New method for producing PBI films without organic solvents
The PPA process for PBI films, which involves neutralizing gel PBI films in water baths and controlled drying, addresses the limitations of organic solvent-based methods by reducing costs and environmental impact while enhancing film properties for diverse applications.
Patent Information
- Application Number
- JP2024119265
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-09-13
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-09-13
AI Technical Summary
Existing methods for producing Polybenzimidazole (PBI) films require the use of organic solvents, which are costly, time-consuming, and environmentally unfriendly, limiting the range of monomers that can be incorporated and posing health risks to workers.
A novel method involving the PPA process where gel PBI films are neutralized in water baths and subjected to controlled drying, eliminating the need for organic solvents and allowing a wider range of monomers to be used, resulting in PBI films that are cheaper, faster, and generate less chemical waste.
The solvent-free process reduces production costs, time, and environmental impact while enabling the production of PBI films with improved properties, such as high thermal stability and chemical resistance, suitable for applications like redox flow batteries and aerospace coatings.
Smart Images

Figure 2024164016000019 
Figure 2024164016000020 
Figure 2024164016000021
Abstract
Description
[Technical field]
[0001] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH This invention was made with Government support under DE-AR0000767 awarded by the Department of Energy. The Government has certain rights in this invention.
[0002] 1) Field of the invention The present invention relates to a novel method for producing PBI films starting from a gel PBI membrane polymerized and cast in a PPA process, in which the acid-absorbed gel PBI is neutralized in a series of water baths and, optionally together with a substrate or porous material, undergoes controlled drying to obtain a PBI film without the use of organic solvents. [Background technology]
[0003] 2) Description of related technologies Polybenzimidazole (PBI) is a glassy thermoplastic with particularly good thermal stability (Tg of 427°C), broad chemical resistance, and the ability to function as a proton acceptor or donor. PBI has unique properties that make it suitable for transporting protons, hydrogen, and water. For these reasons, PBI is well suited for H2 / CO2 separation membranes, fuel cell proton exchange membranes, and pervaporation dehydration membranes for organic chemicals, which are often used at high temperatures.
[0004] A novel synthesis process for producing high molecular weight PBI, the "PPA process", was developed at Rensselaer Polytechnic Institute in collaboration with BASF Fuel Cell GmbH. The general synthesis of PBI by this method requires the combination of tetraamines and dicarboxylic acids in polyphosphoric acid (PPA) in a dry environment. Stepwise polycondensation reactions are typically carried out at about 200 °C for 16-24 h in a nitrogen atmosphere to produce a polymer with high molecular weight. The solution is cast directly from the PPA as a thin film on the substrate, and upon absorption of water, the PPA hydrolyzes in situ to form phosphoric acid. It is noted that for PBI, PPA is a good solvent, whereas PA is a poor solvent. Under controlled hydrolysis conditions, mechanically stable PBI gel membranes highly doped with phosphoric acid are produced.
[0005] In one commercial application, PA-doped m-PBI fuel cell membranes have been produced that maintain thermal and physical stability during high temperature operation. The PPA process produces membranes with much higher proton diffusion coefficients and electrical conductivity, and creates membranes with better proton transport structure than conventionally imbibed PBI membranes. In addition, intrinsic viscosity data shows that the PPA process produces polymers with much higher molecular weights. The improved membrane morphology and increased molecular weight show that the polymers are capable of retaining much more phosphoric acid than conventional cast PBI membranes. Increasing the PA doping level typically improves the membrane conductivity and may also enhance cell performance.
[0006] PBI films are known to have very good properties such as high temperature stability, non-flammability, and high chemical resistance. So far, the method for producing PBI films has involved polymerization, dissolving the resulting polymer in an organic solvent such as dimethylacetamide (DMAc), casting the film, and removing the solvent by a series of washes. Summary of the Invention [Problem to be solved by the invention]
[0007] Therefore, the objective of the present disclosure is to provide a new and improved method for producing PBI films starting from a gel PBI membrane polymerized and cast in a PPA process. As described below in this disclosure, the acid-imbibed gel PBI can be neutralized in a series of water baths, subjected to controlled drying, and applied between two porous materials or onto a suitable substrate as desired to obtain a PBI film without the use or utilization of organic solvents. In addition, the PBI gel synthesized in the PPA process allows the use of a wider range of monomers due to their low solubility in organic solvents. Thus, the present invention provides for the first time access to a wider range of PBI chemicals that can be processed into films. [Means for solving the problem]
[0008] The above object is achieved according to the present disclosure by providing, in one embodiment, a method for manufacturing a PBI film. The method may include forming a gel PBI film via a PPA process, rinsing the gel PBI film, constraining the gel PBI film in at least the XY plane direction, and drying the rinsed gel PBI film, where no organic solvent is used throughout the method. Furthermore, the gel PBI film may be rinsed with a cleaning solution. Still further, the rinsed gel PBI film may be applied to at least one substrate. Still further, the rinsed gel PBI film may be applied to a porous substrate. Still further, the constraining of the PBI film may apply tension to the PBI film in the X, Y, or Z plane direction. Still further, the PBI film may be formed via a continuous forming process. Still further, the polybenzimidazole of the PBI film may be formed from the following repeating units: [ka] [ka] or any combination thereof, wherein n and m are , each independently being 1 or greater, about 10 or greater, or about 100 or greater. Still further, the method can form a film.
[0009] In a further embodiment, a PBI film is formed. The film may include forming a gel PBI film via a PPA process, rinsing the gel PBI film, constraining the gel PBI film in at least the XY plane direction, and drying the rinsed gel PBI film to form a PBI film, where no organic solvent is used throughout the process to form the film. Still further, the film may be used as a coating. Still further, the film may have a thickness of 5 to 150 μm. Still further, the film has a breaking stress of at least 25 MPa. Still further, the polybenzimidazole of the PBI film may have the following repeating units: [ka] [ka] or any combination thereof, wherein n and and m are each independently 1 or greater, about 10 or greater, or about 100 or greater. Still further, the film may comprise a PBI polymer that is substantially insoluble in organic solvents. Still further, the film may absorb an organic or inorganic acid or base to form an ionically conductive membrane.
[0010] Structures designed to carry out the invention will now be described, together with other features of the invention, which will become more readily understood by reading the following specification and by referring to the accompanying drawings, which form a part hereof, and in which examples of the invention are shown. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 shows a graph of the cell cycling current for the membranes of the present disclosure. [Diagram 2] FIG. 2 shows a further graph of cell cycling current for membranes of the present disclosure. [Diagram 3] FIG. 3 shows the VRFB Oxidative Stability Test for the membrane of the present disclosure. [Figure 4] FIG. 4 shows the polymerization scheme of s-PBI in PPA and the cross-linking modification reaction of the membrane. [Diagram 5] FIG. 5 shows Table 1 - ex-situ properties of s-PBI gel films compared to dense m-PBI films. [Figure 6] FIG. 6 shows the performance of the membranes of the present disclosure compared to commercially available membranes. [Figure 7] FIG. 7 shows a graph of the measured out-of-situ properties of a membrane of the present disclosure compared to a typical PBI gel membrane. [Figure 8] FIG. 8 shows a complete ex situ measurement of the membrane of the present disclosure. [Figure 9] FIG. 9 shows the transmittance compared to the conductivity for para-PBI. [Figure 10] FIG. 10 shows the transmittance compared to the conductivity in Mrp PBI. [Figure 11] FIG. 11 shows cell test results for membranes formed according to the present disclosure. [Figure 12] FIG. 12 shows the voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) for 1.7× stretched para-PBI. [Figure 13] FIG. 13 shows the voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) for 1.5× stretched para-PBI. [Figure 14] FIG. 14 shows the voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) for dry para-PBI. [Figure 15]FIG. 15 shows the voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) for stretched s-PBI. [Figure 16] FIG. 16 shows the voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) for dry s-PBI. [Figure 17] FIG. 17 shows the voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) for VRB test cells of conventionally imbibed dense m-PBI Comparative Example 1. [Figure 18] FIG. 18 shows the mechanical properties of para-PBI films formed via the PPA process and processed via the methods of the present disclosure. [Figure 19] FIG. 19 shows the mechanical properties of Di-OH-PBI films formed in accordance with the present disclosure. [Figure 20] FIG. 20 shows the mechanical properties of s-PBI copolymer films formed in accordance with the present disclosure. [Figure 21] FIG. 21 shows the mechanical properties of meta / para-PBI copolymer films formed in accordance with the present disclosure. [Figure 22] FIG. 22 shows a comparative example using m-PBI cast from an organic solution. [Figure 23] FIG. 23 illustrates a continuous PBI film formation process that can be used in the present disclosure. [Figure 24] FIG. 24 shows that the membranes produced by the methods disclosed herein exhibited lower creep resistance than the standard PPA process membranes. [Diagram 25] FIG. 25 shows the polarization curves in H2 / air. [Figure 26] FIG. 26 shows the polarization curves in H2 / O2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Those skilled in the art will appreciate that certain objectives may be met by one or more aspects of the present invention, while certain other objectives may be met by one or more other aspects. Each objective may not be equally applicable in all respects to all aspects of the present invention. Thus, the aforementioned objectives may be viewed as alternatives with respect to any one aspect of the present invention. These and other objects and features of the present invention will become more fully apparent from the following detailed description taken in conjunction with the accompanying drawings and examples. However, it should be understood that the foregoing summary of the present invention and the following detailed description are of preferred embodiments and are not intended to limit the present invention or other alternative embodiments of the present invention. In particular, while the present invention is described herein with reference to certain specific embodiments, it is understood that the descriptions are illustrative of the present invention and are not to be construed as limiting the present invention. Those skilled in the art will appreciate various modifications and applications without departing from the spirit and scope of the present invention as set forth in the appended claims. Similarly, other objects, features, benefits, and advantages of the present invention will become apparent from this summary and certain embodiments described below, and will be readily apparent to those skilled in the art. Such objects, features, benefits, and advantages will become apparent from the above, taken in conjunction with the accompanying examples, data, drawings, and all reasonable inferences to be derived therefrom, either alone or together with a consideration of the references incorporated herein.
[0013] The present invention will be described in more detail below with reference to the drawings.Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the subject matter disclosed herein belongs.Although any methods, devices, and materials similar or equivalent to those described herein may be used in the practice or testing of the subject matter disclosed herein, representative methods, devices, and materials are described herein.
[0014] Unless otherwise noted, terms and phrases used in this document, and variations thereof, should be construed in an open rather than limiting sense unless expressly stated otherwise. Similarly, a group of items joined by the conjunction "and" should not be construed as requiring that each and every one of those items be present in the group, but rather as "and / or," unless expressly stated otherwise. Similarly, a group of items joined by the conjunction "or" should not be construed as requiring mutual exclusivity among the group, but rather as "and / or," unless expressly stated otherwise.
[0015] Additionally, although items, elements, or components of the disclosure may be described or claimed in the singular, the plural is also contemplated within the scope of the disclosure unless limitation to the singular is expressly stated. The presence in some cases of broadening words and phrases, such as "one or more," "at least," "including but not limited to," or other similar phrases, should not be construed as implying that a narrower case is intended or required in cases where such broadening phrases may not be present.
[0016] This invention details a novel method for producing PBI films without the use of organic solvents. Eliminating the need for organic solvents provides a new route to produce PBI films that is cheaper, takes less time, significantly reduces worker exposure, and generates less chemical waste than previous methods. This novel solvent-free process is scalable and easy to use. This allows for a wider range of PBI chemistries to be made into the films, as the use of organic solvents previously limited the chemistries that could be incorporated into the PBI membrane.
[0017] Provided herein are methods and processes for obtaining chemically resistant and thermally stable PBI films that are synthesized for the first time without the use of organic solvents. Previously, the synthesis of PBI films was an expensive and time-consuming process involving harsh chemicals. The present disclosure provides a method that does not require the use of organic solvents, thereby making the method "greener" and more environmentally friendly. The method is also considered safer, as it reduces worker exposure to organic solvents. By overcoming the need for organic solvents, the method of producing PBI films becomes cheaper and takes less time.
[0018] PBI films produced without organic solvents reduce the associated solvent purchasing costs and eliminate the expensive and time-consuming disposal of hazardous waste generated from the use of organic solvents. The disclosed method for obtaining PBI films is simpler and offers a wider range of PBI chemicals than previously available. Importantly, commercial applications of the disclosure include, but are not limited to, aerospace coatings, wire coatings, microelectronic packaging, protective windows and glass coatings, gas separation membranes, high temperature materials / films, high chemical resistance films, and ion exchange membranes.
[0019] In one embodiment of the present disclosure, sulfonated polybenzimidazole (s-PBI) gel membranes were fabricated and shown to have high stability in concentrated sulfuric acid and strong oxidative vanadium (V) solutions. These membranes were considered candidates for use in vanadium redox flow batteries and compared to the commonly used "conventionally imbibed" meta-polybenzimidazole (m-PBI) membranes cast from N,N'-dimethylacetamide (DMAc) solutions. The s-PBI membranes exhibited high conductivity and low performance degradation in in-cell tests.
[0020] Redox flow batteries are used to convert electrical energy into chemical energy, which can then be converted back into electrical energy as needed. These devices can store grid-scale amounts of energy. However, currently, the high cost of device manufacturing limits the widespread adoption of flow batteries. However, this cost can be mitigated by reducing the size of the electrochemical stack. To effectively achieve this and maintain high power density, the battery must be capable of operating under high current loads. Conventional membranes used in flow batteries are poor ionic conductors and cannot sustain operation under these conditions, thus requiring larger stacks. The present disclosure provides, in part, a PBI-based high-performance battery with high electrical conductivity and low intra-cell resistance that allows the battery to operate at high performance under high current load conditions. These properties allow for the use of smaller, lower-cost electrochemical stacks.
[0021] The PBI gel membranes synthesized from the PPA process may be neutralized and imbibed with electrolytes commonly used in flow batteries. This established process and use of PBI membranes takes advantage of their excellent physical properties for such applications.
[0022] In one case, PBI gel membranes were fabricated for use with sulfuric acid electrolytes commonly used in redox flow batteries. These membranes have higher ionic conductivity than any previously reported on the subject, and can be used in batteries for renewable energy fields and / or for backup / reduction of energy interruptions during peak usage on the current power grid.
[0023] The present disclosure enables higher performance flow batteries operating under high current loads. These operating conditions alleviate the need for large electrochemical stacks, thereby reducing the overall cost of commercial flow battery devices. Furthermore, the membranes of the present disclosure exhibit superior performance due to their high ionic conductivity, which in turn reduces the overall construction cost by reducing the required stack size.
[0024] Figures 1 and 2 show the improved performance of PBI gel membranes at higher current densities. By using and fabricating devices with these membranes, which have inherently higher ionic conductivity, improved battery rate capability is possible. Overall battery cost can be dramatically reduced due to the smaller stack size required. Note: All data shown is for PBI membranes except those marked "BOM".
[0025] Furthermore, the membrane of the present disclosure does not show decomposition in vanadium (V) oxide solution. The applicants understand that no hydrocarbon membrane has this level of chemical stability, suggesting that the PBI gel membrane is an advantageous membrane for long-term use devices. Figure 3 shows the oxidation stability test of VRFB in the membrane of the present disclosure.
[0026] Increasing demands on the energy sector have created new needs for large energy storage devices with additional implications in grid management and backup power, while seamlessly integrating with new renewable energy devices. Redox flow batteries have the potential to both efficiently store large amounts of energy and also meet cost expectations. In vanadium redox flow batteries (VRBs), the major part of the cost is attributable to the vanadium electrolyte. This cost can be offset by cheaper cell stack designs. Currently, commercial VRBs use PFSA membranes in the stack components, which limits their further development due to their low selectivity and high cost. To reduce the cost of VRBs and improve their overall performance, there has been a surge in membrane development tailored to the specific needs of VRBs.
[0027] Phosphoric acid (PA) doped polybenzimidazole (PBI) membranes are best known for their performance in high temperature polymer electrolyte membranes (HT-PEMs). However, PBI membranes have been shown to be favorable candidates for several novel devices such as electrochemical hydrogen separation, SO2 depolarized electrolyzers, and redox flow batteries.
[0028] To date, research on PBI membranes for flow batteries has focused around meta-polybenzimidazole (m-PBI) and its derivatives, which are fabricated by solution casting in N,N'-dimethylacetamide (DMAc) to form a dense film and then imbibing the desired electrolyte into the formed film, a process referred to as the "conventional imbibition process". Membranes fabricated in this way typically have pore sizes in the range of 0.5 nm to 2.0 nm, which is much smaller than the pore sizes (2-4 nm) found in PFSA (e.g. Nafion™) type membranes. This reduction in porosity allows for a dramatic reduction in vanadium ion permeability compared to PFSA membranes, but their extremely low conductivity (<20 mS cm) when imbibed with a typical VRB electrolyte solution remains. -1 ) The focus of these recent studies has been to enhance the proton conductivity while maintaining the inherently low permeability of m-PBI dense films. These techniques include pre-swelling the PBI film with concentrated phosphoric acid before doping with sulfuric acid, creating a sponge-like porous structure using vapor-induced phase inversion and non-solvent-induced phase separation, and grafting various substituents onto the PBI polymer backbone. To the best of the applicant's knowledge, the PPA process as an alternative membrane for redox flow batteries has not been studied. No studies have been conducted on the use of PBI gel membranes formed from
[0029] The conventional imbibition process of PBI membranes is a time-consuming, environmentally unfriendly, and costly technique for membrane fabrication processes. However, Xiao et al. developed a novel polyphosphoric acid (PPA) process for producing PBI gel membranes, which consists of directly casting a polymerization solution containing PBI polymer in PPA. Subsequently, by exposing the cast solution to atmospheric moisture or controlled humidity conditions at room temperature, the PPA solvent, which is a good solvent for PBI, is hydrolyzed to phosphoric acid (PA), which is a poor solvent for PBI. This process induces a gel transition in the solution, which essentially forms a PBI gel membrane that has absorbed the phosphoric acid. These membranes are "pre-absorbed" with phosphoric acid, but have been shown to be capable of undergoing acid exchange of the absorbed electrolyte. Garrick et al. exchanged the phosphoric acid in a sulfonated para-polybenzimidazole (s-PBI) membrane with a 50 wt% sulfuric acid solution for testing in a SO2 depolarized electrolyzer used for hydrogen production. The membrane exhibited high stability in concentrated sulfuric acid, even at 120 °C. Furthermore, the membrane resistance in the SO2 depolarized electrolyzer was found to be almost negligible compared to the anodic overpotential, which is attributed to the high ionic conductivity of s-PBI.Due to the particularly good stability of the PBI derivatives and their high electrical conductivity, the s-PBI polymer gel membrane is envisioned as a possible alternative membrane for vanadium redox flow batteries with improved rate capabilities. EXAMPLES
[0030] material 3,3',4,4'-Tetraaminobiphenyl (TAB, polymer grade, ca. 97.5%) was a gift from BASF Fuel Cell, Inc. and was used as received. Monosodium 2-sulfoterephthalate (purity >98.00%) was purchased from TCI and was used as received. Polyphosphoric acid (115%) was supplied by FMC Corporation and was used as received. a,a'-Dichloro-p-xylene (purity >98.0%) was purchased from TCI and was used as received.
[0031] Polymer Synthesis and Membrane Production A typical polymerization consisted of adding 10.71 g of tetraaminobiphenyl (TAB, 50 mmol) and 13.44 g of monosodium 2-sulfoterephthalate (s-TPA, 50 mmol) to 580 g of polyphosphoric acid, mixing with an overhead stirrer and purging with dry nitrogen. The contents were heated in a high temperature silicone oil bath and the temperature was controlled by a programmable temperature controller with ramp and soak functions. In a typical polymerization, the final reaction temperature was approximately 195°C and held for 12 hours. After the reaction was complete and the viscosity was visually checked, the polymer solution was cast onto a clear glass plate using a doctor blade while controlling the gate thickness to 15 mils. The cast solution was hydrolyzed into a film in a humidity chamber controlled at 25°C and 55% RH.
[0032] acid exchange The cast membrane was placed in a DI water bath and the pH of the water was monitored using pH paper. The water bath was changed every 8 hours until a pH of 7 was recorded. At this point, the membrane was placed in a 2.6 molar sulfuric acid bath for 24 hours to ensure equilibration of the acid dope or the membrane was further modified by a cross-linking reaction.
[0033] Crosslinking after film formation After removing the PA from the PBI gel film, the film was immersed in a bath of 0.0523 M a,a'-dichloro-p-xylene in methanol. The bath was covered, heated to 30°C, and stirred with a magnetic stir bar. The crosslinking reaction was typically allowed to proceed for 6 hours. The film was then repeatedly washed at least three times with DI water and methanol. The film was then washed in 2.6 M a,a'-dichloro-p-xylene in methanol. The plate was then transferred into a sulfuric acid (SA) bath for 24 hours to dope it with acid.
[0034] Film composition The composition of the sulfuric acid doped PBI membranes was determined by measuring the relative amounts of polymer solids, water, and acid in the membrane. The sulfuric acid (SA) content of the membrane was determined by titrating the membrane samples with a standard solution of sodium hydroxide (0.10 M) using a Metrohm 888 DMS Titrando autotitrator. After titration, the samples were washed extensively with DI water and dried under vacuum at 120°C overnight. The dried samples were then weighed to determine the polymer solids of the membrane.
[0035] Equations 1 and 2 can be used to determine the weight percent of polymer and the weight percent of sulfuric acid, respectively:
number
[0036] The number of moles of sulfuric acid per mole of PBI repeat unit (or SA doping level, X) was calculated from the following formula:
number
[0037] conductivity The membrane was immersed in a 2.6 M sulfuric acid solution and a 1.5 M VOSO4 + 2.6 M sulfuric acid solution, respectively, to impregnate the membrane with sulfuric acid and V. 4+ Ions were absorbed. The in-plane conductivity of the membrane was measured by four-terminal electrochemical impedance spectroscopy (EIS) using a FuelCon (TrueData EIS PCM) electrochemical workstation in the frequency range of 1 Hz to 50 kHz. A membrane sample of typical geometry 1.0 cm x 4.0 cm was fixed to the four-electrode head of the measurement method. The membrane conductivity was calculated using the following formula:
number
[0038] Vanadium Permeability Vanadium(IV) (VOSO4) crossover is now available at PermeGear "Sa The measurements were performed using a "side-by-side" direct permeation cell. This cell has two chambers of 45 mL volume separated by the membrane under test. The temperature of the chambers was controlled at 25 °C with a circulating water bath. In a typical test experiment, 1.5 M VOSO4 in 2.6 M sulfuric acid was placed in the donor chamber and 1.5 M MgSO4 in 2.6 M sulfuric acid was placed in the receptor chamber. Vanadium(IV) has a strong absorption characteristic at 248 nm, which was exploited to measure the concentration in the receptor chamber at various time intervals using a Shimadzu UV-2450 UV / Vis spectrometer. VO 2+ The transmittance can be calculated using Fick's law of diffusion, Equation 5:
number
[0039] Figure 4 shows the polymerization scheme of s-PBI in PPA and the crosslinking modification reaction of the membrane. The rate performance of a flow battery is highly dependent on the conductivity of the membrane. The m-PBI membrane produced from the conventional absorption process has a relatively low conductivity, which limits stable operation at high current density. Herein, the inventors have investigated the use of s-PBI, a highly proton conductive membrane, for use in vanadium redox flow batteries.
[0040] FIG. 5 shows the in situ properties of s-PBI gel films compared to Table 1 - dense m-PBI films.
[0041] The out-of-device membrane properties for s-PBI gel membranes (both uncrosslinked and crosslinked) and m-PBI membranes formed from a conventional absorption process are shown in Table 1. See Figure 5. The room temperature conductivity of the membranes was measured using 2.6 M sulfuric acid and V(IV) / H2O2 as the typical cell operating conditions. + The s-PBI gel membrane exhibited a surprisingly high conductivity compared to the m-PBI membrane in both sulfuric acid and acid electrolyte solutions, 13.1 mS cm, respectively. -1 compared to 537-593 mS·cm -1 , and 12.2 mS cm -1 compared to 240-242 mS·cm -1The slight difference between the two s-PBI membranes is probably a result of crosslinking. s-PBI-x in Table 1 is the s-PBI film that underwent crosslinking modification after hydrolysis of the membrane. The crosslinker may form bonds with the imidazole nitrogens and slightly inhibit the proton pathway through the hydrogen bond network. The decrease in conductivity of the gel membrane in vanadium electrolyte solution compared to the solution in which it is absorbed may result from two factors. First, vanadium ions are attracted to the membrane by the negatively charged sulfonate groups (pKa approx. -2) and are unable to pass the protons through the hydrogen bond network. Furthermore, the dramatic decrease in conductivity of the PBI gel film is most likely due to the inherent conductivity of the electrolyte solution containing vanadium ions.
[0042] Since the main driver of proton conductivity is ion mobility, it is not surprising that increasing vanadium concentration reduces the proton conductivity of the electrolyte solution, related only to the increase in the electrolyte solution's viscosity. PBI gel membranes have a very open morphology that enhances proton conductivity not only by allowing proton transport by the Grotthuss mechanism, but also by the mobility of electrolytes in the membrane, and therefore proton transport through the membrane will also be affected by the increase in viscosity due to the incorporation of vanadium ions. .
[0043] Nevertheless, the mobility of electrolytes in PBI gel membranes is a valid argument for why vanadium permeability is significantly higher than in the corresponding dense membranes. This result is not unexpected, even when considering the polymer solids content of the membrane. In Table 1, it is clear that s-PBI has a relatively small amount of polymer per amount of electrolyte in the membrane compared to m-PBI. Given the high permeability of PBI gel membranes to vanadium ions, the inventors have devised a mitigation measure that allows PBI chains to be chemically crosslinked together to fill voids and limit chain mobility. At first glance, the permeability of s-PBI-x is less than ideal, but this slight modification has an effect when compared to the unmodified version without dramatically affecting the conductivity. This technique is not sensitive to the PBI derivative chosen, and can be used to improve the properties of PBI membranes, if desired. At present, the inventors have not found an easy way to determine the crosslink density of gel membranes, as typical gravimetric and rheological techniques are highly inaccurate for as-cast absorbent gel membranes. However, to confirm that crosslinking had occurred, a 50 mg sample of the neutralized dried membrane was heated to reflux in 800 mL of N,N'-dimethylacetamide for 48 h. Under these conditions, no membrane degradation or discoloration of the solution was observed for the crosslinked samples, whereas dissolution was observed for the pristine polymer film. Furthermore, a comparison of the swelling ratios of crosslinked and uncrosslinked membranes yields noteworthy results. When a non-acid solvent (N,N'-dimethylacetamide) was used to ensure suppression of unwanted solvent-polymer interactions, it was found that the uncrosslinked gel (3.94 wt % increase) absorbed approximately 0.75 wt % more solvent than the crosslinked membrane (3.25 wt % increase). The restriction of chain mobility due to chemical crosslinking inhibits solvent swelling of the polymer gel, resulting in less weight gain due to solvent uptake.
[0044] s-PBI gel membranes were synthesized via a PPA process to yield membranes stable in sulfuric acid and oxidizing V(V) solutions. The membranes exhibited high conductivity and good cell performance, especially at high current densities. However, these membranes have an inherently high vanadium ion permeability due to their open morphology and low polymer solids. Vanadium permeability was shown to be inhibited by chemical crosslinking, but is still high compared to dense membranes. However, this crosslinking method is applicable to many PBI chemistries and can be used to further reduce the permeability in PBI gel membranes without significant loss of proton conductivity.
[0045] Currently, PBI gel membranes used in flow batteries offer better performance than those described in the literature. However, penetration of redox species reduces the long-term overall efficiency of the battery. One further aspect of the present disclosure mitigates the high trans-transport properties of typical membranes without significantly compromising performance.
[0046] PBI gel membranes have shown particularly good performance in redox flow batteries. Membranes formed via this process can be neutralized and doped with common electrolytes used in these applications. The use of these membranes allows for operation under high current loads. The inherently high ionic conductivity of the membranes of these authors gives them a cost advantage compared to the membranes of the literature. Under these conditions, the size of the stack can be greatly reduced, mitigating the prohibitive costs for commercialization. Although the membranes used as is offer high performance, their permeability to the redox couple hampers their long-term efficiency.
[0047] Through novel unidirectional and bidirectional stretching methods, the transport mechanism of the redox couple can be inhibited without significantly compromising the overall performance.
[0048] In one aspect of the present disclosure, improvements are provided via post-modification to novel membranes used in redox flow batteries. The properties are changed without affecting the ionic conductivity of the protons.
[0049] In one embodiment, the present disclosure provides a membrane that can function under high current load, reduce the overall cost of the battery, and improve long-term efficiency by reducing the penetration of redox active species. Such membranes can be used in renewable energy fields and / or for backup / reduction of transmission interruptions during peak usage in the current power grid.
[0050] Novel processing techniques for the formed membranes allow for improved performance due to reduced transport of reactive species. These membranes outperform membranes commonly used in current commercial vanadium redox flow batteries. See FIG. 6, which shows the performance of the membranes of the present disclosure compared to commercial non-PBI membranes. Note: All data shown is for PBI membranes except those marked "BOM."
[0051] FIG. 7 shows a graph of the measured out-of-situ properties of the membranes of the present disclosure compared to a typical PBI gel membrane. Novel processing techniques allow for significant changes in membrane properties. These types of changes are not common in commercially available membranes and provide flexibility to end users when designing new devices or retrofitting existing devices. The permeability of the membranes of the following disclosure can be characterized by:
number
[0052] FIG. 8 shows a complete ex situ measurement of the membrane of the present disclosure.
[0053] FIG. 9 shows a comparison of transmittance compared to conductivity for para-BPI.
[0054] FIG. 10 shows a comparison of transmittance compared to conductivity in Mrp BPI. FIG. 11 shows cell test results for membranes formed according to the present disclosure. Overall, the PBI membranes formed according to the present disclosure showed high conductivity and stability in concentrated SA. Additionally, the transmittance of the para-PBI membrane was 4.55E-08 cm 2 / s, while the proton conductivity is maintained at 246 mS / cm at 2.6 M SA. Also, the VRB operated with the modified para-PBI membrane exhibited a proton conductivity of 100–450 mA / cm. 2 The coulombic efficiency is over 98% under high cycle current densities in the range of 1000 Hz to 1000 Hz.
[0055] Example 1: Para-PBI, stretch ratio = 1.7 The para-PBI membrane produced by the PPA process was first rinsed in a series of deionized water baths to remove phosphoric acid. Before proceeding, a pH indicator paper was used to ensure that all acid was removed. The membrane was cut to dimensions of 10 cm x 12 cm and folded twice into four layers. Using an Instron 5843 tensile tester, the membrane was stretched to 1.7 times its original length. It was then sandwiched between two porous glass plates, clamped around the periphery to maintain the dimensions in the xy direction, and allowed to dry overnight. The next day, the dried dense PBI film was removed and placed in a 2.6 M sulfuric acid solution for 24 hours before being characterized. The in-plane ionic conductivity was measured to be 175 mS / cm at room temperature.
[0056] Vanadium (VOSO4) penetration was measured using a PermeGear "side-by-side" direct permeation cell. The cell contains two chambers of 45 mL volume separated by a membrane sample. The test temperature was controlled at 25°C with a circulating water bath. In the test experiment, 1.5 M VOSO4 in 2.6 M sulfuric acid was placed in the donor chamber and 1.5 M MgSO4 in 2.6 M sulfuric acid was placed in the receptor chamber. The vanadium(IV) concentration in the receptor chamber was measured as absorbance at 248 nm using a Shimadzu UV-2450 UV / Vis spectrometer at various time intervals. The VO2+ transmission was then calculated using Fick's law of diffusion:
number
[0057] VRB (vanadium redox flow battery) test cell, 24 cm 2The membrane was assembled with an active area of 1.0 mm and used interdigitated flow fields machined into the carbon plate for the liquid electrolyte. The membrane was sandwiched between identical commercially available carbon paper electrodes that had been heat-treated at 400 °C for 30 h in air, and a polytetrafluoroethylene (PTFE) film was used as a gasket. The cell had two reservoirs on each side containing 100 mL of electrolyte solution consisting of 1.60 M vanadium species with an average oxidation state of 3.55 and a total sulfur content of 4.2 M. The electrolyte was circulated through the cell at a constant flow rate of 120 mL / min by two acid-resistant membrane pumps. Charge / discharge cycle performance was measured using a multichannel potentiostat (Model BT2000, Arbin Instruments Inc., College Station, TX) at 72 mA / cm 2 ~484mA / cm 2 The measurements were performed at a constant current density in the range of 1000 Hz to 1000 Hz. The voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) were measured and recorded. See FIG. 12.
[0058] Example 2: Para-PBI, stretch ratio = 1.5 The para-PBI membrane produced by the PPA process was first rinsed in a series of deionized water baths to remove phosphoric acid. Before proceeding, a pH indicator paper was used to ensure that all acid had been removed. The neutralized membrane was then cut to 10 cm x 12 cm and folded twice into four layers. Using an Instron 5843 tensile tester, the membrane was stretched to 1.5 times its original length. It was then sandwiched between two porous glass plates and clamped around the periphery to measure the xy The axial dimensions were maintained and the film was allowed to dry overnight. The next day, the dry dense PBI film was removed and placed in a 2.6 M sulfuric acid solution for 24 hours before characterization. The in-plane ionic conductivity was measured to be 207.6 mS / cm at room temperature. The VOSO4 permeability was tested as described in Example 1 and was found to be 4.55×10 -8 cm 2 It turned out to be / s.
[0059] A VRB test cell was assembled as described herein. The voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) were measured and recorded. See FIG. 13.
[0060] Example 3: Para-PBI, stretch ratio = 0 The para-PBI membrane produced by the PPA process was first rinsed in a series of deionized water baths to remove phosphoric acid, and pH indicator paper was used to ensure all acid was removed before proceeding. The wet thickness was measured as 356.67±5.8 um. The membrane was cut to dimensions of 45.72 cm x 30.48 cm. The wet membrane was sandwiched between two porous polyethylene sheets and clamped around the perimeter to maintain the xy dimensions. The sandwiched membrane was placed upright on a bench top and allowed to dry at room temperature. After 24 hours, the clamps and porous sheets were removed to yield a dry, dense PBI film. The film had a uniform thickness of 30 μm.
[0061] Example 3A: Flow battery data doped with 2.6M SA The dried film was placed in 2.6 M sulfuric acid for 24 hours and then characterized. The in-plane ionic conductivity was measured to be 95.17 mS / cm at room temperature. The permeability of VOSO4 was tested as described in Example 1 and was found to be 2.65×10 -8 cm 2 / s was measured.
[0062] A VRB test cell was assembled as described in Example 1. The voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) were measured and recorded. See Figure 14.
[0063] Example 3B: Doped with 85% by weight phosphoric acid The dried films were placed in 85 wt % phosphoric acid for 24 h and then characterized. The through-plane ionic conductivity was measured by four-probe AC impedance spectroscopy using the method of Zahn et al. The measurements were performed using a 3D IM6e spectrometer over the frequency range of 1 Hz to 100 kHz with an amplitude of 5 mV. A two-component model with an ohmic resistor and a capacitor in parallel was used to fit the experimental data. The conductivity of the membrane at different temperatures was calculated from the membrane resistance obtained from the model simulation using the following equation:
number
[0064] Example 4: s-PBI, stretching ratio=1.5 11.0824 g of 3,3',4,4'-tetraaminobiphenyl (TAB, 51.72 mmol), 13.9034 g of 2-sulfoterephthalic acid monosodium salt (2STPA, 51.85 mmol), and 600 g of polyphosphoric acid (PPA) were added to a 1000 mL reaction kettle equipped with an overhead mechanical stirrer (4 wt % monomer charge). ). It was polymerized at 220 °C for 48 hours in a nitrogen atmosphere. The solution was applied to a glass substrate with a gate thickness of 20 mils by doctor blade, followed by hydrolysis for 24 hours. The phosphoric acid-imbibed s-PBI membrane was rinsed in a series of deionized water baths to remove the phosphoric acid. Before proceeding, a pH indicator paper was used to ensure that all the acid was removed. It was cut to a dimension of 10 cm × 12 cm and folded twice into four layers. The membrane was stretched to 1.5 times its original length using an Instron 5843 tensile tester. It was then sandwiched between two porous glass plates, clamped around the periphery to maintain the dimensions in the xy direction, and allowed to dry overnight. The next day, the dried dense PBI film was removed and characterized after being placed in a 2.6 M sulfuric acid solution for 24 hours. The in-plane ionic conductivity was measured to be 179.7 mS / cm at room temperature. The transmittance of VOSO4 was tested as described in Example 1 and was found to be 2.60 × 10 -9 cm 2 / s was measured.
[0065] A VRB test cell was constructed as described in Example 1. The voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) were measured and recorded. See Figure 15.
[0066] Example 5: s-PBI, stretch rate=0 11.0824g of 3,3',4,4'-tetraaminobiphenyl (TAB, 51.72mmol), 13.9034g of 2-sulfoterephthalic acid monosodium salt (2STPA, 51.85mmol), and 600g of polyphosphoric acid (PPA) were added to a 1000mL reaction kettle equipped with an overhead mechanical stirrer (4wt% monomer loading). Polymerization was carried out at 220°C for 48 hours in a nitrogen atmosphere. The solution was applied to a glass substrate with a gate thickness of 20 mils by doctor blade and subsequently hydrolyzed for 24 hours. The phosphoric acid imbibed s-PBI membrane was rinsed in a series of deionized water baths to remove the phosphoric acid. Before proceeding, pH indicator paper was used to ensure that all the acid had been removed. The wet thickness was measured to be 251.8±34um. The wet membrane was sandwiched between two porous polyethylene sheets, clamped around the perimeter to maintain the xy dimensions, and allowed to dry overnight. After 24 hours, the clamps and porous sheets were removed to yield a dry, dense PBI film. The film had a uniform thickness of 37.7 um. The dried film was placed in 2.6 M sulfuric acid for 24 hours and then characterized. The in-plane ionic conductivity was measured to be 65.71 mS / cm at room temperature. The transmittance of VOSO4 was tested as described herein and was found to be 7.76 × 10 -9 cm 2 / s was measured.
[0067] A VRB test cell was constructed as described herein. The voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) were measured and recorded. See FIG. 16.
[0068] Example 6: Di-OH-PBI, stretching rate=0 6.615g of 3,3',4,4'-tetraaminobiphenyl (TAB, 30.87mmol), 6.119g of 2,5-dihydroxyterephthalic acid (DiOH-TPA, 30.88mmol), and 401.29g of polyphosphoric acid (PPA) were added to the reaction kettle and stirred with an overhead mechanical stirrer under nitrogen. Polymerization was carried out at 220°C for 24 hours under nitrogen. The solution was applied to a glass substrate with a gate thickness of 20 mils by doctor blade and subsequently hydrolyzed for 24 hours. The phosphoric acid imbibed membrane was rinsed in a series of deionized water baths to remove the phosphoric acid. Before proceeding, pH indicator paper was used to ensure that all the acid had been removed. The wet thickness was measured to be 404.44±10um. The wet membrane was sandwiched between two porous polyethylene sheets, clamped around the periphery to maintain the dimensions in the xy direction, and allowed to dry overnight. After 24 hours, the clamps and the porous sheet were removed to obtain a dry dense PBI film. This film had a uniform thickness of 31.1 um. The dried film was placed in 2.6 M sulfuric acid for 24 hours and then characterized. The in-plane ionic conductivity was measured to be 218.48 mS / cm at room temperature. The transmittance of VOSO4 was measured in this study. Tested as described in the specification, 3.92 x 10 -8 cm 2 / s was measured.
[0069] Comparative Example 1 (para-PBI in gel) The para-PBI membranes produced by the PPA process were first rinsed multiple times in deionized water baths to remove phosphate. Before proceeding, pH indicator paper was used to ensure that all acid was removed. The neutralized membranes were then placed in a 2.6 M sulfuric acid solution for at least 24 hours and then characterized. The VOSO4 permeability was tested as described herein and was found to be 5.73 × 10 -7 cm 2 / s was measured.
[0070] Comparative Example 2 (s-PBI in gel) 11.0824 g of 3,3',4,4'-tetraaminobiphenyl (TAB, 51.72 mmol), 13.9034 g of 2-sulfoterephthalic acid monosodium salt (2STPA, 51.85 mmol), and 600 g of polyphosphoric acid (PPA) were added to a 1000 mL reaction kettle equipped with an overhead mechanical stirrer (4 wt % monomer loading). Polymerization was carried out at 220 °C for 48 h in a nitrogen atmosphere. The solution was applied to a glass substrate with a gate thickness of 20 mils by doctor blade and subsequently hydrolyzed for 24 h. The phosphoric acid-imbibed s-PBI membrane was rinsed in a series of deionized water baths to remove the phosphoric acid. pH indicator paper was used to confirm that all the acid had been removed. The s-PBI membrane was placed in 2.6 M sulfuric acid for 24 h and then characterized. The VOSO4 transmittance was tested as described herein and was 4.89 × 10 -7 cm 2 / s was measured.
[0071] Comparative Example 3 (di-OH-PBI in gel) 6.615 g of 3,3',4,4'-tetraaminobiphenyl (TAB, 30.87 mmol), 6.119 g of 2,5-dihydroxyterephthalic acid (diOH-TPA, 30.88 mmol), and 401.29 g of polyphosphoric acid (PPA) were added to the reaction kettle and stirred with an overhead mechanical stirrer under nitrogen atmosphere. Polymerization was carried out at 220°C for 24 hours under nitrogen atmosphere. The solution was applied to a glass substrate with a gate thickness of 20 mils by doctor blade and subsequently hydrolyzed for 24 hours. The phosphoric acid-imbibed membrane was rinsed in a series of deionized water baths to remove the phosphoric acid. pH indicator paper was used to confirm that all the acid had been removed. The membrane was placed in 2.6 M sulfuric acid for 24 hours and then characterized. The transmittance of VOSO4 was tested as described in Example 1 and was found to be 7.23×10 -7 cm 2 / s was measured.
[0072] Comparative Example 4 (Meta-PBI) Commercially available meta-PBI films prepared by casting and drying from N,N-dimethylacetamide solution were used as received. The films were placed in a 2.6 M sulfuric acid solution for 24 h and then characterized. The in-plane ionic conductivity was measured to be 13.1 mS / cm at room temperature.
[0073] A VRB test cell was constructed as described in Example 1. The voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) were measured and recorded at 72 mA / cm2. See Figure 17. At higher current densities, the cell had no practical performance and was not operable. This is because the voltage is related to the conductivity of the membrane, which is very low.
[0074] Yet another aspect of the present disclosure involves refining the PBI film formation method. PBI films are known to have very good properties such as high temperature stability, non-flammability, and high chemical resistance. So far, the method for making PBI films has involved polymerization, dissolving the resulting polymer in an organic solvent such as dimethylacetamide (DMAc), casting the film, and removing the solvent by a series of washes.
[0075] In one embodiment, the present disclosure provides a novel method for producing PBI films starting from gel PBI membranes polymerized and cast by the PPA process. The acid-absorbed gel PBI is neutralized in a series of water baths and subjected to controlled drying between porous materials to obtain PBI films without the use of organic solvents. In addition, the PBI gels synthesized by the PPA process can use a wider range of monomers due to their low solubility in organic solvents. Thus, the present invention provides for the first time access to a wider range of PBI chemicals that can be processed into films.
[0076] The improved method provided herein is based on polybenzimidazole (PBI) membranes, and more specifically, PBI gel membranes. As used herein, the term "gel" refers generally to a polymer matrix that can incorporate a high content of liquid and maintain a self-supporting structure. For example, the PBI gel membranes described herein can incorporate about 60% or more, about 65% or more, about 75% or more, about 80% or more, or about 85% or more by weight of liquid based on the weight of the composite membrane (total solid plus liquid content) without compromising the structure of the polymer matrix. In one embodiment, the PBI gel membrane can incorporate about 60% to about 95% by weight of liquid while maintaining a self-supporting semi-rigid structure. That is, it can be manipulated to exhibit flexibility without compromising the structure of the polymer matrix. In addition, the PBI gel membrane can be treated to remove liquid from the gel and subsequently reabsorb liquid to reswell without compromising the structure of the polymer matrix.
[0077] The membranes formed by the methods of the present invention, in one aspect, provide high electrical conductivity and low resistance, allowing high performance operation under high current load conditions, which can lead to applications such as batteries using smaller, less expensive electrochemical stacks that provide the same or better performance compared to other technologies. For example, the described redox flow battery membranes, in some embodiments, can exhibit in-plane ionic conductivities of about 100 mS / cm or more, about 200 mS / cm or more, or about 300 mS / cm or more in 2.6 M sulfuric acid solution. The crosslinked membranes can exhibit extremely high in-plane ionic conductivities, such as about 300 mS / cm or more, about 400 mS / cm or more, or about 500 mS / cm or more. For example, the redox flow battery, in some embodiments, can exhibit in-plane ionic conductivities of about 100 mS / cm to about 600 mS / cm in 2.6 M sulfuric acid solution.
[0078] In addition, batteries incorporating the disclosed membranes can be operated at high current densities, e.g., about 100 mA / cm2 or greater, in some embodiments, from about 100 mA / cm2 to about 500 mA / cm2. Furthermore, batteries incorporating the described redox flow battery membranes can be operated with high efficiency. For example, at a current density of 242 mA / cm2, redox flow batteries incorporating the described membranes can exhibit a coulombic efficiency (CE) of about 90% or greater, e.g., in some embodiments, from about 93% to about 99%; an energy efficiency (EE) of about 75% or greater, e.g., in some embodiments, from about 78% to about 85%; and a voltage efficiency (VE) of about 80% or greater, e.g., from about 81% to about 87%. At a current density of 483 mA / cm, the described redox flow batteries can exhibit a CE of 90% or greater, e.g., in some embodiments, from about 94% to about 98%; an EE of about 65% or greater, e.g., in some embodiments, from about 65% to about 75%; and a VE of about 65% or greater, e.g., from about 66% to about 77%.
[0079] As further described herein, the disclosed gel membranes are formed according to a method that includes hydrolysis of a PPA polymer solvent, followed by solidification of the PBI polymer in the hydrolysis product (PA). This in situ hydrolysis and solidification of the polymer results in the formation of an ordered polymer matrix with a molecular structure that differs from that of conventional organic solution cast PBI membranes that are cast as a solution in an organic solvent and subsequently solidified by removal of the organic solvent, e.g., via heating. In particular, it is believed that the PBI gel membrane structure contains a more open and ordered framework compared to conventional PBI membranes, and that the PBI matrix framework provides a stable gel membrane that exhibits the improved electrochemical properties described.
[0080] To form a PBI gel film that can be used in the methods of the present disclosure, a polymeric composition can be formed that includes a PPA and a selected PBI-forming compound, such as a PBI-forming monomer. The monomer content of the polymeric composition can generally be low, for example, in some embodiments, about 10% by weight or less, about 8% by weight or less, or about 5% by weight or less.
[0081] The PBI polymer of the PBI gel film may have any PBI structure commonly known in the art and may be formed by polymerization of PBI-forming compounds including at least one aromatic or heteroaromatic tetraamino compound and at least one aromatic or heteroaromatic polycarboxylic acid or its ester, anhydride, or acid chloride, or at least one aromatic or heteroaromatic diaminocarboxylic acid. Heteroaromatic compounds encompassed herein include aromatic systems containing at least one nitrogen, oxygen, sulfur, or phosphorus atom in the aromatic ring.
[0082] Examples of aromatic and heteroaromatic tetraamino compounds that may be used in forming the PBI gel membrane include, but are not limited to, 2,3,5,6-tetraaminopyridine, 3,3',4,4'-tetraaminodiphenylsulfone, 3,3',4,4'-tetraaminodiphenylether, 3,3',4,4'-tetraaminobiphenyl, 1,2,4,5-tetraaminobenzene, 3,3',4,4'-tetraaminobenzophenone, 3,3',4,4'-tetraaminodiphenylmethane, and 3,3',4,4'-tetraaminodiphenyldimethyl-methane, as well as salts thereof, such as the mono-, di-, tri-, and tetrahydrochloride salts, as well as any combination of aromatic or heteroaromatic tetraamino monomers.
[0083] In one embodiment, the aromatic polycarboxylic acid may include a dicarboxylic acid. The dicarboxylic acid may be used alone or in combination with one or more additional polycarboxylic acid compounds, such as tricarboxylic acids and / or tetracarboxylic acids. When incorporated, the content of tricarboxylic acid or tetracarboxylic acid may generally be about 30 mol% or less, for example, about 0.1 mol% to about 20 mol%, or about 0.5 mol% to about 10 mol%, based on the amount of the one or more dicarboxylic acid compounds. Esters of polycarboxylic acids, such as C1-C20 alkyl esters or C5-C12 aryl esters of polycarboxylic acids, may be used. Anhydrides of polycarboxylic acids or acid chlorides of polycarboxylic acids may be polymerized according to the disclosed method.
[0084] Examples of aromatic dicarboxylic acids include, but are not limited to, pyridine-2,5-dicarboxylic acid, pyridine-3,5-dicarboxylic acid, pyridine-2,6-dicarboxylic acid, pyridine-2,4-dicarboxylic acid, 4-phenyl-2,5-pyridinedicarboxylic acid, 3,5-pyrazoledicarboxylic acid, 2,6-pyrimidinedicarboxylic acid, 2,5-pyrazinedicarboxylic acid, 2,4,6-pyridinetricarboxylic acid, benzimidazole-5,6-dicarboxylic acid, 5-hydroxyisophthalic acid, 4-hydroxyisophthalic acid, 2-hydroxyterephthalic acid, 5-phenyl-2,5-pyridinedicarboxylic ... -aminoisophthalic acid, 5-N,N-dimethylaminoisophthalic acid, 5-N,N-diethylaminoisophthalic acid, 2,5-dihydroxyterephthalic acid, 2,6-dihydroxyisophthalic acid, 4,6-dihydroxyisophthalic acid, 2,3-dihydroxyphthalic acid, 2,4-dihydroxyphthalic acid, 3,4-dihydroxyphthalic acid, 1,8-dihydroxynaphthalene-3,6-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, isophthalic acid, terephthalic acid, phthalic acid, 3-fluorophthalic acid, 5-fluoroisophthalic acid, 2 4,4'-dicarboxylic acid, benzophenone-4,4'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, 4-trifluoromethylphthalic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 4,4'-stilbene dicarboxylic acid, and 4-carboxycinnamic acid, or any combination thereof.
[0085] Examples of aromatic tricarboxylic acids, as well as their esters, anhydrides, and acid chlorides, can include, but are not limited to, 1,3,5-benzenetricarboxylic acid (trimesic acid); 1,2,4-benzenetricarboxylic acid (trimellitic acid); (2-carboxyphenyl)iminodiacetic acid, 3,5,3'-biphenyltricarboxylic acid, and 3,5,4'-biphenyltricarboxylic acid; or any combination thereof.
[0086] Examples of aromatic tetracarboxylic acids, as well as their esters, anhydrides, and acid chlorides, may include, but are not limited to, 3,5,3',5'-biphenyltetracarboxylic acid; benzene-1,2,4,5-tetracarboxylic acid; benzophenonetetracarboxylic acid; 3,3',4,4'-biphenyltetracarboxylic acid; 2,2',3,3'-biphenyltetracarboxylic acid; 1,2,5,6-naphthalenetetracarboxylic acid; and 1,4,5,8-naphthalenetetracarboxylic acid; or any combination thereof.
[0087] Heteroaromatic carboxylic acids can include heteroaromatic dicarboxylic acids, heteroaromatic tricarboxylic acids, and heteroaromatic tetracarboxylic acids, including the corresponding esters, such as C1-C20 alkyl esters, C5-C12 aryl esters, or acid anhydrides or acid chlorides of heteroaromatic carboxylic acids. Examples of heteroaromatic carboxylic acids include, but are not limited to, pyridine-2,5-dicarboxylic acid, pyridine-3,5-dicarboxylic acid, pyridine-2,6-dicarboxylic acid, pyridine-2,4-dicarboxylic acid, 4-phenyl-2,5-pyridinedicarboxylic acid, 3,5-pyrazoledicarboxylic acid, 2,6-pyrimidinedicarboxylic acid, 2,5-pyrazinedicarboxylic acid, 2,4,6-pyridinetricarboxylic acid, benzimidazole-5,6-dicarboxylic acid, and also their C1-C20 alkyl esters or their C5-C12 aryl esters, or their acid anhydrides, or their acid chlorides, or any combination thereof.
[0088] In one embodiment, the polymerizable composition may comprise a diaminocarboxylic acid, examples of which include, but are not limited to, diaminobenzoic acid and the mono- and dihydrochloride derivatives thereof, and 1,2-diamino-3'-carboxylic acid 4,4'-diphenyl ether, or any combination thereof.
[0089] The PPA that may be used in the polymeric composition may be a commercially available PPA available, for example, from Riedel-de Haen. The PPA may include concentrated grades of PA (H3PO4) of greater than 100%. At high concentrations, the individual H3PO4 units are polymerized by dehydration, and the PPA has the formula H n+2 P n O 3n+1 (n>1).
[0090] PPA[H n+2 P n O 3n+1(n>1)] may have a P2O5 content of about 70 wt% or more, e.g., about 75 wt% or more, or about 82 wt% or more, e.g., about 70 wt% to about 86 wt%, in some embodiments, as calculated by acid titration. The polymerization composition may generally be in the form of a solution of monomer / compound or a dispersion / suspension of monomer / compound in the PPA, depending on the nature of the compound to be polymerized and any additional components of the polymerization solution.
[0091] The polymerization may be carried out at a temperature and for a period of time until adequate polymerization of the compounds occurs, which can generally be determined by an increase in the viscosity of the polymerized composition. The increase in viscosity can be determined by visual inspection, through determination of the intrinsic viscosity, or by any other suitable means. For example, the polymerization may be continued until the polymerized composition exhibits an intrinsic viscosity of about 0.8 dL / g or more, in some embodiments, for example, about 1.0 dL / g or more, or about 1.5 dL / g or more. The polymerization temperature may generally be about 220° C. or less, such as about 200° C. or less, and in some embodiments, about 100° C. to 195° C. The polymerization may be carried out for a period of time ranging from a few minutes (e.g., about 5 minutes) to a few hours (e.g., about 100 hours). In one embodiment, the polymerized composition may be heated in a stepwise manner, for example in three or more steps, each step lasting from about 10 minutes to about 5 hours, with the temperature increasing by about 15° C. or more for each step. Of course, the specific polymerization conditions can vary depending on the reactivity and concentration of the specific monomers, as will be appreciated by one of ordinary skill in the art, and no specific polymerization conditions are required in the formation of a redox flow battery membrane.
[0092] Exemplary PBI polymer repeat units of a PBI gel membrane include, but are not limited to: [ka] [ka] [ka] or any combination thereof, where in some embodiments n and m are each independently 1 or more, about 10 or more, or about 100 or more.
[0093] The PBI polymers of the membranes disclosed herein may include any repeating units, including any derivatization generally known in the art, examples of which are well within the knowledge of one of ordinary skill in the art, representative examples of which are described, for example, in U.S. Patent Application Publication No. 2013 / 0183603 by Benicewicz, et al., which is incorporated herein by reference.
[0094] After polymerization, the polymer may remain dissolved in the PPA solvent, and the PBI polymer solution may be processed to form a gel film precursor having a desired thickness. Advantageously, the polymer solution, as well as the gel film precursor formed therefrom, and the final gel film and redox flow battery membrane, may be organic solvent free.
[0095] The membrane precursor may be formed according to any suitable forming process, including but not limited to casting, spray coating, knife coating, etc. For example, the gel membrane precursor may be formed to a thickness of about 20 micrometers (μm) to about 4000 μm in one embodiment, and in some embodiments, may be formed to a thickness of about 30 μm to about 3500 μm, or about 50 μm to about 1000 μm, etc.
[0096] To solidify the polymer and form a PBI gel film, the PBI polymer solution can be treated in the presence of water and / or moisture to hydrolyze at least a portion of the PPA in the solution, which hydrolyzes to form PA and water, thereby inducing a sol-gel transition of the PBI polymer solution and solidification of the polymer, since the PBI polymer is less soluble in PA than PPA.
[0097] The hydrolysis treatment may be carried out at a temperature and for a time sufficient to solidify the gel film so that it is self-supporting and can be manipulated without destruction, while maintaining a high liquid content (e.g., a liquid content of about 60% or more by weight of the total solid and liquid content of the film). For example, the hydrolysis treatment may be carried out at a temperature of about 0° C. to about 150° C., e.g., about 10° C. to about 120° C., or about 20° C. to about 90° C., in some embodiments, at ambient temperature (e.g., in a relative humidity contact environment of about 35% to 100%).
[0098] Hydrolysis may be carried out by contacting the gel film precursor with HO, e.g., in liquid or vapor form, and / or in the presence of other components. For example, the gel film precursor may be contacted with water vapor and / or liquid water and / or steam and / or an aqueous PA solution (e.g., a PA solution with a PA concentration of about 10% to about 90% by weight, e.g., about 30% to about 70% by weight, or about 45% to about 55% by weight). The treatment may be carried out under standard pressure, although this is not a requirement of the formation process, and in some embodiments, the hydrolysis treatment may be carried out under altered pressure.
[0099] In one embodiment, hydrolysis may be performed in an air-conditioned environment where the H2O content can be tightly controlled. For example, control of the water content of the local environment may be performed through control of the temperature or saturation of the fluid in contact with the precursor film. For example, a carrier gas such as air, nitrogen, carbon dioxide, or other suitable gas may carry H2O, e.g., steam, in a controlled amount to contact the precursor film.
[0100] The hydrolysis treatment time may generally vary depending on parameters such as, for example, the H2O content, and the contact form, film thickness, contact temperature, etc. The hydrolysis treatment may generally be carried out for a period of time ranging from a few seconds to a few minutes, for example, when the hydrolysis treatment uses superheated steam, or alternatively, for a period of time ranging from a few days, for example, when the hydrolysis treatment is carried out at ambient temperature and at low relative atmospheric moisture content. In some embodiments, the hydrolysis treatment may be carried out for a period of time ranging from about 10 seconds to about 300 hours, for example, from about 1 minute to about 200 hours. By way of example, in embodiments in which the at least partial hydrolysis of the PPA of the PBI polymer solution is carried out at room temperature (e.g., about 20°C) with ambient air having a relative atmospheric moisture (i.e., relative humidity) content of about 20% to 100%, for example, about 40% to about 80%, the treatment time may generally be from about 5 hours to about 200 hours.
[0101] Upon hydrolysis of at least a portion of the PPA of the PBI polymer solution, the polymer can be solidified to form a PBI gel membrane. The PBI gel membrane, in one embodiment, can have a thickness of about 15 μm to about 3000 μm, for example about 20 μm to about 2000 μm, or about 20 μm to about 1500 μm, although any particular membrane thickness is not essential. In some embodiments, the PBI gel membrane can have a thickness less than that of the membrane precursor. As mentioned above, after hydrolysis, the PBI gel membrane can be self-supporting even at high liquid content, which is believed to be due to the intra- and intermolecular polymer structures present in the solidified polymer matrix.
[0102] The as-formed PBI gel film, in one embodiment, can have a PBI solids content of about 5% to about 40% by weight, e.g., about 8% to about 30% by weight or about 10% to about 25% by weight of the total weight of the film including liquid content. The as-formed PBI gel film can be free-standing, e.g., in some embodiments, has a Young's modulus of about 2.0 MPa or greater, e.g., about 3.0 MPa or greater or about 4.5 MPa or greater, as specified for a PBI gel film (e.g., polybenzimidazole) having a thickness of 403 μm and a PBI content of 5% by weight.
[0103] One obvious application of the disclosed method is in redox flow battery membranes, but the method is not limited to this one aspect and may be used to make PBI films as well as fibers, fibrids, resins, resin beads, papers, microporous resins, sizing agents, coatings, and molded resins. Additionally, the disclosed PBI films may be used in aerospace structures, adhesives, carbon fiber laminates, insulation, syntactic foams, and fabrics. Specific applications include, but are not limited to, aircraft fire seals, fire protection equipment, sock hoods, high temperature gloves, aluminum coated rescue gear, flight suits, hazardous work coveralls, filtration systems, glass handling belts, expansion joints, gaskets, packings, resin fillers, motor insulation, filament wound composites, lacing for reinforcing fibers, chopped fiber reinforcement for resin matrices, acid scavenger applications, sizing agents, heat shields, transformer wraps, asbestos replacements, composites, battery separators, pipe insulation, microelectronics processing, wire coatings, gas separation films, protective windows and glass coatings, high temperature substrate fills, and the like.
[0104] If desired, the PBI gel membrane may be crosslinked to reduce the permeation of the redox ion pairs of the battery electrolyte solution through the membrane without significantly affecting the membrane's desired electrochemical properties. The crosslinking technique and the point in the formation process at which the membrane is crosslinked are not particularly limited. For example, the gel membrane may be crosslinked after rinsing / washing the as-formed gel membrane and before absorption of the supporting electrolyte into the membrane. However, in other embodiments, the membrane may be crosslinked before rinsing / washing or after absorption of the supporting electrolyte into the membrane.
[0105] In one embodiment, the PBI gel film may be crosslinked simply by heating in the presence of atmospheric oxygen. Crosslinking may also be performed by the action of radiation, such as IR (having a wavelength of about 700 nm to about 1 mm), including near-infrared (IR) radiation (radiation having a wavelength of about 700 to about 2000 nm or an energy in the range of about 0.6 to about 1.75 eV).
[0106] To effect crosslinking, the PBI polymer may contain reactive functional groups in the polymer chain to crosslink with itself or with a crosslinker, i.e., a multifunctional compound capable of reacting with one or more functional groups (e.g., amines) of the PBI polymer. The crosslinker may contain any suitable functional group for effecting crosslinking. Suitable crosslinkers are not particularly limited, examples of which include, but are not limited to, epichlorohydrin, diepoxides, diisocyanates, α,ω-dihaloalkanes, diacrylates, and bisacrylamides, and specific examples of which include, but are not limited to, α,α'-dichloro-p-xylene, chloromethyl methyl ether, bis(chloromethyl)ether, terephthaloyl chloride, succinyl chloride, and dimethyl succinate, as well as combinations of crosslinkers. In one embodiment, 1 to 20 equivalents of crosslinker per available aromatic ring may be used, although the crosslinked embodiment of the membrane is not limited to any particular crosslink density.
[0107] Additionally, the PBIs of the present disclosure may be imbibed with a supporting electrolyte. The choice of supporting electrolyte may generally depend on the specific characteristics of the redox flow battery in which the membrane is used and may include acidic supporting electrolytes, basic supporting electrolytes, or even neutral species (e.g., water). For example, the membrane may be imbibed with inorganic acids (e.g., strong inorganic acids), such as hydrochloric acid, nitric acid, fluorosulfonic acid, or sulfuric acid, or mixtures thereof, or strong organic acids, such as acetic acid, formic acid, p-toluenesulfonic acid, or trifluoromethanesulfonic acid, or mixtures thereof, as well as mixtures of different types of acids, e.g., combinations of inorganic and organic acids. Other examples of supporting electrolytes that may be imbibed with the membrane include, but are not limited to, sodium chloride, potassium chloride, sodium hydroxide, potassium hydroxide, sodium sulfide, potassium sulfide, and combinations thereof. By way of example, the supporting electrolyte may include H2SO4, HBr, HBr / HCl mixtures, HCl, NaS2, NaS2 / NaBr mixtures, Br2 in HBr, Br2 in H2SO4, Br2 in HBr / H2SO4 mixtures, etc. In one embodiment, a tetraalkylammonium supporting cation may be absorbed into the membrane, such as Et4N + and Bu4N + are two non-limiting examples. Tetrafluoroboric acid (BF 4- ), perchloric acid (ClO 4- ), or hexafluorophosphate (PF 6- ), or combinations thereof, are further examples of supporting electrolytes that may be imbibed into the membrane.
[0108] The concentration of the supporting electrolyte in the membrane is not particularly limited, and generally, the solution to be absorbed into the membrane may contain the supporting electrolyte at a concentration of up to about 25 moles / liter (M) in some embodiments, for example, from about 0.1 M to about 25 M, from about 0.5 M to about 10 M, or from about 1 M to about 5 M.
[0109] The film may be imbibed with the supporting electrolyte according to any suitable method, for example: Absorption of the supporting electrolyte into the film may, in one embodiment, be carried out by immersing the film in a solution of the supporting electrolyte for a period ranging from a few minutes to a few hours or days, in an environment of elevated temperature as desired.
[0110] This disclosure details a novel method for producing PBI films without the use of organic solvents. Eliminating the need for organic solvents provides a new route to produce PBI films that is cheaper, faster, and generates less chemical waste than previous methods. This novel solvent-free method also allows a wider variety of PBI chemicals to be made into films.
[0111] The applications of the PBI-based films of the present disclosure are varied. For films intended for use as ionic conductors in electrochemical applications, the dry films may be further treated to "reswell" the membrane and absorb bases, acids, or other ionic conductors, so that the films are not limited to use only in redox flow batteries. When reswelled, the films exhibit low permeability to redox couples and other materials, yet still exhibit high ionic conductivity for electrochemical applications.
[0112] The following examples will better illustrate the present disclosure.
[0113] Example 7: Para-PBI film The para-PBI membrane produced by the PPA process was first rinsed with a detergent to remove phosphate, which may include various solutions including mildly basic water, deionized water, or other suitable detergents known to those skilled in the art, and in one embodiment, the detergent may be a series of deionized water baths, and pH indicator paper was used to ensure all acid was removed before proceeding. See FIG. 18. The wet thickness was measured as 356.67±5.8 um, and the membrane was cut to dimensions of 45.72 cm×30.48 cm. The wet membrane was sandwiched between two porous polyethylene sheets, clamped around the periphery to maintain dimensions in the xy directions, and allowed to dry overnight. After 24 hours, the polyethylene sheets were removed to obtain a dry dense PBI film. The film had a uniform thickness of 30 μm. The film showed a survival rate of more than 85% by weight as measured by thermogravimetric analysis (TGA) at 500° C. in a nitrogen atmosphere.
[0114] The mechanical properties of the dense films were measured using an Instron 5843 tensile tester. Five samples were cut according to the ASTM D638 (Type V) standard and the elastic modulus (measured as the slope at 1% strain), break stress, and break strain were measured. Figure 18 shows the tensile test results of the para-PBI membranes produced according to the present disclosure.
[0115] Example 8: Di-OH-PBI film 401.30 g of polyphosphoric acid was added to a reaction kettle containing 6.6161 g (30.88 mmol) of 3,3',4,4'-tetraaminobiphenyl and 6.1177 g (30.88 mmol) of 2,5-dihydroxyterephthalic acid. With stirring under nitrogen atmosphere, polymerization was initiated at 40°C for 1 hour, increased to 140°C for 2 hours, soaked at 140°C for 4 hours, increased to 195°C for 3 hours, and soaked at 195°C for 14 hours. The solution was then coated onto a polyester film by a doctor blade, followed by hydrolysis at room temperature and 55% relative humidity.
[0116] The Di-OH-PBI film was then rinsed in a series of deionized water baths to remove the phosphoric acid and pH indicator paper was used to ensure all acid was removed before proceeding. The wet thickness was measured to be 348.33 ± 43.4 um. The wet film was sandwiched between two porous polyethylene sheets, clamped around the periphery to maintain dimensions in the xy direction, and allowed to dry overnight. After 24 hours, the polyethylene sheets were removed to yield a dry, dense PBI film. This film was then dried overnight. The lum had a thickness of 24.67±3.8 um.
[0117] The mechanical properties of the dense films were measured using an Instron 5843 tensile tester. Four samples were cut according to the ASTM D638 (Type V) standard, and the elastic modulus (measured as the slope at 1% strain), breaking stress, and breaking strain were measured. See Figure 19.
[0118] Example 9: s-PBI film 384 g of polyphosphoric acid was added to a reaction kettle containing 7.1063 g (33.17 mmol) of 3,3',4,4'-tetraaminobiphenyl and 8.8937 g (33.16 mmol) of 2-sulfoterephthalic acid monosodium salt. Polymerization was allowed to proceed for 48 hours at 190°C with stirring under a nitrogen atmosphere. The solution was then coated onto a polyester film by a doctor blade and subsequently hydrolyzed at room temperature and 55% relative humidity.
[0119] The s-PBI membrane was then rinsed in a series of deionized water baths to remove the phosphate, and pH indicator paper was used to ensure all acid had been removed before proceeding. The wet thickness was measured to be 276.33 ± 22.59 um. The wet membrane was sandwiched between two porous polyethylene sheets, clamped around the periphery to maintain dimensions in the xy direction, and allowed to dry overnight. After 24 hours, the polyethylene sheets were removed to yield a dry, dense PBI film. The film had a thickness of 33.0 ± 3.0 um.
[0120] The mechanical properties of the dense films were measured using an Instron 5843 tensile tester. Five samples were cut according to the ASTM D638 (Type V) standard, and the elastic modulus (measured as the slope at 1% strain), breaking stress, and breaking strain were measured. See Figure 20.
[0121] Example 10: Meta / Para-PBI Copolymer Film 1027 g of polyphosphoric acid was added to a reaction kettle containing 64.2810 g (300.00 mmol) of 3,3',4,4'-tetraaminobiphenyl, 43.6118 g (262.52 mmol) of isophthalic acid, and 6.2303 g (37.50 mmol) of terephthalic acid. The mixture was polymerized at 190°C for 20 hours under stirring under nitrogen atmosphere. The solution was then coated onto a polyethylene film by a doctor blade and subsequently hydrolyzed at room temperature and 55% relative humidity.
[0122] The meta / para-PBI copolymer film was then rinsed in a series of deionized water baths to remove the phosphoric acid, and pH indicator paper was used to ensure all acid was removed before proceeding. The wet thickness was measured to be 197 ± 15.70 um. The wet film was sandwiched between two porous polyethylene sheets, clamped around the periphery to maintain dimensions in the xy direction, and allowed to dry overnight. After 24 hours, the polyethylene sheets were removed to yield a dry, dense PBI film. The film had a thickness of 62.67 ± 7.97 um.
[0123] The mechanical properties of the dense films were measured using an Instron 5843 tensile tester. Five samples were cut according to the ASTM D638 (Type V) standard, and the elastic modulus (measured as the slope at 1% strain), breaking stress, and breaking strain were measured. See Figure 21.
[0124] Example 11: Para-PBI film dried on one support substrate In this example, the para-PBI membrane produced by the PPA process was first rinsed in a series of deionized water baths to remove phosphate, and pH indicator paper was used to ensure all acid was removed before proceeding. The wet thickness was measured to be 350 μm. The wet membrane was then dried on a single support substrate. The PBI film was clamped onto a piece of porous polyethylene sheet to maintain its dimensions in the xy direction and allowed to dry. After 8 hours, a dry dense PBI film remained, which was removed from the porous polyethylene sheet. The film was 42 □m thick, observed to be of high quality, and appeared to be consistent with the film produced in Example 1 above.
[0125] Comparative Example 5: Commercially available meta-PBI films cast from organic solvents m-PBI was obtained commercially, solution cast (from N,N-dimethylacetamide) and used as received. The mechanical properties of the dense films were measured using an Instron 5843 tensile tester. Eight samples were cut according to ASTM D638 (Type V) standard and the elastic modulus at 1% strain, yield stress, yield strain, break stress, and break strain were measured. See FIG. 22.
[0126] In addition, PBI membranes made according to the present disclosure may be redoped with phosphoric acid. These redoped membranes may exhibit better creep resistance and may be directly applicable at least for fuel cell applications.
[0127] Example 12: Dried para-PBI film doped with 85 wt% phosphoric acid The para-PBI membrane produced by the PPA process was first rinsed in a series of deionized water baths to remove phosphoric acid (PA) and pH indicator paper was used to ensure all acid was removed before proceeding. The wet thickness was measured as 356.67 ± 5.8 μm and the membrane was cut to dimensions of 45.72 cm × 30.48 cm. The wet membrane was sandwiched between two porous polyethylene sheets, clamped around the periphery to maintain dimensions in the xy direction, and allowed to dry overnight. After 24 hours, the polyethylene sheets were removed to obtain a dry dense PBI film. The film had a uniform thickness of 30 μm. The dried film was placed in 85 wt% phosphoric acid for 24 hours before characterization and fuel cell testing. The membrane thickness after PA doping was 150 μm.
[0128] The ionic conductivity through the thickness was measured by four-terminal AC impedance spectroscopy using a Zahner IM6e spectrometer over the frequency range of 1 Hz to 100 kHz at an amplitude of 5 mV. A two-component model with an ohmic resistor and a capacitor in parallel was used to fit the experimental data. The conductivity of the film at different temperatures was calculated from the film resistance obtained from the model simulation using the following equation:
number
[0129] Compressive creep and creep recovery tests were performed using a TA Instruments RSAIII Dynamic Mechanical Analyzer. Membrane samples were cut with a diameter of approximately 7 mm and a thickness of approximately 1.2-1.7 mm. Prior to creep testing, all samples were preconditioned at 180°C for 24 hours. In a typical experiment, a constant compressive force corresponding to a stress level of 0.1 MPa was applied to the sample and held for 20 hours, after which the force was removed for 3 hours. All experiments were performed at 180°C, and strain and stress were recorded as a function of time. Creep compliance was calculated by dividing the time-dependent strain by the applied stress. The creep resistance was calculated by the following formula: In this experiment, the creep test was repeated three times for each membrane. In one embodiment, the film of the present disclosure may have a breaking stress of at least 25 MPa. Figure 24 shows that the membrane produced by this method exhibited much better (lower) creep resistance than the standard PPA process membrane.
[0130] A membrane electrode assembly (MEA) consisting of a phosphoric acid-doped para-PBI membrane was placed on a 10 cm 2 The cells were assembled into a single cell hardware and tested using a commercial fuel cell test station (Fuel cell Technology, Inc.). The device was controlled by a self-programmed LabView software (National Instruments in Austin, TX). Prior to testing, the cells were heated at 160 °C and 0.2 A / cm with H2 supplied to the anode and air supplied to the cathode. 2 A trial run of at least 24 hours was performed by operating at a current density of 1.25 V. Polarization curves were recorded at 160, 180, and 200° C. with stoichiometric flow rates of H2 / air=1.2 / 2.0 and H2 / O2=1.2 / 2.0. FIG. 25 shows the polarization curves with H2 / air, and FIG. 26 shows the polarization curves with H2 / O2.
[0131] These examples disclose placing the PBI gel membrane in contact with a substrate such as a porous sheet during the drying process. The substrate may comprise a variety of materials such as a porous or non-porous substrate. In addition, the disclosure also discloses that the various PBI gels may be sandwiched between two porous sheets, a porous sheet and a non-porous sheet, or simply in contact with one porous or non-porous sheet without a sheet on the other side of the PBI gel membrane. The membrane may be dried in a continuous process with or without a support sheet. As shown in FIG. 23, a flow of drying gas may be used on one or both sides of a supported or free-standing membrane to facilitate the drying process.
[0132] With respect to processing, the PBI membrane of the present disclosure may be restrained and / or tensioned in the X, Y, and Z plane directions. In this specification, "restrained" may be used to mean that the PBI membrane is simply fixed in place without applying a stretching or tensioning force to the PBI membrane to stretch the membrane from its original shape. On the other hand, "tensioned" may be used to mean that a stretching or tensioning force is applied to the PBI membrane to make it taut across the membrane surface in the X and / or Y plane directions or to extend its length in the X and / or Y plane directions. In a preferred embodiment, the PBI membrane is restrained and / or tensioned in the X, Y, and Z plane directions, but is unrestrained and untensioned in the Z plane direction. Furthermore, drying the membrane may simply be air drying the PBI membrane. However, in further embodiments, a gas such as dry gas, air, or nitrogen may be supplied onto the restrained or tensioned film to facilitate the drying process. Still further, the PBI film may be restrained widthwise and a dry gas, air, nitrogen, may be passed over either one or both sides of the tensioned film.
[0133] The present disclosure also has direct implications for the application of film processing in PBI films formed according to the present disclosure. In one embodiment, the present disclosure may be combined with continuous film-forming processes known to those skilled in the art. For example, as shown in FIG. 23, a continuous formation process 100 may be used to form a PBI membrane 102 via a continuous process, where a preformed PBI membrane 102 may be directly deposited, either simultaneously or separately, on a film tensioner surface 104 that may restrain the film in the X, Y, and / or Z plane directions or tension the PBI membrane 102 by pulling it in the X, Y, and / or Z plane directions. Alternatively, the PBI membrane 102 may be applied as a solution 105 to a substrate surface 106 known to those skilled in the art, such as a quench drum, air roller, porous surface, etc., to form the PBI membrane 102. In a bath containing a mixture of phosphoric acid and water that helps complete the sol-gel process, and additionally, removing the phosphoric acid and replacing it with water. An additional step of immersing the casting solution and substrate in a water bath may be added. Thus, the methods of the present disclosure may be adapted for continuous assembly processes of either preformed or freshly formed PBI membranes 102, all under the direction of a controller 108. Drying gas, represented by arrow A, may be applied to the top surface 110 and / or bottom surface 112 of the PBI membrane throughout the process 100. Additionally, serpentine rolls 114 may be used to help tension the PBI membrane 102 as it passes along the continuous formation process 100, as well as to allow for further drying. After the PBI membrane 102 is tensioned and dried, it may be further processed 116 by cutting, winding, etc., as known to those skilled in the art for processing the PBI membrane 102.
[0134] This disclosure offers many benefits to the PBI industry. First, no organic solvents are used in the formation process. Second, this opens the door to PBI polymers that have received little attention in the past precisely because they could not be dissolved in organic solvents. This method allows a wider variety of chemicals to be used.
[0135] Furthermore, the methods of the present disclosure can be used to form films having thicknesses of 5 to 150 microns, more preferably 5 to 100 microns, and even more preferably 10 to 50 microns.
[0136] Although the subject matter of the present invention has been described in detail with respect to specific embodiments and methods thereof, it is understood that those skilled in the art can easily obtain modifications, variations, and equivalents to such embodiments upon understanding the above content. Therefore, the scope of the present disclosure is exemplary and not limiting, and the present disclosure does not exclude the inclusion of modifications, variations, and / or additions to the subject matter of the present invention that would be readily apparent to those skilled in the art using the teachings disclosed herein.
Claims
1. A dried PBI film having a breaking stress of 25 MPa or more.
2. PBI is a repeating unit of: [chemical 1-1] [Case 1-2] [Case 1-3] wherein n and m are each independently 1 or greater.
3. VOSO 4 Transmittance is 2.6 x 10 -9 cm 2 / s ~ 4.89 x 10 -7 cm 2 3. The dried PBI film of claim 1, wherein the viscosity is 100 / s.
4. The dried PBI film of any one of claims 1 to 3, which is crosslinked.
5. 13. A redox flow battery comprising the dry PBI film of claim 1 imbibed with a supporting electrolyte.
6. 6. The redox flow battery of claim 5, wherein the supporting electrolyte comprises sulfuric acid.
7. The redox flow battery of claim 5 or 6, wherein the supporting electrolyte is present at a concentration of 0.1 M to 25 M.
8. The redox flow battery according to any one of claims 5 to 7, which is a vanadium redox flow battery.
9. The PBI film has a current density of 100 mA / cm 2 ~450mA / cm 2 The redox flow battery according to any one of claims 5 to 8, which exhibits a coulombic efficiency of 98% or more under a battery cycle current density of 1000 mAh or more.
Citation Information
Patent Citations
Polybenzimidazole coated metal part
JP1996142262A
A polymer composition, a polymer film containing this polymer composition, a method for producing the same, and a fuel cell containing this film.
JP2011516619A
Application of aromatic polymer ion exchange membranes and their composite membranes to acidic electrolyte flow energy storage batteries
JP2013507742A
Mechanically stable polyazole
JP2014500567A