Heat-generating mold powder
The composition of metal, calcium peroxide, and sodium oxide in exothermic mold powder addresses the issue of hygroscopic nitrates by ensuring uniform dispersibility and rapid crystallization, improving cooling uniformity and slab quality in continuous steel casting.
Patent Information
- Application Number
- JP2023078878
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-11
AI Technical Summary
Nitrates used in exothermic mold powder for continuous steel casting are hygroscopic, leading to solidification during storage, which affects uniform dispersibility and results in insufficient heat generation, causing slag bears and uneven cooling, potentially leading to slab cracking, especially in medium carbon steel.
A composition of 1.0% to 5.0% metal, 0.1% to 3.0% calcium peroxide, and 15.0% or less sodium oxide, which ensures uniform dispersibility and rapid crystallization, preventing excessive heat removal and improving cooling uniformity.
The solution effectively suppresses slag bears and ensures uniform cooling, enhancing the quality of slabs by preventing excessive heat removal, particularly suitable for medium carbon steel casting.
Smart Images

Figure 2024162899000001 
Figure 2024162899000002 
Figure 2024162899000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an exothermic mold powder suitable for continuous casting of steel. [Background technology]
[0002] In continuous casting of steel, molten steel stored in a tundish is poured into a mold through an immersion nozzle to be cooled and solidified, while the solidified shell is continuously drawn downwards through the mold using rolls, thereby continuously producing cast pieces of various shapes such as slabs, blooms, and billets. Powdered or granular mold powder is poured onto the surface of the molten steel in the mold. The mold powder melts due to the heat of the molten steel (hereinafter, the mold powder in the molten state is referred to as "molten slag"), forming a molten slag layer that covers the surface of the molten steel, and the molten slag flows between the solidified shell and the mold, and is discharged and consumed in parallel with the solidified shell. The main roles of the mold powder from the time it is poured until it is consumed are as follows: (1) Ensuring lubrication between the solidified shell and the mold (2) Control of heat flux from the solidified shell to the mold (control of the cooling rate of the solidified shell) (3) Absorption of non-metallic inclusions that float to the surface of molten steel and purification of molten steel (4) Insulation of the molten steel surface (5) Prevention of oxidation of the molten steel surface
[0003] Among these roles, there is one that uses the oxidation and exothermic reaction between a metal or the like as a heat-generating material and an oxidizing agent to improve "(4) heat retention of the molten steel surface." This is called exothermic mold powder.
[0004] Patent Document 1 discloses an exothermic front powder for continuous casting (a type of exothermic mold powder) that contains 3 to 20 mass % of a metal or alloy and 3 to 15 mass % of an alkali metal nitrate as an oxidizing agent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-136766 A [Patent Document 2] JP 2004-001017 A Summary of the Invention [Problem to be solved by the invention]
[0006] The nitrate disclosed in Patent Document 1 is useful as an oxidizing agent. However, nitrate is hygroscopic. When the exothermic mold powder absorbs moisture during storage, the nitrate solidifies. When the nitrate solidifies, the uniform dispersion decreases, so the function of the nitrate as an oxidizing agent decreases, the amount of heat generated becomes insufficient, and poor melting occurs, and slag bears (also called slag rims) may adhere to the inner circumference of the mold above the meniscus. When the slag bears occur and grow, they cause uneven slag flow between the mold and the solidified shell, which may cause cracks in the cast piece due to uneven heat extraction. Therefore, it is necessary to suppress the slag bears in the exothermic mold powder in order to cool the solidified shell uniformly.
[0007] In addition, since medium carbon steel is particularly susceptible to cracking, exothermic molding powder for medium carbon steel must quickly prevent excessive heat from being removed from the slab in the upper part of the mold, and must have slow cooling characteristics due to rapid crystallization between the mold and the solidified shell, i.e., high crystallization temperature and high crystallization rate. To achieve such characteristics, low Na content is required. 2 However, such a low NaO composition is sometimes aimed at (Patent Document 2, etc.). 2 In the O composition, it is difficult to add nitrates that contain Na, such as sodium nitrate.
[0008] The present disclosure has been made in consideration of the above-mentioned circumstances, and its object is to provide an exothermic molding powder that is excellent in suppressing slag bears and is easy to crystallize even under rapid cooling conditions. [Means for solving the problem]
[0009] One aspect of the present disclosure is The raw material contains 1.0% by mass or more and less than 5.0% by mass of metal and 0.1% by mass or more and less than 3.0% by mass of calcium peroxide, The chemical composition of the raw material is 15.0 mass% or less (including zero) of Na 2 The present invention relates to an exothermic molding powder characterized by containing O.
[0010] The exothermic molding powder according to one embodiment of the present disclosure is excellent in suppressing slag bears and crystallizes even under rapid cooling conditions. Therefore, the exothermic molding powder according to one embodiment of the present disclosure is excellent in uniformity of cooling of the solidified shell and can quickly prevent excessive heat removal from the slab in the upper part of the mold, i.e., has excellent slow cooling characteristics and can improve the quality of the slab. Therefore, the exothermic molding powder according to one embodiment of the present disclosure is particularly suitable for continuous casting of medium carbon steel.
[0011] In one aspect of the present disclosure, The chemical composition includes 4.0 mass% or less (including zero) of Na. 2 It is preferable that the glass contains O. The crystallization rate is increased, the glass crystallizes even under rapid cooling conditions, and the glass has excellent slow cooling characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] A preferred embodiment of the present disclosure will be described in detail below. Note that the embodiment described below does not unduly limit the contents of the present disclosure described in the claims, and all of the configurations described in the embodiment are not necessarily essential as a means for solving the problems of the present disclosure.
[0013] The exothermic molding powder of this embodiment contains, as a raw material blend, 1.0 mass% or more and less than 5.0 mass% metal and 0.1 mass% or more and less than 3.0 mass% calcium peroxide, and as a chemical composition of the raw material, 15.0 mass% or less (including zero) Na 2The exothermic molding powder of this embodiment is excellent in suppressing slag bears, and also crystallizes under rapid cooling conditions. Therefore, the uniformity of cooling of the solidified shell is excellent, and excessive heat removal from the slab in the upper part of the mold can be quickly prevented, that is, the slow cooling characteristics are excellent, and the quality of the slab can be improved. Therefore, the exothermic molding powder of this embodiment is particularly suitable for continuous casting of medium carbon steel.
[0014] <Metal> The exothermic molding powder of this embodiment contains 1.0 mass% or more and less than 5.0 mass% of metal as a raw material blend. The metal functions as a heat generating material and contains an alloy, for example, one or more selected from Si, Al, Ca-Si, Al-Mg, Al-Ca-Mg, Fe-Si, etc. The metal content is preferably 1.0 mass% or more and 4.0 mass% or less, more preferably 1.0 mass% or more and 2.0 mass% or less. When the metal content is in a suitable range, the amount of heat generated can be maximized. The form of the metal is not particularly limited, but examples include powder and granules.
[0015] <Calcium peroxide (CaO 2 )> The exothermic molding powder of this embodiment contains calcium peroxide in a raw material blend of 0.1% by mass or more and less than 3.0% by mass. Calcium peroxide functions as an oxidizing agent for metals, but since it has low hygroscopicity, fusion between raw materials hardly occurs, and it disperses uniformly by kneading, and since its decomposition temperature is lower than that of sodium nitrate, it oxidizes metals quickly even at low temperatures. Therefore, the oxidation and exothermic reaction of metals proceeds uniformly even at low temperatures, suppressing the generation of slag bears. The calcium peroxide may be in the form of a pure substance, or may be a formulation to which auxiliary raw materials are added for safe and easy handling. Various commercially available products can be used as the formulation. In the case of a formulation, the content of calcium peroxide is converted to the pure substance. If the content of calcium peroxide is less than 0.1% by mass, oxidation and heat generation are insufficient, and if it is 3.0% by mass or more, oxidation and heat generation are excessive, and the molten slag layer becomes excessively thick, which is not preferable. The content of calcium peroxide is preferably 0.5 to 1.0% by mass, and more preferably 0.6 to 0.9% by mass.
[0016] <Na 2 O> The exothermic molding powder of this embodiment has a chemical composition of the raw material containing 15.0 mass% or less (including zero) Na. 2 It contains O. This increases the crystallization rate of the exothermic molding powder, and it crystallizes even under rapid cooling conditions, quickly preventing excessive heat removal from the slab in the upper part of the mold. In other words, it has excellent slow cooling characteristics and can improve the quality of the slab. This is particularly suitable for continuous casting of medium carbon steel. 2 The O content is preferably 4.0% by mass or less (including zero), and more preferably 3.5% by mass or less (including zero). 2 It is preferred because it does not contain O.
[0017] <Main raw materials> The main raw material constituting the exothermic molding powder of the present embodiment is not particularly limited as long as it is generally used for molding powders, and for example, CaO SiO 2 Portland cement, limestone, quicklime, calcium silicate, synthetic calcium silicate, wollastonite, phosphorus slag, blast furnace slag, dicalcium silicate, sodium carbonate, calcium carbonate, perlite, fly ash, glass powder, silica fume, silica flower, silica sand, silica powder, diatomaceous earth, feldspar, etc. CaO SiO 2 Mass ratio of raw materials (CaO / SiO 2 ) is not particularly limited as long as it is one generally used in molding powders.
[0018] <Auxiliary raw materials> The exothermic mold powder of this embodiment may contain, as auxiliary raw materials, flux raw materials, carbon raw materials, and / or other raw materials generally used in mold powders. The flux raw materials have the role of adjusting the softening point, viscosity, and / or crystallization speed, and for example, fluoride raw materials such as sodium fluoride, lithium fluoride, cryolite, fluorite (calcium fluoride), and magnesium fluoride, carbonate raw materials such as sodium carbonate, lithium carbonate, magnesium carbonate, manganese carbonate, aluminum carbonate, and magnesium carbonate, boric acid, borax, and colemanite can be used. The carbon raw materials have the role of adjusting the slag formation speed of the exothermic mold powder, and for example, coke, graphite, carbon black, and the like can be used. As other raw materials, magnesia, alumina, and the like can be used. In addition, a trace amount of Fe as an inevitable component can be used. 2 O 3 , P 2 O 5 , S, etc. are also permitted.
[0019] <Form of exothermic mold powder> The form of the exothermic molding powder of this embodiment is not particularly limited as long as it is one generally used for molding powders, and for example, powder, extrusion molding granules, hollow spray granules, stirring granules, etc. can be used. EXAMPLES
[0020] Hereinafter, embodiments of the present disclosure will be described in detail.
[0021] 1. Sample Preparation SiO as the main raw material 2 A sample of exothermic mold powder was prepared by kneading calcium silicate, a CaO-based raw material, fluoride raw material, carbonate raw material, carbon raw material, alumina raw material, and / or other raw material magnesia as auxiliary raw materials, calcium peroxide or nitrate raw material as an oxidizing agent, and metal silicon as a metal. All raw materials were powder. The composition of the sample raw materials and the Na content in the chemical composition of the raw materials were 2 The O content is shown in Tables 1 to 6. [Table 1] [Table 2] [Table 3] [Table 4] [Table 5] [Table 6]
[0022] In Examples 1 to 5 and Comparative Examples 1 and 2 in Table 1, the metallic silicon content was fixed at 1.0 mass% and the calcium peroxide content was varied in the raw material composition. In Examples 6 to 10 and Comparative Examples 3 and 4 in Table 2, the metallic silicon content was fixed at 2.0 mass% and the calcium peroxide content was varied. In Examples 11 to 15 and Comparative Examples 5 and 6 in Table 3, the metallic silicon content was fixed at 3.0 mass% and the calcium peroxide content was varied. In Examples 16 to 20 and Comparative Examples 7 and 8 in Table 4, the metallic silicon content was fixed at 4.0 mass% and the calcium peroxide content was varied. In Examples 21 to 28 and Comparative Examples 9 and 10 in Table 5, the Na content in the chemical composition of the raw materials was fixed at 1.0 mass% and the calcium peroxide content was varied. 2 The content of O was reduced. In Comparative Examples 9 and 10, sodium nitrate was used as the oxidizing agent. Table 6 shows Comparative Examples 11 to 16. In Comparative Examples 11 and 12, conventional sodium nitrate was used. In Comparative Example 11, as described later, the heat generation start time was evaluated. In Comparative Examples 13 and 14, the Na content in the chemical composition of the raw material was reduced. 2 The content of O was increased. In Comparative Examples 15 and 16, the content of metallic silicon was increased to 5.0 mass %.
[0023] 2. Measurement and evaluation methods The above samples were subjected to the following measurements and evaluations.
[0024] <Time when fever started> The time from the start of heating the sample to the start of heat generation was measured by differential thermal analysis. That is, a crucible filled with 16 g of the sample and a crucible filled with 16 g of alumina fine powder as a reference sample were simultaneously inserted into an electric furnace at 900°C, and the differential thermal change was recorded to determine the time when heat generation began.
[0025] A slow heat generation start time indicates that the oxidation of the metal and the heat generation reaction are delayed, making it easier for slag to form, while a fast heat generation start time indicates that the powder melts quickly. If there is a difference of ±60 seconds or more compared to the standard Comparative Example 11, it is rated as too slow or too fast (×), if there is a difference of ±15 seconds or more but less than 60 seconds, it is rated as slightly slow or fast but acceptable (△) because it is problematic in practical use, and if the difference is less than ±15 seconds, it is rated as good (◯) as it is equivalent to the standard Comparative Example 11.
[0026] <Melting property> Pig iron was melted in a high-frequency induction furnace, and 400 g of a sample was scattered on the molten iron at 1500°C. The melting properties of the sample were evaluated by visually observing the occurrence of sintered chunks during the melting process.
[0027] The smaller the ratio of decarburized sintered mass to the unmelted powder, the better the melting properties. Observing the inside of the furnace from directly above, when the area ratio of unmelted powder to molten slag is 1:1, if the ratio of decarburized sintered mass to the unmelted powder is less than 25%, it is evaluated as good (◯), if it is between 25% and less than 50%, it is acceptable (△) because there is no problem in practical use, and if it is 50% or more, it is evaluated as unacceptable (×).
[0028] <Crystallization rate> The crystallization rate of the sample was evaluated based on the crystal formation state in the slag film under rapid cooling conditions. The sample was melted in an electric furnace at 1300°C to form molten slag, and a water-cooled stainless steel pipe was immersed in the molten slag to form a slag film on the outer circumference of the stainless steel pipe. The immersion times were 10 and 30 seconds.
[0029] The larger the proportion of the crystalline structure formed on the surface of the slag film in the entire slag film (crystalline area ratio), the faster the crystallization rate, i.e., the easier it is to crystallize, which is preferable. If the crystalline area ratio was 50% or more after 10 seconds of immersion, the crystallization rate was evaluated as fast (◯), if it was 50% or more after 30 seconds of immersion, it was evaluated as acceptable (△) since there was no practical problem, and if it was less than 50% after 30 seconds of immersion, the crystallization rate was evaluated as slow (×).
[0030] <Overall rating> The overall evaluation was as follows: if all three of the above evaluations were ◯, it was excellent (◎); if there were two ◯ and no ×, it was good (◯); if there was one or less ◯ and no ×, it was fair (△); and if there was one or more ×, it was poor (×).
[0031] 3. Measurement and evaluation results The measurement and evaluation results are shown in Tables 1 to 6.
[0032] As can be seen from Tables 1 to 5, all of the Examples had better heat generation start times than Comparative Examples 1 to 10, which did not contain calcium peroxide or contained 3.0 mass% or more of calcium peroxide in the raw material blend. Therefore, it is considered that the calcium peroxide content in the raw material blend should be 0.1 mass% or more and less than 3.0 mass%, with 0.5 to 1.0 mass% being preferable, and 0.6 to 0.9 mass% being more preferable. On the other hand, Comparative Examples 1, 3, 5, and 7, which did not contain calcium peroxide, showed heat generation start times that were too slow, while Comparative Examples 2, 4, 6, and 7, which contained 3.0 mass% or more of calcium peroxide, showed heat generation start times that were too fast.
[0033] From Table 5, the Na content in the chemical composition of the raw material 2 In Examples 21 to 28, in which the O content was reduced, the crystallization rate was good. 2 Comparative Examples 13 and 14 (Table 6), in which the content of O was increased, showed poor crystallization speed. 2 The O content is considered to be 15.0 mass % or less (including zero), preferably 4.0 mass % or less (including zero), and more preferably 3.5 mass % or less (including zero).
[0034] As seen from Tables 1 to 5, all of the Examples had good heat generation start times, while Comparative Examples 15 and 16 (Table 6), in which the content of metallic silicon was increased, showed poor melting properties. Therefore, it is considered that the metallic silicon content in the raw material composition is 1.0 mass% or more and less than 5.0 mass%, preferably 1.0 mass% or more and 4.0 mass% or less, and more preferably 1.0 mass% or more and 2.0 mass% or less.
[0035] Although the present embodiment has been described in detail as above, it will be easily understood by those skilled in the art that many modifications are possible without substantially departing from the novel matters and effects of the present disclosure. Therefore, all such modifications are included in the scope of the present disclosure. For example, a term described at least once in the specification together with a different term having a broader meaning or the same meaning may be replaced with that different term anywhere in the specification. In addition, the configuration and operation of the manufacturing apparatus, etc. of the present embodiment are not limited to those described in the present embodiment, and various modifications are possible.
Claims
1. The raw material composition includes 1.0 mass% or more and less than 5.0 mass% of metal and 0.1 mass% or more and less than 3.0 mass% of calcium peroxide, The chemical composition of the raw material is 15.0 mass% or less (including zero) of Na 2 An exothermic molding powder comprising O.
2. The exothermic molding powder according to claim 1, The chemical composition includes 4.0 mass% or less (including zero) of Na. 2 An exothermic molding powder comprising O.
Citation Information
Patent Citations
Exothermic flux for continuous casting
JP1978070039A
Front powder for continuous casting
JP1991169467A
Method for preventing surface oxidation (deckel) at the time of starting reused tundish
JP1997276996A
Mold powder for continuous casting of steel
JP2004001017A
Exothermic front powder for continuous casting
JP2019136766A