date: 2024-11-21DIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023078528
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing lithium ion secondary battery separators face issues with thermal shrinkage and rupture during high-temperature conditions, leading to potential short circuits and safety risks, despite the presence of a heat-resistant layer.

Method used

An aqueous resin composition containing specific acrylic polymers, such as alkyl (meth)acrylate and N-methylol (meth)acrylamide, is used to form a heat-resistant layer, with a polymerization initiator at 0.05 to 0.25 parts by mass, enhancing the separator's heat shrinkage resistance.

Benefits of technology

The composition provides a separator with excellent heat shrinkage resistance, reducing the risk of short circuits and improving safety in high-capacity lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162708000001
    Figure 2024162708000001
Patent Text Reader

Abstract

To provide an aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator, with which a separator excellent in heat shrinkage resistance can be obtained.SOLUTION: An aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator is used. The aqueous resin composition for the heat-resistant layer of the lithium ion secondary battery separator contains: an acrylic polymer (A) having, as essential raw materials, alkyl(meth)acrylate (a1) having an alkyl group with 4 or more carbon atoms, and one or more monomers (a2) selected from the group consisting of N-methylol(meth)acrylamide and an unsaturated monomer having a carboxyl group; and an aqueous medium (B). The alkyl(meth) acrylate (a1) in monomer raw martials of the acrylic polymer (A) is 50-95 mass%; the monomers (a2) are 1-5 mass%; and a polymerization initiator in a main reaction of the acrylic polymer (A) is 0.05-0.25 pts.mass for 100 pts.mass of the monomer raw materials.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery. [Background technology]

[0002] Polyolefin porous membranes exhibit excellent electrical insulation and ion permeability, and are therefore widely used as separators in batteries, capacitors, etc. In particular, in recent years, as portable devices have become more multifunctional and lighter in weight, lithium ion secondary batteries with high output density and high capacity density have come to be used as their power sources, and polyolefin porous membranes are mainly used as separators for such batteries.

[0003] Lithium-ion secondary batteries have high power density and capacity density, but because they use organic solvents in the electrolyte, the electrolyte can decompose due to heat generated by abnormal events such as short circuits and overcharging, and in the worst case, can even catch fire. To prevent such events, lithium-ion secondary batteries have several built-in safety features, one of which is the separator shutdown feature. When the battery generates abnormal heat, the micropores in the separator are blocked by thermal melting, suppressing ionic conduction in the electrolyte and stopping the progress of the electrochemical reaction. In general, the lower the shutdown temperature, the higher the safety. One of the reasons why polyethylene is used as a separator component is that it has a moderate shutdown temperature.

[0004] However, in high-energy batteries, even if the electrochemical reaction is stopped by shutting down the battery, the temperature inside the battery continues to rise, resulting in the separator shrinking due to heat and rupturing, causing a short circuit between the two electrodes.

[0005] For the purpose of producing a highly safe battery, a technique has been proposed in which a separator is formed by laminating a heat-resistant layer on a first porous layer mainly composed of a thermoplastic resin (see, for example, Patent Document 1).

[0006] However, as the capacity of batteries has been increased, high-capacity batteries tend to generate a large amount of heat during abnormal heating and are prone to being exposed to higher temperature environments. Although the separator described in this publication is considered to be safer than a normal separator that does not have a heat-resistant layer, there is still room for improvement in terms of suppressing the thermal contraction of the separator even in a high-temperature environment and reducing the risk of short-circuiting between the two electrodes due to the separator rupture. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 3756815 specification Summary of the Invention [Problem to be solved by the invention]

[0008] The problem to be solved by the present invention is to provide an aqueous resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery, which can provide a separator having excellent heat shrinkage resistance. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by using an aqueous resin composition containing a specific acrylic polymer and an aqueous medium, thereby completing the present invention.

[0010] That is, the present invention relates to an aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator, which contains an acrylic polymer (A) having, as essential raw materials, an alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms and one or more monomers (a2) selected from the group consisting of N-methylol (meth)acrylamide and unsaturated monomers having a carboxyl group, and an aqueous medium (B), wherein the alkyl (meth)acrylate (a1) is 50 to 95 mass % and the monomer (a2) is 1 to 5 mass % in the monomer raw materials of the acrylic polymer (A), and the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05 to 0.25 parts by mass per 100 parts by mass of the monomer raw materials. Effect of the Invention

[0011] INDUSTRIAL APPLICABILITY The aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator of the present invention can be suitably used as a binder for the heat-resistant layer of a lithium ion secondary battery separator since it can provide a separator having excellent heat shrinkage resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The aqueous resin composition for a heat-resistant layer of a lithium-ion secondary battery separator of the present invention is an aqueous resin composition for a heat-resistant layer of a lithium-ion secondary battery separator, which contains an acrylic polymer (A) having, as essential raw materials, an alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms and one or more monomers (a2) selected from the group consisting of N-methylol (meth)acrylamide and unsaturated monomers having a carboxyl group, and an aqueous medium (B), in which the alkyl (meth)acrylate (a1) and the monomer (a2) in the monomer raw materials of the acrylic polymer (A) account for 50 to 95 mass % and 1 to 5 mass %, respectively, and the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05 to 0.25 parts by mass relative to 100 parts by mass of the monomer raw materials.

[0013] In the present invention, "(meth)acrylamide" refers to either or both of acrylamide and methacrylamide, "(meth)acrylate" refers to either or both of acrylate and methacrylate, "(meth)acrylic acid" refers to either or both of acrylic acid and methacrylic acid, and "(meth)acryloyl" refers to either or both of acryloyl and methacryloyl.

[0014] The radical polymer (A) is made from essential raw materials: an alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms, and one or more monomers (a2) selected from the group consisting of N-methylol (meth)acrylamide and unsaturated monomers having a carboxyl group.

[0015] The alkyl (meth)acrylate (a1) is a monomer having an alkyl group having 4 or more carbon atoms, and examples thereof include n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate. Among these, from the viewpoint of the heat shrinkage resistance of the separator obtained, those having an alkyl group having 4 to 8 carbon atoms are preferred. These acrylic monomers (a1) can be used alone or in combination of two or more. )

[0016] The content of the alkyl (meth)acrylate (a1) in the monomer raw material of the acrylic polymer (A) is 50 to 95 mass %, and from the viewpoint of further improving the heat shrinkage resistance, it is preferably 55 to 95 mass %.

[0017] The monomer (a2) may be N-methylol (meth)acrylamide or an unsaturated monomer having a carboxyl group. These monomers (a2) may be used alone or in combination of two or more.

[0018] Examples of the unsaturated monomer having a carboxyl group include unsaturated monocarboxylic acids such as (meth)acrylic acid and crotonic acid; and unsaturated dicarboxylic acids such as itaconic acid (anhydride), maleic acid (anhydride), and fumaric acid. Among these, unsaturated monocarboxylic acids are preferred. The content of the monomer (a2) in the monomer raw material of the acrylic polymer (A) is 1 to 5% by mass, and is preferably 1 to 3% by mass because this further improves the heat shrinkage resistance.

[0019] The acrylic polymer (A) contains the alkyl (meth)acrylate (a1) and the monomer (a2) as essential raw materials, but other monomers than these may be used as monomer raw materials.

[0020] Examples of the other monomers include alkyl (meth)acrylates having an alkyl group having 1 to 3 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, and propyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, N-(2-hydroxyethyl)(meth)acrylamide, glycerin mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl phthalate, and monomers having a hydroxyl group at the end. monomers having a hydroxyl group, such as lactone-modified (meth)acrylates having the above formula; (meth)acrylates having an amino group, such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, and N,N-diethylaminopropyl (meth)acrylate; monomers having an N-hydroxymethylamide group, such as N-hydroxymethyl(meth)acrylamide; monomers having an N-alkoxymethylamide group, such as N-butoxymethylacrylamide; (meth)acrylates having a glycidyl group, such as glycidyl (meth)acrylate; monomers having an alkoxysilyl group, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropyltriethoxysilane, and 3-(meth)acryloyloxypropylmethyldimethoxysilane;Examples of the polyalkylene glycol (meth)acrylates include polyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, polybutylene glycol (meth)acrylate, and methoxypolybutylene glycol (meth)acrylate; vinyl monomers such as styrene, α-methylstyrene, paramethylstyrene, chloromethylstyrene, vinyl acetate, and (meth)acrylonitrile; tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate; and di(meth)acrylates such as ethylene glycol di(meth)acrylate and propylene glycol di(meth)acrylate. These monomers can be used alone or in combination of two or more.

[0021] The acrylic polymer (A) can be produced by various methods, but the emulsion polymerization method is preferred because the acrylic polymer (A) can be easily obtained.

[0022] Examples of the method for obtaining the acrylic polymer (A) by emulsion polymerization include a method in which monomers serving as raw materials for the acrylic polymer (A) are radically polymerized in an aqueous medium in the presence of an emulsifier and a polymerization initiator at a temperature of 50 to 100°C.

[0023] Examples of the emulsifier include anionic emulsifiers such as sulfate esters and their salts of higher alcohols, alkylbenzene sulfonates, polyoxyethylene alkylphenyl sulfonates, polyoxyethylene alkyl diphenyl ether sulfonates, sulfate half ester salts of polyoxyethylene alkyl ethers, alkyl diphenyl ether disulfonates, and dialkyl succinate sulfonates; nonionic emulsifiers such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene diphenyl ethers, polyoxyethylene-polyoxypropylene block copolymers, and acetylene diols; cationic emulsifiers such as alkyl ammonium salts; and amphoteric emulsifiers such as alkyl (amide) betaines and alkyl dimethyl amine oxides. These emulsifiers can be used alone or in combination of two or more. It is preferable to use these emulsifiers in an amount of 0.5 to 5.0% by mass based on the total amount of monomers that are the raw materials for the polymer.

[0024] Examples of the polymerization initiator include azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), and azobiscyanovaleric acid; organic peroxides such as tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butylperoxy-2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, benzoyl peroxide, and tert-butyl hydroperoxide; and inorganic peroxides such as hydrogen peroxide, ammonium persulfate, potassium persulfate, and sodium persulfate. These polymerization initiators can be used alone or in combination of two or more.

[0025] The amount of the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05 to 0.25 parts by mass relative to 100 parts by mass of the monomer raw material, since the heat shrinkage resistance is improved. The main reaction of the acrylic polymer (A) in the present invention refers to a process in which the monomer raw material and the polymerization initiator are added dropwise or the like to a reaction system to carry out the reaction. After the addition of the monomer raw material to the reaction system is completed, additional polymerization initiator can be added, but this additional polymerization initiator is excluded from the polymerization initiator in the main reaction of the acrylic polymer (A).

[0026] The aqueous medium (B) may be water, an organic solvent miscible with water, or a mixture thereof. Examples of the organic solvent miscible with water include alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; polyalkylene glycols such as ethylene glycol, diethylene glycol, and propylene glycol; alkyl ethers of polyalkylene glycols; and lactams such as N-methyl-2-pyrrolidone. In the present invention, only water may be used, or a mixture of water and an organic solvent miscible with water may be used, or only an organic solvent miscible with water may be used. From the viewpoint of safety and environmental load, only water or a mixture of water and an organic solvent miscible with water is preferred, and only water is particularly preferred.

[0027] As the aqueous medium (B), it is simple and preferable to use the aqueous medium used when producing the acrylic polymer (A) by emulsion polymerization or the like.

[0028] Furthermore, by carrying out a solvent removal step as necessary, the amount of organic solvent in the resin composition of the present invention can be reduced.

[0029] The aqueous resin composition of the present invention obtained by the above method preferably contains the acrylic polymer (A) in an amount of 5 to 60% by mass, more preferably 30 to 55% by mass, based on the total amount of the aqueous resin composition, since this further improves coating workability.

[0030] In addition, the aqueous resin composition of the present invention preferably contains the aqueous medium (B) in an amount of 40 to 95 mass %, more preferably 45 to 70 mass %, based on the total amount of the aqueous resin composition, in order to further improve coating workability.

[0031] The aqueous resin composition of the present invention may contain, as necessary, additives such as a curing agent, a curing catalyst, a lubricant, a filler, a thixotropic agent, a tackifier, a wax, a heat stabilizer, a light resistance stabilizer, a fluorescent whitening agent, a foaming agent, a pH adjuster, a leveling agent, a gelling inhibitor, a dispersion stabilizer, an antioxidant, a radical scavenger, a heat resistance imparting agent, an inorganic filler, an organic filler, a plasticizer, a reinforcing agent, a catalyst, an antibacterial agent, a mildew inhibitor, a rust inhibitor, a thermoplastic resin, a thermosetting resin, a pigment, a dye, an electrical conductivity imparting agent, an antistatic agent, a moisture permeability improving agent, a water repellent, an oil repellent, a hollow foam, a compound containing crystal water, a flame retardant, a water absorbing agent, a moisture absorbing agent, a deodorizer, a foam stabilizer, an antifoaming agent, an antifungal agent, an antiseptic, an anti-algae agent, a pigment dispersant, an antiblocking agent, an antihydrolysis agent, and a pigment.

[0032] Since the aqueous resin composition of the present invention can provide a separator having excellent heat shrinkage resistance, it can be suitably used as a binder for a heat-resistant layer of a lithium ion secondary battery.

[0033] The slurry for a heat-resistant layer of a lithium ion secondary battery separator of the present invention contains the aqueous resin composition of the present invention, and preferably further contains non-conductive particles and a water-soluble polymer.

[0034] The slurry for the heat-resistant layer preferably contains 0.1 to 100 parts by mass of the acrylic polymer (A) and 0.1 to 100 parts by mass of the water-soluble polymer relative to 100 parts by mass of the non-conductive particles.

[0035] As the non-conductive particles, for example, inorganic particles or organic particles can be used, with inorganic particles being preferred.

[0036] Examples of the inorganic particles include oxide particles such as aluminum oxide (alumina), silicon oxide, magnesium oxide, titanium oxide, BaTiO2, ZrO, and alumina-silica composite oxide, nitride particles such as aluminum nitride and boron nitride, covalent crystal particles such as silicon and diamond, sparingly soluble ion crystal particles such as barium sulfate, calcium fluoride, and barium fluoride, and clay particles such as talc and montmorillonite, and among these, aluminum oxide (alumina) is preferred. These inorganic particles can be used alone or in combination of two or more kinds.

[0037] Examples of the organic particles include polyethylene, polystyrene, polydivinylbenzene, styrene-divinylbenzene copolymer crosslinked products, various crosslinked polymer particles such as polyimide, polyamide, polyamideimide, melamine resin, phenolic resin, and benzoguanamine-formaldehyde condensate, and heat-resistant polymer particles such as polysulfone, polyacrylonitrile, polyaramid, polyacetal, and thermoplastic polyimide. These organic particles can be used alone or in combination of two or more kinds.

[0038] Examples of the water-soluble polymer include cellulose-based polymers such as carboxymethyl cellulose, methyl cellulose, and hydroxypropyl cellulose, and their ammonium salts and alkali metal salts; poly(meth)acrylic acid and their ammonium salts and alkali metal salts; polyvinyl alcohol compounds such as polyvinyl alcohol, copolymers of acrylic acid or acrylic acid salts with vinyl alcohol, copolymers of maleic anhydride or maleic acid or fumaric acid with vinyl alcohol; polyethylene glycol, polyethylene oxide, polyvinylpyrrolidone, modified polyacrylic acid, oxidized starch, starch phosphate, casein, various modified starches, etc. These water-soluble polymers can be used alone or in combination of two or more kinds.

[0039] Examples of the particulate polymer include crosslinked poly(meth)acrylic acid particles, crosslinked poly(meth)acrylic acid ester particles, crosslinked polystyrene particles, copolymer crosslinked resin particles of (meth)acrylic acid ester and styrene, melamine resin particles, nylon particles, polyimide particles, polyamideimide particles, phenol resin particles, polytetrafluoroethylene particles, fluororesin particles, silicone resin particles, etc. These particulate polymers can be used alone or in combination of two or more kinds.

[0040] The heat-resistant layer in the present invention can be formed by applying the slurry for the heat-resistant layer onto the separator. The method for applying the slurry for the heat-resistant layer onto the substrate can be, for example, a doctor blade method, a dip method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, a brush coating method, etc. In this case, the slurry for the heat-resistant layer may be applied to only one side of the substrate, or may be applied to both sides.

[0041] Examples of methods for drying the slurry composition for the heat-resistant layer on the substrate include drying methods using warm air, hot air, or low-humidity air, vacuum drying, and drying methods using infrared rays, electron beams, etc. By drying the slurry composition for the heat-resistant layer on the substrate in this manner, the separator of the present invention having a heat-resistant layer formed on the substrate can be obtained. EXAMPLES

[0042] The present invention will now be described in more detail with reference to specific examples.

[0043] (Example 1: Production and evaluation of aqueous resin composition (1)) In a 1.0L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 50.0 parts by mass of ion-exchanged water was charged and heated to 80°C, and then monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-methylol acrylamide, 90.0 parts by mass of n-butyl acrylate, and 7.5 parts by mass of acrylonitrile emulsified with an emulsifier aqueous solution in which 1.5 parts by mass of anionic emulsifier (Dai-ichi Kogyo Seiyaku's "Hitenol LA-12") was dissolved in 35.5 parts by mass of ion-exchanged water) and 10 parts by mass of a 2% by mass aqueous solution of sodium persulfate were dropped for 3 hours to carry out a reaction. After the reaction was completed, the mixture was held at the same temperature for 2 hours, cooled, and adjusted to 45.3% nonvolatile content and 8.1 using ion-exchanged water and 12.5% ​​aqueous ammonia solution to obtain an aqueous resin composition (1). The viscosity of this aqueous resin composition at 25°C was 18 mPa·s.

[0044] (Example 2: Production and evaluation of aqueous resin composition (2)) In a 1.0L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 50.0 parts by mass of ion-exchanged water was charged and heated to 80°C, and then a monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-methylol acrylamide, 60.0 parts by mass of n-butyl acrylate, and 37.5 parts by mass of acrylonitrile emulsified with an emulsifier aqueous solution in which 1.5 parts by mass of an anionic emulsifier (Dai-ichi Kogyo Seiyaku's "Hitenol N-08") was dissolved in 35.5 parts by mass of ion-exchanged water) and 10 parts by mass of a 2% by mass aqueous solution of sodium persulfate were added dropwise for 3 hours to carry out a reaction. After the reaction was completed, the mixture was held at the same temperature for 2 hours, cooled, and the nonvolatile content was adjusted to 45.1% by mass and the pH was adjusted to 8.2 using ion-exchanged water and a 12.5% ​​aqueous ammonia solution, to obtain an aqueous resin composition (2). The viscosity of this aqueous resin composition at 25°C was 15 mPa·s.

[0045] (Example 3: Production and evaluation of aqueous resin composition (3)) In a 1.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 50.0 parts by mass of ion-exchanged water was charged and heated to 80°C, and then a monomer premix (a mixture of 2.0 parts by mass of acrylic acid, 2.5 parts by mass of N-methylol acrylamide, 89.0 parts by mass of n-butyl acrylate, and 6.5 parts by mass of acrylonitrile emulsified with an emulsifier aqueous solution in which 1.5 parts by mass of an anionic emulsifier (Dai-ichi Kogyo Seiyaku's "Hitenol N-08") was dissolved in 35.5 parts by mass of ion-exchanged water) and 10 parts by mass of a 1% by mass aqueous sodium persulfate solution were added dropwise for 3 hours to carry out a reaction. After the reaction was completed, the mixture was held at the same temperature for 2 hours, cooled, and adjusted to 45.4% by mass of nonvolatile matter and 8.0 by mass using ion-exchanged water and a 12.5% ​​aqueous ammonia solution to obtain an aqueous resin composition (3). The viscosity of this aqueous resin composition at 25°C was 32 mPa·s.

[0046] (Example 4: Production and evaluation of aqueous resin composition (4)) In a 1.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 50.0 parts by mass of ion-exchanged water was charged and heated to 80°C, and then monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-methylol acrylamide, 90.0 parts by mass of 2-ethylhexyl acrylate, and 7.5 parts by mass of acrylonitrile emulsified with an emulsifier aqueous solution in which 1.5 parts by mass of anionic emulsifier (Dai-ichi Kogyo Seiyaku's "Hitenol LA-12") was dissolved in 35.5 parts by mass of ion-exchanged water) and 10 parts by mass of a 1% by mass aqueous sodium persulfate solution were added dropwise for 3 hours to carry out a reaction. After the reaction was completed, the mixture was held at the same temperature for 2 hours, cooled, and the nonvolatile content was adjusted to 45.2% by mass and the pH was adjusted to 8.2 using ion-exchanged water and a 12.5% ​​aqueous ammonia solution, to obtain an aqueous resin composition (1). The viscosity of this aqueous resin composition at 25°C was 26 mPa·s. (Example 5: Production and evaluation of aqueous resin composition (5)) In a 1.0 L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 50.0 parts by mass of ion-exchanged water was charged and heated to 80°C, and then a monomer premix (a mixture of 1.0 part by mass of methacrylic acid, 1.5 parts by mass of N-methylol acrylamide, 81.5 parts by mass of n-butyl acrylate, 5.0 parts by mass of acrylonitrile, 8.0 parts by mass of methyl methacrylate, 1.5 parts by mass of n-butyl methacrylate, and 1.5 parts by mass of 2-ethylhexyl acrylate emulsified with an aqueous emulsifier solution in which 1.5 parts by mass of anionic emulsifier ("Hitenol N-08" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was dissolved in 35.5 parts by mass of ion-exchanged water) and 10 parts by mass of a 2% by mass aqueous sodium persulfate solution were added dropwise for 3 hours to carry out a reaction. After the reaction was completed, the mixture was held at the same temperature for 2 hours, cooled, and adjusted to a non-volatile content of 45.5% by mass and a pH of 8.3 using ion-exchanged water and a 12.5% ​​aqueous ammonia solution to obtain an aqueous resin composition (5). The viscosity of this aqueous resin composition at 25°C was 18 mPa s.

[0047] (Comparative Example 1: Production and Evaluation of Aqueous Resin Composition (R1)) In a 5 MPa pressure vessel equipped with a stirrer, 100.0 parts by mass of the monomer composition, 0.3 parts by mass of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts by mass of ion-exchanged water, and 0.3 parts by mass of potassium persulfate as a polymerization initiator were placed, thoroughly stirred, and then heated to 50°C to initiate polymerization. The monomer composition consisted of 92.8 parts by mass of n-butyl acrylate, 2.0 parts by mass of acrylonitrile, 2.0 parts by mass of methacrylic acid, 1.6 parts by mass of N-methylolacrylamide, and 1.6 parts by mass of acrylamide. When the polymerization conversion rate reached 96%, the mixture was cooled to stop the reaction, and a mixture containing a particulate polymer was obtained. A 5% aqueous sodium hydroxide solution was added to the mixture containing the particulate polymer to adjust the pH to 6, and unreacted monomers were removed by heating and vacuum distillation, and then the mixture was cooled to 30°C or less to obtain an aqueous resin composition (R1) as an aqueous dispersion containing a particulate (meth)acrylic polymer.

[0048] (Comparative Example 2: Production and Evaluation of Aqueous Resin Composition (R2)) In a 1.0L reaction vessel equipped with a stirrer, a thermometer, a cooler, and a nitrogen blower, 50.0 parts by mass of ion-exchanged water was charged and heated to 80°C, and then monomer premix (a mixture of 1.0 parts by mass of acrylic acid, 1.5 parts by mass of N-methylol acrylamide, 90.0 parts by mass of lauryl methacrylate, and 7.5 parts by mass of acrylonitrile emulsified with an emulsifier aqueous solution in which 1.5 parts by mass of anionic emulsifier (Dai-ichi Kogyo Seiyaku's "Hitenol LA-12") was dissolved in 35.5 parts by mass of ion-exchanged water) and 10 parts by mass of a 3% by mass aqueous solution of sodium persulfate were added dropwise for 3 hours to carry out a reaction. After the reaction was completed, the mixture was held at the same temperature for 2 hours, cooled, and the non-volatile content was adjusted to 45.3% by mass and the pH was adjusted to 8.1 using ion-exchanged water and a 12.5% ​​aqueous ammonia solution to obtain an aqueous resin composition (R2). The viscosity of this aqueous resin composition at 25°C was 18 mPa·s.

[0049] [Preparation of heat-resistant layer slurry] While stirring at 5,000 rpm with a homodisper, 100 parts by mass of 1% by mass carboxymethylcellulose (manufactured by Daicel Chemical Industries, Ltd., "DN-800H") was gradually added to 100 parts by mass of alumina (manufactured by Sumitomo Chemical Industries, Ltd., "AKP3000") to carry out dispersion. After these were uniformly mixed, 12.5 parts by mass of the aqueous resin composition obtained above and 52.4 parts by mass of ion-exchanged water were added and mixed uniformly to prepare a heat-resistant layer slurry.

[0050] [Preparation of separator with heat-resistant layer] The heat-resistant layer slurry obtained above was applied to both sides of a 12 μm-thick polyethylene separator substrate using a bar coater so that the film thickness after drying would be 4 μm, to obtain a separator having a heat-resistant layer. The drying temperature was 80° C. and the drying time was 5 minutes.

[0051] [Evaluation of heat shrink resistance] The separator with the heat-resistant layer prepared above was cut into 5 cm squares, and placed between thick paper in a hot air dryer at 180°C for 1 hour to perform a heat resistance test. After the test, the length and width of the separator were measured, and the shrinkage rate in the vertical direction (MD shrinkage rate (%)) and the shrinkage rate in the horizontal direction (TD shrinkage rate (%)) were calculated to evaluate the heat shrinkage resistance. Shrinkage rate (%) = separator length after test / separator length before test × 100 (%)

[0052] The evaluation results of Examples 1 to 4 and Comparative Example 1 are shown in Table 1.

[0053] [Table 1]

[0054] It was confirmed that the heat-resistant layers obtained from the aqueous resin compositions of the present invention, that is, Examples 1 to 5, were excellent in heat shrinkage resistance.

[0055] On the other hand, in Comparative Examples 1 and 2, the amount of polymerization initiator used relative to the monomer raw material of the acrylic polymer (a1) was greater than the upper limit of the present invention, but it was confirmed that the heat shrinkage resistance was insufficient.

Claims

1. The aqueous resin composition for a heat-resistant layer of a separator for a lithium ion secondary battery contains an acrylic polymer (A) whose essential raw materials are an alkyl (meth)acrylate (a1) having an alkyl group having 4 or more carbon atoms and one or more monomers (a2) selected from the group consisting of N-methylol (meth)acrylamide and unsaturated monomers having a carboxyl group, and an aqueous medium (B), wherein the alkyl (meth)acrylate (a1) is 50 to 95 mass % and the monomer (a2) is 1 to 5 mass % in the monomer raw materials for the acrylic polymer (A), and the polymerization initiator in the main reaction of the acrylic polymer (A) is 0.05 to 0.25 parts by mass per 100 parts by mass of the monomer raw materials.

2. A slurry for a heat-resistant layer of a lithium ion secondary battery separator, comprising the aqueous resin composition for a heat-resistant layer of a lithium ion secondary battery separator according to claim 1.

3. A lithium ion secondary battery separator having a heat-resistant layer obtained by using the slurry for a lithium ion secondary battery separator heat-resistant layer according to claim 2.

Citation Information

Patent Citations

  • Copolymer composition for multilayer porous film

    JP2012219240A

  • Binder composition for power storage device, slurry for power storage device porous layer, power storage device porous layer, separator with power storage device porous layer, lithium ion secondary battery, and method for improving applicability on separator

    JP2018092701A

  • Binder composition for heat-resistant layer of non-aqueous secondary battery, slurry composition for heat-resistant layer of non-aqueous secondary battery, heat-resistant layer of non-aqueous secondary battery, and non-aqueous secondary battery

    WO2021039673A1

  • Binder for secondary battery functional layer, slurry composition for secondary battery functional layer, secondary battery functional layer, and secondary battery

    WO2022114033A1

  • Battery separator and battery

    JP3756815B2