Artificial hair fiber
The use of a vinyl chloride resin and maleimide copolymer composition in artificial hair fibers addresses issues of heat shrinkage and gloss, resulting in improved spinnability and appearance.
Patent Information
- Application Number
- JP2024133818
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-03-15
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing artificial hair fibers exhibit high heat shrinkage, high gloss, and poor spinnability, which affects their performance and appearance.
A resin composition comprising 50 to 99% vinyl chloride resin and 1 to 50% maleimide copolymer, with specific monomer unit ratios and molecular weights, is used to create artificial hair fibers that minimize heat shrinkage and improve spinnability.
The fibers demonstrate low heat shrinkage, reduced gloss, and enhanced spinnability, making them more comparable to human hair in appearance and processing.
Smart Images

Figure 2024164060000001 
Figure 2024164060000002
Abstract
Description
[Technical field]
[0001] The present invention relates to fibers used for artificial hair such as wigs, hair toupees, and false hair that can be detached from the head (hereinafter, simply referred to as "fibers for artificial hair"). [Background technology]
[0002] Polyvinyl chloride fibers have excellent strength, elongation, etc., and are widely used as fibers for artificial hair that constitute hair accessories. Various efforts have been made to improve the appearance of such fibers for artificial hair in order to make the synthetic resin fibers resemble human hair.
[0003] It has been disclosed that by using a composition containing a polyvinyl chloride resin, a chlorinated polyvinyl chloride resin, and a polymaleimide resin, it is possible to obtain polyvinyl chloride fibers that have little thermal shrinkage even in an atmosphere of 100°C or higher (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2004-225164 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a fiber for artificial hair which has little heat shrinkage, low gloss and excellent spinnability. [Means for solving the problem]
[0006] As a result of investigations by the present inventors, it has been found that by using a resin composition containing a vinyl chloride resin and a maleimide copolymer having a specific composition, it is possible to obtain artificial hair fibers which have little thermal shrinkage, low gloss and excellent spinnability. That is, the present invention provides: (1) A fiber for artificial hair, which is composed of a resin composition containing a vinyl chloride resin and a maleimide copolymer, the vinyl chloride resin being contained in an amount of 50 to 99% by mass in 100% by mass of the resin composition, the maleimide copolymer being contained in an amount of 1 to 50% by mass in 100% by mass of the resin composition, and the maleimide copolymer having 5 to 30% by mass of the maleimide monomer units when the total of aromatic vinyl monomer units, vinyl cyanide monomer units, unsaturated acid anhydride monomer units and maleimide monomer units is taken as 100% by mass. (2) The fiber for artificial hair according to (1), wherein the maleimide copolymer contains 50 to 90% by mass of the aromatic vinyl monomer units, 0.5 to 25% by mass of the vinyl cyanide monomer units, and 0 to 10% by mass of the unsaturated acid anhydride monomer units, when the total of the aromatic vinyl monomer units, the vinyl cyanide monomer units, the unsaturated acid anhydride monomer units, and the maleimide monomer units is taken as 100% by mass. (3) The fiber for artificial hair according to (1) or (2), wherein the ratio of the content of the vinyl chloride resin to the content of the maleimide copolymer is 80 to 99 parts by mass / 1 to 20 parts by mass. (4) The fiber for artificial hair according to any one of (1) to (3), wherein the maleimide copolymer has a weight average molecular weight of 25,000 to 120,000. (5) A hair accessory comprising the artificial hair fiber according to any one of (1) to (4). Regarding. Effect of the Invention
[0007] According to the present invention, it is possible to provide a fiber for artificial hair which has little heat shrinkage, low gloss and excellent spinnability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Terminology explanation> In the present specification, for example, the description "A to B" means A or more and B or less.
[0009] Hereinafter, the embodiments of the present invention will be described in detail. The present invention is not limited to these, and various modifications are possible without departing from the spirit of the present invention. In addition, the embodiments described below can be combined with each other.
[0010] <Artificial hair fibers> The resin composition constituting the artificial hair fiber of this embodiment contains a vinyl chloride resin and a maleimide copolymer. In addition, other synthetic resins may be contained within a range that does not impair the effects of the present invention. Examples of other synthetic resins include vinyl copolymers, specifically, AS resin (acrylonitrile styrene resin) and PLA resin (polylactic acid resin).
[0011] The ratio of the vinyl chloride resin to the maleimide copolymer in the resin composition constituting the artificial hair fiber of this embodiment is preferably 80-99 parts by mass / 1-20 parts by mass (vinyl chloride resin / maleimide copolymer), and more preferably 85-95 parts by mass / 5-15 parts by mass. When the ratio of the vinyl chloride resin to the maleimide copolymer is within this range, the spinnability is good and the heat shrinkage rate of the artificial hair fiber is suppressed.
[0012] <Vinyl chloride resin> The vinyl chloride resin is not particularly limited, and examples thereof include homopolymer resins, which are homopolymers of vinyl chloride, and various copolymer resins. The vinyl chloride resins may be used alone or in combination of two or more types. By using such resins, the quality of the artificial hair fiber, such as the processability and the touch, tends to be improved. The artificial hair fiber of this embodiment may be made of one type of fiber, or may be a mixture of two or more types of fibers made of different materials. The resin composition constituting the artificial hair fiber of this embodiment contains 50 to 99 mass % of vinyl chloride resin, preferably 65 to 95 mass %, and more preferably 65 to 90 mass %, based on 100 mass % of the resin composition.Specifically, for example, it is 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 99 mass %, and may be within a range between any two of the numerical values exemplified here.
[0013] In this embodiment, the vinyl chloride resin may be a non-crosslinked vinyl chloride resin or a crosslinked vinyl chloride resin.
[0014] <Non-crosslinked vinyl chloride resin> The non-crosslinked vinyl chloride resin may be a homopolymer resin or a copolymer resin. The copolymer resin in the non-crosslinked vinyl chloride resin is not particularly limited, but may be, for example, a copolymer resin of vinyl chloride and vinyl esters, such as vinyl chloride-vinyl acetate copolymer resin and vinyl chloride-vinyl propionate copolymer resin; a copolymer resin of vinyl chloride and acrylic esters, such as vinyl chloride-butyl acrylate copolymer resin and vinyl chloride-2-ethylhexyl acrylate copolymer resin; a copolymer resin of vinyl chloride and olefins, such as vinyl chloride-ethylene copolymer resin and vinyl chloride-propylene copolymer resin; or a vinyl chloride-acrylonitrile copolymer resin.
[0015] Among these, vinyl chloride homopolymer is preferable, since the use of such a resin tends to further improve spinnability.
[0016] The viscosity average degree of polymerization V1 of the non-crosslinked vinyl chloride resin is preferably 450 to 1700, more preferably 550 to 1600, and further preferably 650 to 1500. When the viscosity average degree of polymerization V1 is 450 or more, the strength of the fiber for artificial hair tends to be further improved. Also, when the viscosity average degree of polymerization V1 is 1700 or less, the fiber is less likely to break, and the productivity tends to be further improved.
[0017] The viscosity average degree of polymerization can be calculated according to JIS-K6721 by dissolving 200 mg of resin in 50 mL of nitrobenzene, measuring the specific viscosity of this polymer solution in a thermostatic bath at 30° C. using an Ubbelohde viscometer.
[0018] The content of the non-crosslinked vinyl chloride resin is preferably 50 to 99% by mass, more preferably 65 to 97% by mass, based on 100% by mass of the resin composition. Specifically, the content is, for example, 50, 65, 65, 70, 75, 80, 85, 90, 95, or 99% by mass, and may be within a range between any two of the numerical values exemplified here. When the content of the non-crosslinked vinyl chloride resin is 50% by mass or more, the spinnability of the artificial hair fiber tends to be further improved.
[0019] <Cross-linked polyvinyl chloride resin> The "crosslinked" of the crosslinked vinyl chloride resin means that the polymer chain has a branch point and is non-linear, whereas the "non-crosslinked" of the non-crosslinked vinyl chloride resin means that the polymer chain has no branch point and is linear.
[0020] Such a crosslinked vinyl chloride resin is obtained by adding a polyfunctional monomer during polymerization. The polyfunctional monomer used in this case is not particularly limited, but examples thereof include diacrylate compounds such as polyethylene glycol diacrylate and bisphenol A modified diacrylate. The crosslinked vinyl chloride resin has a crosslinked structure and is a mixture of a gel component mainly composed of vinyl chloride insoluble in tetrahydrofuran and a polyvinyl chloride component soluble in tetrahydrofuran.
[0021] The viscosity average degree of polymerization V2 of the component of the crosslinked vinyl chloride resin that dissolves in tetrahydrofuran is preferably 700 to 2300, more preferably 700 to 1800, and even more preferably 750 to 1500. When the viscosity average degree of polymerization V2 of the component that dissolves in tetrahydrofuran is within the above range, the weaving property and spinnability of the artificial hair fiber tend to be further improved.
[0022] The viscosity average degree of polymerization of the components of cross-linked vinyl chloride resin that dissolve in tetrahydrofuran is measured as follows: 1 g of cross-linked vinyl chloride resin is added to 60 mL of tetrahydrofuran and allowed to stand for approximately 24 hours. The resin is then thoroughly dissolved using an ultrasonic cleaner. The insoluble matter in the tetrahydrofuran solution is separated using an ultracentrifuge (30,000 rpm x 1 hour), and the supernatant THF solvent is collected. The THF solvent is then volatilized, and the viscosity average degree of polymerization is measured in the same manner as for non-cross-linked vinyl chloride resin.
[0023] The content of the cross-linked vinyl chloride resin is preferably 1 to 10 mass%, more preferably 3 to 7 mass%, based on 100 mass% of the resin composition. When the content of the cross-linked vinyl chloride resin is 1 mass% or more, the effect of reducing the gloss of the artificial hair fiber tends to be obtained. When the content of the cross-linked vinyl chloride resin is 10 mass% or less, the spinnability of the artificial hair fiber tends to be further improved.
[0024] <Chlorine content in polyvinyl chloride resin> The chlorine content of the vinyl chloride resin of the present embodiment is preferably 50.0 to 60.0%, and more preferably 55.0 to 57.0%. When the chlorine content of the vinyl chloride resin is within this range, excellent spinnability can be obtained.
[0025] <Vinyl chloride resin with high chlorine content> The vinyl chloride resin of the present embodiment may contain a vinyl chloride resin having a high chlorine content within a range that does not impair the effects of the present invention. For example, the resin composition may contain, in 100% by mass, preferably less than 4%, more preferably less than 3%, and even more preferably less than 2% of a chlorinated vinyl chloride resin having a chlorine content of more than 60.0%. The vinyl chloride resin of the present embodiment may not substantially contain, in 100% by mass of the resin composition, a chlorinated vinyl chloride resin having a chlorine content of more than 60.0%. By controlling the content of the chlorinated vinyl chloride resin having a chlorine content of more than 60.0% within such a range, excellent spinnability and the effect of reducing the heat shrinkage rate can be obtained.
[0026] <Method for Producing Vinyl Chloride Resin> The method for producing the vinyl chloride resin is not particularly limited, and conventionally known bulk polymerization, solution polymerization, emulsion polymerization, etc. are used.
[0027] <Vinyl Copolymer>
[0028] The resin composition constituting the fiber for artificial hair of the present embodiment preferably contains 5 to 30% by mass, more preferably 5 to 25% by mass of a vinyl copolymer in 100% by mass of the resin composition. When the content of the vinyl copolymer is 5% by mass or more, the specific gravity of the fiber for artificial hair tends to be low. When the content of the vinyl copolymer is 30% by mass or less, the flame retardancy of the fiber for artificial hair tends to be improved.
[0029] <AS Resin> AS resin is a copolymer having a styrene-based monomer unit and a vinyl cyanide-based monomer unit. For example, there is a styrene-acrylonitrile copolymer.
[0030] As other copolymerizable monomers of AS resin, (meth)acrylate monomers such as methyl methacrylate, butyl acrylate, and ethyl acrylate, (meth)acrylic acid monomers such as methacrylic acid and acrylic acid, and N-substituted maleimide monomers such as N-phenylmaleimide can be used.
[0031] The constituent units of the AS resin are preferably 60 to 90% by mass of the styrene-based monomer unit and 10 to 40% by mass of the vinyl cyanide-based monomer unit in 100% by mass of the AS resin, more preferably 65 to 80% by mass of the styrene-based monomer unit and 20 to 35% by mass of the vinyl cyanide-based monomer unit. If the constituent units are within the above range, the spinnability is excellent. The styrene-based monomer unit and the vinyl cyanide-based monomer unit are values measured by 13C-NMR. The other copolymerizable monomers contained in 100% by mass of the AS resin are preferably 0 to 20% by mass, more preferably 0 to 10% by mass.
[0032] <Method for Producing AS Resin> As a method for producing an AS resin, a known method can be adopted. For example, it can be produced by bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc. As the operation method of the reaction apparatus, any of continuous, batch (batchwise), and semi-batch types can be applied. From the viewpoints of quality and productivity, bulk polymerization or solution polymerization is preferable, and a continuous type is preferable. Examples of the solvent for bulk polymerization or solution polymerization include alkylbenzenes such as benzene, toluene, ethylbenzene, and xylene, ketones such as acetone and methyl ethyl ketone, and aliphatic hydrocarbons such as hexane and cyclohexane.
[0033] In the bulk polymerization or solution polymerization of AS resin, a polymerization initiator and a chain transfer agent can be used, and the polymerization temperature is preferably in the range of 120 to 170° C. Examples of the polymerization initiator include peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(t-butylperoxy)butane, 2,2-di(4,4-di-t-butylperoxycyclohexyl)propane, and 1,1-di(t-amylperoxy)cyclohexane; hydroperoxides such as cumene hydroperoxide and t-butyl hydroperoxide; alkyl peroxides such as t-butyl peroxyacetate and t-amyl peroxyisononanoate; dialkyl peroxides such as t-butylcumyl peroxide, di-t-butyl peroxide, dicumyl peroxide, and di-t-hexyl peroxide; peroxyesters such as t-butylperoxyacetate, t-butylperoxybenzoate, and t-butylperoxyisopropyl monocarbonate; peroxycarbonates such as t-butylperoxyisopropyl carbonate and polyethertetrakis(t-butylperoxycarbonate); N,N'-azobis(cyclohexane-1-carbonitrile), N,N'-azobis(2-methylbutyronitrile), N,N'-azobis(2,4-dimethylvaleronitrile), and N,N'-azobis[2-(hydroxymethyl)propionitrile]; and these may be used alone or in combination of two or more. Examples of chain transfer agents include n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, α-methylstyrene dimer, ethyl thioglycolate, limonene, and terpinolene.
[0034] A known method can be used to remove volatile components such as unreacted monomers and the solvent used in the solution polymerization from the solution after the polymerization of AS resin is completed. For example, a vacuum devolatilization tank equipped with a preheater or a devolatilization extruder equipped with a vent can be used. The devolatilized molten AS resin is transferred to the granulation process, extruded into strands through a multi-hole die, and processed into pellets by the cold cut method, the air hot cut method, or the underwater hot cut method.
[0035] The weight average molecular weight of the AS resin is preferably 50,000 to 200,000, more preferably 60,000 to 150,000, from the viewpoint of kneadability with vinyl chloride resin. Specifically, for example, it is 5, 7, 9, 11, 13, 15, 17, 19, or 200,000, and may be within a range between any two of the numerical values exemplified here. The weight average molecular weight of the AS resin is a value measured in THF solvent using gel permeation chromatography (GPC) in terms of polystyrene, and is a value measured in the same manner as the maleimide copolymer (A). The weight average molecular weight can be adjusted by the type and amount of chain transfer agent, solvent concentration, polymerization temperature, and type and amount of polymerization initiator during polymerization.
[0036] <Maleimide copolymer> The maleimide-based copolymer in this embodiment contains an aromatic vinyl-based monomer unit, a vinyl cyanide-based monomer unit, an unsaturated acid anhydride monomer unit, and a maleimide-based monomer unit. The resin composition constituting the artificial hair fiber of this embodiment contains 1 to 50 mass% of the maleimide copolymer in 100 mass% of the resin composition. It preferably contains 5 to 40 mass%, and more preferably 5 to 30 mass%. Specifically, it is, for example, 1, 5, 8, 10, 12, 15, 20, 25, 30, 35, 40, 45, or 50 mass%, and may be within a range between any two of the numerical values exemplified here.
[0037] The monomer units contained in the maleimide copolymer will be described below.
[0038] <Aromatic vinyl monomer unit> Examples of aromatic vinyl monomers that can be used in the maleimide copolymer according to the present embodiment include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, ethylstyrene, p-tert-butylstyrene, α-methylstyrene, and α-methyl-p-methylstyrene. Among these, styrene is preferred because it can suppress coloring of artificial hair fibers. The styrene monomers may be used alone or in combination of two or more.
[0039] The maleimide copolymer according to the present embodiment preferably contains 50 to 90 mass% of aromatic vinyl monomer units, more preferably 60 to 85 mass%, and even more preferably 65 to 80 mass%, when the total of aromatic vinyl monomer units, vinyl cyanide monomer units, unsaturated acid anhydride monomer units, and maleimide monomer units is taken as 100 mass%. Specifically, for example, it is 50, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90 mass%, and may be within a range between any two of the numerical values exemplified here. If the amount of aromatic vinyl monomer units is less than 50% by mass, the amount of other monomer components contained in the maleimide copolymer will increase relatively, which may result in the maleimide copolymer not melting and being unable to be kneaded with the vinyl chloride resin, or the yellowness index (YI) of the maleimide copolymer will increase, causing problems with coloring of the artificial hair fiber. If the amount of aromatic vinyl monomer units is more than 90% by mass, the heat shrinkage rate of the artificial hair fiber may not be sufficiently suppressed.
[0040] <Vinyl cyanide monomer unit> Examples of vinyl cyanide monomer units that can be used in the maleimide copolymer according to the present embodiment include acrylonitrile, methacrylonitrile, ethacrylonitrile, fumaronitrile, etc. Among these, acrylonitrile is preferred from the viewpoints of suppressing coloration of the artificial hair fiber and suppressing the thermal shrinkage rate of the artificial hair fiber. The vinyl cyanide monomer may be used alone or in combination of two or more kinds.
[0041] The maleimide copolymer according to the present embodiment preferably contains 0.5 to 25% by mass of the vinyl cyanide monomer unit, when the total of the aromatic vinyl monomer unit, the vinyl cyanide monomer unit, the unsaturated acid anhydride monomer unit and the maleimide monomer unit is taken as 100% by mass, more preferably 5 to 20% by mass, and even more preferably 5 to 15% by mass. Specifically, for example, it is 0.5, 1, 5, 10, 15, 20, or 25% by mass, and may be within a range between any two of the numerical values exemplified here. If the amount of the vinyl cyanide monomer unit exceeds 30% by mass, the yellowness index (YI) of the maleimide copolymer increases, and coloring of the artificial hair fiber may become a problem.
[0042] <Unsaturated acid anhydride monomer unit> Examples of the unsaturated acid anhydride monomer unit that can be used in the maleimide copolymer according to the present embodiment include maleic anhydride, itaconic anhydride, citraconic anhydride, and aconitic anhydride. Among these, maleic anhydride is preferred from the viewpoint of suppressing the thermal shrinkage rate of the artificial hair fiber. The unsaturated acid anhydride monomer unit may be used alone or in combination of two or more kinds.
[0043] The maleimide copolymer according to the present embodiment preferably contains 0 to 10 mass% of unsaturated acid anhydride monomer units, more preferably 0.5 to 5 mass%, when the total of aromatic vinyl monomer units, cyanide vinyl monomer units, unsaturated acid anhydride monomer units and maleimide monomer units is 100 mass%. Specifically, for example, it is 0, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 mass%, and may be within a range between any two of the numerical values exemplified here. If the amount of unsaturated acid anhydride monomer units exceeds 10 mass%, the flowability decreases, and the kneadability with vinyl chloride resin may decrease.
[0044] <Maleimide monomer unit> Examples of the maleimide monomer units that can be used in the maleimide copolymer according to the present embodiment include N-alkylmaleimides such as N-methylmaleimide, N-butylmaleimide, and N-cyclohexylmaleimide, and N-arylmaleimides such as N-phenylmaleimide, N-chlorophenylmaleimide, N-methylphenylmaleimide, N-methoxyphenylmaleimide, and N-tribromophenylmaleimide. Among these, N-arylmaleimide is preferred from the viewpoint of suppressing the thermal shrinkage rate of the artificial hair fiber, and N-phenylmaleimide is more preferred. The maleimide monomers may be used alone or in combination of two or more kinds. To incorporate maleimide monomer units into a maleimide copolymer, for example, a raw material consisting of unsaturated dicarboxylic acid monomer units may be copolymerized with another monomer, and the resulting copolymer may be imidized with ammonia or a primary amine. Alternatively, a raw material consisting of a maleimide monomer may be copolymerized with another monomer.
[0045] The maleimide copolymer according to the present embodiment contains 5 to 30% by mass of maleimide monomer units, preferably 5% by mass or more and less than 25% by mass, more preferably 10 to 20% by mass, when the total of aromatic vinyl monomer units, vinyl cyanide monomer units, unsaturated acid anhydride monomer units and maleimide monomer units is taken as 100% by mass. Specifically, for example, it is 5, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, or 30% by mass, and may be within a range between any two of the numerical values exemplified here. If the amount of maleimide monomer units is less than 5% by mass, the thermal shrinkage rate of the artificial hair fiber may not be sufficiently suppressed, and if it exceeds 30% by mass, the maleimide copolymer may not melt with the vinyl chloride resin and may not be kneaded.
[0046] <Copolymerizable monomer> The maleimide copolymer according to the present embodiment may be copolymerized with a copolymerizable monomer other than an aromatic vinyl monomer, a vinyl cyanide monomer, an unsaturated acid anhydride monomer unit, and a maleimide monomer, as long as the effect of the present invention is not impaired. Examples of monomers copolymerizable with the maleimide copolymer include acrylic acid ester monomers such as methyl acrylate, ethyl acrylate, and butyl acrylate, methacrylic acid ester monomers such as methyl methacrylate and ethyl methacrylate, vinyl carboxylic acid monomers such as acrylic acid and methacrylic acid, acrylic acid amide, and methacrylic acid amide. The monomers copolymerizable with the maleimide copolymer may be used alone or in combination of two or more. Such monomers can be copolymerized to the extent that the effects of the present invention are not impaired. From the viewpoint of suppressing the thermal shrinkage rate of the artificial hair fiber, however, the amount of such monomers is preferably 20% by mass or less, and more preferably 10% by mass or less, when the total amount of the aromatic vinyl monomer units, the vinyl cyanide monomer units, the unsaturated acid anhydride monomer units and the maleimide monomer units is taken as 100% by mass.
[0047] <Physical properties of maleimide copolymer> <Melt viscosity of maleimide copolymer> The melt viscosity of the maleimide copolymer in this embodiment is preferably 100 to 100,000 Pa·sec, more preferably 200 to 70,000 Pa·sec. Specifically, for example, it may be 100, 200, 500, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10,000, 20,000, 30,000, 40,000, 50,000, or 100,000 Pa·sec, and may be within a range between any two of the numerical values exemplified here. If it is less than 100 Pa·sec, the thermal shrinkage rate of the artificial hair fiber may not be sufficiently suppressed, and if it exceeds 100,000 Pa·sec, the maleimide copolymer of the resin composition may not melt with the vinyl chloride resin and may not be kneaded. The melt viscosity was measured using a capillary rheometer 1D manufactured by Toyo Seiki Seisakusho Co., Ltd., with a capillary die of L=40 mm and D=1 mm.
[0048] The melt viscosity of the maleimide copolymer can be adjusted by adjusting the compounding ratio of the monomer units constituting the maleimide copolymer. For example, the melt viscosity can be increased by increasing the content of the vinyl cyanide monomer units in the maleimide copolymer, or by increasing the content of the maleimide monomer units in the maleimide copolymer. The melt viscosity can also be increased by increasing the weight average molecular weight of the maleimide copolymer. These adjustment methods can be used in combination.
[0049] <Weight average molecular weight of maleimide copolymer> The weight average molecular weight of the maleimide copolymer in this embodiment is preferably 25,000 to 120,000, more preferably 25,000 to 100,000, and more preferably 30,000 to 80,000. Specifically, for example, it is 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, or 120,000, and may be within a range between any two of the numerical values exemplified here. If the weight average molecular weight is less than 25,000, the thermal shrinkage rate of the artificial hair fiber may not be sufficiently suppressed, and if it exceeds 120,000, the torque during kneading of the resin composition containing the vinyl chloride resin and the maleimide copolymer may increase. The weight average molecular weight is a value calculated as polystyrene by gel permeation chromatography (GPC), and can be measured under the following conditions. Measurement name: SYSTEM-21 Shodex (manufactured by Showa Denko Co., Ltd.) Column: Three PL gel MIXED-B columns (Polymer Laboratories) in series Temperature: 40℃ Detection: Differential refractive index Solvent: Tetrahydrofuran Concentration: 2% by mass Calibration curve: Created using standard polystyrene (PS) (Polymer Laboratories)
[0050] As a method for obtaining a maleimide-based copolymer having a preferred weight-average molecular weight (Mw) in the range of 25,000 to 120,000, there is a method for adjusting the amount of solvent and chain transfer agent added in addition to the method for adjusting the polymerization temperature, polymerization time, and amount of polymerization initiator added. Another method is known in which the molecular weight of the obtained copolymer is reduced by decomposition.
[0051] <Method of producing maleimide copolymer> The polymerization mode of the maleimide copolymer includes, for example, solution polymerization and bulk polymerization. From the viewpoint that a maleimide copolymer having a more uniform copolymer composition can be obtained by performing polymerization while performing addition, solution polymerization is preferred. The solvent for solution polymerization is preferably non-polymerizable from the viewpoint that by-products are unlikely to be produced and adverse effects are small. For example, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and acetophenone, ethers such as tetrahydrofuran and 1,4-dioxane, aromatic hydrocarbons such as benzene, toluene, xylene, and chlorobenzene, N,N-dimethylformamide, dimethyl sulfoxide, and N-methyl-2-pyrrolidone are preferred, and methyl ethyl ketone and methyl isobutyl ketone are preferred from the viewpoint of ease of solvent removal during volatilization and recovery of the maleimide copolymer. The polymerization process can be any of a continuous polymerization method, a batch method (batch method), and a semi-batch method.
[0052] The method for producing the maleimide copolymer is not particularly limited, but is preferably obtained by radical polymerization, and the polymerization temperature is preferably in the range of 80 to 150° C. The polymerization initiator is not particularly limited, but for example, known azo compounds such as azobisisobutyronitrile, azobiscyclohexanecarbonitrile, azobismethylpropionitrile, and azobismethylbutyronitrile, and known organic peroxides such as benzoyl peroxide, t-butylperoxybenzoate, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexanoate, di-t-butylperoxide, dicumyl peroxide, and ethyl-3,3-di-(t-butylperoxy)butyrate can be used, and one or more of these may be used in combination. From the viewpoint of polymerization reaction rate and polymerization rate control, it is preferable to use an azo compound or organic peroxide with a 10-hour half-life of 70 to 120°C. The amount of polymerization initiator used is not particularly limited, but is preferably 0.1 to 1.5% by mass, more preferably 0.1 to 1.0% by mass, based on 100% by mass of all monomer units. If the amount of polymerization initiator used is 0.1% by mass or more, a sufficient polymerization rate can be obtained, which is preferable. If the amount of polymerization initiator used is 1.5% by mass or less, the polymerization rate can be suppressed, making it easy to control the reaction and to obtain the target molecular weight.
[0053] A chain transfer agent can be used in the production of maleimide copolymers. The chain transfer agent used is not particularly limited, but examples thereof include n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, α-methylstyrene dimer, ethyl thioglycolate, limonene, and terpinolene. The amount of chain transfer agent used is not particularly limited as long as it is within a range in which the target molecular weight can be obtained, but is preferably 0.01 to 0.8% by mass, and more preferably 0.1 to 0.5% by mass, relative to 100% by mass of the total monomer units. If the amount of chain transfer agent used is 0.01% by mass to 0.8% by mass, the target molecular weight can be easily obtained.
[0054] The method of introducing maleimide monomer units into a maleimide copolymer includes a method of copolymerizing a maleimide monomer, an aromatic vinyl monomer, and a vinyl cyanide monomer (direct method), or a method of copolymerizing an unsaturated dicarboxylic anhydride, an aromatic vinyl monomer, and a vinyl cyanide monomer in advance, and then reacting the unsaturated dicarboxylic anhydride group with ammonia or a primary amine to convert the unsaturated dicarboxylic anhydride group into a maleimide monomer unit (post-imidization method). The post-imidization method is preferred because it reduces the amount of maleimide monomer remaining in the copolymer.
[0055] Examples of primary amines used in the post-imidization method include alkylamines such as methylamine, ethylamine, n-propylamine, iso-propylamine, n-butylamine, n-pentylamine, n-hexylamine, n-octylamine, cyclohexylamine, and decylamine, and aromatic amines such as chlorine- or bromine-substituted alkylamines, aniline, toluidine, and naphthylamine, among which aniline and cyclohexylamine are preferred. These primary amines may be used alone or in combination of two or more. The amount of primary amine added is not particularly limited, but is preferably 0.7 to 1.1 molar equivalents relative to the unsaturated dicarboxylic anhydride group, and more preferably 0.85 to 1.05 molar equivalents. If the amount is 0.7 molar equivalents or more relative to the unsaturated dicarboxylic anhydride monomer unit in the maleimide-based copolymer, the thermal stability is good, which is preferable. Also, if the amount is 1.1 molar equivalents or less, the amount of primary amine remaining in the maleimide-based copolymer is reduced, which is preferable.
[0056] A catalyst may be used when introducing the maleimide monomer unit by the post-imidization method. The catalyst can improve the dehydration ring-closing reaction in the reaction between ammonia or a primary amine and an unsaturated dicarboxylic anhydride group, particularly in the reaction of converting an unsaturated dicarboxylic anhydride group to a maleimide group. The type of catalyst is not particularly limited, but for example, a tertiary amine can be used. The tertiary amine is not particularly limited, but for example, trimethylamine, triethylamine, tripropylamine, tributylamine, N,N-dimethylaniline, N,N-diethylaniline, etc. are included. The amount of the tertiary amine added is not particularly limited, but it is preferably 0.01 molar equivalent or more relative to the unsaturated dicarboxylic anhydride group. The temperature of the imidization reaction in the present invention is preferably 100 to 250°C, more preferably 120 to 200°C. If the temperature of the imidization reaction is 100°C or more, the reaction rate is sufficiently fast and it is preferable in terms of productivity. It is preferable that the temperature of the imidization reaction is 250° C. or lower, since this can suppress the deterioration of the physical properties of the maleimide copolymer due to thermal degradation.
[0057] A known method can be used to remove volatile matters such as the solvent used in the solution polymerization and unreacted monomers from the solution after the completion of solution polymerization of the maleimide copolymer or the solution after the completion of post-imidization (devolatilization method). For example, a vacuum devolatilization tank equipped with a heater or a devolatilization extruder equipped with a vent can be used. The devolatilized molten maleimide copolymer is transferred to a granulation process, extruded into strands through a multi-hole die, and processed into pellets by a cold cut method, an air hot cut method, or an underwater hot cut method. When the vinyl chloride resin is in powder form, it is preferable to pulverize the maleimide copolymer of the present embodiment into powder form before use. There is no particular limitation on the pulverization method, and any known pulverization technique can be used. Examples of pulverization devices that can be suitably used include turbo mill pulverizers, turbo disk mill pulverizers, turbo cutter pulverizers, jet mill pulverizers, impact pulverizers, hammer pulverizers, and vibration pulverizers.
[0058] <Other additives> Other additives may be used in the artificial hair fiber of this embodiment as necessary. The other additives may be attached to the surface of the artificial hair fiber or may be mixed into the resin composition constituting the fiber.
[0059] Other additives are not particularly limited, but examples thereof include flame retardants, heat stabilizers, and lubricants. When a compound corresponding to the above-mentioned specific compound is attached to the surface of the artificial hair fiber as a heat stabilizer or lubricant, the amount of the compound is limited to the total content of the above-mentioned specific compound.
[0060] <Flame retardants> The flame retardant is not particularly limited as long as it is a conventionally known one, and examples thereof include bromine compounds, halogen compounds, phosphorus-containing compounds, phosphorus-halogen compounds, nitrogen compounds, and metal hydroxide-phosphorus-nitrogen compounds. Among these, bromine compounds, which are bromine-based flame retardants, phosphorus-containing compounds, which are phosphorus-based flame retardants, and nitrogen compounds, which are nitrogen-based flame retardants, are preferred.
[0061] The content of the flame retardant is preferably 3 to 30 parts by mass, and more preferably 10 to 20 parts by mass, based on 100 parts by mass of the resin composition.
[0062] <Heat stabilizer> The heat stabilizer is not particularly limited as long as it is a conventionally known one, and examples thereof include tin-based heat stabilizers, Ca-Zn-based heat stabilizers, hydrotalcite-based heat stabilizers, epoxy-based heat stabilizers, and β-diketone-based heat stabilizers. Among these, Ca-Zn-based heat stabilizers and hydrotalcite-based heat stabilizers are preferred. By using such heat stabilizers, the product life of the artificial hair product can be extended, discoloration of the fibers can be suppressed, and thermal decomposition of the composition during fiber formation can be suppressed. The heat stabilizers may be used alone or in combination of two or more types.
[0063] The tin-based heat stabilizer is not particularly limited, and examples thereof include mercaptotin-based heat stabilizers such as dimethyltin mercapto, dimethyltin mercaptide, dibutyltin mercapto, dioctyltin mercapto, dioctyltin mercapto polymer, and dioctyltin mercaptoacetate; maleate-tin-based heat stabilizers such as dimethyltin maleate, dibutyltin maleate, dioctyltin maleate, and dioctyltin maleate polymer; and laurate-tin-based heat stabilizers such as dimethyltin laurate, dibutyltin laurate, and dioctyltin laurate.
[0064] The Ca-Zn-based heat stabilizer is not particularly limited, but examples thereof include zinc stearate, calcium stearate, zinc 12-hydroxystearate, and calcium 12-hydroxystearate.
[0065] Examples of hydrotalcite-based heat stabilizers include, but are not limited to, complex salt compounds consisting of magnesium and / or an alkali metal and aluminum or zinc, complex salt compounds consisting of magnesium and aluminum, and compounds obtained by dehydrating the crystal water of these complex salt compounds.
[0066] The epoxy-based heat stabilizer is not particularly limited, but examples thereof include epoxidized soybean oil and epoxidized linseed oil.
[0067] The β-diketone-based heat stabilizer is not particularly limited, but examples thereof include stearoylbenzoylmethane and dibenzoylmethane.
[0068] The content of the heat stabilizer is preferably 0.1 to 5.0 parts by mass, and more preferably 1.0 to 3.0 parts by mass, relative to 100 parts by mass of the vinyl chloride resin. By having the content of the heat stabilizer within the above range, the product life of the artificial hair product is extended, discoloration of the fibers is suppressed, and thermal decomposition of the composition when forming the fibers tends to be suppressed.
[0069] <Lubricant> The lubricant is not particularly limited as long as it is a conventionally known lubricant, and examples thereof include metal soap-based lubricants, higher fatty acid-based lubricants, ester-based lubricants, and higher alcohol-based lubricants. By using such a lubricant, in addition to the touch, it is also effective to control the melting state of the composition and the adhesion state between the composition and the metal surfaces of the screw, cylinder, die, etc. in the extruder. The lubricant may be used alone or in combination of two or more kinds.
[0070] The metal soap-based lubricant is not particularly limited, but examples thereof include metal soaps such as stearates, laurates, palmitates, and oleates of Na, Mg, Al, Ca, Ba, and the like.
[0071] Examples of higher fatty acid lubricants include saturated fatty acids such as stearic acid, palmitic acid, myristic acid, lauric acid, and capric acid, unsaturated fatty acids such as oleic acid, and mixtures thereof.
[0072] Examples of higher alcohol lubricants include stearyl alcohol, palmityl alcohol, myristyl alcohol, lauryl alcohol, and oleyl alcohol.
[0073] Examples of the ester-based lubricants include ester-based lubricants consisting of alcohol and fatty acid, pentaerythritol-based lubricants such as monoesters, diesters, triesters, tetraesters of pentaerythritol or dipentaerythritol with higher fatty acids, or mixtures thereof, and montanic acid wax-based lubricants which are esters of montanic acid with higher alcohols such as stearyl alcohol, palmityl alcohol, myristyl alcohol, lauryl alcohol, and oleyl alcohol.
[0074] The content of the lubricant is preferably 0.2 to 5.0 parts by mass, more preferably 1.0 to 4.0 parts by mass, based on 100 parts by mass of the vinyl chloride resin. By having the content of the lubricant within the above range, it is possible to suppress an increase in die pressure during yarn obstruction, yarn breakage, an increase in nozzle pressure, and the like, and production efficiency tends to be further improved.
[0075] In addition to the above, the additives that can be used include processing aids, matting agents, plasticizers, reinforcing agents, ultraviolet absorbers, antioxidants, antistatic agents, fillers, pigments, coloring improvers, conductivity imparting agents, fragrances, and the like.
[0076] <Manufacturing method for artificial hair fibers> The method for producing the artificial hair fiber of this embodiment is not particularly limited, but may be, for example, a method having a step of spinning a resin composition for artificial hair containing the vinyl chloride resin and the maleimide copolymer, and optionally an additive, to obtain a synthetic resin fiber.
[0077] <Preparation of Resin Composition for Artificial Hair Fiber> The resin composition for artificial hair fibers to be spun may be a pellet compound obtained by mixing a resin composition containing a vinyl chloride resin and a maleimide copolymer, and additives used as necessary, using a Henschel mixer, a super mixer, a ribbon blender, or the like, and melt-mixing the resulting powder compound.
[0078] In addition, for producing the pellet compound, kneaders such as a single screw extruder, a counter-rotating twin screw extruder, a conical twin screw extruder, a co-rotating twin screw extruder, a co-kneader, a planetary gear extruder, and a roll kneader can be used.
[0079] The conditions for producing the pellet compound are not particularly limited, but in order to prevent thermal degradation of the resin composition for artificial hair fibers, it is preferable to set the resin temperature to 185° C. or less. Also, in order to remove small amounts of metal pieces from the screw and fibers attached to the protective gloves that may be mixed into the pellet compound, a mesh can be placed near the tip of the screw.
[0080] The cold cutting method can be used to manufacture pellet compounds. It is possible to adopt a means to remove chips (fine powder generated during pellet manufacturing) that may be mixed in during cold cutting. In addition, it is preferable to replace the cutter as needed, since the blade of the cutter may chip after long-term use, making chips more likely to be generated.
[0081] <Spinning process> In the spinning process, the resin composition for artificial hair fibers obtained as described above, for example, a pellet compound, can be extruded and melt spun at a cylinder temperature of 150° C. to 190° C. and a nozzle temperature of 180±15° C. The cross-sectional shape of the nozzle used in this case can be appropriately set according to the cross-sectional shape of the artificial hair fiber to be produced.
[0082] The undrawn fibers melt-spun from the nozzle are introduced into a heating cylinder (heating cylinder temperature: 250° C.) and instantaneously heat-treated, and then taken up by a take-up machine installed at a position about 4.5 m directly below the nozzle. During this take-up, the take-up speed can be adjusted so that the fineness of the undrawn yarn becomes the desired thickness.
[0083] When the resin composition for artificial hair fibers is made into an undrawn yarn, a conventionally known extruder can be used, such as a single screw extruder, a counter-rotating twin screw extruder, or a conical twin screw extruder.
[0084] <Stretching and heat treatment> The undrawn fibers obtained as described above can be subjected to drawing treatment and heat treatment. As an example, the undrawn fibers are drawn 3 times with a drawing machine (at 105°C in air atmosphere) and then heat-treated 0.75 times with a heat treatment machine (at 110°C in air atmosphere) (heat-shrunk until the entire fiber length is 75% of the length before treatment) to produce fibers for artificial hair with a fineness of 58 to 62 denier.
[0085] <Gear processing> Furthermore, the artificial hair fiber obtained as described above may be gear processed as necessary. Gear processing is a method of crimping a fiber bundle by passing it between two meshing high-temperature gears, and the material of the gear used, the shape of the gear waves, the number of gears, etc. are not particularly limited. The crimp wave shape can change depending on the fiber material, fineness, pressure conditions between the gears, etc., but the crimp wave shape can be controlled by the depth of the gear wave groove, the surface temperature of the gear, and the processing speed.
[0086] There are no particular limitations on the gear processing conditions, but preferably, the depth of the gear waveform groove is 0.2 mm to 6 mm, more preferably 0.5 mm to 5 mm, the gear surface temperature is 30 to 100°C, more preferably 40 to 80°C, and the processing speed is 0.5 to 10 m / min, more preferably 1.0 to 8.0 m / min.
[0087] <Products using artificial hair fibers> The artificial hair fiber of this embodiment can be suitably used as head accessories such as hair wigs, hair pieces, braids, and hair extensions. EXAMPLES
[0088] The specific embodiments of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples in any way.
[0089] <Preparation of maleimide copolymer> <Production Example of Maleimide Copolymer (A-1)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 73 parts by mass of styrene, 18 parts by mass of acrylonitrile, 1 part by mass of maleic anhydride, 0.22 parts by mass of α-methylstyrene dimer, and 26 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92 ° C. over 40 minutes while stirring. After the temperature was raised to 92 ° C., a solution in which 7 parts by mass of maleic anhydride and 1.0 part by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 35 parts by mass of methyl ethyl ketone was continuously added over 4.5 hours. After the addition was completed, the temperature was raised to 120 ° C. and the reaction was carried out for 1 hour to terminate the polymerization. Then, 6 parts by mass of aniline and 0.1 parts by mass of triethylamine were added to the polymerization liquid and the reaction was carried out at 140 ° C. for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer A-1. The analytical results of the obtained maleimide copolymer are shown in Table 1.
[0090] <Production Example of Maleimide Copolymer (A-2)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 64 parts by mass of styrene, 20 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, 0.5 parts by mass of α-methylstyrene dimer, and 31 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92 ° C. over 40 minutes while stirring. After the temperature was raised to 92 ° C., a solution in which 14 parts by mass of maleic anhydride and 0.60 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 69 parts by mass of methyl ethyl ketone was continuously added over 5.5 hours. After the addition was completed, the temperature was raised to 120 ° C. and the reaction was carried out for 1 hour to terminate the polymerization. Then, 12 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization liquid and the reaction was carried out at 140 ° C. for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer A-2. The analytical results of the obtained maleimide copolymer are shown in Table 1.
[0091] <Production Example of Maleimide Copolymer (A-3)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 79 parts by mass of styrene, 9 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, 0.52 parts by mass of α-methylstyrene dimer, and 33 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92 ° C. over 40 minutes while stirring. After the temperature was raised to 92 ° C., a solution in which 9 parts by mass of maleic anhydride and 0.60 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 47 parts by mass of methyl ethyl ketone was continuously added over 5 hours. After the addition was completed, the temperature was raised to 120 ° C. and the polymerization was completed by reacting for 1.5 hours. Then, 9 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization liquid and reacted at 140 ° C. for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer A-3. The analytical results of the obtained maleimide copolymer are shown in Tables 1 and 2.
[0092] <Production Example of Maleimide Copolymer (A-4)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 85 parts by mass of styrene, 7 parts by mass of acrylonitrile, 1 part by mass of maleic anhydride, 0.72 parts by mass of α-methylstyrene dimer, and 30 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92°C over 40 minutes while stirring. After the temperature was raised to 92°C, a solution in which 7 parts by mass of maleic anhydride and 0.80 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 33 parts by mass of methyl ethyl ketone was continuously added over 6 hours. After the addition was completed, the temperature was raised to 120°C and the reaction was carried out for 1 hour to terminate the polymerization. Then, 5 parts by mass of aniline and 0.1 parts by mass of triethylamine were added to the polymerization liquid and the reaction was carried out at 140°C for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer A-4. The analytical results of the obtained maleimide copolymer are shown in Table 1.
[0093] <Production Example of Maleimide Copolymer (A-5)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 25 parts by mass of styrene, 26 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, 0.53 parts by mass of α-methylstyrene dimer, and 30 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92°C over 40 minutes while stirring. After the temperature was raised to 92°C, a solution in which 34 parts by mass of styrene, 13 parts by mass of maleic anhydride, and 0.22 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 67 parts by mass of methyl ethyl ketone was continuously added over 3 hours while maintaining the temperature at 92°C. Furthermore, after the addition of maleic anhydride was completed, a solution in which 0.18 parts by mass of t-butylperoxy-2-ethylhexanoate was dissolved in 1 part by mass of methyl ethyl ketone was continuously added over 2.5 hours. After the addition was completed, the temperature was raised to 120°C, and the reaction was carried out for 1 hour to complete the polymerization. Then, 12 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization solution and reacted at 140° C. for 7 hours. After the reaction was completed, the imidization reaction solution was fed into a vent-type screw extruder, and the volatile matter was removed to obtain pellets of maleimide copolymer A-5. The analytical results of the obtained maleimide copolymer are shown in Table 1.
[0094] <Production Example of Maleimide Copolymer (A-6)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 23 parts by mass of styrene, 26 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, 0.32 parts by mass of α-methylstyrene dimer, and 32 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92°C over 40 minutes while stirring. After the temperature was raised to 92°C, a solution in which 33 parts by mass of styrene, 16 parts by mass of maleic anhydride, and 0.22 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 81 parts by mass of methyl ethyl ketone was continuously added over 3 hours while maintaining the temperature at 92°C. Furthermore, after the addition of maleic anhydride was completed, a solution in which 0.18 parts by mass of t-butylperoxy-2-ethylhexanoate was dissolved in 1 part by mass of methyl ethyl ketone was continuously added over 2.5 hours. After the addition was completed, the temperature was raised to 120°C, and the reaction was carried out for 1 hour to complete the polymerization. Then, 14 parts by mass of aniline and 0.3 parts by mass of triethylamine were added to the polymerization solution and reacted at 140° C. for 7 hours. After the reaction was completed, the imidization reaction solution was fed into a vent-type screw extruder, and the volatile matter was removed to obtain pellets of maleimide copolymer A-6. The analytical results of the obtained maleimide copolymer are shown in Table 1.
[0095] <Production Example of Maleimide Copolymer (A-7)> In a 120-liter autoclave equipped with a stirrer, 94 parts by mass of styrene, 2 parts by mass of acrylonitrile, Parts by mass, 0.4 parts by mass of maleic anhydride, 0.58 parts by mass of α-methylstyrene dimer, and 28 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and then the temperature was raised to 92 ° C. over 40 minutes while stirring. After the temperature was raised to 92 ° C., a solution in which 4 parts by mass of maleic anhydride and 1.0 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 18 parts by mass of methyl ethyl ketone was continuously added over 7.5 hours while maintaining the temperature at 92 ° C. After the addition was completed, the temperature was raised to 120 ° C. and the polymerization was completed by reacting for 1 hour. Then, 3 parts by mass of aniline and 0.1 parts by mass of triethylamine were added to the polymerization liquid and reacted at 140 ° C. for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatiles were removed to obtain a pellet-shaped maleimide copolymer A-7. The analysis results of the obtained maleimide copolymer are shown in Table 1.
[0096] <Production Example of Maleimide Copolymer (A-8)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 88 parts by mass of styrene, 1 part by mass of maleic anhydride, 0.48 parts by mass of α-methylstyrene dimer, and 29 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92°C over 40 minutes while stirring. After the temperature was raised to 92°C, a solution in which 11 parts by mass of maleic anhydride and 1.20 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 56 parts by mass of methyl ethyl ketone was continuously added over 8.5 hours. After the addition was completed, the temperature was raised to 120°C and the reaction was carried out for 1 hour to terminate the polymerization. Then, 9 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization liquid and the reaction was carried out at 140°C for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer A-8. The analysis results of the obtained maleimide copolymer are shown in Table 1.
[0097] <Production Example of Maleimide Copolymer (A-9)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 27 parts by mass of styrene, 33 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, 0.11 parts by mass of α-methylstyrene dimer, and 24 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and then the temperature was raised to 92°C over 40 minutes while stirring. After the temperature was raised to 92°C, a solution in which 31 parts by mass of styrene, 7 parts by mass of maleic anhydride, and 0.38 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 37 parts by mass of methyl ethyl ketone was continuously added over 3.5 hours while maintaining the temperature at 92°C. Furthermore, after the addition of maleic anhydride was completed, a solution in which 0.22 parts by mass of t-butylperoxy-2-ethylhexanoate was dissolved in 2 parts by mass of methyl ethyl ketone was continuously added over 2 hours. After the addition was completed, the temperature was raised to 120°C, and the reaction was carried out for 1 hour to complete the polymerization. Thereafter, 6 parts by mass of aniline and 0.1 parts by mass of triethylamine were added to the polymerization solution and reacted at 140° C. for 7 hours. After the reaction was completed, the imidization reaction solution was fed into a vent-type screw extruder, and the volatile matter was removed to obtain pellets of maleimide copolymer A-9. The analytical results of the obtained maleimide copolymer are shown in Table 1.
[0098] <Production Example of Maleimide Copolymer (A-10)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 63 parts by mass of styrene, 22 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, 0.59 parts by mass of α-methylstyrene dimer, and 30 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92 ° C. over 40 minutes while stirring. After the temperature was raised to 92 ° C., a solution in which 13 parts by mass of maleic anhydride and 0.44 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 69 parts by mass of methyl ethyl ketone was continuously added over 4 hours while maintaining the temperature at 92 ° C. After the addition of maleic anhydride was completed, a solution in which 0.16 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 1 part by mass of methyl ethyl ketone was continuously added over 1.5 hours. After the addition was completed, the temperature was raised to 120 ° C., and the reaction was carried out for 1 hour to complete the polymerization. Then, 3 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization solution and reacted at 140° C. for 7 hours. After the reaction was completed, the imidization reaction solution was fed into a vent-type screw extruder, and the volatile matter was removed to obtain pellets of maleimide copolymer A-10. The analytical results of the obtained maleimide copolymer are shown in Table 1.
[0099] <Production Example of Maleimide Copolymer (A-11)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 79 parts by mass of styrene, 9 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, 1.00 parts by mass of α-methylstyrene dimer, and 33 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92°C over 40 minutes while stirring. After the temperature was raised to 92°C, a solution in which 9 parts by mass of maleic anhydride and 0.60 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 47 parts by mass of methyl ethyl ketone was continuously added over 5 hours. After the addition was completed, the temperature was raised to 120°C and the reaction was carried out for 1.5 hours to terminate the polymerization. Then, 9 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization liquid and the reaction was carried out at 140°C for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer A-11. The analytical results of the obtained maleimide copolymer are shown in Table 2.
[0100] <Production Example of Maleimide Copolymer (A-12)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 79 parts by mass of styrene, 9 parts by mass of acrylonitrile, 2 parts by mass of maleic anhydride, and 33 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92 ° C. over 40 minutes while stirring. After the temperature was raised to 92 ° C., a solution in which 9 parts by mass of maleic anhydride and 0.60 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 47 parts by mass of methyl ethyl ketone was continuously added over 5 hours. After the addition was completed, the temperature was raised to 120 ° C. and the reaction was carried out for 1.5 hours to terminate the polymerization. Then, 9 parts by mass of aniline and 0.2 parts by mass of triethylamine were added to the polymerization liquid and the reaction was carried out at 140 ° C. for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer A-12. The analysis results of the obtained maleimide copolymer are shown in Table 2.
[0101] <Production Example of Maleimide Copolymer (B-1)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 77 parts by mass of styrene, 19 parts by mass of acrylonitrile, 1 part by mass of maleic anhydride, and 25 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92 ° C. over 40 minutes while stirring. After the temperature was raised to 92 ° C., a solution in which 3 parts by mass of maleic anhydride and 0.82 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 23 parts by mass of methyl ethyl ketone was continuously added over 4.5 hours while maintaining the temperature at 92 ° C. After the addition of maleic anhydride was completed, a solution in which 0.18 parts by mass of t-butylperoxy-2-ethylhexanoate was dissolved in 1 part by mass of methyl ethyl ketone was continuously added over 1 hour. After the addition was completed, the temperature was raised to 120 ° C., and the polymerization was terminated by reacting for 1 hour. Thereafter, 2 parts by mass of aniline and 0.1 parts by mass of triethylamine were added to the polymerization liquid and reacted at 140 ° C. for 7 hours. After the reaction was completed, the imidization reaction solution was fed into a vent-type screw extruder, and the volatile matter was removed to obtain pellets of maleimide copolymer B-1. The analytical results of the obtained maleimide copolymer are shown in Table 2.
[0102] <Production Example of Maleimide Copolymer (B-2)> In an autoclave with a volume of about 120 liters equipped with a stirrer, 22 parts by mass of styrene, 10 parts by mass of acrylonitrile, 3 parts by mass of maleic anhydride, 0.45 parts by mass of α-methylstyrene dimer, and 39 parts by mass of methyl ethyl ketone were charged, and the gas phase was replaced with nitrogen gas, and the temperature was raised to 92°C over 40 minutes while stirring. After the temperature was raised to 92°C, a solution in which 41 parts by mass of styrene, 23 parts by mass of maleic anhydride, and 0.42 parts by mass of t-butylperoxy-2-ethylhexanoate were dissolved in 116 parts by mass of methyl ethyl ketone was continuously added over 5 hours. After the addition was completed, the temperature was raised to 120°C and the reaction was carried out for 1 hour to terminate the polymerization. Then, 23 parts by mass of aniline and 0.4 parts by mass of triethylamine were added to the polymerization liquid and the reaction was carried out at 140°C for 7 hours. The imidization reaction liquid after the reaction was charged into a vent-type screw extruder, and the volatile matter was removed to obtain a pellet-shaped maleimide copolymer B-2. The analytical results of the obtained maleimide copolymer are shown in Table 2.
[0103] <Weight average molecular weight of maleimide copolymer> The weight average molecular weight of the maleimide copolymer is a value calculated as polystyrene by gel permeation chromatography (GPC), and was measured under the following conditions. Measurement name: SYSTEM-21 Shodex (manufactured by Showa Denko Co., Ltd.) Column: Three PL gel MIXED-B columns (Polymer Laboratories) in series Temperature: 40℃ Detection: Differential refractive index Solvent: Tetrahydrofuran Concentration: 2% by mass Calibration curve: Created using standard polystyrene (PS) (Polymer Laboratories)
[0104] <Melt viscosity of maleimide copolymer> The melt viscosity of the maleimide copolymer was measured using a capillary die with L=40 mm and D=1 mm at 190° C. and a shear rate of 100 / sec. The measuring device used was a Capillary Rheometer 1D manufactured by Toyo Seiki Seisakusho Co., Ltd.
[0105] <Fiber preparation> A non-crosslinked vinyl chloride resin, a crosslinked vinyl chloride resin, an AS resin, and a maleimide copolymer were mixed in a blender in the ratios shown in Tables 1 and 2 below, and compounded to produce pellets using an extruder with a diameter of 40 mm at a cylinder temperature in the range of 130 to 170° C. The resulting pellets were then melt-spun in the extruder. (Raw materials used) The raw materials used in each of the examples and comparative examples are shown below. (1) Polyvinyl chloride resin Non-crosslinked polyvinyl chloride resin (manufactured by Taiyo Vinyl, product name TH1000, viscosity average degree of polymerization 1000) Cross-linked polyvinyl chloride resin (Shin-Etsu Chemical Co., Ltd., product name GR800T, viscosity average degree of polymerization of component soluble in tetrahydrofuran: 800) (2) Vinyl copolymer resin AS resin (GR-AT-6S manufactured by Denka Co., Ltd., styrene monomer unit 68% by mass, vinyl cyanide monomer unit 32% by mass, weight average molecular weight 90,000) (3) Maleimide copolymer (A-1) to (A-12) and (B-1) to (B-2) obtained according to the above-mentioned Production Examples were used.
[0106] The fiber was then heat-treated for about 0.5 to 1.5 seconds in a heating cylinder installed directly under the nozzle to obtain a fiber of 150 dtex. The melt-spun fiber was then stretched 300% in an air atmosphere at 100°C, and the stretched fiber was then heat-shrunk in an air atmosphere at 120°C until the entire fiber length was 75% of the length before the treatment, to obtain a fiber for artificial hair of 670 dtex. The results of evaluations of the obtained fiber for artificial hair are shown in Tables 1 and 2.
[0107] <Various measurements and evaluations> Various characteristics and physical properties were measured and evaluated by the methods described below.
[0108] <Heat shrinkage rate> A sample with a length of 100 mm was prepared from the artificial hair fibers of the Examples and Comparative Examples, and was immersed in 95°C warm water for 30 seconds. The length of the sample was measured before and after immersion. The thermal shrinkage was calculated according to the following formula (1). Heat shrinkage rate (%) = {(length before immersion) - (length after immersion at 95°C for 30 seconds)} / (length before immersion) x 100 (1)
[0109] <Gloss> The artificial hair fibers of the Examples and Comparative Examples were bundled into a bundle of 200 mm in length and 20 g in mass, and ten artificial hair fiber processing technicians (with more than 5 years of work experience) observed the bundle under sunlight and visually compared it with human hair to evaluate the luster according to the following criteria. (Evaluation Criteria) ◎: More than 9 out of 10 people judged that they could not see any difference from human hair. Good: 6 to 8 out of 10 people judged that they could not see any difference from human hair. △: 3 to 5 out of 10 people judged that they could not recognize the difference from human hair. ×: Less than 2 out of 10 people judged that they could not recognize the difference from human hair.
[0110] <Spinnability> While undrawn yarn was being produced by melt spinning, the occurrence of yarn breakage was visually observed, and the spinnability was evaluated according to the following criteria. (Evaluation Criteria) ◎: Thread breakage occurs once or less per hour 〇: Thread breaks 2-3 times / hour ×: Thread breakage occurs 4 or more times per hour
[0111] [Table 1]
[0112] [Table 2]
[0113] From the results of Tables 1 and 2, it can be seen that the artificial hair fibers according to the Examples have low heat shrinkage, low gloss, and excellent spinnability. On the other hand, it can be seen that the artificial hair fibers according to the Comparative Examples are inferior to the Examples in one or more aspects of heat shrinkage rate, gloss, and spinnability. Moreover, Comparative Example 2 could not be melt-kneaded, and artificial hair fibers could not be obtained. [Industrial Applicability]
[0114] INDUSTRIAL APPLICABILITY The present invention has industrial applicability as a fiber for artificial hair used for artificial hair such as wigs, hair toupees, and false hair that can be detached from the head.
Claims
1. An artificial hair fiber made of a resin composition containing a vinyl chloride resin and a maleimide copolymer, The vinyl chloride resin is contained in an amount of 50 to 99% by mass based on 100% by mass of the resin composition, The maleimide copolymer is contained in an amount of 1 to 50% by mass based on 100% by mass of a resin composition, The maleimide-based copolymer has 5 to 30% by mass of the maleimide-based monomer units, when the total of the aromatic vinyl-based monomer units, the vinyl cyanide-based monomer units, the unsaturated acid anhydride monomer units and the maleimide-based monomer units is taken as 100% by mass.
2. 2. The fiber for artificial hair according to claim 1, wherein the maleimide-based copolymer contains 50 to 90% by mass of the aromatic vinyl-based monomer units, 0.5 to 25% by mass of the vinyl cyanide-based monomer units, and 0 to 10% by mass of the unsaturated acid anhydride monomer units, when the total of the aromatic vinyl-based monomer units, the vinyl cyanide-based monomer units, the unsaturated acid anhydride monomer units, and the maleimide-based monomer units is taken as 100% by mass.
3. 3. The fiber for artificial hair according to claim 1, wherein the ratio of the content of said vinyl chloride resin to the content of said maleimide copolymer is 80 to 99 parts by mass / 1 to 20 parts by mass.
4. The maleimide copolymer has a weight average molecular weight of 25,000 to 120,000. The fiber for artificial hair according to any one of claims 1 to 3.
5. A hair accessory comprising the artificial hair fiber according to any one of claims 1 to 4.
Citation Information
Patent Citations
Polyvinyl chloride-based fiber
JP2004225164A