Negative-electrode active material and preparation method thereof, secondary battery, and battery module, battery pack and apparatus that comprise secondary battery

The use of a negative electrode active material with artificial graphite and amorphous carbon coating addresses the issue of slow charging in secondary batteries by improving ion diffusion and reducing polarization, enhancing rapid charging and cycle performance.

JP2024164133AActive Publication Date: 2024-11-26CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024140007
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2040-10-15

AI Technical Summary

Technical Problem

Conventional secondary batteries suffer from long charging times, which cause range anxiety for electric vehicle users, limiting their widespread adoption due to inadequate rapid charging performance and cycle life.

Method used

A negative electrode active material comprising artificial graphite with a coating layer of amorphous carbon, characterized by specific particle size distributions and uniformity, enhances active ion diffusion and reduces polarization, thereby improving charging rates and cycle performance.

Benefits of technology

The proposed negative electrode active material significantly enhances rapid charging ability and cycle performance of secondary batteries, ensuring high energy density and efficient ion transport even at high lithium occlusion states.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164133000001_ABST
    Figure 2024164133000001_ABST
Patent Text Reader

Abstract

To provide secondary batteries with good fast-charging performance.SOLUTION: This application provides a negative-electrode active material and a preparation method thereof, a secondary battery, and a battery module, a battery pack and an apparatus that comprise the secondary battery. The negative-electrode active material comprises: a core containing artificial graphite; and a coating layer covering at least part of a surface of the core and containing amorphous carbon. The negative-electrode active material has a volume-based particle size distribution satisfying Dv99≤24 μm, and an average volume-based particle size Dv50 satisfying 8 μm≤Dv50≤15 μm, where Dv99 is a particle size corresponding to a cumulative volume distribution percentage of the negative-electrode active material reaching 99%, and Dv50 is a particle size corresponding to a cumulative volume distribution percentage of the negative-electrode active material reaching 50%.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application belongs to the field of secondary battery technology, and specifically relates to a negative electrode active material, a method for producing the same, a secondary battery, a battery module including the secondary battery, a battery pack, and an apparatus. [Background technology]

[0002] The secondary battery is charged and discharged by the shuttle of active ions between the positive and negative electrodes, and has outstanding characteristics such as high energy density, long cycle life, no pollution, no memory effect, etc. Therefore, as a clean energy source, the secondary battery is widely used in the fields of large devices such as electronic products and electric vehicles, and is in line with the sustainable development strategy for the environment and energy.

[0003] However, while conventional fuel vehicles can be refueled quickly and in a timely manner, electric vehicles are generally charged at a low rate, which requires a long charging time, which makes users anxious about the driving range and limits the rapid popularization of electric vehicles. Therefore, in order to improve the market competitiveness of electric vehicles, it is necessary to provide a secondary battery with good fast charging performance. Summary of the Invention

[0004] An object of the present application is to provide a negative electrode active material that improves the charging performance and cycle performance of a secondary battery, a method for producing the same, a secondary battery, a battery module including the secondary battery, a battery pack, and an apparatus.

[0005] In order to achieve the above object of the invention, a first aspect of the present application is a composite material having a core containing artificial graphite and a coating layer containing amorphous carbon that coats at least a part of the surface of the core, the composite material having a volume particle size distribution D v 99≦24 μm and average volume particle size D v 50 is 8μm≦D v Provide a negative electrode active material that satisfies 50≦15μm. D v 99 is the particle size corresponding to the cumulative volume distribution percentage of the negative electrode active material reaching 99%, and D v50 is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 50%.

[0006] Surprisingly, it has been found that the negative plate has high active ion solid-phase diffusion performance when the negative active material of the present application is used. Even in the high lithium absorption state at the end of charging, the active ions can have a high diffusion rate in the negative plate, effectively reducing ohmic and concentration polarization, thus greatly increasing the charging speed and charging depth of the entire negative plate, and significantly improving the fast charging ability of the battery. Furthermore, the cycle performance of the battery is also significantly improved.

[0007] In any embodiment of the present application, the negative electrode active material has a thickness of 17 μm≦D v 99≦24 μm, and optionally, 18 μm≦D v 99≦21μm. D of negative electrode active material v When 99 is within the above range, the rapid charging capability and cycle performance of the battery can be further improved.

[0008] In any embodiment of the present application, the negative electrode active material has a thickness of 9 μm≦D v 50≦13 μm, and optionally, 11 μm≦D v 50≦13μm. D of negative electrode active material v When 50 is within the appropriate range, the rapid charging capability and cycle performance of the battery can be further improved.

[0009] In any embodiment of the present application, the particle size uniformity of the negative electrode active material is 0.25 to 0.45, and preferably 0.32 to 0.38. When the particle size uniformity of the negative electrode active material is within the above range, the rapid charging capability of the battery can be further improved, and the negative electrode plate can be provided with a high compaction density, thereby improving the energy density of the battery.

[0010] In any embodiment of the present application, the particle size specific surface area of ​​the negative electrode active material is 0.4 m 2 / g~0.75m 2 / g, preferably 0.5m2 / g~0.65m 2 When the particle size-specific surface area of ​​the negative electrode active material is within the appropriate range, the rapid charging performance and cycle performance of the battery can be further improved, and the energy density of the battery can be improved.

[0011] In any embodiment of the present application, the negative electrode active material includes secondary particles, and the number ratio of the secondary particles in the negative electrode active material is ≧50%. Optionally, the number ratio of the secondary particles in the negative electrode active material is 70% to 95%. When the negative electrode active material includes an appropriate amount of secondary particles, the rapid charging ability, cycle performance, and storage performance of the battery can be further improved.

[0012] In any embodiment of the present application, the negative electrode active material has a capacitance of 0.6≦(D v 90-D v 10) / D v 50≦1.8, and optionally, 0.8≦(D v 90-D v 10) / D v 50≦1.4. D v 90 is the particle size corresponding to the cumulative volume distribution percentage of the negative electrode active material reaching 90%, and D v 10 is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 10%. v 90-D v 10) / D v The appropriate value of 50 is advantageous for further improving the rapid charging capability of the battery.

[0013] In any embodiment of the present application, the volume particle size distribution D v 90 is 13 μm to 18 μm, and optionally 14 μm to 17 μm. v If 90 is within the above range, the rapid charging capability of the battery can be further improved.

[0014] In any embodiment of the present application, the volume particle size distribution D v10 is 5 μm to 10 μm, and optionally 6 μm to 8 μm. v When 10 is within the above range, it is advantageous for improving the cycle performance and storage performance of the battery.

[0015] In any embodiment of the present application, the graphitization degree of the negative electrode active material is 91.0% to 96.0%, and preferably 94.0% to 95.0%. When the graphitization degree of the negative electrode active material is within the above range, the rapid charging capability of the battery can be further improved.

[0016] In any embodiment of the present application, the gram capacity of the negative electrode active material is 345mAh / g to 360mAh / g, and preferably 350mAh / g to 358mAh / g. When the gram capacity of the negative electrode active material is within an appropriate range, the energy density of the battery can be improved, and the rapid charging ability and cycle performance of the battery can be improved.

[0017] In any embodiment of the present application, the tap density of the negative electrode active material is 0.9 g / cm 3 ~1.3g / cm 3 and preferably 1.0 g / cm 3 ~1.1g / cm 3 When the tap density of the negative electrode active material is within a given range, the rapid charging capability of the battery can be improved, and the energy density of the battery can be improved.

[0018] In any embodiment of the present application, the powder compaction density of the negative electrode active material at a pressure of 2 kN is 1.55 g / cm 3 ~1.67g / cm 3 and preferably 1.60 g / cm 3 ~1.65g / cm 3 When the powder compaction density of the negative electrode active material at a pressure of 2 kN is within a given range, the particles in the negative electrode film layer can be closely attached to each other, and good electrolyte wetting tunnels can be formed, improving the rapid charging ability and cycle performance of the battery.

[0019] A second aspect of the present application is A) providing a core comprising artificial graphite; The core is coated so that a coating layer containing amorphous carbon is formed on at least a part of the surface of the core. v 99≦24μm and 8μm≦D v and B) a step of obtaining a negative electrode active material that satisfies 50≦15 μm.

[0020] In any embodiment of the present application, the preparation of artificial graphite according to step A) comprises: a) providing a coke feedstock; b) subjecting the coke raw material to a shaping process to obtain a precursor; Step c) of granulating the precursor to obtain a granulated product; The granules are graphitized to obtain a volume average particle diameter D v 50 is 6 μm to 14 μm and the volume particle size distribution D v and d) obtaining artificial graphite having a particle size of 17 μm to 26 μm.

[0021] In any embodiment of the present application, the volume average particle size D v 50 is 9 μm to 15 μm and has a volume particle size distribution D v 99 is 17μm to 24μm.

[0022] In any embodiment of the present application, the volume average particle diameter D v 50 is 8 μm to 13 μm and has a volume particle size distribution D v 99 is 16μm to 22μm.

[0023] In any embodiment of the present application, the volume average particle diameter D v 50 is 7 μm to 12 μm and has a volume particle size distribution D v 99 is 15μm to 21μm.

[0024] In any embodiment of the present application, the particle size uniformity of the precursor is U1, and satisfies 0.2≦U1≦0.55. Optionally, 0.3≦U1≦0.45.

[0025] In any embodiment of the present application, the grain size uniformity of the artificial graphite is U2, which satisfies 0.22≦U2≦0.48. Optionally, 0.3≦U2≦0.4.

[0026] In any embodiment of the present application, the volatile matter content of the coke raw material is C1, the particle size uniformity of the precursor is U1, and the adhesive is added during the granulation process in step c), the amount of adhesive used is C2, and the preparation method satisfies 21%≦(C1+C2) / U1×100%≦50%, and optionally 31%≦(C1+C2) / U1×100%≦35%.

[0027] In any embodiment of the present application, the volatile matter content C1 of the coke feedstock satisfies 1%≦C1≦12%. Optionally, 5%≦C1≦9%.

[0028] In any embodiment of the present application, the coke feedstock comprises one or more of petroleum based non-needle coke, petroleum based needle coke. Optionally, the coke feedstock comprises petroleum green coke.

[0029] In any embodiment of the present application, step B) includes step e) of coating the core with an organic carbon source and forming an amorphous carbon coating layer on at least a portion of the surface of the core by heat treatment to obtain a negative electrode active material.

[0030] In any embodiment of the present application, the amount of organic carbon source added in step e) is C3, and the preparation method satisfies 20%≦(C1+C2+C3) / U2×100%≦56%, 1.2%≦C3×residual carbon rate≦2.5%.

[0031] The negative electrode active material obtained by the manufacturing method of the present application has a core containing artificial graphite and a coating layer containing amorphous carbon that coats the surface of the core, and the negative electrode active material is D v 99≦24μm and 8μm≦D v By satisfying the requirement of 50≦15 μm, the rapid charging capability of a battery using the negative electrode active material can be significantly improved, and the cycle performance of the battery can also be significantly improved.

[0032] A third aspect provides a secondary battery including a negative electrode plate having a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector and including a negative electrode active material including the negative electrode active material described in the present application.

[0033] The secondary battery according to the present application uses the negative electrode active material described in the present application, and therefore can have high energy density, rapid charging capability, and cycle performance.

[0034] A fourth aspect of the present application provides a battery module including a secondary battery according to the present application.

[0035] A fifth aspect of the present application provides a battery pack including a secondary battery or a battery module according to the present application.

[0036] A device according to a sixth aspect of the present application includes at least one of a secondary battery, a battery module, or a battery pack according to the present application.

[0037] The battery module, battery pack, and device of the present application include the secondary battery of the present application, and therefore have at least the same advantages as the secondary battery. [Brief description of the drawings]

[0038] In order to more clearly explain the aspects of the embodiments of the present application, the following briefly describes the drawings that need to be used in the embodiments of the present application. Obviously, the drawings described below are only some of the embodiments of the present application, and those skilled in the art can obtain other drawings based on the drawings without performing creative labor. [Figure 1]FIG. 2 is a scanning electron microscope (SEM) view at 1000 times magnification of one embodiment of a negative electrode active material according to the present application. [Diagram 2] FIG. 2 is a scanning electron microscope (SEM) view at 5000 times magnification of another embodiment of a negative electrode active material according to the present application. [Diagram 3] 1 is a photograph of a cross-sectional shape (CP) of a negative electrode plate after the negative electrode active material according to the present application is formed into a negative electrode plate, the cross-sectional shape being ion-polished at a magnification of 5000 times. [Figure 4] FIG. 2 is a transmission electron microscope (TEM) view at 60,000 times magnification of one embodiment of a negative electrode active material according to the present application. [Diagram 5] FIG. 1 is a schematic diagram illustrating an embodiment of a secondary battery. [Figure 6] FIG. 6 is an exploded view of FIG. 5. [Figure 7] FIG. 1 is a schematic diagram illustrating an embodiment of a battery module. [Figure 8] FIG. 1 is a schematic diagram illustrating an embodiment of a battery pack. [Figure 9] FIG. 9 is an exploded view of FIG. [Figure 10] FIG. 1 is a schematic diagram showing an embodiment of an apparatus that uses a secondary battery as a power source. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] In order to make the inventive object, aspects and beneficial technical effects of the present application clearer, the present application will be described in more detail with reference to the following examples. It should be understood that the examples described herein are merely for the purpose of illustrating the present application, and are not intended to limit the present application.

[0040] For simplicity, this specification only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range. Any lower limit can also be combined with another lower limit to form an unspecified range, and any upper limit can also be combined with another upper limit to form an unspecified range. Although not specified, each point or individual value between the endpoints of the range is included in this range. Therefore, each point or individual value can be combined with other points or individual values ​​as its own lower limit or upper limit, or can be combined with other lower limits or upper limits to form an unspecified range.

[0041] In the description of this specification, unless otherwise specified, "more than or equal to" and "less than or equal to" are inclusive of the number, and "multiple types" in "one type or multiple types" means two types or more than two types.

[0042] In the description of this specification, unless otherwise stated, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions satisfy "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and A and B are both true (or exist).

[0043] The above content of the present application is not intended to describe all of the embodiments or all of the implementations disclosed in the present application. As follows, the description will more specifically illustrate exemplary embodiments by way of examples. In several places in the present specification, a series of examples are provided to provide teachings, and these examples can be used in various combination forms. In each example, the examples are merely representative and should not be construed as exhaustive.

[0044] A secondary battery, also called a rechargeable battery or a storage battery, is a battery that can be continuously used by activating the active material through charging after discharging.

[0045] A secondary battery generally includes a positive electrode plate, a negative electrode plate, a separator, and an electrolyte. During the charging and discharging process of the battery, active ions (e.g., lithium ions) shuttle between the positive electrode plate and the negative electrode plate to be absorbed and released. The separator is provided between the positive electrode plate and the negative electrode plate, and mainly serves to prevent short circuits between the positive and negative electrodes, and is also permeable to ions. The electrolyte mainly serves to conduct ions between the positive and negative electrodes.

[0046] The inventors have found that the key to improving the rapid charging ability of a secondary battery is to improve the dynamic performance of the negative electrode. The negative electrode plate generally has a negative electrode current collector and a negative electrode film layer containing a negative electrode active material. The negative electrode active material generally refers to a material involved in the absorption and release of active ions in the negative electrode plate during the charging and discharging process of the battery. Currently, in order to improve the dynamic performance of a battery, the method of reducing the thickness of the negative electrode film layer or reducing the compaction density of the negative electrode film layer is often adopted. However, a large amount of research has shown that the above-mentioned methods for improving the dynamic performance of a battery can only improve the dynamic performance of the battery to a certain extent in a low SOC state (i.e., early charging) in actual use, and the improvement of the dynamic performance of the battery in a high SOC state (i.e., end charging) in actual use is small, and the rapid charging ability of the secondary battery cannot be effectively improved. In addition, the energy density of the battery is also significantly reduced.

[0047] In general, in the manufacturing process of the negative electrode active material, the volume average particle diameter D v 50 is attracting attention, and particles with a cumulative volume distribution percentage of 99% or more from the small particle size side are few in number, so the D v However, the inventors of the present invention have conducted extensive research and found that the D v We were surprised to discover that by keeping the content of 99 within a specific range, the rapid lithium absorption capability of the negative electrode active material in a high lithium absorption state (corresponding to a high SOC state of the battery) can be significantly improved, thereby overcoming the above bottleneck and improving the rapid charging capability of the secondary battery in a high SOC state.

[0048] Accordingly, the present application provides a composite material having a core containing artificial graphite and a coating layer containing amorphous carbon that coats at least a portion of the surface of the core, the composite material having a volume particle size distribution D v 99≦24μm and the average volume particle size D v 50 is 8μm≦D v Provide a negative electrode active material that satisfies the requirement of 50≦15 μm.

[0049] The inventors have found that, after extensive research, the use of the negative electrode active material according to the present application allows the battery to have high active ion solid-phase diffusion performance on the premise of having high energy density. Even in a high lithium absorption state at the end of charging (high SOC state), the negative electrode active material particles can maintain good electrochemical reaction activity, and the active ions can be quickly absorbed and moved in the bulk phase of the negative electrode active material, effectively improving the diffusion rate of the active ions in the negative electrode plate, and reducing ohmic and concentration polarization, greatly increasing the charging rate and charging depth of the entire negative electrode plate. Therefore, the present application allows the battery to perform high-power charging in all SOC states, and can significantly improve the rapid charging ability. In addition, since the active ion migration performance between the positive and negative electrodes in the battery is excellent and the polarization is small, the cycle performance can also be significantly improved. In general, a low SOC state generally refers to 30% SOC or less, and a high SOC state generally refers to 60% SOC or more.

[0050] The artificial graphite referred to in this application generally refers to a graphite material obtained through a high-temperature graphitization treatment, and the degree of graphitization crystallization is generally high.

[0051] Amorphous carbon, as used herein, generally refers to carbon materials that have a low degree of graphitic crystallization.

[0052] In general, the lattice structure of artificial graphite tends to be a layered arrangement with long-range order, while the lattice structure of amorphous carbon tends to be disordered. Generally, the lattice arrangement can be observed by transmission electron microscope (TEM) images.

[0053] In some embodiments, the core may have one or more of the following shapes: a block shape, a sheet shape, and a roughly spherical shape.

[0054] In some embodiments, the thickness of the coating layer is ≧2 nm, optionally between 2 nm and 20 nm, for example, between 2 nm and 15 nm, between 2 nm and 10 nm, between 5 nm and 10 nm.

[0055] In some embodiments, the coverage of the coating layer on the core surface is ≧50%, and optionally 60% to 100%.

[0056] In some embodiments, the negative electrode active material is D v 99≦23.8 μm, ≦23.5 μm, ≦23 μm, ≦22.5 μm, ≦22 μm, ≦21 μm, or ≦20 μm can be satisfied.

[0057] In some embodiments, the negative electrode active material is D v 99≧15 μm, ≧16 μm, ≧17 μm, ≧18 μm, ≧19 μm.

[0058] In some embodiments, the negative electrode active material has a thickness of 15 μm≦D v 99≦24μm, for example, 16μm≦D v 99≦22μm, 17μm≦D v 99≦24μm, 17μm≦D v 99≦23μm, 15μm≦D v 99≦21μm, 18μm≦D v 99≦21μm, 19μm≦D v 99≦21μm, 19μm≦D v 99≦22μm, 19μm≦D v 99≦23μm, 20μm≦D v 99≦22μm, 20μm≦D v 99≦21.5μm or 20μm≦D v 99≦21 μm.

[0059] Negative electrode active material D vWhen 99 is within the appropriate range, it can further improve the solid-phase diffusion rate of active ions when the negative electrode is in a high lithium absorption state, reduce polarization, and help reduce the number of relatively small particles, allowing the particles to absorb more active ions. It also forms a smooth tunnel structure in the negative electrode film layer, shortens the liquid phase conduction path, and further improves the fast charging ability and cycle performance of the battery. D v By using an appropriate negative electrode active material, the secondary battery can achieve both high rapid charging capability and cycle performance.

[0060] In some embodiments, the negative electrode active material is D v 50≦14 μm, ≦13 μm, or ≦12 μm. Optionally, D v 50≧8 μm, ≧9 μm, ≧10 μm, or ≧11 μm. For example, the negative electrode active material has a thickness of 8 μm≦D v 50≦14μm, 9μm≦D v 50≦13μm, 10μm≦D v 50≦14μm, 12μm≦D v 50≦14μm, 12μm≦D v 50≦13μm or 11μm≦D v The condition 50≦13μm can be satisfied.

[0061] Negative electrode active material D v When D 50 is within the appropriate range, it is favorable for shortening the migration path of the active ions in the negative active material particles, and for forming a smooth porous structure in the negative electrode membrane layer, so that the negative plate has a good solid-phase diffusion rate of the active ions and a good liquid-phase transport performance, and further improves the rapid charging ability of the battery. v When the ratio of the positive electrode active material to the negative electrode active material is within the appropriate range, it can further ensure that the negative electrode active material has a high gram capacity, which is favorable for the battery to obtain a high energy density, and it can also reduce the side reaction of the electrolyte at the negative electrode and improve the cycle performance of the battery.

[0062] In some embodiments, the particle size uniformity of the negative electrode active material is 0.25 to 0.45, and may be, for example, 0.28 to 0.4, 0.32 to 0.4, 0.32 to 0.38, 0.30 to 0.36, 0.31 to 0.35, or 0.32 to 0.36. The particle size uniformity of the negative electrode active material is determined by the particle size of all particles in the negative electrode active material being smaller than the volume average particle size D v 50, and reflects the uniformity of the particle size distribution of the negative active material. When the particle size uniformity of the negative active material is within the above range, it is easy to form a short liquid phase transport path in the negative electrode film layer, and a large contact area can be obtained between the particles, which is favorable for the electron conduction and the transport of active ions in the negative electrode plate, and further improves the rapid charging ability of the battery. In addition, the particles in the negative electrode film layer can be closely attached to each other, which increases the compaction density of the negative electrode plate and improves the energy density of the battery.

[0063] In some embodiments, the negative electrode active material has a molecular weight of 0.6≦(D v 90-D v 10) / D v 50≦1.8. v 90-D v 10) / D v 50 is, for example, 0.8 to 1.4, 0.9 to 1.3, 1.0 to 1.25, or 1.2 to 1.6. v 90-D v 10) / D v 50 is the volume average particle diameter D v The degree of deviation from 50 is reflected in the negative electrode active material (D v 90-D v 10) / D v When 50 is appropriate, it is favorable to improve the processability of the negative electrode slurry and the negative electrode film layer, to make the entire negative electrode film layer have high particle distribution uniformity, and to make different regions of the negative electrode film layer have high active ion transport performance, and further improve the fast charging ability of the battery.

[0064] In some embodiments, the volume particle size distribution D of the negative electrode active materialv The negative electrode active material D 90 is 13 μm to 18 μm, and may be, for example, 13 μm to 16 μm, 14 μm to 17 μm, or 15 μm to 18 μm. v When 90 is within the appropriate range, the solid-phase diffusion rate of the active ions in the negative electrode film layer can be further improved, and the rapid charging ability of the battery can be further improved. In addition, the negative electrode active material can have a high gram capacity, which helps to improve the energy density of the battery.

[0065] In some embodiments, the volume particle size distribution D of the negative electrode active material v The diameter 10 is 5 μm to 10 μm, and may be, for example, 6 μm to 8 μm. Since the content of small particles in the negative electrode active material is small, the side reaction between the electrolyte and the material can be reduced, and the cycle performance and storage performance of the battery can be improved.

[0066] In some embodiments, the particle size specific surface area of ​​the negative electrode active material is 0.4 m 2 / g~0.75m 2 / g, for example, 0.4m 2 / g~0.7m 2 / g, 0.42m 2 / g~0.68m 2 / g, 0.46m 2 / g~0.55m 2 / g, 0.5m 2 / g~0.68m 2 / g, or 0.5m 2 / g~0.65m 2 / g.

[0067] The "particle size specific surface area" of the negative electrode active material according to the present application is different from the "specific surface area" of general negative electrode active materials. Currently, the specific surface area (SSA) of negative electrode active materials in the industry is often obtained using the gas adsorption BET method, and is used to represent only the physical adsorption specific surface area of ​​the negative electrode active material. The "particle size specific surface area" of the negative electrode active material according to the present application is obtained using a laser diffraction particle size analysis method, and represents the degree to which the shape of the negative electrode active material deviates from sphericity.

[0068] The inventors have found that when the particle size-specific surface area of ​​the negative electrode active material is within a suitable range, the ion release passage in the negative electrode film layer can be increased, the charge exchange impedance can be reduced, and a smoother tunnel can be formed in the negative electrode film layer, the wettability of the electrolyte can be improved, and the transport speed of the solid phase and liquid phase of the active ions in the negative electrode plate can be further improved, so that the rapid charging performance and cycle performance of the battery can be further improved. In addition, the appropriate particle size-specific surface area of ​​the negative electrode active material can improve the compaction density of the negative electrode film layer and improve the energy density of the battery.

[0069] In some embodiments, the negative electrode active material includes secondary particles, as shown in FIG. 1 and FIG. 2. Optionally, the number ratio of the secondary particles in the negative electrode active material is ≧50%. For example, the number ratio of the secondary particles in the negative electrode active material is 50%-100%, 60%-100%, 60%-90%, 70%-100%, 70%-95%, 70%-90%, 70%-80%, or 75%-85%. When the negative electrode active material includes a large amount of secondary particles, the number of active ion release paths in the negative electrode film layer increases, which further improves the rapid charging ability of the battery, reduces polarization, and improves the cycle performance. In particular, when the negative electrode active material includes both secondary particles and primary particles, it can reduce side reactions of the electrolyte in the negative electrode, and further improve the cycle performance and storage performance of the battery.

[0070] In some embodiments, the graphitization degree of the negative electrode active material is 91.0% to 96.0%, and may be, for example, 94.0% to 95.0%, or 93.0% to 94.5%. When the graphitization degree of the negative electrode active material is within the above range, the particle structure can have a large interlayer distance and low powder resistance, and the rapid charging ability can be further improved.

[0071] In some embodiments, the gram capacity of the negative electrode active material is 345mAh / g to 360mAh / g, and may be, for example, 350mAh / g to 358mAh / g, 351mAh / g to 356mAh / g, or 352mAh / g to 355mAh / g. Since the gram capacity of the negative electrode active material is high, the energy density of the battery can be improved. The gram capacity of the negative electrode active material within the above range means that the migration path of the active ions of the active material is short, and the rapid charging ability of the battery can be improved.

[0072] In some embodiments, the tap density of the negative electrode active material is 0.9 g / cm 3 ~1.3g / cm 3 For example, 1.0 g / cm 3 ~1.1g / cm 3 When the tap density of the negative electrode active material is within a given range, the particles in the negative electrode coating layer can be in good contact with each other, improving the fast charging ability of the battery. Also, the particles can be densely stacked with each other, improving the energy density of the battery.

[0073] In some embodiments, the negative electrode active material has a powder compaction density of 1.55 g / cm at a pressure of 2 kN. 3 ~1.67g / cm 3 For example, 1.60 g / cm 3 ~1.65g / cm 3 When the powder compaction density of the negative electrode active material at a pressure of 2 kN is within a given range, the particles in the negative electrode film layer can be closely attached to each other and good electrolyte wetting tunnels can be formed, thereby improving the rapid charging capability and cycle performance of the battery.

[0074] In this application, the negative electrode active material D v 99, D v 90, D v 50, D v10. The particle size uniformity and particle size specific surface area can be measured by laser diffraction particle size analysis, for example, referring to GB / T19077-2016 standard, using a laser particle size analyzer (such as Malvern Master Size 3000).

[0075] D v 99 is the particle size corresponding to the cumulative volume distribution percentage of the negative electrode active material reaching 99%, and D v D 90 is the particle size corresponding to the cumulative volume distribution percentage of the negative active material reaching 90%, v D 50 is the particle size corresponding to when the cumulative volume distribution percentage of the negative active material reaches 50%, v 10 is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 10%.

[0076] In the present application, the negative active material is made into a negative plate, and the negative plate is subjected to ion polishing cross-sectional shape (CP) measurement, thereby making it possible to observe the material type of the core. For example, the measurement method may be as follows. First, the made negative plate is cut into a sample to be measured of a certain size (e.g., 2 cm x 2 cm), and the negative plate is fixed to a sample stage with paraffin. Next, the sample stage is inserted into a sample holder, locked and fixed, and the power of an argon ion cross-sectional polishing device (e.g., IB-19500CP) is turned on and a vacuum (e.g., 10 -4 Pa), set the argon gas flow rate (e.g., 0.15 MPa), voltage (e.g., 8 KV) and polishing time (e.g., 2 hours), adjust the sample stage to the rocking mode, and start polishing. Sample measurement can refer to JY / T010-1996. Randomly select an area on the sample to be measured for scanning measurement, and obtain an ion-polished cross-sectional profile (CP) photograph of the negative plate at a certain magnification (e.g., 5000 times). For example, as can be seen from FIG. 3 of the present application, the core of the negative active material of the present application is artificial graphite.

[0077] In this application, the structure of the negative electrode active material (e.g., core and coating layer) can be measured using equipment and methods known in the art. For example, the operation can be performed in the following steps. Select a microgrid of a certain diameter (e.g., 3 mm in diameter), pinch the edge of the microgrid with pointed tweezers, turn the film surface upward (observe the surface that is shiny under the lamp, i.e., the film surface), lightly and flatly place it on a white filter paper, take an appropriate amount of graphite particle sample (e.g., 1 g), place it in a beaker containing an appropriate amount of ethanol, perform ultrasonic oscillation for 10 min to 30 min, and aspirate with a glass capillary, then drop 2 to 3 drops of the test sample onto the microgrid, bake in an oven for 5 min, and then place the microgrid on which the test sample has been dropped onto the sample stage, and measure it at a certain magnification (e.g., 60,000 times) using a transmission electron microscope (e.g., Hitachi HF-3300S Cs-corrected STEM), and a transmission electron microscope (TEM) diagram of the test sample can be obtained. For example, as is clear from FIG. 4 of the present application, the negative electrode active material of the present application includes a core and a coating layer.

[0078] In this application, the primary particles and secondary particles have the meanings known in the art. The primary particles refer to particles in a non-aggregated state, and the secondary particles refer to particles in an aggregated state in which two or more primary particles are aggregated. The primary particles and the secondary particles can be easily distinguished by taking SEM images with a scanning electron microscope.

[0079] The ratio of the number of secondary particles in the negative active material can be measured using a method known in the art. An exemplary measurement method is to lay and adhere the negative active material to a conductive adhesive to prepare a sample to be measured with a length x width = 6 cm x 1.1 cm, and measure the particle shape using a scanning electron microscope (e.g. ZEISS Sigma 300). For the measurement, JY / T010-1996 can be referred to. In order to ensure the accuracy of the measurement result, a plurality of (e.g. 5) different regions in the sample to be measured are randomly selected and scanned, and the percentage of the number of secondary particles in each region to the total number of particles is calculated at a certain magnification (e.g. 1000 times), to obtain the ratio of the number of secondary particles in the region, and the average value of the measurement results of the plurality of measurement regions is the ratio of the number of secondary particles in the negative active material. In order to ensure the accuracy of the measurement result, the above measurement can be repeated for a plurality of samples (e.g. 10 pieces), and the average value of each sample can be the final measurement result.

[0080] The graphitization degree of the negative electrode active material has a meaning known in the art and can be measured by a method known in the art. The graphitization degree can be measured, for example, by using an X-ray diffraction apparatus (e.g., Bruker D8 Discover) with reference to JIS K0131-1996 and JB / T4220-2011. 002 Measure the size of the 002 ) / (0.344-0.3354)×100%. 002 is the interlayer distance of the graphite crystal structure in nanometers (nm). In the X-ray diffraction analysis measurement, a copper target is used as the anode target, CuKα radiation is used as the radiation source, the radiation wavelength λ=1.5418 Å, the 2θ angle range of the scan is 20° to 80°, and the scan speed may be 4° / min.

[0081] The tap density of the negative electrode active material has a meaning known in the art, and can be measured by a method known in the art. For example, it can be measured by a powder tap density meter with reference to the GB / T5162-2006 standard. When using the FZS4-4B tap density meter of Beijing Iron and Steel Research Institute, the measurement parameters are vibration frequency: 250±15 times / min, amplitude: 3±0.2mm, vibration number: 5000 times, and scale cylinder: 25mL.

[0082] The powder compaction density of the negative electrode active material at a pressure of 2 kN has a meaning known in the art and can be measured using a method known in the art. For example, it is measured by an electronic pressure tester (e.g., UTM7305 type) with reference to the GB / T24533-2009 standard. An exemplary measurement method is to weigh 1 g of the negative electrode active material and measure the powder compaction density at a pressure of 1.327 cm 2 The powder compaction density of the negative electrode active material at a pressure of 2 kN is calculated and recorded.

[0083] The gram capacity of the negative electrode active material has a meaning known in the art and can be measured using methods known in the art. An exemplary measurement method is as follows. The prepared negative electrode active material, carbon black (Super P) as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive are uniformly mixed in a mass ratio of 91.6:1.8:6.6 with a solvent N-methylpyrrolidone (NMP) to prepare a slurry, and the prepared slurry is applied to a copper foil current collector and dried in an oven before use. A metallic lithium sheet is used as the counter electrode, and a polyethylene (PE) film is used as the separator. Ethylene carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte, with the concentration of LiPF6 being 1 mol / L. A CR2430 type coin battery is assembled in an argon atmosphere glove box. The obtained coin battery is left to stand for 12 hours, then discharged at a constant current of 0.05C to 0.005V at 25°C, left to stand for 10 minutes, discharged at a constant current of 50μA to 0.005V, left to stand for 10 minutes, discharged at a constant current of 10μA to 0.005V, and then charged at a constant current of 0.1C to 2V, and the charge capacity is recorded. The ratio of the charge capacity to the mass of the negative electrode active material is the gram capacity of the prepared negative electrode active material.

[0084] The above-mentioned various parameters of the negative electrode active material may be measured by directly taking a sample of the negative electrode active material, or may be measured by sampling from a secondary battery.

[0085] When sampling the above-mentioned sample from the secondary battery, for example, sampling can be performed by the following steps.

[0086] (1) Discharge the secondary battery (for safety reasons, the battery is generally fully discharged), remove the battery, and then take out the negative plate. The negative plate is then immersed in dimethyl carbonate (DMC) for a certain period of time (e.g., 2 to 10 hours). After that, the negative plate is taken out and dried at a certain temperature for a certain period of time (e.g., 60°C, 4 hours). After drying, the negative plate is taken out.

[0087] (2) The negative electrode plate dried in step (1) is baked at a certain temperature and time (e.g., 400°C, 2 h), and an arbitrary area is selected from the baked negative electrode plate, and the negative electrode active material is sampled (the powder can be scraped off with a blade to be sampled).

[0088] (3) The negative electrode active materials collected in step (2) are each subjected to a sieving process (e.g., sieving through a 200 mesh sieve) to finally obtain samples of the negative electrode active materials that can be used to measure the parameters of each of the above materials in the present application.

[0089] The present application next provides a method for preparing a negative electrode active material, and the above-mentioned negative electrode active material can be obtained based on this preparation method. The preparation method for the negative electrode active material can include the following steps A) and B).

[0090] A) Providing a core comprising synthetic graphite.

[0091] B) coating the core so that a coating layer containing amorphous carbon is formed on at least a portion of the surface of the core; v 99≦24μm and 8μm≦D v A negative electrode active material having a particle size of 50≦15 μm is obtained.

[0092] In some embodiments, in step A), the method for producing artificial graphite comprises: a) providing a coke feedstock; b) subjecting the coke raw material to a shaping process to obtain a precursor; Step c) of granulating the precursor to obtain a granulated product; The granules are subjected to a graphitization treatment, v 50 is 6μm to 14μm, and D v and step d) obtaining artificial graphite having a particle size of 17 μm to 26 μm.

[0093] In some embodiments, the coke feedstock D v 50 becomes 7μm~12μm, D vThe coke raw material D 99 is 15μm to 21μm. v 50 and D v 99 can be adjusted. v 50 and D v If the D 99 is within a given range, it is advantageous for improving the subsequent shaping and granulation processes, and the final negative electrode active material has a suitable secondary particle content and a suitable D v 50 and D v Optionally, the coke feedstock D v 50 is 8 μm to 12 μm, 8 μm to 11.5 μm, or 9 μm to 11 μm. Optionally, the D v 99 is 16 μm to 21 μm, 17 μm to 21 μm, 17 μm to 20 μm, or 17 μm to 19 μm.

[0094] In step a), the coke raw material may be a commercially available product or may be obtained by crushing a coke material. In some embodiments, the coke raw material may be subjected to a crushing process to obtain the D of the coke raw material. v 50 and D v 99 can be controlled within a desired range. The coke raw material can be pulverized using equipment and methods known in the art, such as a jet mill, a mechanical mill, or a roll mill. Since many undersized particles are always produced during pulverization, and oversized particles may also be present, classification can be performed after pulverization as necessary to remove undersized and oversized particles in the pulverized powder. After classification, a coke raw material having a desired particle size distribution can be obtained. Classification can be performed using equipment and methods known in the art, such as a classification sieve, a gravity classifier, or a centrifugal classifier.

[0095] The grinding process of the coke raw material can be carried out in a process unit including a grinder, a classifier and an intake fan. In the grinding process, the D of the obtained coke raw material can be controlled by adjusting the supply frequency, grinding frequency, classification frequency and intake frequency. v 50 and D v99 can be adjusted and controlled within a desired range. Compared with the low classification frequency in the conventional pulverization process, the method of the present application can improve the classification frequency, which is advantageous for removing undersized particles. Compared with the high suction frequency in the conventional pulverization process, the method of the present application can reduce the suction frequency, which is advantageous for removing oversized particles. In addition, compared with the wide frequency range controlled in the conventional pulverization process, the method of the present application can further control the main engine frequency, classification frequency, and suction frequency within a narrow frequency range, which can narrow the particle size distribution width of the coke raw material, for example, the D v 50 and D v 99 in a narrow range. Also, by synchronously adjusting and controlling the feeding frequency, the feeding amount can be controlled, which can further improve the material grinding effect.

[0096] In some embodiments, the supply frequency may be between 10 Hz and 40 Hz, for example between 25 Hz and 35 Hz.

[0097] In some embodiments, the grinding frequency may be between 20 Hz and 50 Hz, for example between 35 Hz and 45 Hz.

[0098] In some embodiments, the classification frequency may be between 20 Hz and 50 Hz, for example between 40 Hz and 50 Hz.

[0099] In some embodiments, the inhalation frequency may be between 30Hz and 55Hz, for example between 35Hz and 45Hz.

[0100] Those skilled in the art can select and adjust one or more of the above process conditions according to the actual operating conditions to finally obtain D v 50 is 7μm to 12μm and D v It is possible to obtain a coke raw material having a particle size of 15 μm to 21 μm.

[0101] In some embodiments, the coke feedstock in step a) may comprise one or more of petroleum based non-needle coke, petroleum based needle coke. Optionally, the coke feedstock comprises petroleum green coke.

[0102] In some embodiments, the volatile content C1 of the coke raw material described in step a) satisfies 1%≦C1≦12%. Optionally, the volatile content C1 of the coke raw material is 3%-10%, 5%-9%, 6%-8%, 7%-8.5%, or 7.5%-8.5%, etc. The appropriate volatile content of the coke raw material is favorable for improving the particle size distribution of the material in the subsequent granulation process, and helps the negative electrode active material have a desired particle size distribution. In addition, the appropriate volatile content of the coke raw material can also ensure that the prepared artificial graphite has high structural strength, improve the cycle life of the negative electrode active material, and improve the cycle performance of the battery.

[0103] The volatile content of the coke feedstock can be measured by methods known in the art, for example, with reference to SH / T0026-1990.

[0104] In step b), the corners of the coke raw material particles can be polished by shaping, which is advantageous for the subsequent granulation process, and the secondary particles in the obtained negative electrode active material have high structural stability. The shaping process can be performed on the coke raw material using equipment and methods known in the art, such as a shaping machine or other shaping devices.

[0105] In some embodiments, the coke raw material is shaped and then classified to obtain the precursor D v 50 is 8μm~13μm, D v 99 is 16μm to 22μm, and the final negative electrode active material has an appropriate secondary particle content and an appropriate D v 50 and D v 99. Optionally, the precursor D v50 is 9 μm to 12 μm, 9 μm to 11 μm, 10 μm to 12 μm, or 10 μm to 11 μm. D of the precursor v 99 is 17 μm to 22 μm or less, 18 μm to 21 μm or less, or 18 μm to 20 μm or less. The classification process can be performed using equipment and methods known in the art, such as a classification sieve, a gravity classifier, or a centrifugal classifier.

[0106] The shaping and classification process can be performed in a process unit including a shaping machine, a classifier, and an intake fan. In the shaping and classification process, the shaping frequency (e.g., the main and auxiliary machine frequencies of the shaping machine), the classification frequency, and the intake frequency are adjusted to control the D of the obtained precursor. v 50 and D v The inventors found that, compared with the conventional shaping and classification processes, the method of the present application can improve the shaping frequency in the treatment process, appropriately extend the shaping time, and further reduce the classification frequency and intake frequency in the treatment process, thereby improving the D of the obtained precursor. v 50 and D v Adjust and control 99 within the target range.

[0107] The obtained precursor may further have a suitable particle size uniformity (U1), which helps to improve the particle size uniformity of the obtained negative electrode active material.

[0108] In some embodiments, the particle size uniformity U1 of the precursor satisfies 0.2≦U1≦0.55, such as 0.2≦U1≦0.5, 0.25≦U1≦0.45, 0.3≦U1≦0.45, 0.3≦U1≦0.4, 0.35≦U1≦0.55, or 0.35≦U1≦0.45.

[0109] In some embodiments, in step b), the main machine frequency of the shaping machine is controlled to 35 Hz to 40 Hz, the auxiliary machine frequency is controlled to 60 Hz to 70 Hz, the classification frequency is controlled to 40 Hz to 50 Hz, the intake frequency is controlled to 10 Hz to 25 Hz, and the shaping time is controlled to 160 s to 180 s, thereby performing shaping and classification treatment on the coke raw material, and D v 50 is 8 μm to 13 μm and Dv Obtain precursors with sizes between 16 μm and 22 μm.

[0110] In step c), the precursor is granulated to aggregate the independently dispersed primary particles to form secondary particles, which improves the isotropy of the artificial graphite, allows active ions to be absorbed into the particles from all directions, improves the lithium absorption rate of the solid phase, and reduces polarization.

[0111] In some embodiments, D of the granulation obtained in step c) v 50 is 9μm to 15μm, D v 99 may be 17 μm to 24 μm. Optionally, the D v 50 is 10 μm to 14 μm, 11 μm to 15 μm, or 11 μm to 13 μm. Optionally, the granulation D v 99 is 18 μm to 24 μm or 19 μm to 22 μm. v 50 and D v If 99 is within the appropriate range, the D v 50 and D v This is advantageous in bringing 99 into the desired range.

[0112] In step c), granulation can be performed using equipment known in the art, such as a granulator. The granulator generally includes a stirring reactor and a module for controlling the temperature of the reactor. By adjusting and controlling the stirring rotation speed, temperature rise rate, granulation temperature, temperature fall rate, etc. during the granulation process, the degree of granulation can be adjusted and controlled, and the D of the obtained granules can be adjusted and controlled. v 50 and D v Furthermore, by adjusting the above granulation process, the D 99 of the finally obtained negative electrode active material can be set within a desired range. v 10. D v 90 in the desired range, and the D v 10. D v 90 can be made to meet your needs.

[0113] In some embodiments, the precursor and the adhesive can be mixed and then granulated at high temperature. The mixing temperature may be 20°C to 40°C. Compared with the conventional graphite manufacturing process, the present invention can improve the granulation degree by appropriately increasing the mixing frequency and shortening the mixing time, and the D of the obtained granulated product can be improved. v 50 and D v 99 within the desired range.

[0114] The temperature of the high-temperature granulation can be determined according to the type of adhesive. The adhesive softens at high temperature, and the particles are bonded together to achieve granulation. In some embodiments, the adhesive is pitch. In these examples, the granulation temperature may be 700°C to 800°C. The present application further improves the temperature rise program of the high-temperature granulation process, and adopts a stepwise temperature rise. By setting multiple (e.g., 2 to 4) program temperature rise platforms in the temperature rise process, the granulated material can have a desired particle size distribution. In addition, the particle size uniformity of the granulated material is good, which helps the subsequent artificial graphite and the final negative electrode active material product to have good particle size uniformity.

[0115] In some embodiments, in step c), the mixing frequency is controlled to 35 Hz to 38 Hz, and the mixing time is controlled to 50 min to 65 min. Then, the temperature is increased to 300°C to 400°C at 6 to 10°C / min, and the temperature is maintained for 1 to 2 hours. Then, the temperature is increased to 500°C to 600°C at 6 to 10°C / min, and the temperature is maintained for 1 to 2 hours. Then, the temperature is increased to 700°C to 800°C at 6 to 10°C / min, and the temperature is maintained for 1 to 2 hours. Then, the temperature is naturally decreased to obtain a granulated product.

[0116] In some embodiments, in step c), the amount C2 of the adhesive added during the granulation process is related to the volatile matter content C1 of the coke raw material and the particle size uniformity U1 of the precursor in a relationship of 21%≦(C1+C2) / U1×100%≦50%. Optionally, 25%≦(C1+C2) / U1×100%≦45%, 25%≦((C1+C2) / U1×100%≦38%, 27%≦(C1+C2) / U1×100%≦38%, 30%≦(C1+C2) / U1×100%≦40%, or 31%≦(C1+C2) / U1×100%≦35%. When the above relationship is satisfied between the amount C2 of the binder added during the granulation process, the volatile matter content C1 of the coke raw material, and the particle size uniformity U1 of the precursor, the granulation degree of the negative electrode active material particles can be improved, and the deionization performance and structural stability of the negative electrode active material can be improved.

[0117] The amount C2 of the adhesive added in the granulation process is the percentage of the weight of the adhesive added in the granulation process to the total weight of the precursor. The granulation process is carried out with or without the addition of an adhesive.

[0118] In some embodiments, the amount of adhesive C2 added to the granulation process can satisfy 0%≦C2≦16%, optionally 1%≦C2≦12%, 2%≦C2≦10%, 4%≦C2≦7%, or 5%≦C2≦9%.

[0119] In some embodiments, in step d), the granules are graphitized at a temperature of 2800° C. to 3200° C. to obtain artificial graphite having an appropriate degree of graphitization. Optionally, the graphitization temperature may be 2900° C. to 3100° C.

[0120] In step d), graphitization can be performed using equipment known in the art, such as a graphitization furnace, for example, an Acheson-type graphitization furnace. After the graphitization process is completed, a small amount of oversized particles formed by the granules agglomerating during the high-temperature graphitization can be removed by sieving, and the D of the finally obtained negative electrode active material can be obtained. v 50 and D v It is advantageous to have 99 within the desired range.

[0121] In some embodiments, the D of the artificial graphite obtained in step d) v 50 may be 6.5 μm to 14 μm, 7 μm to 14 μm, 6 μm to 13 μm, 7 μm to 13.5 μm, 8 μm to 12 μm, 9 μm to 12 μm, 9 μm to 11 μm, 10 μm to 13 μm, 10 μm to 12 μm, 6.5 μm to 12 μm, or 6.5 μm to 12.5 μm.

[0122] In some embodiments, the D of the artificial graphite obtained in step d) v 99 may be 18 μm to 24 μm, 19 μm to 26 μm, 21 μm to 26 μm, 20 μm to 25 μm, 20 μm to 23 μm, or 19.5 μm to 22 μm.

[0123] In some embodiments, the particle size uniformity U2 of the artificial graphite obtained in step d) can satisfy 0.22≦U2≦0.48, and optionally 0.25≦U2≦0.45, 0.26≦U2≦0.43, 0.3≦U2≦0.4, or 0.33≦U2≦0.38. If the particle size uniformity of the obtained artificial graphite is within an appropriate range, it is advantageous for the particle size uniformity of the final negative electrode active material to be within a desired range.

[0124] In some embodiments, step B) can include step e) of coating the core with an organic carbon source and forming an amorphous carbon coating layer on at least a portion of the surface of the core by heat treatment to obtain the negative electrode active material.

[0125] In some embodiments, in step e), an amorphous carbon coating layer is formed on at least a portion of the surface of the core, followed by sieving to obtain the negative electrode active material.

[0126] For example, the artificial graphite obtained in step d) can be mixed with an organic carbon source, at least a part of the surface of the artificial graphite can be coated with the organic carbon source, and then the organic carbon source can be carbonized by heat treatment at a temperature of 700° C. to 1800° C. to form an amorphous carbon coating layer on at least a part of the surface of the artificial graphite. Optionally, the temperature of the heat treatment is 1000° C. to 1300° C.

[0127] In some embodiments, the amount C3 of the organic carbon source added during the coating process satisfies the relationship between the volatile content C1 of the coke raw material, the amount C2 of the adhesive added during the granulation process, and the particle size uniformity U2 of the artificial graphite, and the relationship satisfies 20%≦(C1+C2+C3) / U2×100%≦56%. And the organic carbon source satisfies 1.2%≦C3×residual carbon ratio≦2.5%. The amount C3 of the organic carbon source is the percentage of the weight of the organic carbon source added during the coating process relative to the total weight of the artificial graphite. The residual carbon ratio is the residual carbon ratio of the organic carbon source, which can be measured using the LP-5731 coal pitch coking value measuring instrument, and the measurement can be performed by referring to GB / T268 "Method for Determining Residual Carbon in Petroleum Products" and GB / T8727-2008 "Method for Determining Coking Value of Coal Pitch-Based Products".

[0128] When the amount of the organic carbon source added in the coating process satisfies the above relationship, the granulation degree of the negative electrode active material can be improved, and it is advantageous that the particle size uniformity, particle size specific surface area, and number ratio of secondary particles of the negative electrode active material are within the above range. In addition, the amount of the organic carbon source used is within the above range, and the ratio of the coating layer in the negative electrode active material is appropriate, so that the negative electrode active material can achieve both good dynamic performance and long cycle life. Optionally, 30%≦((C1+C2+C3) / U2×100%≦48%. Further optionally, 40%≦(C1+C2+C3) / U2×100%≦48%. Optionally, 1.5%≦C3×residual carbon ratio≦2.4%, 1.8%≦C3×residual carbon ratio≦2.3%, or 2%≦C3×residual carbon ratio≦2.2%.

[0129] Optionally, 2%≦C3≦8%. For example, C3 may be 3%, 4%, 5%, 6% or 7%.

[0130] In some embodiments, the organic carbon source can be selected from one or more of pitch (eg, coal pitch, petroleum pitch), phenolic resin, coconut shells, and the like, more preferably pitch.

[0131] In the above-mentioned preparation process, the coke raw material generally contains some impurity elements (e.g., iron, nickel, chromium, zinc, sulfur, silicon, etc.), and some impurity elements (e.g., iron, copper, etc.) are also introduced in the equipment used in the crushing, shaping, and granulation processes. Generally, the content of impurity elements in the core is small, generally less than 1 ppm.

[0132] In the above-mentioned preparation process, trace amounts of impurity elements are introduced into the coating layer due to the organic carbon source used in the coating process and the equipment used for coating.

[0133] secondary battery

[0134] The present application further provides a secondary battery. The secondary battery includes a positive electrode plate, a negative electrode plate, and an electrolyte. During the charging and discharging process of the battery, active ions shuttle between the positive electrode plate and the negative electrode plate to be absorbed and released. The electrolyte serves to conduct ions between the positive electrode plate and the negative electrode plate.

[0135] [Negative plate]

[0136] In the secondary battery according to the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, and the negative electrode film layer includes any one or more types of negative electrode active materials according to the present application.

[0137] In some embodiments, the negative electrode film layer may optionally contain a certain amount of other commonly used negative electrode active materials in addition to the above-mentioned negative electrode active materials of the present application, such as one or more of natural graphite, other artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based materials may be selected from one or more of elemental silicon, silicon oxide, and silicon carbon composites. The tin-based materials may be selected from one or more of elemental tin, tin oxide, and tin alloys.

[0138] In the secondary battery according to the present application, the negative electrode film layer generally includes a negative electrode active material, an optional adhesive, an optional conductive agent, and other optional auxiliary agents, and is generally formed by coating and drying a negative electrode slurry. The negative electrode slurry is generally formed by dispersing the negative electrode active material, the optional conductive agent, the adhesive, etc. in a solvent and stirring the mixture uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water.

[0139] By way of example, the conductive agent may include one or more of superconducting carbon, carbon black (eg, acetylene black, ketjen black), carbon dots, carbon nanotubes, graphene, carbon nanofibers, and the like.

[0140] By way of example, the adhesive may include one or more of styrene butadiene rubber (SBR), water soluble unsaturated resin SR-1B, water-based acrylic resin, polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).

[0141] Other optional auxiliary agents are, for example, thickeners (eg, sodium carboxymethylcellulose CMC-Na), PTC thermistor materials, and the like.

[0142] In the secondary battery according to the present application, the negative plate does not exclude additional functional layers other than the negative film layer. For example, in some embodiments, the negative plate according to the present application may further include a conductive undercoat layer (e.g., composed of a conductive agent and an adhesive) interposed between the negative current collector and the first negative film layer and provided on the surface of the negative current collector. In some other embodiments, the negative plate according to the present application may further include a coating protection layer that covers the surface of the second negative film layer.

[0143] [Positive plate]

[0144] In the secondary battery according to the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer that is provided on at least one surface of the positive electrode current collector and contains a positive electrode active material. The positive electrode current collector has, for example, two surfaces that face each other in the thickness direction, and the positive electrode film layer is provided on either one or both of the two facing surfaces of the positive electrode current collector.

[0145] In the secondary battery according to the present application, the positive electrode active material may be a positive electrode active material for secondary batteries known in the art. The positive electrode active material may include, for example, at least one or more of lithium transition metal oxides, olivine-type lithium-containing phosphates, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide, lithium nickel oxide, lithium manganate, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganate, lithium nickel cobalt manganate, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of olivine-type lithium-containing phosphates may include, but are not limited to, lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and their modified compounds. The present application is not limited to these materials, and other known materials that have been conventionally available as positive electrode active materials for secondary batteries may be used.

[0146] In some embodiments, in order to further improve the energy density of the battery, the cathode active material can include one or more of the lithium transition metal oxides and their modified compounds represented by Formula 1.

[0147] Li a Ni b Co c M d O e A f ···Formula 1

[0148] In Formula 1, 0.8 ≦ a ≦ 1.2, 0.5 ≦ b < 1, 0 < c < 1, 0 < d < 1, 1 ≦ e ≦ 2, 0 ≦ f ≦ 1, M is selected from one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A is selected from one or more of N, F, S, and Cl.

[0149] In the present application, the modified compound of each of the above materials may be obtained by doping modification or surface coating modification of the cathode active material.

[0150] In the secondary battery according to the present application, the cathode film layer generally includes a cathode active material, an optional binder, and an optional conductive agent, and is generally formed by applying, drying, and cold pressing a cathode slurry. The cathode slurry is generally formed by dispersing a cathode active material, an optional conductive agent, a binder, etc. in a solvent and uniformly stirring. The solvent may be N-methylpyrrolidone (NMP).

[0151] As an example, the binder used in the cathode film layer can include one or more of polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE).

[0152] By way of example, the conductive agent used in the positive electrode membrane layer may include one or more of superconducting carbon, carbon black (e.g., acetylene black, ketjen black), carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0153] In the secondary battery according to the present application, the positive electrode current collector can be a metal foil piece or a composite current collector (a composite current collector can be formed by providing a metal material on a polymer substrate). For example, the positive electrode current collector can be an aluminum foil.

[0154] [Electrolyte]

[0155] The type of electrolyte in the secondary battery according to the present application is not particularly limited and can be selected as necessary. The electrolyte can be selected from at least one of a solid electrolyte and a liquid electrolyte (i.e., an electrolytic solution).

[0156] In some embodiments, the electrolyte is an electrolytic solution that includes an electrolyte salt and a solvent.

[0157] In some embodiments, the electrolyte salt can be selected from one or more of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluoro(oxalato)borate), LiBOB (lithium bis(oxalato)borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorobis(oxalato)phosphate), and LiTFOP (lithium tetrafluoro(oxalato)phosphate).

[0158] In some embodiments, the solvent may be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).

[0159] In some embodiments, the electrolyte optionally includes an additive, for example, an additive that can improve some performance of the battery, such as an additive that improves the overcharge performance of the battery, an additive that improves the high temperature performance of the battery, or an additive that improves the low temperature performance of the battery.

[0160] [Separator]

[0161] Secondary batteries using an electrolyte solution or some secondary batteries using a solid electrolyte further include a separator. The separator is provided between the positive electrode plate and the negative electrode plate and plays a role of isolation. In the present application, the type of separator is not particularly limited, and any known separator with a porous structure having good chemical stability and mechanical stability can be used. In some embodiments, the material of the separator can be selected from one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single layer film or a multilayer composite film. When the separator is a multilayer composite film, the materials of each layer may be the same or different.

[0162] In some embodiments, the positive plate, the negative plate, and the separator can be formed into an electrode assembly by a winding or stacking process.

[0163] In some embodiments, the secondary battery can include an exterior packaging, which is used to package the electrode assembly and electrolyte.

[0164] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.

[0165] The present application does not particularly limit the shape of the secondary battery, and the secondary battery may be cylindrical, rectangular, or any other shape. Fig. 5 shows a secondary battery 5 having a rectangular structure as an example.

[0166] In some embodiments, as shown in FIG. 6, the exterior may include a housing 51 and a cover plate 53. The housing 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate surround and form a storage chamber. The housing 51 has an opening communicating with the storage chamber, and the cover plate 53 covers the opening so as to close the storage chamber. The positive electrode plate, the negative electrode plate, and the separator may form an electrode assembly 52 through a winding process or a stacking process. The electrode assembly 52 is sealed in the storage chamber. The electrolyte is permeated into the electrode assembly 52. ​​The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be adjusted as necessary.

[0167] In some embodiments, the secondary batteries can be assembled into a battery module, and the number of secondary batteries included in the battery module can be multiple, and the specific number can be adjusted based on the application and capacity of the battery module.

[0168] Fig. 7 shows an example of a battery module 4. As shown in Fig. 7, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed with a fastener.

[0169] Optionally, the battery module 4 may further include a housing having an accommodation space for accommodating a plurality of secondary batteries 5.

[0170] In some embodiments, the battery modules can be further assembled into a battery pack, and the number of battery modules included in the battery pack can be adjusted based on the application and capacity of the battery pack.

[0171] 8 and 9 show an example of a battery pack 1. As shown in Fig. 8 and 9, the battery pack 1 may include a battery case and a plurality of battery modules 4 provided in the battery case. The battery case includes an upper case 2 and a lower case 3, and the upper case 2 is configured to cover the lower case 3 to form an enclosed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery case in any manner.

[0172] Device

[0173] The present application further provides a device including at least one of the secondary battery, battery module, or battery pack according to the present application. The secondary battery, battery module, or battery pack may be used as a power source for the device, or may be used as an energy storage means for the device. The device may be, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf car, an electric truck, etc.), a train, a ship, a satellite, an energy storage system, etc. The device can select a secondary battery, a battery module, or a battery pack according to its usage requirements.

[0174] An example of the device is shown in Figure 10. The device may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the demand for high power and high energy density, a battery pack or a battery module may be used.

[0175] Another example of the device may be a mobile phone, a tablet computer, a notebook computer, etc. These devices are generally required to be lightweight and thin, and can use a secondary battery as a power source.

[0176] Working Example

[0177] The following examples will more specifically describe the disclosure of the present application, and these examples are merely illustrative, and various modifications and variations within the scope of the disclosure of the present application will be apparent to those skilled in the art. Unless otherwise specified, all parts, percentages, and ratios described in the following examples are based on weight. In addition, all reagents used in the examples can be purchased or synthesized according to conventional methods, and can be used as is without further treatment, and all instruments used in the examples can be purchased.

[0178] 1. Battery manufacturing

[0179] Example 1

[0180] Preparation of negative electrode active material

[0181] The petroleum raw coke with a volatile content C1 of 7.87% was used. The petroleum raw coke was crushed and v 50 is 11.8 μm and D v The coke raw material with a particle size of 20.1 μm was obtained.

[0182] The coke raw material is shaped and classified, v 50 is 13.0 μm and D v A precursor with a particle size of 21.3 μm was obtained.

[0183] The precursor is granulated using pitch as an adhesive, and the amount of adhesive used C2 is 5%. The resulting granulated material is D v 50 is 13.7 μm, D v 99 is 21.9 μm.

[0184] The granulated material was graphitized at a temperature of 3000°C, and then sieved to obtain artificial graphite. v 99 is 22.9 μm.

[0185] Then, the artificial graphite is coated with pitch, which is an organic carbon source, and then carbonized to obtain a negative electrode active material having an organic carbon source usage amount C3 of 3%. The negative electrode active material includes an artificial graphite core and an amorphous carbon coating layer that coats the surface of the artificial graphite core, and the negative electrode active material is D v 50 is 14.5 μm, D v 99 is 22.3 μm and the gram capacity is 355.2 mAh / g.

[0186] Preparation of negative electrode plate

[0187] The negative electrode active material prepared above, styrene butadiene rubber (SBR) as an adhesive, sodium carboxymethylcellulose (CMC-Na) as a thickener, and carbon black (Super P) as a conductive agent were mixed in a weight ratio of 96.2:1.8:1.2:0.8 with an appropriate amount of deionized water and thoroughly stirred to form a uniform negative electrode slurry. The negative electrode slurry was applied to the surface of copper foil as a negative electrode current collector, and then dried, cold pressed, striped, and cut to obtain a negative electrode plate. The negative electrode plate had a compaction density of 1.65 g / cm. 3 , surface density is 123g / m 2 It is.

[0188] Preparation of the positive electrode plate

[0189] Lithium Nickel Cobalt Manganese Oxide LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), carbon black (Super P) as a conductive agent, and PVDF as an adhesive were thoroughly mixed in an appropriate amount of N-methylpyrrolidone (NMP) in a weight ratio of 97.5:1.5:1 to form a uniform positive electrode slurry, which was then applied to the surface of an aluminum foil as a positive electrode current collector, and the positive electrode plate was obtained through drying, cold pressing, striping, and cutting. The positive electrode plate had a compaction density of 3.5 g / cm. 3 and the areal density is 196 g / m 2 It was.

[0190] Separator

[0191] A polyethylene (PE) film was used as the separator.

[0192] Preparation of electrolyte

[0193] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1, and then thoroughly dried lithium salt LiPF6 was uniformly dissolved in the above solution to obtain an electrolyte solution, with a LiPF6 concentration of 1 mol / L.

[0194] Secondary battery manufacturing

[0195] A positive electrode plate, a separator, and a negative electrode plate are stacked in this order, and a reference electrode (the reference electrode is used for subsequent performance measurement of the battery sample, and can be a lithium sheet, a lithium wire, etc., and the reference electrode should be separated by the separator to prevent contact with either side of the positive or negative electrode plate) is added between the separator and the negative electrode plate. After winding, an electrode assembly is obtained, the electrode assembly is placed in an outer casing, the above-mentioned electrolyte is added, and a secondary battery is obtained after processes such as sealing, standing, formation, and aging.

[0196] In Examples 2 to 20 and Comparative Examples 1 and 2, the preparation method is similar to that of Example 1, but the preparation parameters of the negative electrode active material are adjusted. Details of the different preparation parameters and product parameters are shown in Tables 2 to 5.

[0197] Second, battery performance measurement

[0198] (1) Measurement of quick charging performance

[0199] At 25°C, the secondary batteries produced in the examples and comparative examples were charged at a constant current of 1C (i.e., the current value at which the theoretical capacity is completely discharged within 1 hour) to 4.25V, then charged at a constant voltage of 0.05C, allowed to stand for 5 minutes, and further discharged at a constant current of 1C to 2.8V, and the actual capacity was recorded as C0.

[0200] Next, the battery was charged at a constant current of 0.5C0, 1C0, 1.5C0, 2C0, 2.5C0, 3C0, 3.5C0, 4C0, and 4.5C0 in sequence to a negative electrode final potential of 4.25V or 0V (based on the first one reached). Each time charging was completed, it was necessary to discharge to 2.8V at 1C0. The corresponding negative electrode potentials were recorded when charging to 10%, 20%, 30%...80% SOC (State of Charge) at different charging rates, and the charging rate-negative electrode potential curves at different SOC states were drawn and linearly fitted to obtain the charging rate corresponding to when the negative electrode potential at different SOC states was 0V. This charging rate is the charging window at that SOC state, and each C 20%SOC , C30%SOC , C 40%SOC , C 50%SOC , C 60%SOC , C 70%SOC , C 80%SOC and the formula (60 / C 20%SOC +60 / C 30%SOC +60 / C 40%SOC +60 / C 50%SOC +60 / C 60%SOC +60 / C 70%SOC +60 / C 80%SOC ) × 10%, the charging time T (min) for this battery to be charged from 10% SOC to 80% SOC was calculated. The shorter this time, the better the rapid charging performance of the battery.

[0201] (2) Measurement of cycle performance

[0202] At 25°C, the secondary batteries manufactured in the examples and comparative examples were charged at a constant current of 0.33C to a charge end voltage of 4.25V, then charged at a constant voltage of 0.05C, left to stand for 5 minutes, and further discharged at a constant current of 0.33C to a discharge end voltage of 2.8V, and the initial capacity was recorded as C0. Thereafter, the secondary batteries were charged according to the method described in Table 1, and discharged at 0.33C, and the cycle capacity retention rate (C n / C0×100%) until the discharge capacity C per cycle is 80% n The cycle count was recorded, and the number of cycles was recorded. A higher number of cycles indicates a higher cycle life of the battery.

[0203] [Table 1]

[0204] The measurement results of Examples 1 to 20 and Comparative Examples 1 and 2 are shown in Tables 3 and 5 in detail.

[0205] [Table 2]

[0206] [Table 3]

[0207] As can be seen from the results in Table 3, the negative electrode active material according to the present invention has a core containing artificial graphite and a coating layer containing amorphous carbon that coats the surface of the core, and the negative electrode active material has a D v 99≦24μm and 8μm≦D v By simultaneously satisfying the requirement of 50≦15 μm, a secondary battery using this negative electrode active material can achieve improved rapid charging capability and cycle performance under the condition of high energy density.

[0208] Comparative Example 1 does not satisfy the above conditions, and is therefore inferior in both quick charging capability and cycle performance.

[0209] [Table 4]

[0210] In Table 4, A = (C1 + C2) / U1 × 100%; B = (C1 + C2 + C3) / U2 × 100%

[0211] [Table 5]

[0212] As can be seen from the results of Examples 7 to 11, when the negative electrode active material further satisfies the requirement that the particle size uniformity is within an appropriate range, the rapid charging capability and cycle performance of the battery can be further improved.

[0213] As can be seen from the results of Examples 12 to 20, when the negative electrode active material further satisfies that its particle size-specific surface area or the number ratio of secondary particles is within an appropriate range, the rapid charging capability and cycle performance of the battery can be further improved.

[0214] The above content is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto, and a person skilled in the art can easily think of various equivalent modifications and replacements within the technical scope disclosed in the present application, and all of these modifications and replacements belong to the scope of protection of the present application. Therefore, the scope of protection of the present application should be based on the scope of protection of the claims.

Claims

1. A negative electrode active material having a core containing artificial graphite and a coating layer containing amorphous carbon that coats at least a portion of a surface of the core, The particle size uniformity of the negative electrode active material is 0.25 to 0.45, and the volume particle size distribution D v 99≦24 μm, D v 99 is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 99%.

2. The volume particle size distribution D of the negative electrode active material v 99 is 17 μm≦D v The negative electrode active material according to claim 1 , which satisfies 99≦24 μm.

3. The average volume particle diameter D of the negative electrode active material v 50 is 9 μm≦D v 50≦13 μm, D v 3. The negative electrode active material according to claim 1, wherein 50 is a particle size corresponding to a cumulative volume distribution percentage of the negative electrode active material reaching 50%.

4. The negative electrode active material according to any one of claims 1 to 3, wherein the particle size uniformity of the negative electrode active material is 0.32 to 0.

38.

5. The particle size specific surface area of ​​the negative electrode active material is 0.4 m 2 / g to 0.75 m 2 The negative electrode active material according to any one of claims 1 to 4, wherein the negative electrode active material has a molecular weight of 1000 or more and a molecular weight of 1000 or more.

6. The negative electrode active material according to any one of claims 1 to 5, wherein the negative electrode active material contains secondary particles, and a ratio of the number of the secondary particles in the negative electrode active material is ≧50%.

7. The negative electrode active material has a density of 0.6≦(D v 90-D v 10) / D v 50≦1.8 is satisfied, D v D 90 is the particle size corresponding to the cumulative volume distribution percentage of the negative active material reaching 90%, v D10 is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 10%, v 7. The negative electrode active material according to claim 1, wherein 50 is a particle size corresponding to a cumulative volume distribution percentage of the negative electrode active material reaching 50%.

8. The volume particle size distribution D of the negative electrode active material v The negative electrode active material according to any one of claims 1 to 7, wherein 90 is 13 µm to 18 µm.

9. The volume particle size distribution D of the negative electrode active material v The negative electrode active material according to any one of claims 1 to 8, wherein 10 is 5 µm to 10 µm.

10. The negative electrode active material further comprises (1) the degree of graphitization of the negative electrode active material is 91.0% to 96.0%; (2) the gram capacity of the negative electrode active material is 345 mAh / g to 360 mAh / g; (3) The tap density of the negative electrode active material is 0.9 g / cm 3 ~1.3g / cm 3 And, (4) The powder compaction density of the negative electrode active material at a pressure of 2 kN is 1.55 g / cm 3 ~1.67g / cm 3 The negative electrode active material according to any one of claims 1 to 9, which satisfies one or more of the following conditions.

11. A) providing a core comprising synthetic graphite; The core is coated, and a coating layer containing amorphous carbon is formed on at least a part of the surface of the core. The particle size uniformity of the negative electrode active material is 0.25 to 0.

45. v A method for producing a negative electrode active material, comprising: a step B) obtaining a negative electrode active material satisfying a particle size distribution of 99≦24 μm, v 99 is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 99%.

12. In the step A), the artificial graphite is produced by a) providing a coke feedstock; b) subjecting the coke raw material to a shaping process to obtain a precursor; Step c) of granulating the precursor to obtain a granulated product; The granules are graphitized to obtain a volume average particle diameter D v 50 is 6 μm to 14 μm and the volume particle size distribution D v and step d) of obtaining artificial graphite having a particle size of 17 μm to 26 μm, v 12. The method according to claim 11, wherein 50 is the particle size corresponding to when the cumulative volume distribution percentage of the negative electrode active material reaches 50%.

13. The volume average particle diameter D of the granules v 50 is 9 μm to 15 μm, and the volume particle size distribution D v 13. The method of claim 12, wherein 99 is 17 μm to 24 μm.

14. The volume average particle diameter D of the precursor v 50 is 8 μm to 13 μm, and the volume particle size distribution D v The method according to any one of claims 12 to 13, wherein 99 is between 16 μm and 22 μm.

15. The volume average particle diameter D of the coke raw material v 50 is 7 μm to 12 μm, and the volume particle size distribution D v The method according to any one of claims 12 to 14, wherein 99 is between 15 μm and 21 μm.

16. The particle size uniformity of the precursor is U 1 And 0.2≦U 1 ≦0.55, or The particle size uniformity of the artificial graphite is U 2 And 0.22≦U 2 The method according to any one of claims 12 to 15, wherein the ratio satisfies ≦0.

48.

17. The volatile matter content of the coke raw material is C 1 The particle size uniformity of the precursor is U 1 In the granulation process of step c), an adhesive is added, and the amount of the adhesive used is C 2 and 21%≦(C 1 +C 2 ) / U 1 The method according to any one of claims 12 to 16, wherein x 100%≦50% is satisfied.

18. The volatile matter content C of the coke raw material 1 1%≦C 1 The method according to any one of claims 12 to 17, wherein the .lambda. / .lambda. ratio satisfies ≦12%.

19. 19. The method of any one of claims 12 to 18, wherein the coke feedstock comprises one or more of petroleum based non-acicular coke, petroleum based needle coke.

20. The step B) comprises: The method according to any one of claims 11 to 19, further comprising a step e) of coating the core with an organic carbon source and forming an amorphous carbon coating layer on at least a portion of a surface of the core by heat treatment to obtain the negative electrode active material.

21. The step B) includes coating the core with an organic carbon source and forming an amorphous carbon coating layer on at least a part of the surface of the core by heat treatment to obtain the negative electrode active material, and the volatile matter content of the coke raw material is reduced to C 1 An adhesive is added during the granulation process of step c), and the amount of the adhesive used is C 2 The particle size uniformity of the artificial graphite is U 2 The amount of the organic carbon source used is C 3 and 20%≦(C 1 +C 2 +C 3 ) / U 2 × 100% ≦ 56%, 1.2% ≦ C 3 The method according to any one of claims 12 to 19, wherein the residual carbon rate is ≦2.5%.

22. A secondary battery comprising a negative electrode plate containing the negative electrode active material according to any one of claims 1 to 10.

23. A battery module comprising the secondary battery according to claim 22.

24. A battery pack comprising the secondary battery according to claim 22 or the battery module according to claim 23.

25. An apparatus including at least one of the secondary battery according to claim 22, the battery module according to claim 23, or the battery pack according to claim 24.

Citation Information

Patent Citations

  • Lithium battery negative electrode material and preparation method thereof

    CN110767888A

  • Negative electrode active material, and electrochemical device and electronic device using same

    CN111354944A

  • Negative electrode material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte battery using the same

    JP2010251315A

  • Negative electrode material for nonaqueous secondary battery, negative electrode using the same, and nonaqueous secondary battery

    JP2012216532A

  • Negative electrode active material and lithium battery employing the same material