Granulation binder, active material granules using the same, and method for manufacturing active material granules

A silicate or phosphate-based skeleton forming agent addresses the limitations of conventional binders by creating a robust, heat-resistant electrode structure, improving cycle life and safety in non-aqueous electrolyte secondary batteries, especially with alloy-based active materials.

JP2024164034AActive Publication Date: 2024-11-26ATTACCATO LIMITED LIABILITY COMPANY
View PDF 21 Cites 0 Cited by

Patent Information

Application Number
JP2024124674
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26
Estimated Expiration
2036-10-14

AI Technical Summary

Technical Problem

Conventional organic binders for non-aqueous electrolyte secondary batteries face issues such as swelling in high-temperature electrolytes, low thermal conductivity, flammability, and poor adhesion, leading to reduced safety and performance, especially when used with alloy-based active materials that undergo significant volume changes during charging and discharging.

Method used

Employing a skeleton forming agent containing silicate or phosphate with siloxane or aluminophosphate bonds, which forms a strong, heat-resistant skeleton in the electrode, enhancing mechanical stability and cycle life characteristics without using the binder as a traditional adhesive.

Benefits of technology

The solution provides electrodes with improved heat resistance, high strength, and extended cycle life, while reducing the risk of cracking and peeling, even with high-conductivity active materials, thereby enhancing battery safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164034000001_ABST
    Figure 2024164034000001_ABST
Patent Text Reader

Abstract

To provide an electrode having excellent cycle life characteristics.SOLUTION: An electrode for a non-aqueous electrolyte secondary battery includes a skeleton-forming agent including a silicate or a phosphate having a siloxane bond as a component, present on the surface of an active material layer and inside the active material layer, and the skeleton of the active material layer is formed by the skeleton-forming agent.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode for a non-aqueous electrolyte secondary battery. [Background technology]

[0002] Secondary batteries are now used in a wide range of applications, from electronic devices to automobiles and large-scale power storage systems, and the market is expected to grow to more than 10 trillion yen. In particular, information and communication devices such as smartphones and tablet terminals have become extremely popular, with their penetration rate exceeding 30% worldwide.

[0003] In addition, the range of applications of secondary batteries is expanding to include power sources for next-generation automobiles, such as electric vehicles (EVs) and plug-in hybrid vehicles (PHEVs). Furthermore, since the Great East Japan Earthquake in 2011, secondary batteries have been used for home backup power sources, natural energy storage, load leveling, and other purposes, and the uses of secondary batteries are expanding. In this way, secondary batteries are also indispensable in the introduction of energy-saving and new energy technologies.

[0004] Traditionally, alkaline secondary batteries such as nickel-cadmium batteries and nickel-hydrogen batteries have been the mainstream of secondary batteries, but the use of non-aqueous electrolyte secondary batteries, especially lithium secondary batteries (lithium ion batteries), is increasing due to their features of small size, light weight, high voltage, and no memory effect. A non-aqueous electrolyte secondary battery is composed of a positive electrode, a negative electrode, a separator, an electrolytic solution or electrolyte, and a battery case (storage case).

[0005] Electrodes such as positive and negative electrodes are composed of an active material, a conductive assistant, an organic polymer binder, and a current collector. In general, electrodes are manufactured by mixing the active material, the conductive assistant, and the organic binder in a solvent to form a slurry, coating the slurry on a current collector, drying it, and rolling it with a roll press or the like.

[0006] The electrode is rolled after drying in order to shrink the volume of the active material layer of the electrode, i.e., the coating layer consisting of the active material, conductive additive, and binder, thereby increasing the contact area with the conductive additive and current collector, thereby firmly establishing an electronic conductive network in the active material layer and improving electronic conductivity.

[0007] Binders are used to bind active materials together, active materials and conductive additives, active materials and current collectors, conductive additives and current collectors, etc. Binders can be broadly divided into "solution type" binders that are dissolved in a solvent and used in liquid form, "dispersion type (emulsion / latex type)" binders that are used by dispersing solids in a solvent, and "reactive type" binders that are used by reacting binder precursors with heat or light.

[0008] Binders can also be divided into water-based and organic solvent-based binders depending on the type of solvent. For example, polyvinylidene fluoride (PVdF) is a soluble binder, and organic solvents such as N-methyl-2-pyrrolidone (NMP) are used when making electrode slurry. Styrene butadiene rubber (SBR) is a dispersed binder, and SBR fine particles are dispersed in water for use. Polyimide (PI) is a reactive binder, and a PI precursor is dissolved or dispersed in a solvent such as NMP and heated to promote imidization and crosslinking reactions, resulting in a tough PI.

[0009] Although it depends on the molecular weight and substituents of the binder, soluble binders include polyvinylidene fluoride (PVdF) and ethylene vinyl acetate (EVA). Dispersed binders include styrene butadiene rubber (SBR), polytetrafluoroethylene (PTFE), urethane rubber, polypropylene (PP), polyethylene (PE), polyvinyl acetate (PVAc), and nitrocellulose. Reactive binders include polyimide (PI), polyamide (PA), polyamideimide (PAI), polybenzimidazole (PBI), and polybenzoxazole (PBO).

[0010] In addition, organic solvent binders such as N-methyl-2-pyrrolidone (NMP) are considered to have a negative impact on the environment, and therefore must be recovered when drying the electrodes, which increases the cost of electrode production. In addition, organic solvent binders swell in high-temperature electrolytes and increase electrode resistance, making them difficult to use in high-temperature environments.

[0011] Water-based soluble binders are inferior in oxidation resistance or reduction resistance, and many of them are gradually decomposed by repeated charging and discharging, so sufficient life characteristics cannot be obtained. In addition, they lack output characteristics due to low ionic conductivity. Dispersion-type binders have the advantage that water can be used as a solvent, but the dispersion stability is easily impaired by the degree of acidity or alkalinity (pH), water concentration, or environmental temperature, and they are prone to segregation, aggregation, precipitation, etc. during mixing of the electrode slurry. In addition, the binder particles dispersed in water have a particle size of 1 to 800 nm, and when the water is evaporated by drying, the particles fuse together to form a film. This film has no electrical conductivity or ionic conductivity, so even a slight difference in the amount used can have a significant effect on the output characteristics and life characteristics of the battery.

[0012] When the above-mentioned soluble or dispersed binders are combined with active materials that undergo drastic volume changes during charging and discharging, such as sulfur (S), silicon (Si), tin (Sn), and aluminum (Al), stable life characteristics cannot be obtained, and the charge / discharge capacity drops to less than half after just a few cycles.

[0013] On the other hand, reactive binders are excellent in terms of heat resistance, binding properties, and chemical resistance. PI in particular exhibits high heat resistance and binding properties, and can provide stable life characteristics even with active materials that undergo large volume changes. The binder is also less likely to swell even in high-temperature electrolytes.

[0014] According to Non-Patent Document 1, by combining PI with a high-strength current collector, deterioration of the current collector can be prevented and the life characteristics can be further improved.

[0015] Patent Document 1 discloses that a LiFePO4 / SiO-based lithium-ion secondary battery using PI for the positive and negative electrodes can be stably charged and discharged even at a high temperature of 120°C. On the other hand, when PI is used, it has excellent adhesion to the current collector, so when combined with an active material that has a large volume change, wrinkles and cracks may occur in the current collector during initial charge and discharge. Therefore, it is necessary to use iron foil or stainless steel foil, which has high mechanical strength, for the current collector.

[0016] Other than the above organic binders, there have been few reports in the field of non-aqueous electrolyte secondary batteries, but Patent Documents 2 to 4 disclose techniques using inorganic binders in secondary battery electrodes. Patent Document 2 proposes an electrode mixture for non-aqueous electrolyte secondary batteries, an electrode, and a non-aqueous electrolyte secondary battery that contain an amorphous carbon material containing an inorganic binder, a conductive agent, a binder, and a solvent, and have a viscosity in the range of 2000 mPa·s to 10000 mPa·s. It is also shown that the inclusion of an inorganic binder may suppress the decomposition reaction of the binder.

[0017] A physically and chemically stable lithium ion battery is provided by using an inorganic binder in Patent Documents 3 and 4. Meanwhile, as described above, an electrode generally comprises an active material layer (a layer made of an active material, a conductive assistant, and a binder) and a current collector, but there are also cases where a layer different from the active material layer is provided on the active material layer.

[0018] For example, Patent Document 5 proposes a non-aqueous secondary battery using an electrode sheet having a layer mainly made of a metal or semi-metal oxide and at least one auxiliary layer containing water-insoluble particles. The auxiliary layer provided on the electrode sheet is composed of water-insoluble conductive particles and a binder, and may further contain particles that are substantially non-conductive. The particles that are substantially non-conductive are oxides, and oxides containing compounds that are soluble in both acidic and alkaline conditions are preferred. It is noted that the binder used in the auxiliary layer can be the same as the binder used in forming the electrode mixture.

[0019] Such secondary batteries are widely used in various shapes such as cylindrical, square, laminated, etc. For batteries with a relatively small capacity, cylindrical types are used because of their pressure resistance and ease of sealing, while for batteries with a relatively large capacity, square types are used because of their ease of handling.

[0020] In terms of the electrode structure of secondary batteries, they are roughly divided into two types: stacked type and wound type. That is, in stacked type batteries, electrodes in which positive and negative electrodes are alternately stacked with a separator between them are housed in a battery case. Most stacked type batteries have a rectangular battery case. On the other hand, in wound type batteries, the positive and negative electrodes are housed in a battery case in a spirally wound state with a separator between them. Wound type battery cases are available in cylindrical and rectangular shapes. [Prior art documents] [Patent documents]

[0021] [Patent Document 1] Patent 5728721 [Patent Document 2] Patent 5293020 [Patent Document 3] JP 11-144736 [Patent Document 4] Patent Publication No. 10-523411 [Patent Document 5] International Publication No. 1996 / 027910 [Non-patent literature]

[0022] [Non-Patent Document 1] Takashi Mukai et al., Development of Lithium-ion Battery Active Materials and Electrode Material Technology, Science & Technology Co., Ltd., pp.269-311(2014), ISBN:978-4-86428-089-1 [Non-Patent Document 2] Masahiro Yanagida et al., Abstracts of the 83rd Electrochemical Society, 1T28, (2016) Summary of the Invention [Problem to be solved by the invention]

[0023] As described above, in Non-Patent Document 1 and Patent Document 1, when a thin copper foil or the like is used for the current collector, wrinkles, cracks, etc. occur, and the electrode is not viable (see FIG. 19). On the other hand, if a high-strength iron foil or stainless steel foil is used for the current collector, wrinkles, cracks, etc. can be made less likely to occur even if the current collector is thin. However, since the current collector has very high strength and excellent toughness, the process of punching out the electrode is difficult, and the active material layer falls off during cutting, and burrs are generated on the cut surface.

[0024] In addition, PI is so resistant to chemicals that it is insoluble in almost all organic solvents. Therefore, to prepare the electrode slurry, a PI precursor such as polyamic acid (polyamide acid) is dissolved in NMP and used, and then heated at 200°C or higher to proceed with an imidization reaction (dehydration cyclization reaction) to obtain PI. After the imidization reaction, a crosslinking reaction occurs by heat treatment at a higher temperature, and PI with high mechanical strength is obtained. From the viewpoint of the electrode life, it is preferable to heat treat the electrode at a high temperature to the extent that the PI is not carbonized. However, heat treatment at 200°C or higher not only reduces the flexibility of the electrode, making it difficult to handle, but also oxidizes the active material and the surface of the current collector, which can cause irreversible capacity. Heat treatment at a high temperature also leads to an increase in power consumption during electrode production.

[0025] Some PI binders are imidized to form PI and dispersed in a solvent, but if one that has already been imidized is used when added to the slurry, the electrode will have poor adhesion strength and poor life characteristics. In addition, many reactive binders, including PI, absorb alkali metal ions during initial charging, but cannot remove them during discharge, which causes irreversible capacity. For example, depending on the molecular structure, PI has an irreversible capacity of 500 to 1000 mAh / g. Therefore, electrodes using reactive binders have low initial charge / discharge efficiency and a large decrease in battery capacity.

[0026] Incidentally, in order to confirm the safety of the battery, a nail penetration test is being conducted. When a nail is inserted into a fully charged battery, heat generation exceeding 600 °C may be observed even in a battery of the nominal capacity 1 Ah class. Non-Patent Document 1 shows that a battery using an Si-based active material is greatly improved in the nail penetration safety of the battery. Further, it has been shown that a battery using an Si-based negative electrode and a heat-resistant nonwoven separator has further improved safety.

[0027] Non-Patent Document 2 has studied this phenomenon, and the results show that when the electronic conductivity of the active material layer of the electrode is high, the heat generation temperature of the battery and the nail at the time of nail penetration becomes high, and when the electronic conductivity of the electrode active material layer is low, the heat generation temperature of the battery and the nail at the time of nail penetration also becomes low. That is, the electronic conductivity of the electrode active material layer greatly contributes to the nail penetration safety of the battery. When the electronic conductivity of the active material layer is high, the current value flowing through the nail increases, and the heat generation amount of the nail and the battery also increases. When the electronic conductivity is low, the current value flowing through the nail decreases, and the heat generation amount per unit time decreases.

[0028] The alloy-based active material improves the electronic conductivity when alloyed with an alkali metal. For example, Si in the discharged state is a semiconductor and has a low electronic conductivity, but Li in the charged state x Si alloy (0 < x ≤ 4.4) is a conductor and has a high electronic conductivity. That is, in the Si-based negative electrode, it is considered that the Si-based active material in the short-circuited portion is delithiated due to an internal short circuit, the electronic conductivity of the electrode rapidly decreases, and the current is interrupted, thereby suppressing the temperature rise of the battery.

[0029] However, in an electrode with a large amount of conductive assistant in the active material layer or an electrode using a material in which a highly conductive material is coated or compounded with the active material, the electronic conductivity of the active material layer becomes high. Even if an Si-based material is used, the above current interruption mechanism hardly functions, and the temperature rise of the battery cannot be sufficiently suppressed. Therefore, in order to design a battery that emphasizes safety, an electrode with a low conductivity of the active material layer must be used. Conversely, in an electrode composition that emphasizes safety, since the electronic conductivity is low, there is a high possibility of obtaining a low-output battery.

[0030] Even in batteries that use electrodes with low electronic conductivity in the active material layer, momentary heat generation during an internal short circuit cannot be eliminated, and if this heat causes the binder to carbonize, the electrode's electronic conductivity will increase and safety will be compromised. Even with organic reactive binders, which have excellent heat resistance, the heat resistance temperature is limited to around 400°C, and if the temperature rise caused by an internal short circuit exceeds the binder's heat resistance temperature, the binder will carbonize, so there is a demand for binders that do not carbonize.

[0031] In addition, it is generally known that active materials with small volume changes have good life characteristics. For example, the charging reaction of Si (Si + 4.4Li + +4.4e - →Li 4.4 The volume of the SiO2 charge reaction (SiO+8.4Li + +8.4e - →Li 4.4 In the case of Li4SiO4 (Si+Li4SiO4), excluding the volume change due to the initial Li4SiO4 formation, the volume change is about 2.7 times larger, so SiO shows superior life characteristics compared to Si.

[0032] As another example, in a negative electrode that uses a mixture of Si and alumina, as the Si ratio decreases, the capacity decreases compared to a pure Si negative electrode, but the life characteristics tend to improve. Alumina is inactive with Li and does not contribute to the charge / discharge reaction, but it acts as a buffer for the volume change of Si, making it possible to reduce the volume change of the entire electrode.

[0033] For example, the charging reaction of a Si negative electrode, as shown in Equation 1 below, causes a volume change of about four times compared to before charging, and the stress on the electrode binder also increases by about four times. Si+4.4Li + +4.4e - →Li 4.4 Si (eq. 1)

[0034] If an anode is made by adding an equal molar amount of Al2O3 to Si, Al2O3 is inactive with Li, so from a macroscopic point of view, the charging reaction will be as shown in formula (2). With such an electrode, the volume change of the electrode will be half that of a pure Si electrode, and the stress on the electrode binder will also be half. Therefore, it is expected that as the Si ratio decreases, the capacity of an electrode that mixes a material with smaller volume change than Si decreases, but the life characteristics will tend to improve. 0.5Si+0.5Al2O3+2.2Li + +2.2e - →0.5Li 4.4 Si+0.5Al2O3 (eq. 2)

[0035] However, in actual life characteristics, although there is a slight improvement in life, the degradation rate of Si in each cycle does not change much. This is because, from a microscopic perspective, the volume change of the Si particles themselves is about four times, so the stress on the electrode binder remains the same as in formula 1, and ultimately, stress is concentrated in the bonding parts. In particular, in electrodes in which electrode materials or electrode materials and current collectors are point-bonded with a binder, the bonding parts receive concentrated stress due to the volume change, losing their bonding ability and easily destroying the conductive network of the electrode.

[0036] On the other hand, if the binder is surface-bonded, the bonding part distributes the stress evenly, so the conductive network is less likely to be destroyed, but the binder inhibits the movement of ions, so the output characteristics decrease. Although it depends on the type of binder, point bonding is more likely to occur when the amount of binder is small, and surface bonding is more likely to occur when the amount of binder is large.

[0037] Among the many binders available, the only binders that can stably charge and discharge alloy-based active materials are reactive binders such as PI. However, reactive binders require the use of organic solvents during slurry production and a heat treatment process at 200°C or higher, and the resulting electrodes have a large irreversible capacity derived from the binder, and there are also limitations in terms of safety.

[0038] In addition, reactive binders alone are not sufficient to provide sufficient life characteristics, and it is necessary to combine them with SiO or high-strength current collector foil. Organic materials have low melting points, are easily soluble in organic solvents, and are flammable, while inorganic materials have high melting points, are difficult to dissolve in organic solvents, are non-flammable, and have high thermal conductivity. Therefore, if a binder composed of inorganic materials can be used, there is a high possibility that an electrode with high heat resistance, excellent electrolyte resistance, and heat dissipation properties can be obtained.

[0039] However, most inorganic binders have not been suitable for use in electrodes of non-aqueous electrolyte secondary batteries. Inorganic binders can be broadly divided into four types: silicate-based, phosphate-based, sol-based, and cement-based. Among these, the present inventors have focused on silicate-based and phosphate-based binders, particularly alkali metal silicate-based binders, which have strong binding properties against metals, oxides, and carbon, and heat resistance of 1000°C or higher.

[0040] The silicate-based binder may be an alkali metal silicate, a silicate of a guanidine compound, or a silicate of an ammonium compound. A silicate-based inorganic binder is a compound whose molecular skeleton is mainly composed of silicon (Si) and oxygen (O) with a siloxane bond (-Si-O-Si-), and is different from an organic binder whose skeleton is mainly composed of carbon (see Figure 21a).

[0041] In addition, some of the Si sites in the siloxane bond may be substituted with transition metal elements such as Al, Zr, Ti, Mg, Mo, Sr, Ca, Zn, Ba, B, W, Ta, Ce, Hf, and Y.

[0042] There are many types of silicates, including polysilicates such as orthosilicate (A4SiO4), metasilicate (A2SiO3), pyrosilicate (A6Si2O7), disilicate (A2Si2O5), and tetrasilicate (A2Si4O9), as well as A2Si2O5, A2Si3O7, and A2Si4O9, which may be hydrates. In terms of their structure, they can be broadly classified into crystalline silicates and non-crystalline silicates (A=alkali metal element, guanidine compound, or ammonium compound). As the proportion of A in the silicate increases, the melting point of such silicates tends to decrease, and at the same time, they become soluble in water.

[0043] In industry, the proportion of A in silicates can be continuously changed, and any salt can be adjusted. The general molecular formula of silicates is expressed in the form A2O·nSiO2.

[0044] Due to this difference in molecular structure, organic binders exhibit higher heat resistance and oxidation resistance than organic binders, and are used in a variety of fields, including fire retardants, waterproofing agents, bleaches, detergents, soaps, coating agents, sealants, and civil engineering ground strengthening agents. However, there have been few reports of their use in non-aqueous electrolyte secondary batteries.

[0045] The phosphate-based salt may be, in addition to aluminum phosphate, magnesium phosphate, or calcium phosphate.

[0046] When phosphate-based inorganic binders are heated, water is removed from the hydroxyl groups, forming covalent bonds between phosphorus and oxygen, and a dehydration condensation reaction occurs. This dehydration condensation reaction can occur at up to six sites per molecule centered on the transition metal (M), resulting in a three-dimensional polymerized transition metal phosphate. In other words, it is a compound whose main molecular skeleton is phosphorus (P), oxygen (O), and transition metal (M) with aluminophosphate bonds, and is different from organic binders which have a skeleton mainly made of carbon (see Figure 21b).

[0047] In addition, a portion of the transition metal sites may be substituted with a transition metal element such as Al, Mg, Ca, Cu, Fe, Ba, Ti, Mn, Mo, Mg, Si, Sr, Ca, Zn, Ba, B, W, Ta, Ce, Hf, or Y.

[0048] Specifically, aluminum phosphates include monobasic aluminum phosphate (Al(H2PO4)3), dibasic aluminum phosphate (Al2(H2PO4)3), and dibasic aluminum metaphosphate (Al(PO3)3). Magnesium phosphates include monobasic magnesium phosphate (Mg(H2PO4)3), dibasic magnesium phosphate (MgHPO4), and dibasic magnesium metaphosphate (Mg(PO3)2). Calcium phosphates include monobasic calcium phosphate (Ca(H2PO4)3), dibasic calcium phosphate (CaHPO4), tribasic calcium phosphate (Ca3(H2PO4)2), and dibasic calcium metaphosphate (Ca(PO3)2), which may be hydrates. In terms of their structure, they can be broadly classified into crystalline phosphates and noncrystalline phosphates.

[0049] In industry, the ratio of M and P in phosphate can be continuously changed, and any salt can be adjusted. The general molecular formula of phosphate is M nH. x It is expressed in the form PO4 (M = Al, Mg, Ca).

[0050] A sol-based material is a colloidal solution in which oxide particles are dispersed in water. The particle size of the oxide is 10 nm or more and 200 nm or less, and hydroxyl groups are present on the surface. For example, when the oxide is SiO2, a siloxane bond is formed by dehydration condensation, but since this siloxane bond is formed inside the oxide particle, the binding strength is weaker than that of silicic acid salts. In addition, pH control is important, and there is a problem that it is difficult to maintain a stable sol state. In the present invention, a sol-based material is not preferably used as a skeleton forming agent because it is difficult to penetrate into the active material layer.

[0051] Patent Document 2 shows that the decomposition reaction of the binder can be suppressed by including an inorganic binder in the binder. This is because carbon materials (graphite, soft carbon, hard carbon, etc.) have a low solubility in water at 0.1V (vs. Li + Since the charge / discharge plateau potential is near 0.05V / Li and the electrode has a strong reducing power, it is believed that the decomposition reaction is suppressed by the inorganic binder, which has excellent resistance to reduction.

[0052] However, since the alloy-based material has a higher charge / discharge plateau potential than the carbon material and a weaker reducing power than the carbon-based electrode, the binder decomposition reaction does not occur much, so the life characteristics of the alloy-based electrode are not significantly improved even if the binder decomposition reaction is suppressed.

[0053] Patent Document 2 also indicates that the inorganic binder contains inorganic particles, and that the particle size of the inorganic particles is preferably 1 nm to 100 nm, more preferably 1 nm to 50 nm, and even more preferably 1 nm to 10 nm. It also indicates that by setting the particle size in this range, a binder having superior dispersibility and adhesive strength of the electrode mixture can be obtained.

[0054] Inorganic particles have a larger specific gravity than carbon materials, so as the particle size of inorganic particles increases, the particle settling speed increases, and dispersibility and adhesive strength decrease. Therefore, it is effective to use particles of 100 nm or less. However, when drying after electrode coating, there is a problem that particles of 100 nm or less prevent the escape of evaporated moisture, causing the coating film to foam, reducing the binding with the current collector, and making it difficult to obtain a uniform electrode. In addition, such electrodes are brittle because they do not contain an organic binder with excellent flexibility, and are damaged when the electrode is bent. Therefore, they are not suitable for wound-type batteries.

[0055] On the other hand, alloy-based active materials are known to have higher capacities than conventional carbon-based active materials. For example, Si has a high electric capacity of 2800 to 4000 mAh / g, SiO has a high electric capacity of 1300 to 2000 mAh / g, Sn has a high electric capacity of 700 to 1000 mAh / g, and S has a high electric capacity of 800 to 1500 mAh / g. Therefore, even a small error can cause a large variation in the electrode capacity, which can deteriorate the life characteristics and output characteristics. In addition, the viscosity of the electrode slurry is difficult to control because it changes dramatically depending on the amount of solvent used.

[0056] Patent Documents 3 and 4 provide physically and chemically stable lithium ion batteries using inorganic binders. Examples of electrodes include a graphite negative electrode (graphite anode) and a LiCoO2 positive electrode (LiCoO2 cathode). The graphite negative electrode is composed of 1.0 g of lithium hydroxide, 23.4 g of inorganic binder (lithium polysilicate), and 45.0 g of graphite powder.

[0057] Therefore, if the total solid content of the active material, conductive assistant, and binder is taken as 100 mass %, the active material is 64.8 mass % and the inorganic binder is 33.7 mass %.

[0058] The LiCoO2 positive electrode was composed of 1.0 g of lithium hydroxide, 1.9 g of graphite powder, 2.9 g of C-100 carbon black, 24 g of inorganic binder (lithium polysilicate), and 85.6 g of graphite powder.

[0059] Therefore, if the total solid content of the active material, conductive assistant, and binder is 100 mass%, the active material is 74.2 mass% and the inorganic binder is 20.8 mass%. Note that Patent Documents 3 and 4 do not mention inorganic particles in the inorganic binder, and no inorganic particles are included in the examples.

[0060] The above-mentioned Patent Documents 2 to 4 all aim to improve the decomposition reaction of the binder and swelling caused by the electrolyte, which were difficult to achieve with conventional organic binders. By using an alloy material such as Si-based or Sn-based as the active material and a binder that does not easily swell in the electrolyte, it is possible to expand the operating temperature of the electrode and achieve a high capacity.

[0061] However, because silicate-based binders are strongly alkaline and phosphate-based binders are strongly acidic, the alloy-based active material dissolves during electrode slurry preparation, generating hydrogen gas and foaming the slurry. In particular, the temperature rises during electrode drying, increasing the amount of hydrogen gas generated, making it difficult to produce uniform electrodes. In addition, if a current collector that is not resistant to alkali or acid is used, the current collector will deteriorate.

[0062] For example, when the Si active material comes into contact with an alkali metal silicate, the reaction - +H2O→SiO3 - The reaction +2H2↑ occurs. Therefore, the only choice is an active material that is resistant to alkali or acid, that is, a carbon-based material. In addition, the binder, which is one of the components of the electrode, is used to bind the active material to the active material, the active material to the conductive assistant, the active material to the current collector, and the conductive assistant to the current collector. However, since the current battery uses an organic binder such as PVdF or SBR, its thermal conductivity is low compared to inorganic materials such as the active material, the conductive assistant, and the current collector, and it is difficult to transfer heat. In addition, since the specific gravity of inorganic binders such as silicate-based and phosphate-based binders is large compared to conventional organic binders, the amount of binder used when preparing the electrode must be 20% by mass or more, assuming that the total solid content of the active material, the conductive assistant, and the binder is 100% by mass, in order to show sufficient binding strength. In particular, when a material with a large volume change is used, 30 to 70% by mass is required. As a result, the proportion of active material in the electrode decreases, and the electrode energy density decreases.

[0063] As described above, the inventors of the present application initially conducted extensive research into the application of silicate-based or phosphate-based binders, but found that when silicate-based or phosphate-based binders are used as binders, many problems arise under the current circumstances, and they are not viable as practical electrodes. Therefore, the inventors conducted extensive research into the application of silicate-based or phosphate-based binders to electrodes, rather than as binders, and came up with the present invention. The present invention can solve the above-mentioned conventional problems as well as problems newly discovered by the inventors. [Means for solving the problem]

[0064] The skeleton-forming agent according to the present invention is used in electrodes of non-aqueous electrolyte secondary batteries, and is characterized in that it contains a silicate having a siloxane bond as a component, or a phosphate having an aluminophosphate bond as a component. According to this configuration, by using a skeleton-forming agent containing a silicate or a phosphate in an electrode, it is possible to obtain an electrode that has excellent heat resistance, high strength, and improved cycle life characteristics.

[0065] Furthermore, this framework-forming agent and the silicate have a crystalline or amorphous structure represented by the general formula A2O·nSiO2, where A is at least one of Li, Na, K, a triethanolammonium group, a tetramethanolammonium group, a tetraethanolammonium group, and a granidine group, and n is 0.5 or more and 5.0 or less.

[0066] Preferably, in the skeletal forming agent, A in the general formula is Li or Na, and n is 1.6 to 3.9, more preferably 2.0 to 3.5. A is preferably Na from the viewpoint of excellent mechanical strength, binding, and abrasion resistance of the skeletal formation. In addition, Li is excellent in input / output characteristics of the battery because it can obtain a skeletal forming body with high ion conductivity. However, even if it is Na, if the number n of SiO2 exceeds 5.0, the binding with the active material layer and the separator is poor, and peeling and cracking are significantly likely to occur due to external factors such as volume change of the electrode during charging and discharging and nail penetration tests. In addition, the viscosity becomes too low, and the dispersion stability with ceramics described later decreases.

[0067] Conversely, if n is less than 0.5, the skeleton forming agent will have high viscosity, making it difficult for the skeleton forming agent to penetrate into or be applied to the electrode active material layer or the separator, and will generate a large amount of heat when kneaded with the ceramics.

[0068] The silicate is preferably amorphous. Amorphous silicate does not crack in a specific direction like crystals, improving the life characteristics of the electrode. In addition, resistance to hydrofluoric acid is improved, making it difficult for the electrode to collapse due to hydrofluoric acid.

[0069] Amorphous solids usually consist of disordered molecular arrangements and do not possess a distinct crystal lattice. Amorphous solids are also more soluble than crystalline forms and do not have a definite melting point. Thus, the absence of distinct peaks in powder X-ray diffraction (XRD) patterns and the absence of melting endothermic peaks in differential thermal analysis (DTA) and differential scanning calorimetry (DSC) curves indicate amorphous forms.

[0070] That is, amorphous silicates do not show the sharp peaks characteristic of crystalline forms in XRD, but show a typical broad peak, a so-called halo pattern, at diffraction angles (2θ) in the range of 15° to 40° using Cu-Kα radiation. More specifically, they show essentially the same XRD pattern as shown in FIG.

[0071] However, even if a halo pattern is obtained by XRD, it does not necessarily mean that the material is amorphous. However, this only applies under limited conditions where the crystal grains are less than 5 nm, according to the Scherrer equation shown in Equation 3. In other words, if the crystal grains are 5 nm or larger, the diffraction lines will be broad and will not show a pattern similar to that of amorphous materials. D(Å)=0.9λ / (β×cosθ) (Formula 3) (In the formula, D is the size of the crystal grain, λ is the wavelength of the X-ray tube, β is the broadening of the diffraction line due to the size of the crystal grain, and θ is the diffraction angle.)

[0072] In addition, when the amorphous state changes to a crystalline state, a large amount of heat is generated, and by measuring this, it is possible to determine the crystalline state of the silicate. Amorphous silicate can be obtained by heat treating the electrode at a temperature between 80°C and 600°C at a heating rate of 10°C / h or more.

[0073] Preferably, the solid content concentration of the silicate in the skeleton-forming agent is from 0.1% by mass to 30% by mass, more preferably from 0.1% by mass to 15% by mass.

[0074] The skeleton-forming agent further contains a surfactant, and the surfactant is 0.001% by mass or more and 5.0% by mass or less. With this configuration, the skeleton-forming agent has improved lyophilicity to the active material layer, and the skeleton-forming agent penetrates the active material layer uniformly. Thus, a uniform skeleton is formed in the active material layer, and cycle life characteristics are further improved. If the skeleton-forming agent is less than 0.001% by mass, the skeleton-forming agent does not penetrate easily into the active material layer, which contains a large amount of carbon-based materials such as graphite, hard carbon, and conductive additives. If the skeleton-forming agent is more than 5% by mass, a defoaming agent is required, and without the defoaming agent, the surface of the active material layer will foam, making it difficult to form a strong skeleton.

[0075] The skeleton-forming agent further contains alkali-resistant inorganic particles. According to this configuration, when the skeleton-forming agent is applied to an electrode, the inorganic particles are laminated on the surface of the active material layer of the electrode, covering the active material layer with a layer of inorganic particles, and the inorganic particles also penetrate into the active material layer.

[0076] This allows a strong skeleton to be formed in the active material layer, and the occurrence of peeling and cracking during drying can be suppressed. Also, voids are formed between the inorganic particles, resulting in good lyophilicity with the electrolyte. The layer of inorganic particles also results in an electrode with excellent heat resistance, high strength, and excellent wear resistance. The layer of inorganic particles also serves as a separator, making it possible to construct a battery without using a separate separator.

[0077] Preferably, in this skeleton forming agent, when the total solid content including the silicate and the alkali-resistant inorganic particles is taken as 100 mass%, the silicate is 5 mass% or more and 80 mass% or less, the alkali-resistant inorganic particles are 20 mass% or more and 95 mass% or less, and the median diameter (D 50 ) is 0.2 μm or more and 20 μm or less.

[0078] Here, the median diameter (D 50 ) refers to the volumetric particle size in laser diffraction / scattering particle size distribution measurement. Laser diffraction / scattering particle size distribution measurement is a method for measuring particle size by utilizing the phenomenon in which the light intensity distribution of diffracted / scattered light differs depending on the particle size when a laser beam is applied to the particle.

[0079] By including the alkali-resistant inorganic particles in the skeleton-forming agent, the skeleton-forming agent is less likely to foam when dried at high temperatures. If the skeleton-forming agent foams, the binding strength with the active material layer and the separator is reduced, making it difficult to obtain sufficient strength.

[0080] The median diameter (D 50 The reason why the thickness is set to 0.2 μm or more and 20 μm or less is that pores are formed between the inorganic particles, resulting in good lyophilicity with the electrolyte. From the viewpoint of the output characteristics of the battery, the thickness is more preferably 0.25 μm or more and 10 μm or less, and even more preferably 0.3 μm or more and 2 μm or less.

[0081] If the particle size of the inorganic particles is larger than this range, the thixotropy is reduced and the particles tend to show dilatancy, resulting in a decrease in dispersion stability when the inorganic particles are added to the skeleton-forming agent. Conversely, if the particle size is smaller than this range, when a skeleton with a thickness of more than 2 μm is formed, there is no escape route for the water vaporized during drying, causing the coating to foam, decreasing the binding to the current collector, and making it difficult to obtain a uniform electrode.

[0082] The reason why the inorganic particles need to be alkali resistant is that silicates exhibit strong alkalinity (pH 12 or higher). In addition to the alkali resistance, the framework forming agent is preferably inorganic particles that are excellent in resistance to dissolution in an electrolyte.

[0083] Examples of inorganic particles that satisfy such conditions include oxides, hydroxides, nitrides, carbides, carbonates, and sulfates of at least one element selected from the group consisting of Al, Zr, Ti, Si, Mg, Mo, Sr, Ca, Zn, Ba, B, W, Ta, Ce, Hf, and Y. Among these, from the viewpoint of being a material that is less susceptible to oxidative decomposition or reductive decomposition during charging and discharging of a battery and has a small irreversible capacity, it is preferable to contain Al2O3, ZrO2, TiO2, SiO2, CaO, MgO, CeO, Y2O3, AlN, WC, SiC, B4C, BN, TaC, TiC, TiB2, HfB2, Si3N4, TiN, CaCO3, MgSO4, Al2(SO4)3, CaSO4, and ZrSiO4.

[0084] In addition, from the viewpoint of being a material with low irreversible capacity of the battery, it is preferable to contain Al2O3, ZrO2, TiO2, SiO2, MgO, CeO, Y2O3, WC, SiC, B4C, TaC, TiC, Si3N4, TiN, CaCO3, MgSO4, CaSO4, and ZrSiO4. These materials have the effect of suppressing the large volumetric shrinkage of silicates that occurs during drying, and can maintain sufficient strength even when dried at low temperatures.

[0085] Phosphates, on the other hand, have the general formula M nH x It has a crystalline or amorphous structure represented by PO4, where M is at least one of Al, Ca, and Mg, x is 0 or more and 2 or less, and n is 0.5 or more and 5 or less.

[0086] From the viewpoint of excellent mechanical strength, binding property, and abrasion resistance of the skeleton formation, M is preferably Al. From the viewpoint of excellent binding property of the skeleton formation, x is preferably 1 to 2, and more preferably 2. From the viewpoint of excellent mechanical strength, binding property, and abrasion resistance of the skeleton formation, n is preferably 0.5 to 5.0, and more preferably 2.5 to 3.5. As in the case of silicates, phosphates are also preferably amorphous.

[0087] Preferably, the skeleton-forming agent has a solids concentration of the phosphate of 0.1% by mass or more and 30% by mass or less, more preferably 0.1% by mass or more and 15% by mass or less.

[0088] Moreover, it is preferable that the framework forming agent contains a surfactant, and the content of the surfactant is 0.001% by mass or more and 5.0% by mass or less.

[0089] In addition, the skeletal forming agent preferably further contains acid-resistant inorganic particles. According to this configuration, when the skeletal forming agent is applied to an electrode, the inorganic particles are laminated on the surface of the active material layer of the electrode, the active material layer is covered with a layer of inorganic particles, and the inorganic particles also penetrate into the active material layer.

[0090] This allows a strong skeleton to be formed in the active material layer, and the occurrence of peeling and cracking during drying can be suppressed. Also, voids are formed between the inorganic particles, resulting in good lyophilicity with the electrolyte. The layer of inorganic particles also results in an electrode with excellent heat resistance, high strength, and excellent wear resistance. The layer of inorganic particles also serves as a separator, making it possible to construct a battery without using a separate separator.

[0091] Preferably, in this skeleton forming agent, when the total solid content including the phosphate and the acid-resistant inorganic particles is taken as 100 mass%, the phosphate is 5 mass% or more and 80 mass% or less, the acid-resistant inorganic particles are 20 mass% or more and 95 mass% or less, and the median diameter (D 50 ) is 0.2 μm or more and 20 μm or less.

[0092] By including the acid-resistant inorganic particles in the skeleton-forming agent, the skeleton-forming agent is less likely to foam when dried at high temperatures. If the skeleton-forming agent foams, the binding strength with the active material layer and the separator is reduced, making it difficult to obtain sufficient strength. The median diameter (D 50 ) is preferably 0.2 μm or more and 20 μm or less.

[0093] The reason why the inorganic particles need to be acid resistant is that phosphates exhibit strong acidity (pH 1 to 2). In addition, it is desirable for the framework forming agent to be inorganic particles that are excellent in resistance to dissolution in an electrolyte in addition to the acid resistance.

[0094] Examples of inorganic particles that satisfy such conditions include oxides, hydroxides, nitrides, carbides, carbonates, and sulfates of at least one element selected from the group consisting of Al, Zr, Ti, Si, Mo, Sr, Ba, B, W, Ta, Ce, Hf, and Y. Among these, from the viewpoint of being a material that is less susceptible to oxidative or reductive decomposition during charging and discharging of the battery and has a small irreversible capacity, it is preferable to contain Al2O3, ZrO2, TiO2, SiO2, CeO, Y2O3, WC, SiC, B4C, BN, TaC, TiC, TiB2, HfB2, Si3N4, TiN, and ZrSiO4.

[0095] In addition, from the viewpoint of being a material with low irreversible capacity of the battery, it is preferable to contain Al2O3, ZrO2, TiO2, SiO2, CeO, Y2O3, WC, SiC, B4C, BN, TaC, TiC, Si3N4, TiN, and ZrSiO4. These materials have the effect of suppressing the large volumetric shrinkage of phosphate that occurs during drying, and can maintain sufficient strength even when dried at low temperatures.

[0096] Of the silicate-based and phosphate-based batteries, the silicate-based batteries are preferred from the standpoints of battery life, input / output characteristics, irreversible capacity, resistance to moisture absorption, heat resistance, and the like.

[0097] The electrode according to the present invention is an electrode for a non-aqueous electrolyte secondary battery, characterized in that the above-mentioned skeletal former is present at least on the surface of the active material layer. According to this configuration, the skeletal former containing silicate or phosphate constitutes the skeleton of the electrode, resulting in an electrode with excellent heat resistance, high strength, and improved cycle life characteristics. Furthermore, while an electrode cannot be formed using a binder containing silicate or phosphate, by applying the skeletal former to the surface of the active material layer, an electrode with excellent cycle life characteristics can be obtained.

[0098] Here, the nonaqueous electrolyte secondary battery is a secondary battery that uses an electrolyte that does not contain water as a main component, and examples of such batteries include lithium secondary batteries (lithium ion batteries), sodium batteries (sodium ion batteries), potassium batteries (potassium ion batteries), etc. The electrodes are not particularly limited as long as they are electrodes used in nonaqueous electrolyte secondary batteries, and the material and shape of the electrodes are also not particularly limited.

[0099] In addition, the electrodes include negative and positive electrodes. First, regarding the negative electrode, the negative electrode active material used in the negative electrode is not particularly limited as long as it is a material capable of reversibly absorbing and releasing alkali metal ions (lithium ions, sodium ions, potassium ions, etc.). For example, at least one element selected from the group consisting of Li, Na, K, C, Mg, Al, Si, P, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Y, Zr, Nb, Mo, Pd, Ag, Cd, In, Sn, Sb, W, Pb, and Bi, or an alloy, composite, oxide, chalcogenide, or halide using these elements may be used.

[0100] The discharge plateau region is 0 to 1 V (vs. Li + From the viewpoint of being observable within the range of 1:1 / Li), at least one element selected from the group consisting of Li, Na, K, C, Mg, Al, Si, Ti, Zn, Ge, Fe, Mn, Ag, Cu, In, Sn, and Pb, or an allotrope, alloy, or oxide using these elements is preferred.

[0101] Furthermore, from the viewpoint of energy density, preferred elements are Al, Si, Zn, Ge, Ag, Sn, etc., and preferred alloys are combinations of Si-Al, Al-Zn, Si-Mg, Si-La, Al-Ge, Si-Ge, Si-Ag, Si-Sn, Si-Ti, Si-Y, Si-Cr, Si-Ni, Si-Zr, Si-V, Si-Nb, Si-Mo, Zn-Sn, Ge-Ag, Ge-Sn, Ge-Sb, Ag-Sn, Ag-Ge, Sn-Sb, etc., and preferred oxides are Fe2O3, CuO, MnO2, NiO, Li4Ti5O 12 , H2Ti 12 O 25 , Na2Ti3O7, etc. are preferred. The alloy may be a complete solid solution type alloy, a eutectic alloy, a hypoeutectic alloy, a hypereutectic alloy, or a peritectic alloy. The surface of the active material particles may be coated with a material or ceramics having excellent electronic conductivity. Two or more of these materials capable of reversibly absorbing and releasing lithium may be used.

[0102] The shape of the active material particles is not particularly limited, and may be spherical, elliptical, faceted, strip-like, fibrous, flake-like, doughnut-like, hollow, etc. The material capable of reversibly absorbing and releasing alkali metal ions (lithium ions, sodium ions, potassium ions) is preferably a substance capable of absorbing and releasing alkali metal ions during the initial charging process and a compound that decomposes into a solid electrolyte.

[0103] The solid electrolyte is not particularly limited as long as it is a substance having ion conductivity, but is preferably a solid electrolyte represented by LiαXβYγ, where 0<α≦4, 0≦β≦2, and 0≦γ≦5. The solid electrolyte can also serve as a buffer material capable of reversibly absorbing and releasing alkali metal ions.

[0104] X is, for example, one or more of Si, Ti, Mg, Ca, Al, V, Ge, Zr, Mo, and Ni, and Y is one or more of O, S, F, Cl, Br, I, P, B2O3, C2O4, CO3, PO4, S, CF3SO3, and SO3. More specifically, for example, LiF, LiCl, LiBr, LiI, Li3N, LiPON, Li2C2O4, Li2CO3, LiAlCl4, Li2O, Li2S, LiSO4, Li2SO4, Li3PO4, Li3VO4, Li4GeO4, Li2Si2O5, Li2SiO3, Li 4SiO4, Li4ZrO4, LiMoO4, LiAlF4, Li3Ni2, LiBF4, LiCF3SO3, NaF, NaCl, NaBr, NaI, Na3N, NaPON, Na2C2O4, Na2CO3, NaAlCl4, Na2O, Na2S, NaSO4, Na2SO4, Na3P O4, Na3VO4, Na4GeO4, Na2Si2O5, Na2SiO3, Na4SiO4, Na4ZrO4, NaMoO4, NaAlF4, Na3Ni2, NaBF4, NaCF3SO3, KF, KCl, KBr, KI, K3N, KPON, K2C2O4, K2CO3, KAlCl4, K2O, K2S, KSO4, K2SO4, K3PO4, K3VO4, K4GeO4, K2Si2O5, K2SiO3, K4SiO4, K4ZrO4, KMoO4, KAlF4, K3Ni2, KBF4, KCF3SO3, and the like. One or more of these can be used.

[0105] Examples of the substance capable of absorbing and releasing alkali metal ions and the compound decomposing into a solid electrolyte include SiO, GeO, GeS, GeS2, SnO, SnO2, SnC2O4, SnO-P2O5, SnO-B2O3, SnS, SnS2, Sb2S3, SnF2, SnCl2, SnI2, SnI4, etc., and two or more of these may be used. However, it is preferable to pre-dope the substance capable of absorbing and releasing alkali metal ions and the compound decomposing into a solid electrolyte before assembling the battery, since the battery capacity will be extremely reduced if the pre-doping is not performed in advance.

[0106] As described in a patent document (JP 2015-088437 A) and a non-patent document ("Collection of Measurement and Analysis Data of Lithium Secondary Battery Components," Chapter 3, Section 30, pp. 200-205, Technical Information Association), the pre-doping method can be performed using known methods such as electrochemical methods, alkali metal attachment methods, and mechanical methods. Although the reason is unclear, in the present invention, when the electrode to be subjected to skeleton formation is made of Si, a Si alloy, a Si composite, a Si oxide, or a mixture containing at least one of these, a particularly significant cycle life improvement effect is exhibited.

[0107] Regarding the particle size of the active material, when an active material powder with a small particle size is used, the collapse of the particles is reduced, and the life characteristics of the electrode tend to be improved. In addition, the specific surface area tends to increase, and the output characteristics tend to be improved. For example, according to a non-patent document (Latest Technology Trends of Rare Metal-Free Secondary Batteries, Chapter 3, Section 1, Item 4, pp. 125-135, CMC Publishing, 2013), it is described that the initial discharge capacity increases and the cycle life is also improved when the particle size of the active material becomes smaller, and it is understood that the particle size of the active material is correlated with the initial charge / discharge efficiency and the cycle life.

[0108] However, nano-order active materials are difficult to handle, so they are preferably granulated before use. For example, Patent No. 5525003 shows a negative electrode using nano-granules that use one or more granulation binders selected from polyimide, polybenzimidazole, styrene butadiene rubber, polyvinylidene fluoride, carboxymethyl cellulose, and polyacrylic acid. Granulating the nano-order active material reduces the stress applied to the copper foil due to the expansion and contraction of the negative electrode active material, and prevents the copper foil from deforming.

[0109] On the other hand, it is also conceivable to use the framework forming agent of the present invention as a binder for granulation of the above-mentioned negative electrode active material. It is said that the smaller the particle diameter of an active material, the better its output characteristics and cycle characteristics are. However, powders made of small particles are easily burned and prone to scattering and aggregation, making them difficult to handle. By using this binder for granulation, it is possible to suppress combustion and make handling easier, and, as mentioned above, to mitigate the volumetric change of the active material. In addition, the primary particles of the active material have a median diameter (D 50 The active material particles (secondary particles) after granulation preferably have a median diameter (D 50 ) It is preferable that the thickness is within the range of 1 μm to 100 μm.

[0110] As a method for granulating the active material, known granulation methods can be applied, such as fluidized bed granulation, stirring granulation, rolling granulation, spray drying, extrusion granulation, rolling granulation, and coating granulation. Among these, the spray drying and fluidized bed granulation are particularly preferred.

[0111] In the spray-drying method, for example, a suspension in which an active material is dispersed in a skeleton forming agent is sprayed from above into a greenhouse heated to 50 to 300°C at a rate of 1 to 30 mL / min and an air pressure of 0.01 to 5 MPa to produce aggregated particles, which are then dried to obtain a granulated product.

[0112] In the fluidized bed granulation method, for example, the powder raw materials are placed in a fluidized bed granulation device, and hot air heated to 50 to 300°C is blown in from below to fluidize and mix the powder raw materials (granule precursor). Water in which a skeleton-forming agent has been dissolved is sprayed from a nozzle above into this mixed powder raw material, and the skeleton-forming agent is sprayed uniformly onto the powder surface at 1 to 30 mL / min and an air pressure of 0.01 to 5 MPa to create agglomerated particles, which are then dried to obtain a granule.

[0113] However, when an active material with poor alkali resistance such as Si or Sn is used, there is a high possibility that it will react with the skeletal forming agent to generate hydrogen gas, and will not function as a negative electrode. Therefore, when the skeletal forming agent of the present invention is used, it is believed that the generation of hydrogen gas can be minimized by spraying the skeletal forming agent onto secondary particles that have been granulated in advance with an organic binder for granulation, and forming a skeleton in the granulated material.

[0114] As the organic binder for granulation, known ones can be used. For example, binders used for positive and negative electrodes may be used, but polybenzimidazole, styrene butadiene rubber, polyvinylidene fluoride, carboxymethyl cellulose, polyvinyl alcohol, polyacrylic acid, cellulose nanofiber, polyimide, polyamide, and polyamideimide are preferred from the viewpoints of chemical stability, heat resistance, reduction resistance, and the like of the granules.

[0115] The amount of the granulation binder is not particularly limited as long as it is an amount capable of binding the active material particles, but is preferably within the range of 0.1 to 30% by mass relative to the granules. In addition to the active material particles and the granulation binder, the granules may contain a conductive assistant for imparting electronic conductivity as necessary. The skeleton forming agent is preferably contained within the range of 0.2 to 30% by mass relative to the granules. The granules thus obtained not only have improved cycle life characteristics, but also have improved coating properties of the slurry.

[0116] The conductive assistant for the negative electrode is not particularly limited as long as it has electronic conductivity, and the above-mentioned metals, carbon materials, conductive polymers, conductive glasses, etc. can be used. Specific examples include acetylene black (AB), ketjen black (KB), furnace black (FB), thermal black, lamp black, channel black, roller black, disc black, carbon black (CB), carbon fiber (for example, vapor-grown carbon fiber named VGCF, which is a registered trademark), carbon nanotubes (CNT), carbon nanohorns, graphite, graphene, glassy carbon, amorphous carbon, etc., and one or more of these may be used.

[0117] When the total of the active material, binder, and conductive assistant contained in the negative electrode is taken as 100 mass%, the conductive assistant is preferably contained in an amount of 0 to 20 mass%. In other words, the conductive assistant is contained as needed. If it exceeds 20 mass%, the ratio of the active material as a battery is small, and the electrode capacity density is likely to be low.

[0118] The negative electrode binder may be any of the commonly used binders, such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, aramid, polyacrylic, styrene butadiene rubber (SBR), ethylene-vinyl acetate copolymer (EVA), styrene-ethylene-butylene-styrene copolymer (SEBS), carboxymethyl cellulose (CMC), xanthan gum, polyvinyl alcohol (PVA), ethylene vinyl alcohol, polyvinyl butyral (PVB), ethylene vinyl alcohol, polyethylene (PE), polypropylene (PP), polyacrylic acid, lithium polyacrylate, sodium polyacrylate, potassium polyacrylate, ammonium polyacrylate, methyl polyacrylate, ethyl polyacrylate, amine polyacrylate, polyacrylic acid, etc. Organic materials such as acrylate esters, epoxy resins, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), nylon, vinyl chloride, silicone rubber, nitrile rubber, cyanoacrylate, urea resin, melamine resin, phenolic resin, latex, polyurethane, silylated urethane, nitrocellulose, dextrin, polyvinylpyrrolidone, vinyl acetate, polystyrene, chloropropylene, resorcinol resin, polyaromatic, modified silicone, methacrylic resin, polybutene, butyl rubber, 2-propenoic acid, cyanoacrylic acid, methyl methacrylate, glycidyl methacrylate, acrylic oligomer, 2-hydroxyethyl acrylate, alginic acid, starch, lacquer, sucrose, glue, casein, and cellulose nanofibers may be used alone or in combination of two or more.

[0119] Further, a mixture of these organic binders and inorganic binders may be used. The inorganic binder may be a silicate-based, phosphate-based, sol-based, cement-based, or other type. For example, lithium silicate, sodium silicate, potassium silicate, cesium silicate, guanidine silicate, ammonium silicate, silicofluoride, borate, lithium aluminate, sodium aluminate, potassium aluminate, aluminosilicate, lithium aluminate, sodium aluminate, potassium aluminate, polyaluminum chloride, polyaluminum sulfate, polyaluminum silicate sulfate, aluminum sulfate, aluminum nitrate, ammonium alum, lithium alum, sodium alum, potassium alum, chrome alum, iron alum, manganese alum, nickel ammonium sulfate, diatomaceous earth, polyzirconoxane, polytitanium tallow, mullite, white carbon, silica sol, colloidal silica, fumed silica, alumina sol, colloidal alumina, fumed alumina, zirconium tallow, silicic acid ... Inorganic materials such as conia sol, colloidal zirconia, fumed zirconia, magnesia sol, colloidal magnesia, fumed magnesia, calcia sol, colloidal calcia, fumed calcia, titania sol, colloidal titania, fumed titania, zeolite, silicoaluminophosphate zeolite, sepiolite, montmorillonite, kaolin, saponite, aluminum phosphate, magnesium phosphate, calcium phosphate, iron phosphate, copper phosphate, zinc phosphate, titanium phosphate, manganese phosphate, barium phosphate, tin phosphate, low melting point glass, plaster, gypsum, magnesium cement, litharge cement, Portland cement, blast furnace cement, fly ash cement, silica cement, phosphate cement, concrete, and solid electrolytes may be used alone or in combination of two or more.

[0120] Among these, from the viewpoints of binding ability, resistance to electrolyte elution, resistance to oxidation-reduction, energy density, and the like, inorganic materials such as lithium silicate, sodium silicate, potassium silicate, guanidine silicate, ammonium silicate, silicofluoride, aluminosilicate, aluminum phosphate, magnesium phosphate, and calcium phosphate are preferred.

[0121] However, when negative electrodes are manufactured using inorganic binders, the specific gravity of the inorganic binder is large, so the electrode energy density per weight tends to be low. In addition, when inorganic binders that are highly acidic or alkaline are used and contain active materials with poor chemical resistance such as Si or Sn, hydrogen gas is generated during the mixing of the slurry, making it difficult to apply the electrode coating and causing foaming during the heating and drying process, making it impossible to manufacture uniform electrodes. In addition, when a current collector with poor chemical resistance is used, the current collector deteriorates.

[0122] Conventionally, when an alloy-based negative electrode active material is used, PI, for example, has been considered to be preferable as a negative electrode binder from the viewpoint of suppressing the volume change of the active material accompanying charge and discharge and improving the cycle life characteristics of the battery. However, in the present invention, since the volume change can be suppressed by the framework forming agent, all of the above-mentioned commonly used binders can be used.

[0123] When the total of the active material, binder, and conductive assistant contained in the negative electrode is taken as 100 mass %, the binder is preferably contained in an amount of 0.1 to 60 mass %, and more preferably 0.5 to 30 mass %.

[0124] If the binder is less than 0.1% by mass, the mechanical strength of the electrode is low, so that the active material is likely to fall off during the formation of the skeleton, which may result in poor cycle life characteristics of the battery.On the other hand, if the binder is more than 60% by mass, the ion conductivity is low, the electrical resistance is high, and the proportion of the active material in the battery is low, so that the electrode capacity density is likely to be low.

[0125] The current collector used for the negative electrode is not particularly limited as long as it has electronic conductivity and can pass current through the negative electrode active material held therein. For example, conductive materials such as C, Ti, Cr, Ni, Cu, Mo, Ru, Rh, Ta, W, Os, Ir, Pt, Al, Au, etc., and alloys containing two or more of these conductive materials (e.g., stainless steel) can be used. When using a conductive material other than the above, it may be a multilayer structure of heterogeneous metals, such as iron coated with Cu or Ni.

[0126] From the viewpoint of high electrical conductivity and good stability in the electrolyte, the current collector is preferably C, Ti, Cr, Au, Fe, Cu, Ni, stainless steel, etc., and more preferably C, Cu, Ni, stainless steel, etc. from the viewpoint of reduction resistance and material cost. When iron is used as the current collector substrate, it is preferable that it is coated with Ni or Cu to prevent oxidation of the surface of the current collector substrate. In addition, since the volume change of the negative electrode material accompanying charge and discharge is large in the conventional alloy-based negative electrode, the current collector substrate is preferably stainless steel or iron, but in the present invention, since the stress applied to the current collector can be relaxed by the framework forming agent, all of the above-mentioned commonly used ones can be used.

[0127] The shape of the current collector may be linear, rod-like, plate-like, foil-like, or porous, and among these, the porous shape may be used since it can increase the packing density and the skeleton forming agent can easily penetrate into the active material layer. Examples of the porous shape include mesh, woven fabric, nonwoven fabric, embossed body, punched body, expanded body, and foamed body, and among these, the shape of the current collecting substrate is preferably embossed or foamed because it has good output characteristics.

[0128] Next, the active material for the positive electrode is not particularly limited as long as it is a positive electrode active material used in a non-aqueous electrolyte secondary battery. Known electrodes including alkali metal transition metal oxide-based, vanadium-based, sulfur-based, solid solution-based (lithium excess-based, sodium excess-based, potassium excess-based), carbon-based, organic-based, etc. can be used.

[0129] Alkali metal transition metal oxides include, for example, LiCoO2, Li0.9 So 0.1 CoO2、LiNiO2、LiNi 0.5 Co 0.5 O2、LiNi 0.33 Mr 0.33 Co 0.33 O2、LiNi 0.5 Mr 0.2 Co 0.3 O2、LiNi 0.6 Mr 0.2 Co 0.2 O2、LiNi 0.8 Mr 0.1 Co 0.1 O2、Li(Ni,Co,Al)O2、LiMnO2、LiMn2O4、LiFePO4、LiFe 0.5 Mr 0.5 PO4、LiMnPO4、Li2MnSiO4、Li2FeSiO4、Li2(Mn,Fe)SiO4、Li2CoSiO4、Li2MgSiO4、Li2CaSiO4、Li2ZnSiO4、LiNb2O5、LiNbO2、LiF eO2、LiMgO2、LiCaO2、LiTiO2、LiTiS2、LiCrO2、LiRuO2、LiCuO2、LiZnO2、LiMoO2、LiMoS2、LiTaO2、LiWO2、NaCoO2、NaNiO2、NaNi 0.33 Mr 0.33 Co 0.33 O2、NaMnO2、NaMn2O4、NaFePO4、NaFe 0.5 Mr 0.5 PO4、NaMnPO4、Na2MnSiO4、Na2FeSiO4、Na2(Mn,Fe)SiO4、Na2CoSiO4、Na2MgSiO4、Na2CaSiO4、Na2ZnSiO4、NaNb2O5、NaNbO2、N aFeO2、NaMgO2、NaCaO2、NaTiO2、NaTiS2、NaCrO2、NaRuO2、NaCuO2、NaZnO2、NaMoO2、NaMoS2、NaTaO2、NaWO2、KCoO2、KNiO2、KNi 0.33 Mr 0.33 Co 0.33 O2、KMnO2、KMn2O4、KFePO4、KFe 0.5 Mr 0.5Examples include PO4, KMnPO4, K2MnSiO4, K2FeSiO4, K2(Mn,Fe)SiO4, K2CoSiO4, K2MgSiO4, K2CaSiO4, K2ZnSiO4, KNb2O5, KNbO2, KFeO2, KMgO2, KCaO2, KTiO2, KTiS2, KCrO2, KRuO2, KCuO2, KZnO2, KMoO2, KMoS2, KTaO2, and KWO2.

[0130] Examples of vanadium-based materials include LiV2O5, LiVO2, Li3VO4, Li3V2(PO4)3, NaV2O5, NaVO2, Na3VO4, Na3V2(PO4)3, KV2O5, KVO2, K3VO4, K3V2(PO4)3, etc. Examples of sulfur-based materials include sulfur, carbon sulfide, polysulfide, polycarbon sulfide, sulfur-modified polyacrylonitrile, disulfide compounds, sulfur-modified rubber, sulfur-modified pitch, sulfur-modified anthracene, metal sulfide, etc. Solid solution systems include, for example, Li2MnO3-LiNiO2, Li2MnO3-LiMnO2, Li2MnO3-LiCoO2, Li2MnO3-Li(Ni,Mn)O2, Li2MnO3-Li(Ni,Co)O2, Li2MnO3-Li(Mn,Co)O2, Li2MnO3-Li(Ni,Mn,Co)O2, Na2MnO3-NaNiO2, Na2MnO3-NaMnO2, Na2MnO3-NaCoO2, Na2MnO3-Na (Ni,Mn)O2, Na2MnO3-Na(Ni,Co)O2, Na2MnO3-Na(Mn,Co)O2, Na2MnO3-Na(Ni,Mn,Co)O2, K2MnO3-KNiO2, K2MnO3-KMnO2, K2MnO3-KCoO2, K2MnO3-K(Ni,Mn)O2, K2MnO3-K(Ni,Co)O2, K2MnO3-K(Mn,Co)O2, K2MnO3-K(Ni,Mn,Co)O2, etc.

[0131] Examples of carbon-based materials include graphite, soft carbon, hard carbon, glassy carbon, etc. Examples of organic-based materials include rubeanic acid, tetracyanoquinodimethane, triquinoxalinylene, phenazine dioxide, trioxotriangulene, indigo carmine, nitronyl nitroxide radical compounds, radialene-based compounds, aliphatic cyclic nitroxyl radicals, benzoquinones, etc.

[0132] The above-mentioned positive electrode active materials may be used alone or in combination of two or more. From the viewpoint of energy density, for example, LiCoO2, LiMn2O4, LiFePO4, LiFe 0.5 Mn 0.5 PO4, LiMnPO4, LiNi 0.33 Mn 0.33 Co 0.33 O2, LiNi 0.5 Mn 0.2 Co 0.3 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2, Li(Ni,Co,Al)O2, solid solution system, vanadium system, and sulfur system are preferred. The shape of the active material particles is not particularly limited, and may be spherical, elliptical, faceted, strip-like, fibrous, flake-like, doughnut-like, or hollow.

[0133] On the other hand, as in the case of the negative electrode, it is also possible to use the framework forming agent of the present invention as a binder for granulation of the above-mentioned positive electrode active material. In that case, the primary particles of the active material have a median diameter (D 50 The active material particles (secondary particles) after granulation preferably have a median diameter (D 50 The particle size is preferably within a range of 1 μm to 100 μm. The method for granulating the active material is substantially the same as the method for granulating the negative electrode active material, and known granulation methods can be used.

[0134] The conductive assistant is not particularly limited as long as it has electronic conductivity, and examples thereof include metals, carbon materials, conductive polymers, conductive glass, etc., but carbon materials are preferred from the viewpoint of high electronic conductivity and oxidation resistance. Specific examples thereof include acetylene black (AB), ketjen black (KB), furnace black (FB), thermal black, lamp black, channel black, roller black, disc black, carbon black (CB), carbon fiber (for example, vapor-grown carbon fiber named VGCF, which is a registered trademark), carbon nanotubes (CNT), carbon nanohorns, graphite, graphene, glassy carbon, amorphous carbon, etc., and one or more of these may be used.

[0135] When the total of the active material, binder, and conductive assistant contained in the positive electrode is taken as 100 mass%, the conductive assistant is preferably contained in an amount of 0 to 20 mass%. In other words, the conductive assistant is contained as necessary. If it exceeds 20 mass%, the proportion of the active material as a battery is small, and the electrode capacity density is likely to be low.

[0136] The positive electrode binder may be any of the commonly used binders, such as polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), ethylene-vinyl acetate copolymer (EVA), styrene-ethylene-butylene-styrene copolymer (SEBS), carboxymethyl cellulose (CMC), xanthan gum, polyvinyl alcohol (PVA), polyvinyl butyral (PVB), ethylene vinyl alcohol, polyethylene (PE), polypropylene (PP), polyacrylic acid, lithium polyacrylate, sodium polyacrylate, potassium polyacrylate, ammonium polyacrylate, methyl polyacrylate, ethyl polyacrylate, amine polyacrylate, polyacrylic ester, epoxy resin, etc. Organic materials such as grease, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), nylon, vinyl chloride, silicone rubber, nitrile rubber, cyanoacrylate, urea resin, melamine resin, phenolic resin, latex, polyurethane, silylated urethane, nitrocellulose, dextrin, polyvinylpyrrolidone, vinyl acetate, polystyrene, chloropropylene, resorcinol resin, polyaromatic, modified silicone, methacrylic resin, polybutene, butyl rubber, 2-propenoic acid, cyanoacrylic acid, methyl methacrylate, glycidyl methacrylate, acrylic oligomer, 2-hydroxyethyl acrylate, polyacetal, alginic acid, starch, sucrose, lacquer, glue, casein, and cellulose nanofiber may be used alone or in combination of two or more. Also, a mixture of these organic binders and inorganic binders may be used.

[0137] The inorganic binder may be, for example, a silicate-based, phosphate-based, sol-based, cement-based, etc. However, if a positive electrode is manufactured using only an inorganic binder, the specific gravity of the inorganic binder is large, so that the electrode energy density per weight tends to be low.

[0138] Conventionally, when a sulfur-based, vanadium-based, or solid solution-based positive electrode active material is used, a binder with high binding properties has been considered preferable from the viewpoint of suppressing the volume change of the active material due to charging and discharging and improving the cycle life characteristics of the battery. However, in the present invention, since it is possible to suppress the volume change with the framework-forming agent, all of the above-mentioned commonly used binders can be used.

[0139] When the total of the active material, binder, and conductive assistant contained in the positive electrode is taken as 100% by mass, the binder is preferably contained in an amount of 0.1 to 60% by mass. If the binder is less than 0.1% by mass, the mechanical strength of the electrode is low, so that the active material is likely to fall off during skeleton formation, and the cycle life characteristics of the battery may deteriorate. On the other hand, if the binder is more than 60% by mass, the ion conductivity is low, the electrical resistance is high, and the proportion of the active material in the battery is low, so that the electrode capacity density is likely to be low.

[0140] The current collector used for the positive electrode is not particularly limited as long as it has electronic conductivity and can pass electricity through the positive electrode active material held therein. For example, conductive materials such as C, Ti, Cr, Ni, Cu, Mo, Ru, Rh, Ta, W, Os, Ir, Pt, Au, Al, and alloys containing two or more of these conductive materials (e.g., stainless steel) can be used. When using conductive materials other than the above, for example, a multilayer structure of heterogeneous metals such as iron coated with Al may be used. From the viewpoint of high electrical conductivity and good stability in the electrolyte, C, Ti, Cr, Au, Al, stainless steel, and the like are preferred as the current collector, and further from the viewpoint of oxidation resistance and material cost, C, Al, stainless steel, and the like are preferred. More preferably, carbon-coated Al and carbon-coated stainless steel are preferred.

[0141] The shape of the current collector may be linear, rod-like, plate-like, foil-like, or porous, and among these, the porous shape may be used since it can increase the packing density and the skeleton forming agent can easily penetrate into the active material layer. Examples of the porous shape include mesh, woven fabric, nonwoven fabric, embossed body, punched body, expanded body, and foamed body, and among these, the shape of the current collecting substrate is preferably embossed or foamed body since it has good output characteristics.

[0142] The electrode is for a non-aqueous electrolyte secondary battery, and the above-mentioned skeletal forming agent is present at least in the active material layer. According to this configuration, by applying the skeletal forming agent to the electrode, the skeletal forming agent penetrates into the active material layer and forms a strong skeleton in the active material layer. This reduces the volume change of the electrode and improves the insulation of the electrode surface.

[0143] In addition, in this electrode, the above-mentioned skeletal former is present in the active material layer, and in the active material layer, there are gaps between the active materials. According to this configuration, by applying the skeletal former to the electrode, the skeletal former penetrates into the active material layer, so that the gaps between the active materials in the active material layer are not completely filled with the skeletal former, and gaps between the active materials remain. This allows the active materials to expand and contract during charging and discharging, and suppresses the occurrence of wrinkles, cracks, and the like in the current collector of the electrode.

[0144] In addition, this electrode has a layer containing the alkali-resistant inorganic particles on the surface of the layer of the silicate-based skeleton-forming agent. According to this configuration, by providing the layer of inorganic particles, a strong skeleton can be formed and peeling and cracking during drying can be suppressed. In addition, the layer of inorganic particles can replace the separator, and it is possible to configure a battery without using a separate separator. Note that when the skeleton-forming agent is a phosphate-based agent, the layer contains acid-resistant inorganic particles.

[0145] Preferably, the electrode has a coating amount of the skeletal forming agent of 0.01 mg / cm per unit area of ​​the electrode coated on one side. 2 More than 3mg / cm 2or less, or the amount of the framework forming agent per unit area of ​​the electrode coated on both sides is 0.02 mg / cm 2 More than 6mg / cm 2 More preferably, the amount of the skeleton-forming agent per unit area of ​​the electrode coated on one side is 0.05 mg / cm or less. 2 More than 3mg / cm 2 or less, or the amount of the framework forming agent per unit area of ​​the electrode coated on both sides is 0.1 mg / cm 2 More than 6mg / cm 2 The following is the result.

[0146] The electrode also comprises an active material capable of being alloyed with an alkali metal or capable of occluding alkali metal ions, an organic binder, and the framework forming agent.

[0147] Preferably, in this electrode, when the total solid content of the active material, conductive assistant, binder, and skeletal former is taken as 100 mass%, the skeletal former is present in an amount of 0.1 mass% or more and 30 mass% or less, more preferably 0.2 mass% or more and 20 mass% or less, and even more preferably 0.5 mass% or more and 10 mass% or less.

[0148] The separator according to the present invention is a separator for a non-aqueous electrolyte secondary battery, characterized in that the above-mentioned framework forming agent is present at least on the surface.

[0149] According to this configuration, the separator has high strength, excellent heat resistance, and improved cycle life characteristics. Here, the separator may be one generally used in non-aqueous electrolyte secondary batteries. The material of the separator is not particularly limited. The separator may be coated or filled with a ceramic layer to prevent meltdown due to local heat generation during a short circuit. The shape of the separator is not particularly limited, and may be a microporous membrane, a woven fabric, a nonwoven fabric, or a powder compact.

[0150] By applying a framework-forming agent to the separator, localized heat generation during a short circuit can cause the separator substrate to melt down, preventing the battery from shorting. In addition, oxidation of the separator on the positive electrode side can be suppressed when the battery is charged, preventing the battery from self-discharging. In addition, the heat resistance of the separator is improved, improving safety against nail penetration and overcharging.

[0151] The silicate-based skeleton-forming agent may also contain inorganic particles such as ceramics having alkali resistance. In this case, the particle size of the ceramics is preferably within the range of 0.2 to 20 μm, more preferably within the range of 0.25 to 10 μm. However, the phosphate-based agent may also contain inorganic particles such as ceramics having acid resistance. In this case, the same applies as the silicate-based agent.

[0152] Alternatively, a separator having improved heat resistance may be used by applying and filling a skeleton forming agent onto the ceramic layer of an existing ceramic-coated separator.

[0153] The porosity of the separator is preferably 30% or more, and more preferably 40% to 90% from the viewpoint of alkali metal ion conductivity and dendrite resistance. The air permeability obtained by the Gurley test method is preferably 3000 seconds / 100cc or less. Here, the porosity is a value calculated from the apparent density of the separator and the true density of the solid content of the constituent material by the formula: porosity (%) = 100 - (apparent density of separator / true density of solid content of material) x 100. The Gurley air permeability is the air permeability resistance measured by the Gurley tester method specified in JIS P 8117.

[0154] Preferably, the separator has a coating amount of the framework forming agent per unit area of ​​the separator coated on one side of the separator of 0.01 mg / cm. 2 More than 3mg / cm 2 or less, or the amount of the framework forming agent per unit area of ​​the separator coated on both sides is 0.02 mg / cm 2 More than 6mg / cm 2 The following is the result.

[0155] The method for producing an electrode according to the present invention is a method for producing an electrode for a non-aqueous electrolyte secondary battery, and includes step A of applying a skeleton-forming agent containing a silicate having a siloxane bond or a skeleton-forming agent containing a phosphate to the surface of an active material layer of the electrode, and step B of drying the electrode. According to this configuration, by using the skeleton-forming agent in the production of the electrode, it is possible to produce an electrode that has excellent heat resistance, high strength, and improved cycle life characteristics.

[0156] In the method for producing an electrode, in the step A, the framework forming agent permeates from the surface of the active material layer to the inside.

[0157] In addition, in the method for producing an electrode, the step A is a step of immersing the electrode in a tank containing the framework forming agent.

[0158] Preferably, in this electrode manufacturing method, the solids concentration of the silicate or phosphate in the framework forming agent is 0.1 to 30 parts by mass, and the step B is a step of heat treating at a temperature of 60° C. or higher. If drying is performed at a temperature lower than 60° C., the binding strength with the electrodes and separator is low and moisture cannot be sufficiently removed, making it difficult to obtain stable life characteristics when assembled into a battery.

[0159] Here, the electrode is manufactured, for example, by mixing an active material, a binder, and a conductive assistant added as necessary to form a slurry, applying the mixture to a current collector, pre-drying the mixture, filling the active material layer with water in which a skeleton-forming agent is dissolved, and performing heat treatment at 60°C or higher to obtain an electrode. That is, the electrode obtained by the slurry coating method is filled with a skeleton-forming agent in the active material layer, and then performing heat treatment to obtain an electrode. The pre-drying is not particularly limited as long as it can volatilize and remove the solvent in the slurry, and an example of the method is a method of performing heat treatment in the air at a temperature of 50 to 200°C.

[0160] In addition, the heat treatment is preferably performed at 80°C or higher, more preferably 100°C or higher, and desirably 110°C or higher, because a higher temperature can shorten the heat treatment time and improve the strength of the skeleton-forming agent. The upper limit of the heat treatment temperature is not particularly limited as long as the current collector does not melt, and may be increased to, for example, about 1000°C, which is the melting point of copper. In the case of conventional electrodes, the upper limit of the temperature was estimated to be much lower than 1000°C because the electrode binder was carbonized and the current collector was softened. However, in the present invention, the skeleton-forming agent exhibits excellent heat resistance and is stronger than the strength of the current collector, so the upper limit of the temperature is 1000°C.

[0161] The heat treatment can be performed for 0.5 to 100 hours. The heat treatment can be performed in the air, but it is preferable to perform the heat treatment in a non-oxidizing atmosphere to prevent oxidation of the current collector. The non-oxidizing atmosphere means an environment in which the amount of oxygen gas present is less than that in air. For example, the heat treatment can be performed in a reduced pressure environment, a vacuum environment, a hydrogen gas atmosphere, a nitrogen gas atmosphere, a rare gas atmosphere, or the like.

[0162] In addition, in the case of an electrode using a material with irreversible capacity, it is preferable to cancel the irreversible capacity by lithium doping. The lithium doping method is not particularly limited, but for example, (i) a method of attaching metallic lithium to a part on an electrode collector where there is no active material layer, injecting the liquid to form a local cell, and doping lithium into the electrode active material, (ii) a method of attaching metallic lithium on the active material layer on the electrode collector, injecting the liquid to forcibly short-circuit the electrode, and doping lithium into the electrode active material, (iii) a method of forming a film of metallic lithium on the active material layer by vapor deposition or sputtering, and doping lithium into the electrode active material by a solid-phase reaction, (iv) a method of electrochemically doping lithium into an electrode before battery construction in an electrolyte, and (v) a method of adding metallic lithium to an active material powder and mixing the powder to dope lithium into the active material.

[0163] As another method for producing an electrode, for example, a method in which an active material or an active material precursor is applied by chemical plating, sputtering, vapor deposition, gas deposition or the like to form an active material layer on a current collector and integrate them, may be used. From the viewpoints of the lyophilicity of the framework-forming agent and the electrode production costs, however, a slurry coating method is preferred.

[0164] The battery according to the present invention is characterized by comprising the above-mentioned electrode or the above-mentioned separator. With this configuration, the battery can have excellent cycle life characteristics and good safety.

[0165] For example, in the case of a battery using the above-mentioned electrodes (positive or negative electrodes), a battery structure in which the positive and negative electrodes are joined via a separator and sealed in a state of being immersed in an electrolyte is conceivable. Note that the battery structure is not limited to this, and the battery can be applied to existing battery forms and structures such as stacked batteries and wound batteries.

[0166] The electrolyte used in this battery may be a liquid or solid that can transfer alkali metal ions from the positive electrode to the negative electrode or from the negative electrode to the positive electrode, and may be the same as the electrolyte used in known non-aqueous electrolyte secondary batteries. Examples of the electrolyte include an electrolyte solution, a gel electrolyte, a solid electrolyte, an ionic liquid, and a molten salt. Here, the electrolyte solution refers to an electrolyte dissolved in a solvent.

[0167] Since the electrolyte must contain an alkali metal ion, the electrolyte salt is not particularly limited as long as it is used in nonaqueous electrolyte secondary batteries, but alkali metal salts such as lithium salts, sodium salts, and potassium salts are preferred. As the alkali metal salt, at least one selected from the group consisting of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium trifluoromethanesulfonate (LiCF3SO4), lithium bistrifluoromethanesulfonylimide (LiN(SO2CF3)2), lithium bispentafluoroethanesulfonylimide (LiN(SO2C2F5)2), lithium bisoxalatoborate (LiBC4O8), sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium trifluoromethanesulfonate, sodium trifluoromethanesulfonimide, potassium hexafluorophosphate, potassium perchlorate, potassium tetrafluoroborate, potassium trifluoromethanesulfonate, potassium trifluoromethanesulfonimide, and the like can be used.

[0168] Examples of the electrolyte solvent include propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), γ-butyrolactone (GBL), methyl-γ-butyrolactone, methyl lactone, 2-methyltetrahydrofuran, 1,3-dioxolane (DOL), 4-methyl-1,3-dioxolane, 1,2-dimethoxyethane, 1,2-diethoxyethane, diethyl ether, furan, dimethylfuran, tetrahydrofuran (THF), methyltetrahydrofuran (MeTHF), tetrahydrofuran (THP), dioxane (DIOX), crown ether, dimethoxymethane (DMM), Dimethoxyethane (DME), diglyme, triglyme, tetraglyme, methyl acetate (MA), ethyl acetate (EA), propyl acetate, isopropyl acetate, butyl acetate, methyl fluoroacetate, ethyl trifluoroacetate, methyl propionate, ethyl propionate, propyl propionate, methyl formate, ethyl formate, propyl formate, ethyl butyrate, propyl butyrate, methyl propyl butyrate, vinyl acetate, methyl cyanoacetate, gamma-valerolactone, sigma-valerolactone, epsilon-caprolactone, gamma-hexalactone, gamma-undecalactone, trimethyl phosphate (TMP), triethyl phosphate (TEP), tri-n-propyl phosphate, trioctyl phosphate, triphenyl phosphate, N,N-Dimethylformamide (DMF), ethylenediamine, pyridine, N-methylimidazole, dimethyl sulfate, dimethyl sulfite, dipropyl sulfite, ethylene sulfite, dimethyl sulfone, ethyl methyl sulfone, diphenyl sulfone, sulfolane, methyl sulfolane, methyl methanesulfonate, methyl benzenesulfonate, methyl trifluoromethanesulfonate, propanesulfone, butanesulfone, dimethylsulfoxide, diphenyl disulfide, dimethyl sulfide, diethyl sulfide, acetonitrile, propanenitrile, adiponitrile, valeronitrile, glutaniline At least one selected from the group consisting of butyl ether, malononitrile, succinonitrile, pimelonitrile, suberonitrile, isobutyronitrile, biphenyl, succinic anhydride, t-butylbenzene, naphthalene, cyclohexylbenzene, benzotriazole, thiophene, toluene, methyl ethyl ketone, benzene, fluorobenzene, hexafluorobenzene, nitromethane, N,N-dimethylformamide, dimethyl sulfoxide, vinylene carbonate (VC), vinyl ethylene carbonate (EVC), fluoroethylene carbonate (FEC), and ethylene sulfite (ES) can be used.

[0169] Ionic liquids and molten salts are classified by the type of cation (positive ion), such as pyridine, alicyclic amine, and aliphatic amine. By selecting the type of anion (negative ion) to be combined with this, a variety of ionic liquids and molten salts can be synthesized. Examples of cations include ammonium ions such as imidazolium salts and pyridinium salts, phosphonium ions, and inorganic ions, while examples of anions include halogen ions such as bromide ions and triflates, boron ions such as tetraphenylborate, and phosphorus ions such as hexafluorophosphate.

[0170] Ionic liquids and molten salts can be obtained by known synthesis methods, for example, by combining a cation such as imidazolinium with an anion such as Br-, Cl-, BF4-, PF6-, (CF3SO2)2N-, CF3SO3-, FeCl4-, etc. Ionic liquids and molten salts can function as an electrolyte without the addition of an electrolyte.

[0171] An electrical device according to the present invention is characterized by comprising the battery described above.

[0172] Examples of electrical equipment include irons, whisks, all-in-one computers, clothes dryers, medical equipment, intercoms, wearable devices, video equipment, air conditioners, air circulators, gardening machinery, motorcycles, ovens, music players, music recorders, hot air heaters, toys, car components, flashlights, loudspeakers, car navigation systems, cassette stoves, home storage batteries, nursing care machinery, humidifiers, dryers, fuel dispensers, water dispensers, suction machines, safes, glue guns, mobile phones, portable information devices, air purifiers, air-conditioned clothing, game consoles, fluorescent lights, lint removers, cordless phones, coffee makers, Heat warmers, ice shaver, kotatsu, copy machines, haircutting equipment, shavers, lawn mowers, automobiles, lighting equipment, dehumidifiers, sealers, shredders, automated external defibrillators, rice cookers, stereos, stoves, speakers, trouser presses, smartphones, rice polishers, washing machines, toilet seats with cleaning functions, sensors, electric fans, submarines, blowers, vacuum cleaners, tablets, body fat scales, fishing tackle, digital cameras, televisions, television receivers, video games, displays, disc changers, desktop computers, railways, televisions, electric carpets, desk lamps, electric stoves, electric pots electric blankets, calculators, electric carts, electric wheelchairs, power tools, electric cars, electric floats, electric toothbrushes, telephones, electric bicycles, electric insect killers, induction cookers, electronic organizers, electronic musical instruments, electronic locks, electronic cards, microwave ovens, electronic mosquito repellents, electronic cigarettes, telephones, toasters, hair dryers, walkie-talkies, watches, drones, food waste processors, laptops, incandescent light bulbs, soldering irons, panel heaters, halogen heaters, fermenters, bread bakers, hybrid cars, personal computers, computer peripherals, hair clippers, panel heaters, video cameras, video decks, airplanes, emergency power supplies Lights, emergency batteries, ships, beauty equipment, printers, copiers, grinders, sprayers, fax machines, forklifts, plug-in hybrid cars, projectors, hair dryers, hair irons, headphones, disaster prevention equipment, security equipment, home theaters, hot sandwich makers, hot plates, pumps, aroma diffusers, massage machines, mixers, mills, movie players, monitors, rice cake makers, water heaters, underfloor heating panels, radios, radio cassette players, lanterns, radio-controlled cars, laminators, remote controls, microwave ovens, water coolers, refrigerators, air coolers, cooling fans, air conditioning equipment, robots,Word processors, GPS, etc. Effect of the Invention

[0173] The skeleton-forming agent according to the present invention, when used in an electrode, can suppress the occurrence of wrinkles, cracks, etc., unlike when used as a binder. In addition, better life characteristics can be obtained than in the past. Furthermore, even when the electronic conductivity of the active material layer is high, heat generation due to internal short circuit can be reduced. [Brief description of the drawings]

[0174] [Figure 1] FIG. 2 is a diagram showing a cross section of an electrode coated with a framework forming agent according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of coating of a framework forming agent according to one embodiment of the present invention. [Diagram 3] 1A to 1C are diagrams illustrating an example of a manufacturing process for an electrode according to an embodiment of the present invention. [Figure 4] FIG. 4 is a graph showing cycle life characteristics of an electrode according to one embodiment of the present invention. [Diagram 5] FIG. 2 is a graph showing the relationship between the skeletal density and the discharge capacity of an electrode according to one embodiment of the present invention. [Figure 6] FIG. 4 is a graph showing cycle life characteristics of an electrode according to one embodiment of the present invention. [Figure 7] FIG. 2 is a graph showing the relationship between the skeletal density and the discharge capacity of an electrode according to one embodiment of the present invention. [Figure 8] FIG. 4 is a graph showing cycle life characteristics of an electrode according to one embodiment of the present invention. [Figure 9] FIG. 1 is a diagram showing the cycle life characteristics of an electrode to which a framework forming agent containing a surfactant according to one embodiment of the present invention is applied. [Figure 10] FIG. 1 is a diagram comparing the cycle life characteristics of an electrode coated with a framework-forming agent according to one embodiment of the present invention and an electrode that is not coated with the framework-forming agent. [Figure 11] FIG. 1 is a diagram comparing the cycle life characteristics of an electrode coated with a framework-forming agent according to one embodiment of the present invention and an electrode that is not coated with the framework-forming agent. [Figure 12] FIG. 1 is a diagram showing a cross section of an electrode coated with a framework forming agent containing inorganic particles according to one embodiment of the present invention. [Figure 13] FIG. 2 is a diagram showing the initial charge / discharge curves of a battery not using a separator according to one embodiment of the present invention. [Figure 14] FIG. 2 is a diagram showing an SEM image of a Si granule to which a framework-forming agent according to one embodiment of the present invention is applied. [Figure 15] FIG. 4 is a diagram showing charge / discharge curves at various rates according to one embodiment of the present invention. [Figure 16] FIG. 1 is a diagram showing the results of a peel test comparing an electrode coated with a framework-forming agent according to one embodiment of the present invention and an electrode that is not coated. [Figure 17] FIG. 1 shows the X-ray diffraction (XRD) pattern of silicate (Na2O·nSiO2) powder. [Figure 18] FIG. 1 shows the cycle life characteristics of a reference electrode containing an alkali metal silicate (Li0.05Na1.95O·2.8SiO2) as a binder and the electrode after 200 cycles. [Figure 19] 1 is a copy of a photograph showing a current collector in a conventional Si negative electrode. [Figure 20] FIG. 13 is a graph showing the results of glow discharge optical emission spectroscopy comparing an electrode coated and impregnated with a framework-forming agent with an electrode not coated and impregnated. [Figure 21] FIG. 1 is a diagram showing a silicate-based molecular formula and a phosphate-based molecular formula. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0175] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, but the present invention is not limited to this embodiment. In particular, in this embodiment, an electrode of a lithium secondary battery (lithium ion battery) will be described as an example, but the present invention is not limited to this. In addition, as a framework forming agent, an alkali metal silicate aqueous solution containing Na2O·3SiO2 will be mainly described as an example, but the present invention is not limited to this.

[0176] -First embodiment- [1. Electrode manufacturing method] First, as an example of this embodiment, a method for manufacturing an electrode of a lithium secondary battery will be described. Note that the electrodes include a negative electrode and a positive electrode, but the manufacturing methods of the negative electrode and the positive electrode are the same, with only the difference being the current collector and the active material. Therefore, the manufacturing method of the negative electrode will be described, and the manufacturing method of the positive electrode will be omitted as appropriate.

[0177] The negative electrode is manufactured by applying an electrode material to copper foil. First, for example, a rolled copper foil with a thickness of 10 μm is manufactured, and the copper foil is wound in a roll shape in advance. The electrode material of the negative electrode is made by baking a carbon precursor to graphitize it, and mixing it with a binder, a conductive assistant, and the like to make a paste. In this embodiment, as an example, PVdF is used as the binder, and acetylene black (AB) is used as the conductive assistant. Then, the electrode material is applied to the surface of the copper foil, and after drying, the pressure is adjusted to complete the negative electrode body.

[0178] The positive electrode is manufactured by applying an electrode material to an aluminum foil. The electrode material of the positive electrode is made into a paste by mixing a lithium-transition metal oxide with a binder and a conductive assistant. In this embodiment, as an example, PVdF is used as the binder and AB is used as the conductive assistant. Hereinafter, the positive electrode body and the negative electrode body are collectively referred to as the electrode body, the copper foil and the aluminum foil are collectively referred to as the current collector, and the electrode material applied to the current collector may be referred to as the active material layer.

[0179] On the other hand, in this embodiment, the skeletal forming agent to be used in the electrode body is prepared in advance. The skeletal forming agent is produced by purifying Na2O·3SiO2, an alkali metal silicate having a siloxane bond, by a dry or wet method, and adjusting the amount of water added. For example, the dry method is according to the following formula 4, and the wet method is according to the following formula 5. At this time, a surfactant is mixed. As an example of the skeletal forming agent of this embodiment, the solid concentration of Na2O·3SiO2 in the skeletal forming agent is 5 mass %, and the surfactant is 0.04 mass %. Na2CO3+3SiO2→Na2O・3SiO2+CO2↑ (Equation 4) 2NaOH+3SiO2→Na2O・3SiO2+H2O (Formula 5)

[0180] Then, the surface of each electrode body is coated with a skeleton-forming agent to coat the active material layer. The skeleton-forming agent can be applied by impregnating the electrode body in a tank containing the skeleton-forming agent, dripping or applying the skeleton-forming agent to the surface of the electrode body, spray coating, screen printing, curtain printing, spin coating, gravure coating, die coating, or the like. The skeleton-forming agent applied to the surface of the electrode body penetrates into the active material layer and enters into gaps between the active material and the conductive assistant. The electrode body is then dried by hot air at 110°C to 160°C, heating, or the like to harden the skeleton-forming agent. As a result, the skeleton-forming agent forms the skeleton of the active material layer.

[0181] Finally, each electrode body, i.e., the negative electrode body and the positive electrode body, is cut to a desired size, and the electrodes with skeleton formation are completed.

[0182] The above-mentioned electrode manufacturing method can be realized by a manufacturing device. A current collector wound in a roll is sent out, an electrode material is applied to the current collector in an active material layer coating device, the electrode material is dried by hot air in a first drying device, a skeleton-forming agent is applied to the surface of the electrode body in a skeleton-forming agent coating device, the skeleton-forming agent is dried and hardened by hot air in a second drying device, and the electrode is wound again in a roll. Finally, the electrode wound in a roll is cut to a desired size.

[0183] According to the above-mentioned electrode manufacturing method, it is possible to continuously manufacture electrodes having high strength, excellent heat resistance, and improved cycle life characteristics. In addition, by using a silicate having a siloxane bond as a skeleton-forming agent instead of a binder, the copper foil does not wrinkle or crack, and the active material layer does not crack or warp, and does not expand due to generated gas, so that the electrode can be used.

[0184] The positive and negative electrodes obtained as described above can be joined together via a separator and sealed in an electrolyte solution to form a lithium secondary battery. A lithium secondary battery having this structure can function as a lithium secondary battery with good safety. The structure of the lithium secondary battery is not particularly limited, and can be applied to existing battery forms and structures such as stacked batteries and wound batteries.

[0185] [2. Electrode configuration] The negative electrode for a non-aqueous electrolyte secondary battery manufactured by the above manufacturing process includes a copper foil current collector and an active material layer on the surface of the current collector, the active material layer containing an active material, a conductive assistant, and a binder. The surface of the active material layer is coated with a hardened skeletal former, and the hardened skeletal former is also present inside the active material layer. The skeletal former inside the active material layer is present in the gaps between the active material, the conductive assistant, and the binder so as to cover them. The density of the skeletal former in the active material layer is, for example, 0.7 mg / cm. 2 and 0.1mg~3mg / cm 2 It is preferable to set it within the range of

[0186] The positive electrode includes an aluminum foil current collector and an active material layer on the surface of the current collector, the active material layer containing an active material, a conductive assistant, and a binder. The surface of the active material layer is coated with a hardened skeletal former, and the hardened skeletal former is also present inside the active material layer. The skeletal former inside the active material layer is present in the gaps between the active material, the conductive assistant, and the binder so as to cover them. The density of the skeletal former in the active material layer is, for example, 0.5 mg / cm. 2 and 0.1mg~3mg / cm 2 It is preferable to set the above.

[0187] The electrodes of this embodiment are of high strength, excellent heat resistance, and have improved cycle life characteristics. Also, as shown in the nail penetration test results described later, the nail penetration safety is also improved. Further, since the skeleton forming agent is applied to the surface of the electrode by coating or impregnation, the skeleton forming agent exists in the gaps inside the active material layer so as to cover the active material, the conductive assistant, and the binder. That is, when the skeleton forming agent is kneaded with the binder and used, the skeleton forming agent exists in the active material layer with substantially no gaps, whereas in the electrodes of this embodiment, a certain gap exists inside the active material layer. This allows for the expansion and contraction of the electrodes and suppresses the occurrence of wrinkles, cracks, etc. in the current collector.

[0188] [3. Configuration of Skeleton Forming Agent] As described above, the solid content concentration of the skeleton forming agent of this embodiment, which is an alkali metal silicate having a siloxane bond, Na2O·3SiO2, is 7.5% by mass, the surfactant is 0.09% by mass, and the remainder is water. Note that the surfactant is not essential, but it improves the lyophilicity to the active material layer and allows the skeleton forming agent to uniformly penetrate into the active material layer.

[0189] Also, although the skeleton forming agent of this embodiment uses sodium silicate, Na2O·3SiO2, as the silicate, it is not limited thereto, and instead of Na, Li, K, a triethanolammonium group, a tetramethanolammonium group, a tetraethanolammonium group, or a guanidine group may be used.

[0190] Note that Na is used because Na is of high strength and has excellent cycle life characteristics. Also, it is possible to use Na and Li in combination, and using Li improves the ionic conductivity. In this case, it is preferable that Li < Na, and in this way, a skeleton forming agent that maintains a certain strength and has good ionic conductivity is obtained. More specifically, when the total of Na and Li is 100 mol%, it is preferable that Na is in the range of 51 to 99% and Li is in the range of 1 to 49%, and it is more preferable that Na is in the range of 70 to 98% and Li is in the range of 2 to 30%.

[0191] In addition, although the skeleton-forming agent of the present embodiment has a coefficient of SiO2 of 3, it is not limited thereto, and it may be 0.5 or more and 5.0 or less, preferably 2.0 or more and 4.5 or less, and more preferably 2.2 or more and 3.8 or less.

[0192] In addition, the skeleton-forming agent of the present embodiment can also be used for coating existing electrodes. By doing so, an electrode with high strength, excellent heat resistance, and improved cycle life characteristics can be obtained.

[0193] In addition, the skeleton-forming agent of the present embodiment can also be used by coating the surface of the separator. By doing so, a separator with high strength, excellent heat resistance, and improved cycle life characteristics can be obtained.

[0194] [4. Examples] Hereinafter, in the present embodiment, examples in which various parameters such as the solid content concentration and skeleton density of the skeleton-forming agent are changed, as well as their tests, results, and effects will be described.

[0195] [Examination of the number of n in Na2O·nSiO2 and the skeleton density] (Examples 1 to 18 and Comparative Example 1) Using Si-C granulated bodies as the electrode active material, under the conditions of 0.2C-rate, cut-off potential of 0.01V to 1.2V (vs. Li+ / Li), and 30°C, the solid content concentration of Na2O·nSiO2 of the skeleton-forming agent was changed from 0 mass% to 20 mass%, and the value of n was changed to 2.0, 2.5, and 3.0. This is a test on the cycle life characteristics. The Si-C granulated bodies (D 50 = 9.8μm) are composed of Si (D 50 = 1.1μm) and artificial graphite (D 50 = 1μm) (Si: artificial graphite = 29:71 mass%) and a granulation aid. They were produced by spray-drying a suspension at a feed rate of 6g / min, a spray pressure of 0.1MPa, and a drying temperature of 80 to 180°C.

[0196] The granulation aid used was polyvinyl alcohol (PVA, Poval 1400). The PVA content was 1% by mass relative to 100% by mass of the solid content consisting of silicon, artificial graphite, and PVA. 50 The value indicates the median diameter measured by the laser diffraction / scattering particle size distribution measurement method.

[0197] Test electrode (1.4mAh / cm 2 ) was prepared by applying a slurry (solid content ratio: 85:3:1:1:10% by mass) consisting of Si-C granules, AB, vapor grown carbon fiber (VGCF), copper flakes, and PVdF to copper foil, immersing it in an aqueous solution containing a specific skeleton-forming agent, and then heat-treating it at 160°C. Metallic lithium foil was used as the counter electrode. A glass nonwoven fabric (GA-100, manufactured by Toyo Roshi Co., Ltd.) and a polyethylene (PE) microporous membrane (20 μm) were used as the separator. 1.0M LiPF6 / (EC:DEC=50:50 vol%, + vinylene carbonate 1% by mass) was used as the electrolyte.

[0198] Table 1 shows the solid concentration of the skeleton-forming agent and the value of n in Na2O·nSiO2 of Examples 1 to 18 and Comparative Example 1. The inorganic skeleton-forming agent was prepared by blending a mixture of Na2CO3 and SiO2 to the composition shown in Table 1 below, heating and melting it at 1000°C or higher, cooling it, and then dissolving it in water.

[0199] [Table 1]

[0200] Fig. 4 is a graph showing the cycle life characteristics of Examples 1 to 18 and Comparative Example 1. As is clear from Fig. 4, the negative electrodes coated with the skeleton forming agent (Examples 1 to 18) have significantly improved life characteristics compared to the negative electrode not coated with the skeleton forming agent (Comparative Example 1). Among these, a solid concentration of Na2O·nSiO2 in the range of 2 to 10 mass% showed particularly excellent cycle life characteristics. The value of n in Na2O·nSiO2 of 3.0 showed particularly excellent cycle life characteristics.

[0201] 5 is a graph showing the relationship between the density (skeleton density) of the skeletal body and the discharge capacity at each cycle in Examples 1 to 18 and Comparative Example 1. As is clear from FIG. 5, in the electrodes using Si-C granules (Si:artificial graphite=29:71% by mass) as the active material, the skeletal density was 0.04 to 3.15 mg / cm 2 It can be seen that a sufficient discharge capacity can be obtained when the skeletal density is 0.1 to 2.5 mg / cm. 2 It is.

[0202] (Examples 19 to 36 and Comparative Example 2) In Examples 19 to 36 and Comparative Example 2, the composition of the Si-C granules as the active material was changed from 29:71% by mass of Si:artificial graphite to 46:54% by mass, and the capacity density of the test electrode was 1.2 mAh / cm 2 Other than that, the tests were the same as the previous tests (Examples 1 to 18 and Comparative Example 1). Table 2 shows the solid content concentrations of the skeleton forming agents and the values ​​of n in Na2O·nSiO2 for Examples 19 to 36 and Comparative Example 2, respectively.

[0203] [Table 2]

[0204] Fig. 6 is a graph showing the cycle life characteristics of Examples 19 to 36 and Comparative Example 2. As is clear from Fig. 6, the negative electrodes coated with the skeleton forming agent (Examples 19 to 36) have significantly improved life characteristics compared to the negative electrode without the skeleton forming agent (Comparative Example 2). Among these, the solid concentration of Na2O·nSiO2 in the range of 2 to 10 mass% showed particularly excellent cycle life characteristics. The value of n in Na2O·nSiO2 of 3.0 showed particularly excellent cycle life characteristics.

[0205] 7 is a graph showing the relationship between the density (skeleton density) of the skeletal body and the discharge capacity at each cycle in Examples 19 to 36 and Comparative Example 2. As is clear from FIG. 7, in electrodes using Si-C granules (Si:artificial graphite=46:54 mass%) as the active material, the skeletal density was 0.03 to 3.45 mg / cm. 2It can be seen that a sufficient discharge capacity can be obtained when the skeletal density is 0.1 to 2.5 mg / cm. 2 It is.

[0206] (Examples 37 to 40 and Comparative Example 3) In Examples 37 to 40, the active material was Si(D 50 = 1.1 μm), and the framework forming agent is Li 0.05 Na 1.95 O 3SiO2, the capacity density of the test electrode is 3.0 mAh / cm 2 The charge / discharge test was conducted under the conditions of 0.1 C-rate and cutoff potential of 0.01 V to 1.4 V (vs. Li+ / Li), and was otherwise the same as the previous tests (Examples 1 to 18 and Comparative Example 1). Table 3 shows the solid content concentration of the skeleton forming agent and the skeleton density of the electrode for Examples 37 to 40 and Comparative Example 3. The inorganic skeleton forming agent was prepared by blending a mixture of Li2CO3, Na2CO3, and SiO2 to the composition shown in Table 3, heating and melting it at 1000°C or higher, cooling, and then dissolving it in water.

[0207] [Table 3]

[0208] FIG. 8 is a graph showing the cycle life characteristics of Examples 37 to 40 and Comparative Example 3. As is clear from FIG. 8, the negative electrodes coated with the skeleton-forming agent (Examples 37 to 40) had an initial discharge capacity of over 1800 mAh / g, whereas the negative electrode without the skeleton-forming agent (Comparative Example 3) had a discharge capacity of 56.7 mAh / g. As can be seen by comparing the negative electrodes coated with the skeleton-forming agent (Examples 37 to 40) and the negative electrode without the skeleton-forming agent (Comparative Example 3), a dramatic improvement in cycle life characteristics was demonstrated. Of these, Li 0.05 Na 1.95 The solid concentration of O·3SiO2 in the range of 0.5 to 2.5 mass% showed particularly excellent cycle life characteristics. In electrodes using Si as the active material, the skeletal density was 0.12 to 0.90 mg / cm 2 It was found that a discharge capacity exceeding 2000 mAh / g could be obtained in this case.

[0209] Next, the batteries of Examples 37 to 40 and Comparative Example 3 were disassembled after charging and discharging (after 20 cycles), and the test electrodes were observed. The active material layer peeled off from the current collector in Comparative Example 3, whereas it did not peel off from the current collector in Examples 37 to 40, and no wrinkles or cracks were observed in the current collector. From these results, it was revealed that the electrodes coated and filled with the framework forming agent had improved adhesion between the active material layer and the current collector, improving the electrode performance.

[0210] <Surfactant study> (Example 41 and Example 42) In Example 41, Si-C granules (Si:artificial graphite = 29:71 mass%) were used as the electrode active material, and the solid content concentration of Na2O·nSiO2 was 6 mass%, the value of n was 2.5, and the skeletal density was 0.84 mg / cm3 as the skeletal forming agent. 2 The other conditions were adjusted to be the same as in Example 10.

[0211] Example 42 was the same as Example 41 except that a nonionic surfactant (registered trademark: Triton X-100) was added in an amount of 0.05% by mass as a skeleton-forming agent.

[0212] FIG. 9 is a graph showing a comparison of cycle life characteristics of an electrode (Example 41) in which a surfactant is not added to the skeletal forming agent and an electrode (Example 42) in which a surfactant is added to the skeletal forming agent. As is clear from FIG. 9, it can be seen that the cycle life characteristics are improved by adding a surfactant. This is because the surfactant improves the lyophilicity of the skeletal forming agent to the active material layer, and a uniform skeleton is formed in the active material layer. In addition, although a nonionic surfactant is used as the surfactant in this embodiment, the surfactant is not limited thereto, and an anionic surfactant, a cationic surfactant, an amphoteric surfactant, or a nonionic surfactant may also be used.

[0213] <Nail penetration safety> (Example 43 and Comparative Example 4) We conducted a safety test on batteries that use negative electrodes that use a framework forming agent. The test method is a nail penetration test, in which a nail is inserted into a battery model to examine whether the battery model emits smoke or catches fire. For the test, we used a 1.1 Ah battery model in which multiple negative electrodes, separators, and positive electrodes are stacked in an aluminum laminate casing and electrolyte is sealed inside. The positive electrode (4.2 mAh / cm 2 ) is LiNi 0.33 Co 0.33 Mn 0.33 The negative electrode (4.6 mAh / cm2) was fabricated by applying a slurry of O2, AB, and PVdF to an aluminum foil (20 μm) and then heat-treating it at 160°C. 2 ) is an artificial graphite (D 50 It was produced by applying a slurry consisting of AB and an acrylic binder to copper foil (10 μm) under a controlled pressure and then heat-treating it at 160°C.

[0214] Example 43 was prepared by immersing the negative electrode in an aqueous solution containing a skeleton-forming agent, followed by heat treatment at 150°C, as shown in Figure 2. The skeleton-forming agent was an aqueous solution of Na2O·3SiO2 and a nonionic surfactant (registered trademark: Triton X-100), with a solid concentration of Na2O·3SiO2 of 6 mass% and a solid concentration of the surfactant of 0.05 mass%. The skeleton density of the electrode was 0.9 mg / cm per side. 2 In this test, the positive and negative electrodes were prepared by coating on both sides, so the skeletal density on both sides was 1.8 mg / cm 2 In addition, a battery using a negative electrode to which no framework-forming agent was applied was used as Comparative Example 4.

[0215] The electrolyte used was 1M LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 50:50 vol%, + vinylene carbonate 1 mass%. The separator used was a polypropylene (PP) microporous membrane (23μm). For the nail penetration test, this battery model was charged to 4.2V at 0.1C-rate, and then an iron nail (φ3mm, round) was pierced into the center of the battery at a speed of 1mm / sec in a 25℃ environment until it penetrated, and the battery voltage, nail temperature, and casing temperature were measured.

[0216] When a nail was pierced in the conventional battery model (Comparative Example 4) using a negative electrode without a framework-forming agent, the battery voltage dropped to 0 V and a large amount of smoke was generated. This was because the separator melted down due to heat generated when a short circuit occurred inside the battery model.

[0217] On the other hand, the battery model using an artificial graphite negative electrode with a framework forming agent (Example 43) maintained a voltage of 3V or more even when a nail was pierced, did not emit smoke, and the temperature of the casing and nail was below 50°C, with almost no heat generation due to short circuit. This is thought to be because the framework present inside the active material layer of the negative electrode coats the active material, etc., blocking the movement of electrons and suppressing short circuit.

[0218] <Electrode peeling test> (Example 43 and Comparative Example 4) A peel test was carried out on the negative electrodes used in the batteries of Example 43 and Comparative Example 4. The peel test was carried out in accordance with JIS K685, in which an adhesive tape (Scotch, No. 845, Book Tape) was pressed onto the active material layer of the negative electrode with a 1 kg roller, and the evaluation was carried out under conditions of a pulling speed of 300 mm / min and an angle of 180° in a 25°C environment. FIG. 16 shows photographs of the negative electrodes and adhesive tapes of Example 43 and Comparative Example 4 after the peel test. As is clear from FIG. 16, the negative electrode of Comparative Example 4, which did not use a skeletal forming agent, has the peeled active material layer attached to the adhesive tape, while the negative electrode of Example 43, which used a skeletal forming agent, has almost no active material layer attached to the adhesive tape. It was shown that the peel strength was improved.

[0219] <Study of negative electrode active material> (Examples 44 to 59 and Comparative Examples 5 to 20) The effects of the presence or absence of a skeletal former were compared using various negative electrode active materials shown in Table 4. Examples 44 to 59 were produced by applying a slurry consisting of the negative electrode active material, AB, and PVdF shown in Table 4 to copper foil (10 μm) under an adjusted pressure, then using a spray gun to coat and impregnate the active material layer with the skeletal former, and heat treating at 160° C. The solid content ratio of the electrode slurry was 88 mass % for the electrode active material, 4 mass % for AB, and 8 mass % for PVdF.

[0220] The framework forming agent is Li 0.05 Na 1.95 The aqueous solution is composed of O·3SiO2 and a non-ionic surfactant (registered trademark: Triton X-100), and Li 0.05 Na 1.95 The solid concentration of O·3SiO2 was 7.5 mass%, and the solid concentration of the surfactant was 0.03 mass%. In this test, the test electrode was prepared by coating on one side.

[0221] The test battery used lithium metal as the counter electrode and 1M LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 50:50 vol%, + vinylene carbonate 1 mass% as the electrolyte. The separator used was a polypropylene (PP / PE / PP) three-layer microporous membrane (25 μm). The charge / discharge test was performed at a current density of 0.1 mA / cm. 2 The test environment temperature was 30°C, and the cut-off potential, the active material density of the electrode (one side), the electrode thickness, and the skeletal density (one side) were as shown in Table 4.

[0222] Table 5 shows the cycle life characteristic test results of each electrode having a skeleton (Examples 44 to 59). Table 6 shows the cycle life characteristic test results of each electrode having no skeleton (Comparative Examples 5 to 20) for comparison. As is clear from a comparison of Tables 5 and 6, the electrodes using Si, SiO, Ge, In, and Fe2O3 as active materials showed excellent cycle life characteristics by using a skeleton-forming agent. Among these, the electrodes using Si as the active material (Example 56 and Comparative Example 17) showed a particularly remarkable difference. This is thought to be because the strong skeleton-forming agent was constructed in the active material layer, suppressing the destruction of the electronic conductive network due to volume change.

[0223] On the other hand, no significant difference was observed in cycle life characteristics with or without a framework former for Ag, Ag2O, Sb, Sb2S3, SnO2, CuO, NiO, artificial graphite, and hard carbon. These active materials have smaller volume changes than Si, SiO, Ge, In, and Fe2O3, which is probably why no clear difference was observed under the test conditions.

[0224] However, in the case of Sn, the cycle life characteristics deteriorated when a skeleton forming agent was used. This is presumably because Sn has a high dissolution rate when added to the skeleton forming agent and could not maintain the shape of the active material, resulting in capacity degradation.

[0225]

Table 4

[0226]

Table 5

[0227]

Table 6

[0228] <Examination of the mixing ratio of Si and graphite> (Examples 60 to 63 and Comparative Examples 21 to 24) In an electrode using a mixture of Si (1 μm) and artificial graphite (19 μm) as the negative electrode active material, the presence or absence of the effect of skeleton formation was compared. Examples 60 to 63 were prepared by coating a slurry composed of the negative electrode active material, AB, and PVdF shown in Table 7 on a copper foil (10 μm), adjusting the pressure, coating and impregnating the active material layer with a skeleton forming agent using a spray gun, and heat-treating at 160 °C.

[0229] Also, for comparison, electrodes without coating and impregnation with a skeleton forming agent were prepared (Comparative Examples 21 to 24). The solid content ratio of the electrode slurry was 88% by mass of the electrode active material, 4% by mass of AB, and 8% by mass of PVdF. The skeleton forming agent is an aqueous solution composed of Li 0.05 Na 1.95 O·3SiO2 and a nonionic surfactant (registered trademark: Triton X-100), and an aqueous solution with a solid content concentration of Li 0.05 Na 1.95 O·3SiO2 of 7.5% by mass and a solid content concentration of the surfactant of 0.03% by mass was used. In this test, the test electrode was prepared by single-sided coating.

[0230] The test battery used lithium metal as the counter electrode and 1M LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 50:50 vol%, + vinylene carbonate 1 mass% as the electrolyte. A polypropylene (PP / PE / PP) three-layer microporous membrane (25μm) was used as the separator. The charge / discharge test was performed with a current density of 0.1C-rate, a test environment temperature of 30°C, and a cut-off potential of 0.0 to 1.4V (vs. Li+ / Li). The skeletal density (one side) is as shown in Table 8. The capacity density of the test electrode was 3.0mAh / cm 2 It was decided.

[0231] Fig. 10 is a graph showing a comparison of cycle life characteristics of Examples 60 to 63 in which a skeletal forming agent was applied and Comparative Examples 21 to 24 in which a skeletal forming agent was not applied. As is clear from Fig. 10, when the total amount of active material contained in the negative electrode is taken as 100 mass%, electrodes with Si of 10 mass% or less (Example 60, Example 61, Comparative Example 21, Comparative Example 22) did not show a significant change, but electrodes with Si of 20 mass% or more (Example 62, Example 63, Comparative Example 23, Comparative Example 24) clearly showed an improvement in life characteristics. In particular, electrodes with Si of 50 mass% (Example 63 and Comparative Example 24) showed an overwhelming improvement in life characteristics by forming a skeletal structure.

[0232] [Table 7]

[0233] [Table 8]

[0234] <Study of various positive electrode materials> The effect of the amount of the skeleton-forming agent applied was compared using each positive electrode active material. The test electrode was prepared by applying a slurry consisting of the positive electrode active material, AB, and PVdF shown in Table 9 to an aluminum foil (20 μm) under an adjusted pressure, impregnating the active material layer with the skeleton-forming agent using a spray gun, and heat-treating at 170° C. The solid content ratio of the electrode slurry was 90 mass% for the electrode active material, 5 mass% for AB, and 5 mass% for PVdF.

[0235] The skeletal forming agent used in Examples 64 to 72 was an aqueous solution of Na2O·2.8SiO2 and a nonionic surfactant (registered trademark: Triton X-100), with a solid concentration of Na2O·3SiO2 of 5.5% by mass and a solid concentration of the surfactant of 0.03% by mass. The skeletal forming agent used in Examples 73 to 81 was an aqueous solution of Na2O·2.8SiO2 and a nonionic surfactant (registered trademark: Triton X-100), with a solid concentration of Na2O·3SiO2 of 1.1% by mass and a solid concentration of the surfactant of 0.03% by mass.

[0236] Table 9 shows the skeletal density per electrode surface and the cutoff potential for each of Examples 64 to 81. However, for Examples 72 and 81, charging was performed up to 4.6 V only in the first charge.

[0237] In this test, the test electrode had an electrode capacity of 2.0 mAh / cm 2 The test battery was prepared by coating one side so that the electrode was coated with lithium metal. The test battery used lithium metal as the counter electrode and 1M LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 50:50 vol% as the electrolyte. The separator used was a polypropylene (PP / PE / PP) three-layer microporous membrane (25 μm). The charge / discharge test was performed at a test environment temperature of 30°C, with a charge / discharge rate of 0.1 C-rate for 1 to 10 cycles.

[0238] Table 10 shows the cycle life characteristic test results for Examples 64 to 81. As is clear from Table 10, 2 The positive electrodes (Examples 64 to 72) having a skeletal density of more than 0.5 mg / cm 2It can be seen that the discharge capacity is smaller than that of the positive electrodes (Examples 73 to 81) having the following skeletal densities: 2 It has been found that it is preferable that:

[0239] [Table 9]

[0240] [Table 10]

[0241] <High temperature durability of positive electrode> (Examples 82 to 84 and Comparative Examples 21 to 23) In Example 82, the electrode capacity is 1.0 mAh / cm 2 , skeletal density is 0.06mg / cm 2 Example 83 is the same as Example 74, except that the electrode capacity is changed to 1.0 mAh / cm 2 , skeletal density is 0.07mg / cm 2 Example 84 is the same as Example 76, except that the electrode capacity was changed to 1.0 mAh / cm 2 , skeletal density is 0.11 mg / cm 2 In Comparative Example 21, the electrode capacity was changed to 1.0 mAh / cm 2 In Comparative Example 22, the electrode capacity was set to 1.0 mAh / cm 2 In Comparative Example 23, the electrode capacity was set to 1.0 mAh / cm 2 The same as Example 81 except that no scaffold was provided.

[0242] All batteries were fabricated using the positive electrodes of Examples 82 to 84 and Comparative Examples 21 to 23. 2The negative electrode was fabricated by applying a slurry consisting of SiO, AB, and polyimide (PI) to a copper foil (40 μm) under an adjusted pressure, and then heat-treating it at 300°C. The solid content ratio of the negative electrode slurry was 79 mass% electrode active material, 3 mass% AB, and 18 mass% PI. Before being assembled into a battery, the negative electrode was electrochemically filled with Li to compensate for the irreversible capacity.

[0243] The test battery used 1M LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 50:50 vol%, + vinylene carbonate 1 mass% as the electrolyte. The separator used glass nonwoven fabric (GA-100, manufactured by Toyo Roshi Co., Ltd.). The charge-discharge test was performed at a test environment temperature of 80°C, with 10 cycles of charge-discharge repeated at a current density of 0.1 C-rate, followed by 30 cycles of charge-discharge at 1 C-rate. The cut-off potential was 4.15V to 2.0V for Example 82 and Comparative Example 21, 4.15V to 2.0V for Example 83 and Comparative Example 22, and 4.25V to 2.0V for Example 84 and Comparative Example 23.

[0244] FIG. 11 is a graph showing a comparison of cycle life characteristics of Examples 82 to 84 in which a skeletal forming agent was applied and Comparative Examples 21 to 23 in which a skeletal forming agent was not applied. As is clear from FIG. 11, it can be seen that Examples 82 to 84 in which a skeletal forming agent was applied have improved cycle life characteristics compared to Comparative Examples 21 to 23. When the PVdF binder is exposed to a high-temperature electrolyte, it absorbs the electrolyte and swells, increasing the electrode resistance, but it is believed that by using electrodes (Examples 82 to 84) coated with a skeletal forming agent that has excellent swelling resistance, the swelling of the binder is suppressed even in an electrolyte solution as hot as 80°C. In addition, the application of the skeletal forming agent to the positive electrode active material layer also suppresses the decomposition of the electrolyte solution, which is believed to have contributed to the improvement of the cycle life characteristics.

[0245] [5. Effects of this embodiment] According to the above embodiment, the following effects are achieved. By using a skeleton-forming agent containing A2O·3SiO2 (A=Na, Li) for the electrode, the electrode has excellent heat resistance, high strength, and improved cycle life characteristics. In addition, a tough current collector is not essential, and the occurrence of wrinkles, cracks, etc. in the current collector can be suppressed. In addition, it is not necessary to use a binder with a large irreversible capacity. In addition, even if the electronic conductivity of the active material layer is high, heat generation due to internal short circuit can be reduced. In addition, the skeleton-forming agent has heat resistance exceeding 1000°C and is not carbonized. Even if an electrode uses an alloy-based material with a large volume change and a binder with low adhesive strength, good life characteristics can be obtained. In addition, the active material layer does not swell much even when it comes into contact with a high-temperature electrolyte.

[0246] -Second embodiment- [1. Structure of the skeleton forming agent and electrode] Next, a second embodiment of the present invention will be described. The main difference between the first and second embodiments is that the skeleton forming agent contains ceramics. Figure 12 shows an image of a cross section of an electrode in the second embodiment, and the skeleton forming agent in the second embodiment contains ceramic powder or solid electrolyte powder that has excellent alkali resistance.

[0247] FIG. 3 shows an example of a manufacturing process. By applying the skeletal forming agent of the second embodiment to the surface of the electrode body, the alumina in the skeletal forming agent is laminated on the surface of the active material layer to form an electrically insulating ceramic layer or solid electrolyte layer, and the skeletal forming agent penetrates into the active material layer.

[0248] This allows a strong skeleton to be formed, and the occurrence of peeling and cracking during drying can be suppressed. In addition, pores are formed between the inorganic particles, providing good lyophilicity with the electrolyte. In addition, the ceramic layer can serve as a separator, making it possible to construct a battery without using a separate separator.

[0249] 2. Working Examples Next, in the second embodiment, examples in which the composition of the skeleton-forming agent and the like are variously changed will be described.

[0250] <Examination of the Ratio of Na2O·3SiO2 and α-Al2O3> (Examples 85 to 87 and Comparative Example 23) Table 11 shows the solid content compositions of the skeleton formers used in Examples 85 to 87. In addition, an electrode using polyimide (PI) as the skeleton former was fabricated (Comparative Example 23). α-Al2O3 powder with a median diameter (D 50 ) of 0.95 μm was used. The solid content concentration of the skeleton former was set to 10% by mass when the solid contents of Na2O·3SiO2 and α-Al2O3 were 100% by mass.

[0251]

Table 11

[0252] The negative electrode (4.0 mAh / cm 2 ) was prepared by coating a slurry composed of SiO, carbon black (CB), and an acrylic binder on a copper foil (10 μm), adjusting the pressure, coating and impregnating the active material layer with the skeleton former shown in Table 11 using a spray gun, and heat-treating at 160 °C. The skeleton density of the electrode was 3.0 mg / cm per side 2 . The solid content ratio of the negative electrode slurry was 90% by mass of SiO, 5% by mass of CB, and 5% by mass of the acrylic binder. Note that the negative electrode electrochemically compensates for the irreversible capacity portion of Li before being assembled into the battery.

[0253] The positive electrode (2.0 mAh / cm 2 ) was prepared by coating a slurry composed of LiFePO4, CB, and an acrylic binder on an aluminum foil (20 μm), adjusting the pressure, and heat-treating at 160 °C. The solid content ratio of the positive electrode slurry was 91% by mass of LiFePO4, 5% by mass of CB, and 4% by mass of the acrylic binder. As the electrolyte for the test battery, 1 M LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 50:50 vol%, + 1% by mass of vinylene carbonate was used.

[0254] In this test, no separator was used. The charge / discharge test was performed at a test environment temperature of 60° C. and at a current density of 0.1 C-rate. The cutoff potential was 4.0V to 2.5V.

[0255] FIG. 13 shows the initial charge / discharge curves of the test batteries of Examples 85 to 87. It can be seen that they function as batteries without using a separator. Note that no battery test was performed for Comparative Example 23. This is because the electrode resistance increased due to the coating of PI on the active material layer, and Li ions could not be electrochemically doped.

[0256] <Study on particle size of alkali-resistant ceramic> As shown in Table 12, the particle size of α-Al2O3 was changed, the skeletal forming agent was applied to the surface of the electrode body, and then dried. The coating property, liquid property, binding property, foaming state, aggregation state, and sedimentation state were observed. 0.05 Na 1.95 The solid concentration of the framework forming agent is Li 0.05 Na 1.95 If the solid content of O.3SiO2 and α-Al2O3 is taken as 100 mass%, it contains 25 mass%. The particle size of the inorganic particles shown in Table 12 is the median diameter (D 50 As shown in Table 12, in the second embodiment, it is found that the particle size of the ceramic is preferably within the range of 0.2 to 20 μm.

[0257] [Table 12]

[0258] [3. Effects of this embodiment] According to the present embodiment, the following effects are obtained. 50By applying a ceramic layer (0.2 to 20 μm thick) to the electrode surface, a strong skeleton can be formed in the active material layer, and peeling and cracking during drying can be suppressed. Also, pores are formed between the inorganic particles, resulting in good lyophilicity with the electrolyte. In addition, the ceramic layer acts as a separator, making it possible to construct a battery without using a separate separator.

[0259] -Other embodiments- <Formation of the skeleton of active material granules> (Examples 88 to 93) This is a test on the manufacturing method of silicon granules using a skeleton forming agent. The Si granules are Si(D 50 A suspension consisting of AB, VGCF and PI was spray-dried at a liquid delivery rate of 5 g / min, a spray pressure of 0.1 MPa and a drying temperature of 80 to 180°C. 50 The solid content ratio of the suspension is as shown in Table 13.

[0260] Next, the Si granules to which the skeletal forming agent was applied were transferred to a fluidized bed, and the granules obtained by spray drying were mixed with skeletal forming agent (Li 0.2 Na 1.8 The granules obtained by spray drying and the skeletal agent were taken as 100% by mass, and the skeletal agent was adjusted to 1% by mass.

[0261] Fig. 14 shows SEM images of the Si granules (Examples 88 to 93) to which the obtained skeleton forming agent was applied. In Example 88, the amount of PI contained in the suspension was small, and it was difficult to obtain spherically shaped granules, but it was found that as the amount of PI increased, it became easier to obtain spherical granules. It was also found that adding fibrous particles such as VGCF made it easier to form sea urchin-shaped granules.

[0262] [Table 13]

[0263] <Aluminum phosphate-based skeleton-forming agent (Example 94)> Test electrode (4.0mAh / cm 2 The electrode was fabricated by applying a slurry consisting of Si (1 μm), CB, and PVdF binder to a copper foil (40 μm) at an adjusted pressure, then using a spray gun to coat and impregnate the active material layer with a skeletal former, followed by heat treatment at 300 °C. The skeletal former was prepared by dissolving aluminum phosphate (Al2O3 3P2O5) in water and adjusting the solid content to 5 mass %. The skeletal density of the electrode was 2.0 mg / cm per side. 2 The solid content ratio of the negative electrode slurry was 90 mass % for Si, 4 mass % for CB, and 8 mass % for the PVdF binder.

[0264] The test battery had a counter electrode of metallic Li, and 1M LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 50:50 vol%, + vinylene carbonate 1 mass% was used as the electrolyte. A glass nonwoven fabric (GA-100, manufactured by Toyo Roshi Co., Ltd.) was used as the separator. The charge / discharge test was performed at a test environment temperature of 30°C, and at current densities of 0.1C-rate, 0.5C-rate, and 1.0C-rate. The cutoff potential was 1.0V to 0.01V. Figure 15 shows the charge / discharge curves at each rate for Example 94. It was found that a stable reversible capacity was also exhibited when aluminum phosphate (Al2O3·3P2O5) was used as the framework forming agent.

[0265] <Evaluation as a binder> Comparative Example 24 This test used a framework forming agent as a binder. The binder was an alkali metal silicate (Li 0.05 Na 1.95 Water was added to adjust the solids concentration of the test negative electrode (2 mAh / cm 2 ) is Si(D 50A slurry consisting of copper foil (10 μm) with a diameter of 1 μm, carbon black, and an inorganic binder was applied to the copper foil and heat-treated at 150° C. The solid content ratio of the electrode slurry was 19 mass % Si, 4 mass % CB, and 76 mass % binder.

[0266] Comparative Example 25 Comparative Example 25 was the same as Comparative Example 24, except that the binder was changed from alkali metal silicate to primary aluminum phosphate (Al2O3·3P2O5). Note that a commercially available reagent (manufactured by Aesar) was used as the aluminum phosphate.

[0267] (Reference example 1) As a binder, alkali metal silicate (Li 0.05 Na 1.95 O 2.8SiO2) and α-Al2O3 (D 50 The mixture was mixed with water to adjust the solid content to 40% by mass. Other conditions were the same as those in Comparative Example 24.

[0268] (Reference example 2) As the binder, aluminum phosphate (Al2O3·3P2O5) and α-Al2O3 (D 50 The mixture was mixed at a ratio of 50:50 by mass, and water was added thereto so that the solid content of the mixture became 40 by mass. The other conditions were the same as those of Comparative Example 25.

[0269] In Comparative Example 25, when the slurry was mixed, Si reacted with the alkali metal silicate, generating hydrogen gas and foaming the slurry. In Comparative Example 25 and Comparative Example 26, when the electrode was pre-dried at 80°C, the active material layer expanded, and a uniform electrode was not obtained. Furthermore, when the electrodes of Comparative Example 25 and Comparative Example 26 were heat-treated at 150°C, the active material layer significantly shrunk in volume, cracked, and fell off from the current collector.

[0270] On the other hand, in Reference Example 1, when the slurry was mixed, Si reacted with the alkali metal silicate to generate hydrogen gas and foam the slurry, but the active material layer did not expand when provisionally dried at 80° C. Furthermore, when this electrode was heat-treated at 150° C., the volumetric shrinkage was suppressed compared to Comparative Example 25, and the active material layer did not crack or fall off from the current collector.

[0271] In Reference Example 2, hydrogen gas was not generated during mixing of the slurry, so the slurry did not foam, and the active material layer did not expand even during temporary drying at 80° C. Furthermore, when this electrode was heat-treated at 150° C., the active material layer did not crack or fall off from the current collector, as compared with Comparative Example 25.

[0272] The reason why the active material layer expanded at 80°C in Comparative Examples 25 and 26 is believed to be that the vaporized gas (water vapor) was trapped in the active material layer when the slurry was dried, causing the active material layer to expand. Furthermore, at 150°C, the active material layer cracked due to the large volumetric shrinkage caused by the alkali metal silicate and aluminum phosphate, causing the active material layer to fall off from the current collector.

[0273] On the other hand, Reference Examples 1 and 2 contain non-binding Al2O3 as a binder, and it is believed that gas is discharged between the Al2O3 and Al2O3 particles when the electrode is dried, and the active material layer does not expand. Furthermore, it is believed that at 150°C, Al2O3 suppresses the volumetric shrinkage of the alkali metal silicate and aluminum phosphate, preventing the active material layer from cracking and falling off from the current collector.

[0274] These phenomena are the same as when, for example, mochi is heated, the water vapor inside becomes trapped within the mochi and expands, but in cookies, which are made primarily from wheat flour, the water vapor can escape through the gaps in the flour, making them less likely to expand like mochi.

[0275] A charge-discharge test was performed using the electrodes of Reference Example 1 and Reference Example 2. A half cell was fabricated using 1M LiPF6 / EC:DEC=50:50vol.%, +VC1% by mass as the electrolyte, a separator made of a polyolefin microporous film (20μm) and a glass nonwoven fabric (GA-100) stacked together, and metal Li as the counter electrode. The charge-discharge test was performed at an environmental temperature of 30°C, a current density of 0.25C-rate, and a cutoff potential of 1.5V to 0.01V.

[0276] A comparison of the initial charge-discharge efficiency shows that the alkali metal silicate system (Reference Example 1) had a 71% initial charge-discharge efficiency, while the aluminum phosphate system (Reference Example 2) had a 67% initial charge-discharge efficiency, meaning that the alkali metal silicate system had a smaller irreversible capacity than the aluminum phosphate system.

[0277] FIG. 18 shows the cycle life characteristics of Reference Example 1 and a photograph of the electrode (collector side) after 200 cycles. The capacity retention rate after 100 cycles was 78% compared to the initial discharge capacity of 2609 mAh / g. It is believed that the formation of a strong inorganic binder (alkali metal silicate) skeleton in the active material layer made the conductive network less likely to be destroyed by the expansion and contraction of Si, resulting in the excellent capacity retention rate. The reason why even a thin copper foil could be used without distortion is believed to be that the strength of the inorganic binder (alkali metal silicate) is higher than that of copper.

[0278] <Confirmation analysis of inorganic skeleton forming agent> (Reference example 3) This test was conducted to confirm whether the skeleton forming agent had penetrated into the electrode. The mock electrode was made of Al2O3(D 50The electrode was fabricated by applying a slurry consisting of α-Al2O3 (α = 9μm), AB, and PVdF binder to copper foil (10μm) at an adjusted pressure, then using a spray gun to coat and impregnate the active material layer with the skeleton-forming agent, and then heat-treating at 150℃. The skeleton-forming agent was prepared by dissolving alkali metal silicate (Na2O 3SiO) in water and adjusting the solid content to 8 mass%. No surfactant was added. The solid content ratio of the mock electrode slurry was 85 mass% α-Al2O3, 5 mass% CB, and 10 mass% PVdF binder.

[0279] (Reference example 4) Reference Example 4 is the same as Reference Example 3 except that the electrode was not coated and impregnated with the framework forming agent for comparison. FIG. 20 shows the results of glow discharge optical emission spectroscopy (GDS) of Reference Example 3 and Reference Example 4. The GDS measurement conditions were a measurement diameter of 4 mmφ and Ne gas pressure of 2000 Pa. The measurement wavelengths were 121 nm for H, 685 nm for F, 130 nm for O, 156 nm for C, 396 nm for Al, and 251 nm for Si. The time on the horizontal axis is the time of sputtering treatment, which is an index corresponding to the depth direction of the active material layer (direction from the electrode surface to the current collector). The intensity on the vertical axis is the emission intensity, which is an index corresponding to the content of the element. As is clear from FIG. 20, the presence of Si could not be confirmed in Reference Example 4, whereas the presence of Si was not constant from the surface to the inside in Reference Example 3, but it was confirmed that Si was present in the deep layer. This result proves that by applying the skeletal forming agent to the electrode surface, the skeletal forming agent can penetrate into the active material layer.

[0280] As described above, the preferred embodiment of the present invention has been described with reference to the drawings, but various additions, modifications, or deletions are possible within the scope of the present invention. For example, various concentrations and ratios such as the solid content concentration of the alkali metal silicate of the skeleton forming agent are not limited to the numerical values ​​of the above-mentioned embodiment. In addition, in the above-mentioned embodiment, the alkali metal silicate is not limited to A2O·3SiO2 (A=Li, Na) Li or Na, and the coefficient of SiO2 is not limited to 2 to 3. In addition, the skeleton forming agent is not limited to aluminum monophosphate (Al2O3·3P2O5) as a phosphate, and the coefficient of P2O5 is not limited to 3. Therefore, such things are also included in the scope of the present invention.

Claims

1. It is a binder used for granulating active materials. A granulation binder comprising a silicate having a siloxane bond or a phosphate having an aluminophosphate bond as a component.

2. The silicate is represented by the general formula A 2 O.nSiO 2 It is a structure represented by A is at least one of Li, Na, K, a triethanolammonium group, a tetramethanolammonium group, a tetraethanolammonium group, and a granidine group, and n is 1.6 or more and 3.9 or less. The negative granulation binder according to claim 1.

3. In the above general formula, A is Li or Na; n is 2.0 or more and 3.5 or less; The granulation binder according to claim 2.

4. The silicate or the phosphate has an amorphous structure. The granulation binder according to claim 1.

5. The active material is an active material containing a Si-based material; The granulation binder according to any one of claims 1 to 4.

6. A granulation binder according to claim 1 and an active material, Active material granules.

7. The surface of the active material is coated with the granulation binder. The active material granule according to claim 6.

8. The particles of the active material have a median diameter (D 50 ) in the range of 1 μm to 100 μm, The active material granule according to claim 6.

9. The primary particles of the active material before granulation with the granulation binder have a median diameter (D 50) in the range of 0.01 μm to 10 μm, The active material granule according to claim 6.

10. The active material includes a Si-based material. The active material granule according to any one of claims 6 to 9.

11. The active material further includes a carbon-based material. The active material granule according to claim 10.

12. A method for producing active material granules, A step A of dispersing an active material in a granulation binder containing a silicate having a siloxane bond or a phosphate having an aluminophosphate bond as a component to obtain a suspension; A step B of spraying the suspension to obtain agglomerates; and a step C of drying the agglomerated particles. A method for producing active material granules.

13. A method for producing active material granules, A step A of fluidizing and mixing the active material at a predetermined temperature to obtain primary granules; A step B of spraying a granulation binder containing a silicate having a siloxane bond or a phosphate having an aluminophosphate bond to the primary granules to obtain an aggregate; and a step C of drying the aggregate. A method for producing active material granules.

14. The step A is a step of further adding an organic binder and mixing it with the active material to obtain primary granules, The method for producing an active material granule according to claim 13.

15. The active material includes a Si-based material. The method for producing an active material granule according to any one of claims 12 to 14.

16. The active material further includes a carbon-based material. The method for producing an active material granule according to claim 15.

Citation Information

Patent Citations

  • Nonaqueous secondary battery

    JP1996298135A

  • Nonaqueous electrolyte battery

    JP1997306541A

  • Lithium ion battery and manufacturing method thereof

    JP2001508916A

  • Lithium battery

    JP2002270152A

  • Composition for electrochemical device electrode binder, composition for electrochemical device electrode, electrochemical device electrode, and electrochemical device

    JP2010170852A