Thermosetting silicone adhesive composition and cured product thereof
The thermosetting silicone adhesive composition cures rapidly by heating, overcoming environmental and surface curing issues, ensuring strong adhesion and rubber strength for complex electronic component assembly.
Patent Information
- Application Number
- JP2023079052
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024163451000013 
Figure 2024163451000014 
Figure 2024163451000015
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat-curable silicone pressure-sensitive adhesive composition and a cured product thereof, and more specifically to a heat-curable silicone pressure-sensitive adhesive composition and a cured product thereof that can be suitably used as a temporary fixing material for transporting objects. [Background technology]
[0002] In recent years, electronic devices such as smartphones, liquid crystal displays, in-vehicle components, etc., are required to not only improve their performance but also to save space and energy. In response to such societal demands, the electric and electronic components mounted on them are becoming smaller and smaller, and the assembly process is becoming more complex and difficult every year.
[0003] A technology that can selectively and simultaneously transfer such miniaturized elements and components has been developed in recent years and is attracting attention. This technology is called micro-transfer printing technology, and it uses the adhesive power of elastomers to pick up microscopic components in one go and transfer them to the desired location.
[0004] As a micro-transfer printing material, an adhesive article in which a silicone adhesive composition is cured and molded on a substrate or the like is used.
[0005] Silicone elastomers are known as adhesive materials for this purpose, and addition heat curing type silicone-based adhesives (Patent Document 1) and ultraviolet curing type silicone-based adhesives (Patent Documents 2 and 3) have been proposed.
[0006] However, when using a thermosetting silicone adhesive that cures through an addition reaction, the cured product may shrink when cooled to room temperature after heat curing, which may result in large dimensional errors in the pattern. Furthermore, addition-curing silicone adhesives can be inhibited from curing by the surface on which the material is applied, which can cause poor curing during material molding, and their use can be limited by the environment around the material.
[0007] On the other hand, ultraviolet-curing silicone pressure-sensitive adhesives have excellent dimensional accuracy and are not inhibited from curing by the surface on which the material is applied, but their use may be limited because they require equipment capable of irradiating ultraviolet light. Furthermore, UV-curable silicone adhesives are strongly affected by oxygen curing inhibition, making it difficult to cure them in the atmosphere, and therefore require UV irradiation in a vacuum or nitrogen atmosphere. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2021-123620 A [Patent Document 2] Patent No. 7131631 [Patent Document 3] Patent No. 7156392 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in view of the above circumstances, and has an object to provide a thermosetting silicone pressure-sensitive adhesive composition which can be cured in a short time by heating, is not inhibited in curing by the environment surrounding the material, and gives a cured product having excellent adhesive properties as a temporary fixing material, and a cured product thereof. [Means for solving the problem]
[0010] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, they discovered that by using an organopolysiloxane having a specific (meth)acryloyloxy-containing group, a monofunctional (meth)acrylate compound not containing a siloxane structure, a peroxide that acts as a radical generator, and an organopolysiloxane resin having a specific (meth)acryloyloxy-containing group, it is possible to obtain a thermosetting silicone composition that cures when heated and gives a cured product that has good adhesion and rubber strength even without containing a non-crosslinkable resin, and thus completed the present invention.
[0011] That is, the present invention provides 1. (A) The following general formula (1) [ka] (In the formula, R 1 each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms; R 2 represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms, R 3 are each independently an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group, p is a number that satisfies 0≦p≦10, and a is a number that satisfies 1≦a≦3. A wavy line represents a bond. In one molecule, there is provided an organopolysiloxane having two groups represented by the formula: (B) a monofunctional (meth)acrylate compound not containing a siloxane structure: 1 to 200 parts by mass, (C) (a) the following general formula (2) [ka] (In the formula, R 1 , R 2 , R 3 , a and p have the same meanings as above. (b) R 4 3SiO 1 / 2 Units (wherein R 4represents a monovalent hydrocarbon group having 1 to 10 carbon atoms.) and (c) SiO 4 / 2 units, and the molar ratio of the sum of the (a) units and the (b) units to the (c) units is in the range of 0.4 to 1.2:1: 1 to 1,000 parts by mass of an organopolysiloxane resin; and (D) Organic peroxide: 0.01~5 parts by mass and not containing a non-crosslinkable organopolysiloxane resin. 2. The thermosetting silicone pressure-sensitive adhesive composition according to 1, which contains 1 to 200 parts by mass of (E) silica per 100 parts by mass of component (A). 3. The thermosetting silicone pressure-sensitive adhesive composition according to 1, further comprising an antistatic agent (F) in an amount of 0.001 to 10 parts by mass per 100 parts by mass of component (A). 4. A cured product of the heat-curable silicone pressure-sensitive adhesive composition according to any one of 1 to 3. 5. The cured product according to 4, having a tensile strength (JIS-K6249) of 1 MPa or more at a thickness of 2.0 mm. 6. An adhesive comprising the cured product according to 4. 7. An adhesive sheet comprising the cured product according to 4. 8. A stamp for transferring a microstructure comprising the cured product according to 4. 9. The stamp for transferring a microstructure according to 8, having at least one convex structure. 10. A microstructure transfer device equipped with the microstructure transfer stamp according to claim 8. 11. A microstructure transfer device equipped with the microstructure transfer stamp according to claim 9. 12. A microstructure-holding substrate having an adhesive layer made of the cured product according to claim 4. 13. A microstructure transfer device equipped with the microstructure holding substrate according to 12. to provide. Effect of the Invention
[0012] The adhesive thermosetting silicone rubber composition of the present invention has good curing properties when heated, and the cured product has excellent adhesiveness and rubber strength as a temporary fixing material. It is not affected by curing inhibition from the surface to which the material is applied, and since it does not contain non-crosslinkable resin, adhesive transfer is also suppressed. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic diagram showing an example of a stamp for transferring a minute structure of the present invention. [Diagram 2] 1 is a schematic diagram showing another example of the stamp for transferring a minute structure of the present invention. FIG. [Diagram 3] 1A to 1C are schematic diagrams illustrating an example of a method for producing a stamp for transferring a microstructure of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be specifically described below. The thermosetting silicone pressure-sensitive adhesive composition according to the present invention comprises: (A) 100 parts by mass of an organopolysiloxane having two groups represented by the following general formula (1) in one molecule; (B) 1 to 200 parts by mass of a monofunctional (meth)acrylate compound not containing a siloxane structure; (C) (a) a unit represented by the following general formula (2), (b) R 4 3SiO 1 / 2 Units (wherein R 4 represents a monovalent hydrocarbon group having 1 to 10 carbon atoms.) and (c) SiO 4 / 2 The organopolysiloxane resin is characterized by comprising 1 to 1,000 parts by mass of an organopolysiloxane resin consisting of (a) units and (b) units, in which the molar ratio of (c) units to the sum of (a) units and (b) units is in the range of 0.4 to 1.2:1, and 0.01 to 5 parts by mass of (D) peroxide, and is free of any non-crosslinked organopolysiloxane resin.
[0015] (A) Organopolysiloxane The component (A) used in the present invention is the crosslinking component of the composition, and is an organopolysiloxane having two groups represented by the following general formula (1) in each molecule and whose main chain is essentially composed of repeating diorganosiloxane units.
[0016] [ka] (The wavy lines represent bonds.)
[0017] In formula (1), R 1 each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, excluding aliphatic unsaturated groups; R 2 represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 5 carbon atoms; R 3 each independently represents an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group; p represents a number satisfying 0≦p≦10; and a represents a number satisfying 1≦a≦3.
[0018] In formula (1), R 1 The monovalent hydrocarbon group having 1 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, cyclohexyl, n-octyl, 2-ethylhexyl, and n-decyl; alkenyl groups such as vinyl, allyl (2-propenyl), 1-propenyl, isopropenyl, and butenyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; and aralkyl groups such as benzyl, phenylethyl, and phenylpropyl. In addition, some or all of the hydrogen atoms bonded to the carbon atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms such as chlorine, fluorine, bromine, etc., or other substituents such as a cyano group. Specific examples of such substituents include halogen-substituted hydrocarbon groups such as chloromethyl, bromoethyl, and trifluoropropyl groups, and cyano-substituted hydrocarbon groups such as a cyanoethyl group. Among these, R 1 As the alkyl group, an alkyl group having 1 to 5 carbon atoms and a phenyl group are preferable, and a methyl group, an ethyl group and a phenyl group are more preferable.
[0019] Also, R 2 The alkylene group having 1 to 20 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include methylene, ethylene, propylene, trimethylene, tetramethylene, isobutylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, and decylene groups. Among these, R 2 is preferably an oxygen atom, a methylene, an ethylene or a trimethylene group, and more preferably an oxygen atom or an ethylene group.
[0020] In addition, R 3 The number of carbon atoms of the alkyl (alkylene) group in the acryloyloxyalkyl group, methacryloyloxyalkyl group, acryloyloxyalkyloxy group, or methacryloyloxyalkyloxy group is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5. Specific examples of these alkyl groups include those in the above R 1 Among the groups exemplified above, those having 1 to 10 carbon atoms are included. R 3 Specific examples of the above include those represented by the following formulas, but are not limited thereto.
[0021] [ka] (In the formula, b represents a number satisfying 1≦b≦4, and R 5represents an alkylene group having 1 to 10 carbon atoms. A wavy line represents a bond.
[0022] The above-mentioned p represents a number satisfying 0≦p≦10, preferably a number satisfying 0≦p≦5, more preferably 0 or 1, and the above-mentioned a represents a number satisfying 1≦a≦3, more preferably 1 or 2.
[0023] The bonding position of the group represented by general formula (1) in the organopolysiloxane molecule of component (A) used in the present invention may be at the terminals of the molecular chain, non-terminals of the molecular chain (i.e., in the middle of the molecular chain or at a side chain of the molecular chain), or both, but from the perspective of flexibility of the cured product, it is desirable for it to be present only at the terminals.
[0024] In the organopolysiloxane molecule of component (A), groups bonded to silicon atoms other than the group represented by general formula (1) above are, for example, the above R 1 In particular, monovalent hydrocarbon groups having 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, excluding aliphatic unsaturated groups. Specific examples of these include the above R 1 Examples of the groups include the same groups as those exemplified in 1. From the viewpoint of ease of synthesis, an alkyl group, an aryl group, or a halogenated alkyl group is preferred, and a methyl group, a phenyl group, or a trifluoropropyl group is more preferred.
[0025] The molecular structure of component (A) is basically a straight-chain or branched-chain main chain consisting of repeating diorganosiloxane units (including straight-chain main chains having a branch as part of the main chain), and straight-chain diorganopolysiloxanes in which both molecular chain terminals are blocked with groups represented by the above general formula (1) are particularly preferred. The component (A) may be a single polymer having these molecular structures, a copolymer having these molecular structures, or a mixture of two or more of these polymers.
[0026] The viscosity of the organopolysiloxane of component (A) at 25°C is preferably 10 to 100,000 mPa·s, more preferably 10 to 50,000 mPa·s, in order to improve the workability of the composition and the mechanical properties of the cured product. This viscosity range usually corresponds to a number average degree of polymerization of about 10 to 2,000, preferably about 50 to 1,100, in the case of a linear organopolysiloxane. In the present invention, the viscosity can be measured using a rotational viscometer (e.g., BL type, BH type, BS type, cone-plate type, rheometer, etc.) (hereinafter the same). In the present invention, the degree of polymerization (or molecular weight) can be determined as the number average degree of polymerization (or number average molecular weight) in terms of polystyrene in gel permeation chromatography (GPC) analysis using, for example, toluene or the like as a developing solvent (the same applies hereinafter).
[0027] Specific examples of the organopolysiloxane of the component (A) include those represented by the following formulas (3) to (5), but are not limited to these.
[0028] [ka] (In the formula, R 1 , R 5 and b have the same meaning as above, Me represents a methyl group, and n is a number that makes the viscosity of the organopolysiloxane the above value, and is preferably a number from 1 to 800, and more preferably a number from 50 to 600.
[0029] Such organopolysiloxanes can be produced by known methods. For example, the polysiloxane represented by the above formula (3) can be obtained by reacting 2-hydroxyethyl acrylate with the hydrosilylation reaction product of a dimethylsiloxane-diphenylsiloxane copolymer capped at both ends with dimethylvinylsiloxy groups and chlorodimethylsilane. The organopolysiloxane represented by the above formula (4) is obtained as the hydrosilylation reaction product of a dimethylsiloxane-diphenylsiloxane copolymer capped at both ends with dimethylvinylsiloxy groups and 3-(1,1,3,3-tetramethyldisiloxanyl)propyl methacrylate (CAS No. 96474-12-3). The organopolysiloxane represented by the above formula (5) can be obtained by reacting 2-hydroxyethyl acrylate with the hydrosilylation product of a dimethylsiloxane-diphenylsiloxane copolymer capped at both ends with dimethylvinylsiloxy groups and dichloromethylsilane.
[0030] (B) Monofunctional (meth)acrylate compound not containing a siloxane structure Specific examples of the monofunctional (meth)acrylate compound (B) not containing a siloxane structure include isoamyl acrylate, lauryl acrylate, stearyl acrylate, ethoxy-diethylene glycol acrylate, methoxy-triethylene glycol acrylate, 2-ethylhexyl-diglycol acrylate, phenoxyethyl acrylate, phenoxydiethylene glycol acrylate, tetrahydrofurfuryl acrylate, isobornyl acrylate, and the like, which may be used alone or in combination of two or more. Among these, isobornyl acrylate is particularly preferable.
[0031] In the present invention, the amount of the monofunctional (meth)acrylate compound of the component (B) is in the range of 1 to 200 parts by mass per 100 parts by mass of the component (A). If the amount of the component (B) is less than 1 part by mass per 100 parts by mass of the component (A), the curability of the composition and the strength and adhesion of the cured product are insufficient. On the other hand, the viscosity of the entire composition can be adjusted by increasing the amount of the component (B), but if the amount exceeds 200 parts by mass per 100 parts by mass of the component (A), the desired adhesion cannot be obtained. In particular, the amount of the component (B) added is preferably 5 to 100 parts by mass, and more preferably 10 to 60 parts by mass, per 100 parts by mass of the component (A).
[0032] (C) Organopolysiloxane resin The component (C) is one of the crosslinking components of the present composition, and is a unit represented by the following general formula (2) (M A units), (b) R 4 3SiO 1 / 2 Units (M units) and (c) SiO 4 / 2 It is an organopolysiloxane resin having a (meth)acryloyloxy-containing group consisting of units (Q units). 4 represents a monovalent hydrocarbon group having 1 to 10 carbon atoms.
[0033] [ka] (In the formula, R 1 , R 2 , R 3 , a and p have the same meanings as above.)
[0034] R 4 are each independently a monovalent hydrocarbon group having 1 to 10 carbon atoms. 4 Specific examples of the monovalent hydrocarbon group having 1 to 10 carbon atoms include the above R 1 Among the groups exemplified above, those having 1 to 10 carbon atoms can be mentioned, among which preferred are alkyl groups having 1 to 5 carbon atoms, such as methyl, ethyl, n-propyl and n-butyl groups; alkenyl groups, such as vinyl groups; and aryl groups having 6 to 10 carbon atoms, such as phenyl and tolyl groups, with methyl, ethyl, vinyl and phenyl groups being more preferred. In addition, the above R 4 The monovalent hydrocarbon radical R 1 Similarly, some or all of the hydrogen atoms bonded to the carbon atoms may be substituted with other substituents as described above.
[0035] In the component (C) of the present invention, (a) the unit represented by the above general formula (2) (M A units), (b) R 4 3SiO 1 / 2 Units (M units) and (c) SiO 4 / 2 The molar ratio of units (Q units) is M AUnit + M unit:Q unit = 0.4~1.2:1. A If the molar ratio of the units to the M units is less than 0.4, the viscosity of the composition becomes very high, whereas if it exceeds 1.2, the mechanical properties of the cured product decrease. In order to set the viscosity of the composition and the mechanical properties of the cured product in a more appropriate range, M A The molar ratio of M units to Q units is M A The ratio of M units to Q units is preferably 0.6 to 1.2:1, and more preferably 0.7 to 1:1.
[0036] Also, M A The rubber properties of the cured product can be adjusted by the molar ratio of M units to M units. A Unit: M unit = 0.01 to 1:1 is preferred, M A The ratio of unit:M unit is more preferably 0.05 to 0.5:1, and further preferably 0.05 to 0.3:1.
[0037] M A The content of the units is preferably 1 to 30 mol %, more preferably 3 to 10 mol %, based on the total siloxane units in the organopolysiloxane resin of component (C), in order to provide good mechanical properties for the cured product.
[0038] In addition, component (C) is R 1 SiO 3 / 2 (R 1 has the same meaning as above.) may be contained as a constituent unit, and in this case, R 1 SiO 3 / 2 Units and SiO 4 / 2 The total unit content is preferably 10 to 90 mol %, and more preferably 20 to 80 mol %, of all siloxane units in the organopolysiloxane resin of component (C).
[0039] The number average molecular weight of component (C) is preferably 500 to 30,000, more preferably 1,000 to 20,000, and even more preferably 1,000 to 10,000. Within such a range, the workability of the composition is improved. The number average molecular weight is a value calculated as a standard polystyrene by gel permeation chromatography (GPC).
[0040] Specific examples of the component (C) include those represented by the formula (2) above, 1 is a methyl group, R 2 is an ethylene group, R 3 is a methacryloyloxyalkyl group and p is 1, and 1 / 2 Units and Me3SiO 1 / 2 units and SiO2 units. In addition, Me represents a methyl group, and Vi represents a vinyl group.
[0041] The amount of organopolysiloxane resin (C) added is in the range of 1 to 1,000 parts by mass, preferably 5 to 500 parts by mass, more preferably 10 to 200 parts by mass, and even more preferably 20 to 150 parts by mass, per 100 parts by mass of component (A). If it is less than 1 part by mass, the rubber strength of the cured product will be low, and if it exceeds 1,000 parts by mass, the adhesive strength will decrease. The component (C) may be used alone or in combination of two or more types.
[0042] (D)Organic peroxide The organic peroxide is not particularly limited, but is preferably one having a one-hour decomposition half-life temperature (hereinafter also referred to as "T1") of 50 to 150°C. For example, any of those known to be used for thermal curing of acrylic functional groups can be used. Specific examples include cumyl peroxyneodecanoate (55.0), di-n-propyl peroxydicarbonate (57.7), diisopropyl peroxydicarbonate (56.2), di-sec-butyl peroxydicarbonate (57.4), 1,1,3,3-tetramethylbutyl peroxyneodecanoate (57.5), di(4-t-butylcyclohexyl) peroxydicarbonate (57.5), di(2-ethylhexyl) peroxydicarbonate (59.1), t-hexyl peroxyneodecanoate (62.8), t-butyl peroxyneodecanoate (64.8), t-butyl peroxyneoheptanoate (68.2), t-hexyl peroxypivalate (71.3), t-butyl peroxypivalate (72.7), di( 3,5,5-trimethylhexanoyl) peroxide (76.8), dilauroyl peroxide (79.5), 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (84.4), disuccinic acid peroxide (87.0), 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane (83.4), t-hexylperoxy-2-ethylhexanoate (90.1), di(4-methylbenzoyl) peroxide (89.3), t-butylperoxy-2-ethylhexanoate (92.1), di(3-methylbenzoyl) peroxide-benzoyl(3-methylbenzoyl) peroxide-dibenzoyl peroxide mixture (91.9), dibenzoyl peroxide (92.0), etc. Among these, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, cumyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-t-butylcyclohexyl)peroxydicarbonate, di(2-ethylhexyl)peroxydicarbonate, t-hexyl peroxyneodecanoate, and t-butyl peroxyneodecanoate are preferred, more preferably 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane and di(4-t-butylcyclohexyl)peroxydicarbonate, and even more preferably 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane. The T1 (unit: °C) of each compound is shown in parentheses following the compound name. Organic peroxides are commercially available, for example, from NOF Corp. Specific examples include Percumyl ND, Peroyl NPP, Peroyl IPP, Peroyl SBP, Perocta ND, Peroyl TCP, Peroyl OPP, Perhexyl ND, Perbutyl ND, and Perhexa 25O.
[0043] The one-hour half-life temperature (T1) of the organic peroxide is preferably from 50 to 150° C., more preferably from 55 to 100° C. Within such a range, the composition has excellent storage stability and good curability. The amount of organic peroxide is 0.01 to 5 parts by mass relative to 100 parts by mass of component (A), and from the viewpoint of the reactivity and curability desired in the present invention, it is preferably 0.1 to 3 parts by mass, and more preferably 1 to 3 parts by mass. If the amount is less than 0.01 parts by mass, the reaction does not proceed sufficiently. If it exceeds 5 parts by mass, the obtained cured product will lack transparency, adhesion, and durability at high temperatures. The component (D) may be used alone or in combination of two or more types.
[0044] (E) Silica Silica, component (E), is an optional component that mainly adjusts the viscosity of the composition, and examples include fumed silica (dry silica) and precipitated silica (wet silica), with fumed silica (dry silica) being preferred. In addition, the incorporation of component (E) further increases the hardness of the cured product, and also has the effect of suppressing displacement when parts, etc. are transferred. The specific surface area of the component (E) is not particularly limited, but is preferably 50 to 400 m 2 / g is preferable, and 100 to 350m 2 / g is more preferable. 2 If the viscosity is less than 400m / g, the thixotropy of the composition may be insufficient. 2 When the specific surface area exceeds 1 / g, the viscosity of the composition becomes excessively high, which may result in poor workability. The specific surface area is a value measured by the BET method. The silica of the component (E) may use either a single type alone, or a combination of two or more types.
[0045] These silicas may be used as they are, but may also be used after being treated with a surface hydrophobizing agent. In this case, silica that has been previously treated with a surface treatment agent may be used, or the surface treatment agent may be added during kneading of the silica, so that kneading and surface treatment may be carried out simultaneously. Examples of these surface treatment agents include alkylalkoxysilanes, alkylchlorosilanes, alkylsilazanes, and silane coupling agents. These may be used alone or in combination of two or more kinds, either simultaneously or at different times.
[0046] When the (E) component is used in the composition of the present invention, the amount added is preferably 1 to 200 parts by mass, more preferably 1 to 150 parts by mass, even more preferably 1 to 100 parts by mass, and still more preferably 1 to 10 parts by mass, per 100 parts by mass of the (A) component.
[0047] (F) Antistatic agent The antistatic agent of the component (F) is an optional component that serves to reduce the surface resistivity and impart antistatic properties to the material. Examples of the antistatic agent include salts of alkali metals or alkaline earth metals, ionic liquids, and the like. Here, the ionic liquid is a molten salt that is liquid at room temperature (25°C), also called a room temperature molten salt, and particularly refers to one having a melting point of 50°C or less. Preferably, it refers to one having a melting point of -100 to 30°C, more preferably -50 to 20°C. Such an ionic liquid has properties such as no vapor pressure (non-volatile), high heat resistance, non-flammability, and chemical stability.
[0048] Examples of the salts of alkali metals or alkaline earth metals include salts of alkali metals such as lithium, sodium, and potassium; salts of alkaline earth metals such as calcium and barium. Specific examples of these include alkali metal salts such as LiClO4, LiCF3SO3, LiN(CF3SO2)2, LiAsF6, LiCl, NaSCN, KSCN, NaCl, NaI, and KI; and alkaline earth metal salts such as Ca(ClO4)2 and Ba(ClO4)2. Among these, lithium salts such as LiClO4, LiCF3SO3, LiN(CF3SO2)2, LiAsF6, and LiCl are preferred from the viewpoints of low resistance and solubility, with LiCF3SO3 and LiN(CF3SO2)2 being particularly preferred.
[0049] Ionic liquids consist of a quaternary ammonium cation and an anion. The quaternary ammonium cation can be imidazolium, pyridinium or an anion of the formula: 6 4N + [In the formula, R 6 are each independently a hydrogen atom or an organic group having 1 to 20 carbon atoms.]
[0050] Above R 6Specific examples of the organic group represented by the formula include monovalent hydrocarbon groups having 1 to 20 carbon atoms, alkoxyalkyl groups, etc., and more specifically, alkyl groups such as methyl, pentyl, hexyl, and heptyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl and phenethyl groups; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cyclooctyl groups; and alkoxyalkyl groups such as ethoxyethyl groups (-CH2CH2OCH2CH3). 6 Two of the organic groups represented by the formula (I) may be bonded to form a ring structure, in which case the two R 6 are combined to form a divalent organic group. The main chain of this divalent organic group may be composed of only carbon, or may contain heteroatoms such as oxygen atoms and nitrogen atoms. Specifically, for example, a divalent hydrocarbon group [for example, an alkylene group having 3 to 10 carbon atoms], the formula: -(CH2) c -O-(CH2) d -[wherein c is an integer of 1 to 5, d is an integer of 1 to 5, and c+d is an integer of 4 to 10].
[0051] Above R 6 4N + Specific examples of the cation represented by the formula (I) include a methyltri-n-octylammonium cation, an ethoxyethylmethylpyrrolidinium cation, and an ethoxyethylmethylmorpholinium cation.
[0052] The anion is not particularly limited, but for example, AlCl4 - , AlCl 10 - , Al2Cl7 - , ClO4 - , PF6 - , BF4 - , CF3SO3 - , (CF3SO2)2N - , (CF3SO2)3C - is preferred, PF6 - , BF4 - , CF3SO3 - , (CF3SO2)2N -is more preferred.
[0053] The antistatic agents may be used alone or in combination of two or more. When the component (F) is used, its amount is preferably 0.001 to 10 parts by mass, and more preferably 0.005 to 10 parts by mass, per 100 parts by mass of the component (A) from the viewpoints of antistatic properties and heat resistance.
[0054] The antistatic performance of the cured product obtained from the thermosetting silicone pressure-sensitive adhesive composition of the present invention is preferably such that, after charging the surface of the cured product with 6 kV of static electricity by corona discharge using a Static Honest Meter (manufactured by Shishido Electrostatic Corporation), the time it takes for the charged voltage to be reduced to half (half-life) is within 2 minutes, and more preferably within 1 minute.
[0055] As mentioned above, the composition of the present invention does not contain a non-crosslinked organopolysiloxane resin. As such an organopolysiloxane resin, (d) R 4 3SiO 1 / 2 Units (R 4 has the same meaning as above.) and (e) SiO 4 / 2 units, and the molar ratio of (d) units to (e) units is in the range of 0.4 to 1.2:1.
[0056] In addition, the composition of the present invention may contain additives such as coloring materials (pigments or dyes), silane coupling agents, adhesion aids, polymerization inhibitors, antioxidants, and light stabilizers, as long as the effects of the present invention are not impaired. Furthermore, the composition of the present invention can also be used by appropriately mixing it with other resin compositions.
[0057] The thermosetting silicone pressure-sensitive adhesive composition of the present invention can be obtained by mixing the above components (A) to (D), and, if necessary, the components (E) and (F) and other components, in any order, followed by stirring, etc. There are no particular limitations on the equipment used for operations such as stirring, but examples of equipment that can be used include a crusher, a three-roll mill, a ball mill, a planetary mixer, etc. These equipment can also be combined as appropriate.
[0058] From the viewpoint of moldability and workability during application, the viscosity of the thermosetting silicone pressure-sensitive adhesive composition of the present invention, measured at 23°C using a rotational viscometer, is preferably 10,000 mPa·s or less, more preferably 5,000 mPa·s or less, even more preferably 4,000 mPa·s or less, and even more preferably 3,500 mPa·s or less. If it exceeds 10,000 mPa·s, workability may be significantly impaired. There is no particular lower limit, but it is preferably 100 mPa·s or more, and more preferably 500 mPa·s or more.
[0059] The thermosetting silicone pressure-sensitive adhesive composition of the present invention cures quickly when heated. The curing conditions are not particularly limited and can be the same as those for known curable silicone compositions. Curing at room temperature or by heating can be performed at a temperature of preferably 20 to 180°C, more preferably 50 to 150°C, for preferably 0.1 to 3 hours, more preferably 0.5 to 2 hours.
[0060] Furthermore, the thermosetting silicone pressure-sensitive adhesive composition of the present invention can be used as a pressure-sensitive adhesive article by applying it to various substrates and curing it by heating. Examples of the substrate include plastic films, glass, metals, etc., and they can be used without any particular limitation. Examples of plastic films include polyethylene films, polypropylene films, polyester films, polyimide films, polyvinyl chloride films, polyvinylidene chloride films, polyvinyl alcohol films, polycarbonate films, polystyrene films, ethylene-vinyl acetate copolymer films, ethylene-vinyl alcohol copolymer films, and triacetyl cellulose films. There are no particular limitations on the thickness or type of glass, and glass that has been subjected to chemical strengthening treatment may also be used. In order to improve the adhesion between the substrate and the pressure-sensitive adhesive layer, the substrate may be previously subjected to a primer treatment, a plasma treatment, or the like.
[0061] The coating method can be appropriately selected from known coating methods such as a method using a spin coater, comma coater, lip coater, roll coater, die coater, knife coater, blade coater, rod coater, kiss coater, gravure coater, etc., screen coating, dip coating, cast coating, etc.
[0062] Since the thermosetting silicone pressure-sensitive adhesive composition of the present invention is a solvent-free composition, potting using a mold is also possible as a method for producing a cured product. Air bubbles may be entrained when pouring into the mold during potting, but these can be degassed by reducing the pressure. As the mold, for example, a resist mold in which desired projections and recesses are formed on a silicon wafer using a photoresist can be used. If it is desired to remove the cured product from the mold after curing, it is preferable to treat the container with a mold release agent before pouring the composition in. As the mold release agent, fluorine-based, silicone-based, etc. can be used.
[0063] The thermosetting silicone pressure-sensitive adhesive composition of the present invention is usually used as is, but when improvements in handleability or coatability onto substrates are required, it is also acceptable to dilute the composition with an organic solvent prior to use as long as the properties of the present invention are not impaired.
[0064] In order to prevent cohesive failure during molding or when used as a microtransfer printing material to transfer fine components such as elements, the cured product of the thermosetting silicone pressure-sensitive adhesive composition of the present invention preferably has a tensile strength (JIS-K6249:2003) at a thickness of 2.0 mm of 1 MPa or more, and more preferably 2 MPa or more.
[0065] Next, one embodiment of the microstructure transfer stamp according to the present invention will be described with reference to the drawings. As shown in Figures 1 and 2, the cured product of the heat-curable silicone pressure-sensitive adhesive composition of the present invention can be used as microstructure transfer stamps 100 and 101 for transferring minute elements, parts, etc.
[0066] In Fig. 1, the stamp 100 for transferring a microstructure is configured to have a cured layer 300 of the thermosetting silicone pressure-sensitive adhesive composition of the present invention on a substrate 200. In this case, the size of the cured layer 300 may be exactly the same size as the substrate 200 as long as it fits within the substrate 200. The size of the substrate is not particularly limited and can be appropriately selected from the range known in the art. The material of the substrate 200 is not particularly limited, and specific examples thereof include plastic film, glass, synthetic quartz, metal, etc. There are also no particular limitations on the thickness or type, and the substrate may be one that has been subjected to chemical strengthening treatment, etc. In order to improve the adhesion between the substrate and the adhesive layer, the substrate may be one that has been previously subjected to primer treatment, plasma treatment, etc. In order to suppress positional deviation during the transfer of the microstructure and to increase the transfer accuracy, it is preferable to use synthetic quartz with high flatness.
[0067] The method for producing the cured product 300 on the substrate 200 is not particularly limited, and may be, for example, any of a method in which an uncured thermosetting silicone pressure-sensitive adhesive composition is directly applied to the substrate 200 and cured, a method in which a sheet-shaped cured product of the thermosetting silicone pressure-sensitive adhesive composition is attached to the substrate 200, and the like. In the method of directly applying and curing a thermosetting silicone adhesive composition onto the substrate 200, the silicone adhesive composition is applied onto the substrate 200, and then cured by heat to obtain a stamp 100 for transferring microstructures. The coating method can be appropriately selected from known coating methods such as a method using a spin coater, comma coater, lip coater, roll coater, die coater, knife coater, blade coater, rod coater, kiss coater, gravure coater, etc., screen coating, dip coating, cast coating, etc. In addition, after applying the silicone adhesive composition to a substrate by these methods, it is possible to obtain a stamp 100 for transferring a microstructure with high flatness by curing the composition by heating while performing press molding, compression molding, or the like.
[0068] In the method of laminating a sheet-like cured product of a thermosetting silicone adhesive composition onto a substrate 200, the material can be molded into a sheet and then laminated onto the substrate 200 to obtain a stamp 100 for transferring a microstructure.
[0069] The method for forming the thermosetting silicone pressure-sensitive adhesive composition into a sheet can be appropriately selected from, for example, roll molding, press molding, transfer molding, compression molding, and other molding methods. The sheet-shaped cured product is preferably molded by sandwiching it between plastic films to prevent adhesion of dust and the like and suppress oxygen inhibition during curing. In addition, if the obtained sheet-shaped cured product is larger than desired, it can be cut to the desired size. In order to increase the adhesion between the sheet-like cured product and the substrate 200, either or both of the bonding surfaces may be subjected to plasma treatment, excimer treatment, chemical treatment, etc. Furthermore, in order to improve the bonding strength, a pressure-sensitive adhesive, a bonding agent, etc. may be used. As the pressure-sensitive adhesive, a silicone-based, acrylic-based, epoxy-based, etc., pressure-sensitive adhesive may be used. The lamination may be performed by roll lamination, vacuum pressing, or the like.
[0070] The thickness of the silicone adhesive cured material layer 300 in the microstructure transferring stamp 100 is preferably from 1 μm to 1 cm, and more preferably from 10 μm to 5 mm, from the viewpoints of moldability and flatness.
[0071] 2, the stamp 101 for transferring a microstructure is configured to have a cured layer 310 of the thermosetting silicone pressure-sensitive adhesive composition of the present invention on a substrate 201. The substrate 201 may be the same as the substrate 200. The cured silicone pressure-sensitive adhesive layer 310 has a convex structure 311 on its surface. A base layer 312 may be provided below the convex structure 311. There is no particular limitation on the method for producing the cured material layer 310 on the substrate 201, and examples thereof include a method of directly molding the cured material layer 310 on the substrate 201 by molding or the like, and a method of laminating a sheet-shaped cured material having a convex structure 311 onto the substrate 201.
[0072] In a method of directly forming a silicone adhesive cured layer 310 on a substrate 201 by molding, for example, as shown in Figure 3, the silicone adhesive composition of the present invention is filled between the substrate 201 and a mold 401, cured by heating and irradiating, and then the mold 401 is demolded to obtain a stamp 101 for transferring microstructures. As the mold 401, for example, a resist mold in which a desired unevenness is formed on a silicon wafer or a quartz substrate using a photoresist, a resin mold in which unevenness is formed by pattern exposure of a thermosetting resin, etc. can be used. In the case of a resin mold, various plastic films can be used as the base material. A method of filling the gap between the substrate 201 and the mold 401 with the silicone adhesive composition includes a method of applying the silicone adhesive composition to either or both of the substrate 201 and the mold 401 and then laminating them together. The above-mentioned methods can be used for the application method and lamination method. There is a possibility that minute air bubbles will remain in the mold 401 during application, but this can be solved by vacuum lamination or degassing by reducing pressure. By applying the silicone adhesive composition to a substrate by these methods, the composition is cured by heating while being subjected to press molding, compression molding, roll press molding, or the like, thereby obtaining the stamp 101 for transferring a minute structure.
[0073] Alternatively, the silicone adhesive composition may be screen-printed using a mesh having a desired pattern, and then cured by heating to obtain the stamp for transferring a microstructure 101. In this case, since the silicone adhesive composition of the present invention has excellent shape retention, the desired pattern shape is not damaged from application to curing.
[0074] In the method of laminating a silicone adhesive sheet-like cured product having a convex structure 311 onto a substrate 201, a silicone adhesive composition is molded into a sheet-like cured product having a convex structure 311, and then laminated to the substrate 201 to obtain a stamp 101 for transferring a microstructure. The method for molding the thermosetting silicone pressure-sensitive adhesive composition into a sheet-like cured product having convex structure 311 can be appropriately selected from molding methods such as roll molding, press molding, transfer molding, and compression molding using a mold having convexities and recesses similar to mold 401. The sheet-shaped cured product is preferably molded by sandwiching it between plastic films or the like in order to prevent adhesion of dust and the like and to suppress oxygen inhibition during curing. If the obtained sheet-shaped cured product is larger than desired, it can be cut to the desired size. Furthermore, in order to increase the adhesion between the sheet-like cured product and the substrate 201, the bonding surfaces thereof may be subjected to plasma treatment, excimer treatment, chemical treatment, etc. Also, in order to increase the bonding strength, the above-mentioned various pressure-sensitive adhesives, adhesives, etc. may be used. The lamination may be performed by roll lamination, vacuum pressing, or the like.
[0075] The size and arrangement of the convex structures 311 can be designed according to the size and desired arrangement of the minute structures to be transferred. The upper surface of the convex structure 311 is flat, and the surface shape is not limited, and examples thereof include a circle, an ellipse, a rectangle, etc. In the case of a rectangle, etc., there is no problem even if the edges are rounded. The width of the upper surface of the convex structure 311 is preferably 0.1 μm to 1 cm, and more preferably 1 μm to 1 mm. Furthermore, there is no limitation on the shape of the side surface of the convex structure 311, and it may be a vertical surface, an inclined surface, or the like. The height of the convex structure 311 is preferably 0.1 μm to 1 cm, and more preferably 1 μm to 1 mm. The pitch distance between adjacent convex structures 311 separated by a space is preferably 0.1 μm to 10 cm, more preferably 0.1 μm to 1 cm, and further preferably 1 μm to 1 mm. The thickness of the base layer 312 is preferably 0.1 μm to 1 cm, and more preferably 1 μm to 5 mm.
[0076] The above-mentioned stamp for transferring a microstructure can be attached to an apparatus and used as a microstructure transferring apparatus. There is no limitation on the method of attachment to the apparatus, but examples include a vacuum chuck, an adhesive sheet, etc. The microstructure transferring apparatus can achieve the transfer of a microstructure by picking up a microstructure such as an element by the adhesiveness of the stamp for transferring a microstructure, moving it to a desired position, and then releasing it.
[0077] As a specific example of the transfer of a microstructure, the microstructure transfer stamp 100 or 101 of the present invention can be used as a holding substrate (donor substrate) for temporarily fixing a peeled semiconductor element so as not to cause displacement during a laser lift off (LLO) process in which a sapphire substrate of a semiconductor element is peeled off from a GaN-based compound crystal layer using laser light. In this case, it is preferable to use synthetic quartz with high flatness as the base material 200 and 201. Furthermore, in order to selectively pick up the semiconductor element temporarily fixed on the holding substrate, a microstructure transfer stamp 100 or 101 having a stronger adhesive force than the holding substrate can be used. The picked-up semiconductor element is then moved to a desired position on the mounting substrate, soldering is performed to bond the semiconductor element to the mounting substrate, and the microstructure transfer stamp is peeled off from the semiconductor element, thereby achieving transfer of the semiconductor element and mounting on the substrate.
[0078] Considering the balance between the releasability and holding property of the transferred object, the adhesive strength of the cured material layer 300, 310 on the holding substrate (donor substrate) is preferably 0.001 to 2 MPa, more preferably 0.002 to 1 MPa. The adhesive strength of the cured material layer 300, 310 on the microstructure transfer stamp for element pickup is preferably greater than that of the holding substrate, preferably 0.01 MPa or more, more preferably 0.1 MPa or more. The method for measuring the adhesive strength is as described in the Examples. EXAMPLES
[0079] The present invention will be described more specifically below with reference to examples and comparative examples, but the present invention is not limited to these examples. The compounds of the components used in the examples are as follows. In the formulae below, Me represents a methyl group, Ph represents a phenyl group, and Vi represents a vinyl group. The viscosities of components (G) and (H) were measured using a rotational viscometer.
[0080] Component (A) [ka] (In the formula, the siloxane units in the parentheses may be arranged in any order.)
[0081] (B) Component (B-1) Isobornyl acrylate (Light Acrylate IB-XA, manufactured by Kyoeisha Chemical Co., Ltd.)
[0082] (C) Component (C-1) A methacryloyloxy group-containing unit represented by the following formula (6), ViMe2SiO 1 / 2 Units, Me3SiO 1 / 2 units and SiO2 units, and 1 / 2 Unit) / (Me3SiO 1 / 2 A 50% by mass xylene solution of organopolysiloxane resin (number average molecular weight 5,700) with a molar ratio of (SiO2 unit) / (SiO2 unit) of 0.07 / 0.10 / 0.67 / 1.00 (C-2) A methacryloyloxy group-containing unit represented by the following formula (6), ViMe2SiO 1 / 2 Units, Me3SiO 1 / 2 units and SiO2 units, and 1 / 2 Unit) / (Me3SiO 1 / 2 A 50% by mass xylene solution of organopolysiloxane resin (number average molecular weight 6,000) with a molar ratio of (SiO2 unit) / (SiO2 unit) of 0.11 / 0.06 / 0.67 / 1.00
[0083] [ka]
[0084] (D) Component (D-1) Hydrocarbon solution containing 50% by mass of 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane (1-hour half-life temperature in benzene: 83.4°C) (NOF Corporation, Perhexa 25O) (E) Component (E-1) Dry silica (Reoloseal DM-30S, manufactured by Tokuyama Corporation, specific surface area 230 m 2 / g) Ingredient (F) (F-1) Adipic acid ester containing 20% by mass of LiN(SO2CF3)2
[0085] Comparative ingredients (G) Component (G-1)(ViMe2SiO 1 / 2 )2(Me2SiO2 / 2 ) 300 Organopolysiloxane with a viscosity of 1 Pa·s at 25°C. (H) Component (H-1)(MeSiO 1 / 2 )2(Me2SiO 2 / 2 ) 17 (MeHSiO 2 / 2 ) 45 Organohydrogenpolysiloxane with a viscosity of 50 mPa·s at 25°C. Component (I) (I-1) A toluene solution of Karstedt catalyst (platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex) with a platinum content of 0.5% by mass. (J) Component (J-1) 3-mercaptopropyltrimethoxysilane, which acts as a platinum group metal catalyst poison (K) Component (K-1) Ethynylmethyldecylcarbinol having the effect of an addition reaction inhibitor
[0086] [Examples 1 to 8 and Comparative Examples 1 and 2] The above components (A) and (C) were mixed in the ratio shown in Table 1, and the xylene was distilled off at 100°C under reduced pressure. The above components (B) and (D), and optionally components (E) and (F) and other components were then blended and mixed to prepare each of the silicone compositions shown in Table 1. The viscosity of the compositions in Table 1 was measured at 23°C using a rotational viscometer. The prepared silicone composition was press-cured at 120° C. for 30 minutes and then heated in an oven at 120° C. for 30 minutes. The sheet had a thickness of 2.0 mm. The hardness and tensile strength of the cured product were measured in accordance with JIS-K6249:2003. The adhesive strength of the cured product was measured using a small tabletop tester EZ-SX manufactured by Shimadzu Corporation. Specifically, a 1 mm square SUS probe was pressed against a 1 mm thick cured product at 1 MPa for 15 seconds, and then pulled at a speed of 200 mm / min, measuring the load applied. The antistatic properties of the cured product were evaluated by charging the surface of a 2 mm thick cured product sheet with 6 kV of static electricity by corona discharge using a Static Honest Meter (manufactured by Shishido Electrostatic Corporation), and then measuring the time it took for the charged voltage to decrease by half (half-life).
[0087] [Table 1]
[0088] As shown in Table 1, the thermosetting silicone pressure-sensitive adhesive compositions prepared in Examples 1 to 8 have appropriate viscosities. The cured products have excellent adhesion and tensile strength, and are useful as temporary fixing materials for transporting fine parts such as elements. Example 7 also has excellent antistatic properties due to the inclusion of component (F-1). On the other hand, in Comparative Example 1, in which the amount of component (C-1) was too much and outside the range of the present invention, the composition solidified and became difficult to handle. Also, in Comparative Example 2, in which curing proceeds by an addition reaction, curing is inhibited by component (J-1), which acts as a catalyst poison, and the composition does not cure, making it unsuitable as a temporary fixing material. As described above, the thermosetting silicone pressure-sensitive adhesive compositions of Examples 1 to 8 can be easily cured by heating, and are not subject to curing inhibition, making it possible to prepare temporary fixing materials for any substrate, and therefore highly useful in many technical fields. The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0089] 100,101 Stamp for transferring microstructures 200,201 Base material 300,310 Cured material layer 311 Convex structure 312 Base Layer Type 401
Claims
1. (A) a compound represented by the following general formula (1): 【Chemistry 1】 (In the formula, R 1 each independently represents a monovalent hydrocarbon group having 1 to 20 carbon atoms; R 2 represents an oxygen atom or an alkylene group having 1 to 20 carbon atoms; R 3 each independently represents an acryloyloxyalkyl group, a methacryloyloxyalkyl group, an acryloyloxyalkyloxy group, or a methacryloyloxyalkyloxy group; p represents a number satisfying 0≦p≦10; and a represents a number satisfying 1≦a≦3. The wavy lines represent bonds.) In one molecule, there is provided an organopolysiloxane having two groups represented by the formula: (B) a monofunctional (meth)acrylate compound not containing a siloxane structure: 1 to 200 parts by mass, (C) (a) a compound represented by the following general formula (2): 【Chemistry 2】 (In the formula, R 1 , R 2 , R 3 , a and p have the same meanings as above. (b) a unit represented by R 4 3 SiO 1 / 2 Units (wherein R 4 represents a monovalent hydrocarbon group having 1 to 10 carbon atoms; and (c) SiO 4 / 2 units, in which the molar ratio of the sum of the (a) units and the (b) units to the (c) units is in the range of 0.4 to 1.2:1:
1. (D) Organic peroxide: 0.01 to 5 parts by mass and is free of a non-crosslinkable organopolysiloxane resin.
2. 2. The thermosetting silicone pressure-sensitive adhesive composition according to claim 1, which comprises (E) silica in an amount of 1 to 200 parts by mass per 100 parts by mass of component (A).
3. 2. The thermosetting silicone pressure-sensitive adhesive composition according to claim 1, further comprising, for each 100 parts by mass of component (A), 0.001 to 10 parts by mass of an antistatic agent (F).
4. A cured product of the heat-curable silicone pressure-sensitive adhesive composition according to any one of claims 1 to 3.
5. The cured product according to claim 4, which has a tensile strength (JIS-K6249) of 1 MPa or more at a thickness of 2.0 mm.
6. A pressure-sensitive adhesive comprising the cured product according to claim 4.
7. A pressure-sensitive adhesive sheet comprising the cured product according to claim 4.
8. A stamp for transferring a microstructure, comprising the cured product according to claim 4.
9. The stamp for transferring a microstructure according to claim 8, which has at least one convex structure.
10. A microstructure transferring apparatus comprising the microstructure transferring stamp according to claim 8.
11. A microstructure transferring apparatus comprising the microstructure transferring stamp according to claim 9.
12. A microstructure-holding substrate having an adhesive layer made of the cured product according to claim 4.
13. A microstructure transferring device comprising the microstructure holding substrate according to claim 12.
Citation Information
Patent Citations
Addition curable silicone adhesive composition and cured product of the same
JP2021123620A
UV-curable silicone adhesive composition and cured product thereof
JP7131631B2
UV-curable silicone adhesive composition and cured product thereof
JP7156392B2