Manufacturing method of fuel cell separator
Laser treatment of stainless steel fuel cell separators modifies the passive film to enhance Cr/Fe and Mn/Fe ratios, effectively addressing corrosion issues and ensuring durability in corrosive conditions.
Patent Information
- Application Number
- JP2023078737
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-11
AI Technical Summary
Conventional stainless steel fuel cell separators face issues with corrosion resistance, particularly when exposed to liquid water during operation, necessitating improved corrosion resistance.
Applying laser treatment to the surface of stainless steel base materials used in fuel cell separators to modify the passive film, enhancing the Cr/Fe and Mn/Fe ratios in the passive film to improve corrosion resistance.
The laser-treated separators exhibit significantly improved corrosion resistance in corrosive environments, preventing corrosion even after prolonged exposure to simulated generated water conditions.
Smart Images

Figure 2024162817000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a separator for a fuel cell. [Background technology]
[0002] 2. Description of the Related Art Solid polymer fuel cells (hereinafter, simply referred to as fuel cells) using an electrolyte membrane can operate at low temperatures and can be made small and lightweight, and therefore their application to automobiles and the like is being considered.
[0003] In such a fuel cell, a plurality of cells (single cells) which are basic units are stacked. The cell includes a membrane electrode assembly having a pair of gas diffusion layers (GDL) arranged on both sides thereof, and a pair of separators which sandwich the assembly. The membrane electrode assembly has a structure in which an anode electrode and a cathode electrode are arranged on both sides of an electrolyte membrane which is an ion exchange membrane.
[0004] Stainless steel separators, which are inexpensive and have excellent corrosion resistance, are widely used as separators for fuel cells. Stainless steel separators generally ensure corrosion resistance by a passive film of chromium oxide (generally Cr2O3), but the specific passive film components actually include oxides and hydroxides such as FeO and FeOH. In addition, if the stainless steel surface is exposed to liquid water such as cooling water used during fuel cell operation or water generated during operation, the stainless steel may corrode. For this reason, when a stainless steel substrate is used for a fuel cell separator, there are some parts that require further improvement in corrosion resistance. Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, in the conventional manufacturing method of stainless steel fuel cell separators, there has been a demand for improved corrosion resistance. Therefore, an object of the present invention is to provide a manufacturing method of fuel cell separators with further improved corrosion resistance. [Means for solving the problem]
[0006] The present inventors have found that the corrosion resistance can be further improved by subjecting the surface of a stainless steel substrate that comes into contact with liquid water to laser treatment, and have completed the present invention.
[0007] That is, the gist of the present invention is as follows. (1) A method for manufacturing a stainless steel fuel cell separator, comprising: subjecting a surface of a stainless steel substrate formed into the shape of a separator to laser treatment so as to come into contact with liquid water, thereby modifying a passive film on the surface of the stainless steel substrate; The passive film of the laser-treated part of the stainless steel substrate surface is determined by X-ray photoelectron spectroscopy (XPS); The ratio of the Cr content (atomic%) to the Fe content (atomic%) (Cr / Fe ratio) is greater than 1 when the ratio before the laser treatment is taken as 1, and / or The ratio of the Mn content (atomic%) to the Fe content (atomic%) (Mn / Fe ratio) is greater than 1 when the ratio before laser treatment is taken as 1. A method for producing a separator for a fuel cell, which is modified to have a passivation film. (2) The energy density of the laser is 10 mJ / mm 2 ~40mJ / mm 2 The method for producing a fuel cell separator according to (1) above, (3) The energy density of the laser is 10 mJ / mm 2 ~20mJ / mm 2 The method for producing a fuel cell separator according to (1) or (2) above, Effect of the Invention
[0008] According to the present invention, it is possible to provide a method for producing a fuel cell separator having improved corrosion resistance. [Brief description of the drawings]
[0009] [Figure 1]1A to 1C show the results of XPS analysis in the depth direction of the passive film before a corrosion test in an example (FIG. 1A: 20 mJ / mm 2 laser-treated area, FIG. 1B: 30 mJ / mm 2 laser-treated area, FIG. 1C: laser-untreated area). [Diagram 2] Fig. 2A shows an XPS spectrum representing the bonding state of Cr in a passive film before a corrosion test in an example, and Fig. 2B shows an XPS spectrum representing the bonding state of O in a passive film before a corrosion test in an example. [Diagram 3] 3A to 3C show the change in Cr / Fe ratio over time in the corrosion test for the laser-treated and untreated areas in the examples (FIG. 3A: 20 mJ / mm2 laser-treated area, FIG. 3B: 30 mJ / mm2 laser-treated area, FIG. 3C: untreated area). [Figure 4] 4A and 4B show the results of XPS analysis of the passive film in the depth direction of the laser-treated area after the corrosion test in the example (FIG. 4A: 20 mJ / mm2 laser-treated area, FIG. 4B: 30 mJ / mm2 laser-treated area). [Diagram 5] 5A and 5B show the results of XPS analysis of the passive film in the depth direction of the untreated area (corroded area) of the laser-treated sample after the corrosion test in the examples (FIG. 5A: untreated area of the sample treated with 20 mJ / mm2 laser, FIG. 5B: untreated area of the sample treated with 30 mJ / mm2 laser). [Figure 6] Fig. 6A shows an XPS spectrum representing the bonding state of Cr in a passive film after a corrosion test in an example, and Fig. 6B shows an XPS spectrum representing the bonding state of O in a passive film after a corrosion test in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Preferred embodiments of the present invention will now be described in detail.
[0011] The present invention relates to a method for manufacturing a stainless steel fuel cell separator from a stainless steel substrate, and the method for manufacturing a fuel cell separator of the present invention includes performing laser treatment on the surface of the stainless steel substrate formed into the shape of the separator that comes into contact with liquid water (product water or cooling water), particularly around the manifold.
[0012] The stainless steel for the stainless steel substrate is not particularly limited, and examples thereof include austenitic stainless steels such as SUS304, SUS316, and SUS430, and ferritic stainless steels such as SUS444, as specified in JIS G 4305:2015.
[0013] The thickness of the stainless steel substrate is not particularly limited, but is usually 80 μm to 200 μm, and preferably 80 μm to 100 μm.
[0014] In the present invention, a laser is irradiated onto the surface of a stainless steel substrate formed into the shape of a separator to modify the passive film on the surface of the stainless steel substrate. The stainless steel substrate can be formed into the shape of a separator by, for example, press molding. The shape of the separator may be any shape that is commonly used for fuel cells, for example, a shape in which a number of grooves are formed in the unevenness along the longitudinal direction, and flow paths for fuel gas, oxidant gas, and coolant are formed, but is not limited to this shape as long as these flow paths can be secured.
[0015] In the present invention, the surface of the stainless steel substrate formed into the shape of a separator is irradiated with a laser to improve the corrosion resistance of the portion treated with the laser (laser-treated portion). A fuel cell separator usually comes into contact with generated water as liquid water on the gas surface side that comes into contact with fuel gas and oxidant gas, and comes into contact with cooling water as liquid water on the cooling surface side opposite to the fuel gas and oxidant gas in the thickness direction. In particular, generated water is likely to accumulate around the manifold through which fuel gas and air flow, and electrochemical corrosion is likely to occur in the cooling water manifold with the cooling water as an electrolyte. In the present invention, since the corrosion resistance is improved in the portion of the stainless steel substrate surface treated with a laser, it is preferable to perform laser treatment on the surface around the manifold that comes into contact with generated water and the periphery of the cooling water manifold that comes into contact with the cooling water and causes electrochemical corrosion. In the present invention, the laser treatment may be performed at least on the portion of the stainless steel substrate surface that comes into contact with liquid water around the manifold, but may also be performed on the entire surface of the stainless steel substrate.
[0016] The laser treatment is preferably carried out so that the laser energy density (hereinafter also referred to as fluence) and treatment speed satisfy the following formula (1). Fluence E (mJ / mm 2 ) / processing speed V(mm / s)=α Equation (1) (In formula (1), α is preferably 0.0033 to 0.0133, more preferably 0.0033 to 0.0067, and particularly preferably 0.0067.)
[0017] The laser fluence is preferably 10 mJ / mm 2 ~40mJ / mm 2 and more preferably 10 mJ / mm 2 ~20mJ / mm 2 or 20mJ / mm 2 Super~40mJ / mm 2 and particularly preferably 10 mJ / mm 2 ~20mJ / mm 2 The laser fluence is 10 mJ / mm 2 ~40mJ / mm 2When the laser fluence is 10 mJ / mm, the passive film having a thickness of several nm on the surface of the stainless steel substrate before the laser treatment can be dissolved, and a new passive film rich in Cr and / or Mn with high corrosion resistance can be formed. 2 ~20mJ / mm 2 In this case, a passivation film richer in Cr and Mn can be formed, which further improves corrosion resistance. In addition, since the energy is low, the life of the laser oscillator is extended, which is also preferable in terms of reducing running costs.
[0018] The processing speed of the laser may be selected so as to satisfy the above formula (1), and is, for example, 1000 mm / s to 5000 m / s, and preferably 2000 mm / s to 4000 mm / s.
[0019] The manufacturing method of the present invention described above provides a stainless steel fuel cell separator with improved corrosion resistance at the laser-treated area. In the fuel cell separator obtained by the manufacturing method of the present invention, the passive film on the surface of the stainless steel base material is modified by the laser treatment to have a passive film with improved corrosion resistance.
[0020] In the fuel cell separator obtained by the manufacturing method of the present invention, the thickness of the passive film of chromium oxide (generally Cr2O3) in the laser-treated portion on the surface of the stainless steel substrate is preferably 1 nm to 50 nm, more preferably 1 nm to 25 nm. The thickness of the passive film in the laser-treated portion varies depending on the fluence of the laser. For example, when the laser fluence is 20 mJ / mm 2 In this case, the thickness of the passive film in the laser-treated area is the same as that before the laser treatment, and is usually about 1 nm to 3 nm. 2 In this case, the thickness of the passive film in the laser-treated area is greater than that before the laser treatment, and is usually about 15 nm to 25 nm.
[0021] In the fuel cell separator obtained by the manufacturing method of the present invention, the passive coating in the laser-treated portion on the surface of the stainless steel substrate is modified to a passive coating in which the ratio of the Cr content (atomic %) to the Fe content (atomic %) (Cr / Fe ratio) determined by X-ray photoelectron spectroscopy (XPS) exceeds 1 when the ratio before the laser treatment is taken as 1, and / or the ratio of the Mn content (atomic %) to the Fe content (atomic %) (Mn / Fe ratio) exceeds 1 when the ratio before the laser treatment is taken as 1. In other words, the passive coating in the laser-treated portion on the surface of the stainless steel substrate is modified to a passive coating in which at least one of the Cr / Fe ratio and the Mn / Fe ratio exceeds 1 when the ratio before the laser treatment is taken as 1.
[0022] In the fuel cell separator obtained by the manufacturing method of the present invention, the Cr / Fe ratio in the passive film in the laser-treated area on the surface of the stainless steel substrate, as determined by XPS analysis, is usually 0.7 to 3.0, with the ratio before laser treatment being taken as 1. The Cr / Fe ratio in the passive film in the laser-treated area varies depending on the laser fluence. For example, when the laser fluence is 20 mJ / mm 2 In this case, the Cr / Fe ratio in the passive film in the laser-treated area is higher than that before the laser treatment. In other words, it is greater than 1 when the ratio before the laser treatment is taken as 1. In addition, when the laser fluence is 30 mJ / mm 2 In this case, the Cr / Fe ratio in the passive film in the laser-treated area is lower than that before the laser treatment.
[0023] In one embodiment, the laser fluence is 20 mJ / mm 2In this case, in the fuel cell separator obtained by the manufacturing method of the present invention, the thickness of the passive film in the laser-treated portion on the surface of the stainless steel substrate is the same as that before the laser treatment, usually about 1 nm to 3 nm, and the Cr / Fe ratio and Mn / Fe ratio in the passive film are higher than those before the laser treatment (i.e., greater than 1 when the ratios before the laser treatment are taken as 1). In this embodiment, the thickness of the passive film in the laser-treated portion is the same as that before the laser treatment, but the Cr / Fe ratio and Mn / Fe ratio in the passive film are significantly increased. In other words, it is presumed that the passive film is composed of oxides richer in Cr and Mn, so that the Fe compounds in the film are relatively reduced, and the corrosion resistance of the laser-treated portion is improved.
[0024] In another embodiment, the laser fluence is 30 mJ / mm 2 In this case, in the fuel cell separator obtained by the manufacturing method of the present invention, the thickness of the passive film in the laser-treated portion of the stainless steel substrate surface is increased from that before the laser treatment, usually about 15 nm to 25 nm, and the Cr / Fe ratio in the passive film is decreased from that before the laser treatment (i.e., less than 1 when the ratio before the laser treatment is taken as 1), and the Mn / Fe ratio in the passive film is increased from that before the laser treatment (i.e., more than 1 when the ratio before the laser treatment is taken as 1). In this embodiment, although the passive film is not a Cr-rich oxide, it is presumed that the corrosion resistance of the laser-treated portion is improved by the further increase in the thickness of the passive film and the improvement in the Mn / Fe ratio. Thus, in the present invention, the improvement in the Mn / Fe ratio in the passive film is also important for improving the corrosion resistance.
[0025] The fuel cell separator of the present invention can be improved in corrosion resistance in a corrosive environment by laser treatment. In the present invention, the corrosive environment refers to a condition in which the separator is immersed in simulated generated water (pH = 3 to 5) at 70°C to 100°C and a potential of 0.8 V to 1.0 V for 24 hours or more.
[0026] In the fuel cell separator of the present invention, the Cr / Fe ratio in the passive film of the laser-treated area on the surface of the stainless steel substrate increases over time in the corrosive environment as determined by XPS analysis. On the other hand, in the unlaser-treated area, the Cr / Fe ratio in the passive film decreases over time. In the manufacturing method for a fuel cell separator of the present invention, by performing laser treatment, the corrosion resistance strength of the obtained fuel cell separator in a corrosive environment is increased, and corrosion can be prevented from progressing at all even in a corrosive environment. EXAMPLES
[0027] The present invention will be described in more detail below with reference to examples, although the technical scope of the present invention is not limited to these examples.
[0028] <Corrosion test> A SUS304 substrate was used as the stainless steel substrate. An energy density (fluence) of 20 mJ / mm was applied to a part of the surface of the SUS304 substrate. 2 or 30mJ / mm 2 Then, laser processing was performed at a processing speed of 3000 mm / s to obtain an evaluation sample.
[0029] A constant potential corrosion test was carried out on the evaluation samples in a corrosive environment simulating generated water. Specifically, the evaluation samples were immersed for 60 hours in simulated generated water (pH = 3) at 70°C to 100°C and a potential of 0.8V to 1.0V was applied. After the corrosion test, the presence or absence of corrosion (discoloration) was visually confirmed.
[0030] In corrosion tests, 20mJ / mm 2 and 30 mJ / mm 2 In all of the evaluation samples at any fluence, the laser-treated area did not discolor and no corrosion was observed, but the untreated area changed color to brown to purple and corrosion was observed. This confirmed that the corrosion resistance of the SUS304 substrate was improved by laser treatment. The difference in the color of corrosion (brown to purple) in the untreated area is thought to be due to variations in the thickness and composition of the passive film on the surface of the SUS304 substrate.
[0031] <Analysis of the mechanism behind improved corrosion resistance> To analyze the mechanism of the improved corrosion resistance confirmed in the corrosion test, X-ray photoelectron spectroscopy (XPS) was performed on the evaluation samples before and after the corrosion test to examine the elements on the surface and in the depth direction of the passive film on the SUS304 substrate surface. XPS analysis was performed using an XPS device (ULVAC; PHI5000 VersaProbeII) under the following conditions: X-ray source; AlKα monochromatic light, output 25 W, voltage 15 kV, irradiation area; φ100 μm, analysis area; 1000 × 200 μm, neutralization gun; ON state, pulse energy (wide; 187.85 eV, narrow; 46.95-117.40 eV), step width (wide; 0.4 eV, narrow; 0.1 eV), shift correction C1s; CC, CH, 284.8 eV. Depth analysis was performed while etching with Ar monomer, voltage 3 kV, irradiation area 2 × 2 mm, and engraving speed (sputtering speed) 6.5 nm / min.
[0032] 1. Surface analysis of the passive film before corrosion testing 1-1. Elemental analysis of the outermost surface of the passive film before corrosion testing The elemental analysis results of the outermost surface of the passive film before the corrosion test are shown in Table 1. As shown in Table 1, the low fluence of 20 mJ / mm 2 In the laser-treated area, the amount of Cr and Mn increased, and the amount of Fe decreased, compared to the untreated area. 2 In the laser-treated area, the amount of Cr was decreased and the amount of Fe, Mn, and O were increased compared to the untreated area. The Cr / Fe ratio in the laser-treated area was higher than that in the non-laser-treated area at a low fluence of 20 mJ / mm. 2 It is higher than the untreated laser treatment, but with a high fluence of 30 mJ / mm 2 The Mn / Fe ratio in the laser-treated area was lower than that in the untreated area, regardless of the fluence. On the other hand, the Mn / Fe ratio in the laser-treated area was higher than that in the untreated area, regardless of the fluence. An increase in the Mn / Fe ratio indicates a relative decrease in the amount of Fe that bonds with oxygen in the passive film, and this is also thought to contribute to improved corrosion resistance.
[0033] [Table 1]
[0034] 1-2. Analysis of the passive film depth before corrosion testing Figures 1A to 1C show the results of XPS analysis (sputtering rate: 6.5 nm / min) of the passive film in the depth direction before the corrosion test (Figure 1A: 20 mJ / mm 2 Laser processing unit, Fig. 1B: 30 mJ / mm 2 (Laser-treated area, Fig. 1C: laser-untreated area). The thickness of the passive film (≒ oxide film) was obtained from Figs. 1A-C. Specifically, the thickness of the passive film is generally defined as half the maximum O amount (oxygen amount), so based on this, the value on the horizontal axis of the graph (sputtering time) was converted to calculate the thickness of the passive film (indicated by the broken line arrow in Figs. 1A-C). As a result, at a laser fluence of 20 mJ / mm 2 The thickness of the passive film is about 2.3 nm (Fig. 1A), and the laser fluence is 30 mJ / mm 2 In the laser-treated area, the thickness of the passive film had increased considerably to approximately 19.5 nm (Fig. 1B), while the thickness of the passive film in the unlaser-treated area was approximately 2.0 nm (Fig. 1C), which was consistent with the commonly known thickness of the passive film on stainless steel (1 to 2 nm).
[0035] For these reasons, the low fluence of 20 mJ / mm 2 It was found that the corrosion resistance of the laser-treated area was improved, even though the thickness of the passive film was almost the same as that of the non-laser-treated area. As can be seen from the XPS spectrum showing the bonding state of Cr in the passive film before the corrosion test shown in Figure 2A and the XPS spectrum showing the bonding state of O in the passive film before the corrosion test shown in Figure 2B, 2 In the laser-treated area, the Cr and O spectra are sharper in the Cr2O3 range than in the untreated area, so it is assumed that the passive film is composed of oxides richer in Cr, which is why the corrosion resistance has improved. 2 In the laser-treated area, the amount of Cr in the passive film is small, but at 20 mJ / mm 2It is presumed that the fact that the Cr and O spectra are sharp in the Cr2O3 range, as in the laser-treated area, and that the passive film is thick contribute to the improvement of corrosion resistance. In this way, it is considered important for improving corrosion resistance that the Cr and O intensities have a sharp shape in the Cr2O3 region in the XPS spectrum, which shows the bonding state of Cr and O in the passive film.
[0036] 2. Surface analysis of the passive film after corrosion testing 2-1. Elemental analysis of the outermost surface of the passive film after corrosion testing The results of elemental analysis of the outermost surface of the passive film after the corrosion test are shown in Table 2. As shown in Table 2, the amount of Fe was smaller and the amount of Cr was larger in the laser-treated area compared to the untreated area (corroded area) regardless of the laser fluence. Figures 3A to 3C show the change in the Cr / Fe ratio for each corrosion test time in the laser-treated and untreated areas (Figure 3A: 20 mJ / mm 2 Laser processing unit, Fig. 3B: 30 mJ / mm 2 (Laser-treated area, Figure 3C: untreated area). As shown in Figures 3A and 3B, the Cr / Fe ratio in the laser-treated area increased with the corrosion test time. This means that the strength of corrosion resistance in the laser-treated area increases in a corrosive environment such as contact with generated water (i.e., corrosion does not progress at all). On the other hand, as shown in Figure 3C, in the unlaser-treated area (SUS304 substrate), the Cr / Fe ratio decreased with the corrosion test time compared to the initial Cr / Fe ratio (before the corrosion test, 0 hr) of the passive film surface, and showed a tendency to eventually become zero. This means that the corrosion resistance of the stainless steel substrate, which has not been modified by laser treatment to modify the passive film, will deteriorate.
[0037] [Table 2]
[0038] 2-2. Analysis of the passive film in the depth direction after corrosion testing The results of 2-1 above were confirmed by XPS analysis of the passive film in the depth direction. Figures 4A and 4B show the results of XPS analysis (sputtering rate: 6.5 nm / min) of the passive film in the laser-treated area in the depth direction after the corrosion test (Figure 4A: 20 mJ / mm 2 Laser processing unit, Fig. 4B: 30 mJ / mm 2 5A and 5B show the results of XPS analysis (sputtering rate: 6.5 nm / min) of the passive film in the depth direction of the unlaser-treated area (corroded area) after the corrosion test (Fig. 5A: 20 mJ / mm 2 Untreated laser-treated sample, Fig. 5B: 30 mJ / mm 2 (Untreated area of the laser-treated sample). As shown in Figures 4A and B, the Cr-rich layer increased in the laser-treated area, and the thickness of the passive film increased (indicated by the broken line arrows (I) and (II) in Figures 4A and B), whereas as shown in Figures 5A and B, the laser-untreated area had changed to an oxide film with almost no Cr present. As can be seen from the XPS spectrum showing the bonding state of Cr in the passive film after the corrosion test shown in Figure 6A and the XPS spectrum showing the bonding state of O in the passive film after the corrosion test shown in Figure 6B, the laser-treated area had a passive film of Cr2O3, whereas the laser-untreated area had changed to an oxide film mainly composed of Fe2O3.
Claims
1. A method for manufacturing a stainless steel fuel cell separator, comprising: subjecting a surface of a stainless steel substrate formed into a separator shape to a contact surface with liquid water, to laser treatment, thereby modifying a passive film on the surface of the stainless steel substrate; The passive film of the laser-treated portion of the stainless steel substrate surface is determined by X-ray photoelectron spectroscopy (XPS); The ratio of the Cr content (atomic %) to the Fe content (atomic %) (Cr / Fe ratio) is greater than 1 when the ratio before the laser treatment is taken as 1, and / or The ratio of the Mn content (atomic %) to the Fe content (atomic %) (Mn / Fe ratio) is greater than 1 when the ratio before the laser treatment is taken as 1. A method for producing a separator for a fuel cell, which is modified to have a passivation film.
2. The energy density of the laser is 10 mJ / mm 2 ~40mJ / mm 2 2. The method for producing a fuel cell separator according to claim 1,
3. The energy density of the laser is 10 mJ / mm 2 ~20mJ / mm 2 3. The method for producing a fuel cell separator according to claim 1 or 2,
Citation Information
Patent Citations
Fuel cell separator, its manufacturing method, and fuel cell
JP2002042827A
Stainless steel for separator of solid polymer fuel cell and its manufacturing method, and solid polymer fuel cell using that stainless steel
JP2004149920A
Fuel cell
JP2005183338A
Performance recovery method of stainless steel separator of solid polymer fuel cell
JP2008027742A
Coating film formation method
JP2017210636A