Photosensitive film laminate, cured product, and printed wiring board
The photosensitive film laminate with controlled surface roughness and composition achieves high blackness and low gloss, addressing the challenge of scratch visibility and ink visibility in solder resist layers, enhancing production yield.
Patent Information
- Application Number
- JP2021161590
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-27
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024164330000001 
Figure 2024164330000002 
Figure 2024164330000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive film laminate. The present invention further relates to a cured product formed using the photosensitive film laminate and a printed wiring board including the cured product. [Background technology]
[0002] In general, in the case of printed wiring boards used in electronic devices, etc., when mounting electronic components on the printed wiring board, a solder resist layer is formed in areas other than connection holes on the board on which the circuit pattern is formed in order to prevent solder from adhering to unnecessary areas.
[0003] In recent years, electronic devices have become lighter, thinner, shorter, and smaller, leading to increased precision and density of printed wiring boards. Currently, solder resist layers are mainly formed using a so-called photosolder resist, in which a photosensitive resin composition is applied to a substrate, dried, exposed to light, and developed to form a pattern, and the patterned resin is then fully cured by heating or irradiating it with light.
[0004] It has also been proposed to form a solder resist layer using a so-called photosensitive film laminate having a photosensitive film without using the liquid photosensitive resin composition as described above. Such a photosensitive film laminate is generally formed by laminating a photosensitive film formed from a photosensitive resin composition on a support film, and a protective film may be laminated on the surface of the photosensitive film as necessary. When using such a photosensitive film laminate, the protective film is peeled off and the laminate is laminated on a wiring board by hot pressing, and the support film is peeled off before exposure or after exposure from the support film side and development is performed to form a patterned solder resist layer. By using a photosensitive film laminate, the drying process after application can be eliminated compared to the case of wet coating, and the surface smoothness and surface hardness of the obtained solder resist layer are also excellent.
[0005] On the other hand, since solder resist is used as the outermost layer of a board and is formed in the final stage of the board manufacturing process, it may be scratched during the board manufacturing process by the use of equipment or transportation tools (for example, Patent Document 1). These scratches may result in a NG judgment in a visual inspection, and the production yield may decrease. In recent years, even minute scratches that do not affect quality can cause a drop in productivity, making this an important requirement, and new improvement methods are being sought.
[0006] On the other hand, in consideration of the case where the printed wiring board is repaired, the names and positions of mounted components may be formed on the solder resist layer using marking ink. Marking inks used are mainly thermosetting and UV curing types formed by pattern printing, or negative alkaline development types formed by exposing through a negative film and removing the unexposed parts with an alkaline aqueous solution (for example, Patent Document 2). When the color of the solder resist layer, which serves as the background color, is a dark color such as green or black, white or yellow marking inks are often used. For this reason, it is desirable for the black solder resist layer to have a high degree of blackness. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-206992 A [Patent Document 2] JP 2002-97239 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, when a photosensitive laminate using a support film as the first film as disclosed in Patent Document 1 is used as a solder resist layer, it is difficult to achieve both suppression of the visibility of scratches and high blackness. That is, if the surface of the photosensitive film has fine irregularities, the surface of the formed solder resist layer becomes whitish brown due to diffuse reflection of light, and the visibility of the marking ink placed thereon decreases. On the other hand, if the surface of the photosensitive film has few irregularities, the surface of the formed solder resist layer has a high blackness, but minute scratches on the surface of the solder resist layer are easily visible. For this reason, it has been difficult to provide a photosensitive film capable of forming a solder resist layer that has a high blackness that is excellent in the visibility of the marking ink, but has a low-gloss uneven surface shape and makes scratches difficult to see.
[0009] Therefore, an object of the present invention is to provide a photosensitive film laminate capable of forming a solder resist layer having a high blackness that provides excellent visibility of marking ink, a low gloss uneven surface shape, and in which scratches are difficult to see. Another object of the present invention is to provide a cured product formed using the photosensitive film laminate and a printed wiring board including the same. [Means for solving the problem]
[0010] The inventors of the present invention believe that the reason why the surface of the solder resist layer formed when the surface of the photosensitive film is made to have a low gloss with fine irregularities and the visibility of the marking ink decreases is because the fine irregularities cause the white light to be diffusely reflected from the solder resist surface, and as a result of repeating various experiments on the surface roughness and blackness of the solder resist layer surface, they have found that by adjusting the surface area per unit area (hereinafter referred to as [surface area / area]) and surface roughness of the photosensitive film surface, it is possible to achieve a high blackness while maintaining a low gloss of the surface of the solder resist layer.The present invention is based on such findings.
[0011] That is, the photosensitive film laminate according to the present invention is A photosensitive film laminate comprising a photosensitive film and a first film provided on one surface of the photosensitive film, the photosensitive film has a textured surface in contact with the first film; The textured surface of the cured photosensitive film meets the following parameters: (A)1.025<surface area / area<1.400 (B) 0.1μm<arithmetic mean surface roughness Ra<0.5μm The present invention is characterized in that:
[0012] In one embodiment of the present invention, the uneven surface of the cured photosensitive film preferably has a 60° gloss of 50 or less.
[0013] In an embodiment of the present invention, the uneven surface of the cured photosensitive film preferably has an L* value of 25 or less in the L*a*b* color space.
[0014] In a preferred embodiment of the present invention, the photosensitive resin composition forming the photosensitive film contains a carboxyl group-containing photosensitive resin, a photopolymerization initiator, and a colorant.
[0015] A cured product according to another aspect of the present invention is characterized in that it is formed using the above-mentioned photosensitive film laminate.
[0016] A printed wiring board according to another aspect of the present invention is characterized by comprising the above-mentioned cured product. Effect of the Invention
[0017] According to the present invention, it is possible to provide a photosensitive film capable of forming a solder resist layer having a high blackness that provides excellent visibility of marking ink, a surface with a low gloss uneven shape, and in which scratches are difficult to see. In the present invention, since scratches on the surface of the solder resist layer are difficult to see, it is possible to improve the production yield. Furthermore, according to the present invention, it is possible to provide a cured product formed using the photosensitive film laminate, and a printed wiring board including the same.
[0018] Problems, configurations and effects other than those described above will become apparent from the following description of the embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The photosensitive film laminate, the cured product, and the printed wiring board according to the present embodiment will be described below. The photosensitive film is a film-shaped photosensitive resin composition that is not laminated with other layers such as a first film or a second film. The photosensitive film laminate according to the present invention will be described below.
[0020] <Photosensitive film laminate> The photosensitive film laminate of the present invention includes a photosensitive film and a first film provided on one side of the photosensitive film, and is suitable for forming a solder resist layer. The photosensitive film laminate of the present invention may further include a second film provided on the other side of the photosensitive film. Each of the components of the photosensitive film laminate of the present invention will now be described.
[0021] [Photosensitive film] The photosensitive film according to the present invention is formed from a photosensitive resin composition and has an uneven surface in contact with the first film. The textured surface of the cured photosensitive film meets the following parameters: (A)1.025<surface area / area<1.400 (B) 0.1μm<arithmetic mean surface roughness Ra<0.5μm The present invention is characterized in that:
[0022] In the present invention, the above-mentioned "surface area / area" and "arithmetic mean surface roughness Ra" refer to values measured by a measuring device conforming to JIS B0601-1994. A specific measurement method will be described below. The "surface area / area" and "arithmetic mean surface roughness Ra" can be measured using a shape measuring laser microscope (for example, VK-X100 manufactured by Keyence Corporation). After starting the shape measuring laser microscope (VK-X100) main body (control unit) and the VK observation application (VK-H1VX manufactured by Keyence Corporation), the sample to be measured is placed on the xy stage. Rotate the lens revolver of the microscope unit (VK-X110 manufactured by Keyence Corporation) to select an objective lens with a magnification of 10 times, and roughly adjust the focus and brightness in the image observation mode of the VK observation application (VK-H1VX manufactured by Keyence Corporation). Operate the xy stage to adjust so that the approximate center of the sample surface is at the center of the screen. Change the 10x objective lens to a 50x magnification, and use the autofocus function in the image observation mode of the VK observation application (VK-H1VX) to focus on the surface of the sample. Select the easy mode in the shape measurement tab of the VK observation application (VK-H1VX), press the measurement start button, measure the surface shape of the sample, and obtain a surface image file. Start the VK analysis application (VK-H1XA, Keyence Corporation), display the obtained surface image file, and then perform tilt correction.
[0023] In the "surface area / area" measurement, the observation measurement range (area) for measuring the surface shape of the sample is 55965 μm 2 For example, an analysis application (VK-H1XA) can be used. Select [Volume / Area] from the measurement analysis menu on the display screen to display the [Volume / Area] window. This refers to the [Surface area / Area] value in the [Total area] measurement in the [Volume / Area] window.
[0024] In addition, for the measurement of the "arithmetic mean surface roughness Ra", a shape measuring laser microscope (VK-X100 manufactured by Keyence Corporation) was used to measure the arithmetic mean surface roughness Ra. After starting the shape measuring laser microscope (VK-X100) main body (control unit) and the VK observation application (VK-H1VX manufactured by Keyence Corporation), the sample (first film) to be measured was placed on the xy stage with the surface having the protruding part of the first film on top. The lens revolver of the microscope unit (VK-X110 manufactured by Keyence Corporation) was turned to select an objective lens with a magnification of 10x, and the focus and brightness were roughly adjusted in the image observation mode of the VK observation application (VK-H1VX manufactured by Keyence Corporation). The xy stage was operated to adjust so that the approximate center of the sample surface was at the center of the screen. The 10x objective lens was replaced with a 50x magnification, and the autofocus function of the image observation mode of the VK observation application (VK-H1VX) was used to focus on the surface of the sample. The simple mode of the shape measurement tab of the VK observation application (VK-H1VX) was selected, the measurement start button was pressed, the surface shape of the sample was measured, and a surface image file was obtained. The VK analysis application (VK-H1XA, manufactured by Keyence Corporation) was started, and the obtained surface image file was displayed, after which tilt correction was performed, and the display area was adjusted to 55,965 μm. 2 The Ra values of the range were measured.
[0025] In order to make the surface form of the photosensitive film after curing fall within the above-mentioned specific "surface area / area" and specific "arithmetic mean surface roughness Ra" ranges, known and commonly used methods can be applied. For example, from the viewpoint of ease of forming such a surface form, it is preferable to form the photosensitive film using a first film having a specific surface form as described below. That is, in the case of a photosensitive film laminate in which the first film is laminated on the photosensitive film of the present invention, it is preferable to form an uneven surface having the above-mentioned specific "surface area / area" and specific arithmetic mean surface roughness Ra on the surface of the photosensitive film after curing by imprinting the specific surface form of the first film on the surface of the photosensitive film. The parameters of the uneven surface of the photosensitive film after curing can be adjusted by the specific surface form of the first film, the composition of the photosensitive resin composition, etc. In addition, it is preferable that the photosensitive film is for forming a solder resist layer.
[0026] In the present invention, by using a photosensitive film having a "surface area / area" ratio calculated as above after curing of more than 1.025 and less than 1.4, it is possible to provide a photosensitive film capable of forming a solder resist layer having a high degree of blackness that provides excellent visibility of marking ink, while having a low-gloss uneven surface shape that makes scratches less visible. Furthermore, when a solder resist layer or the like is formed using a photosensitive film having such a specific surface morphology, it is possible to improve the yield in a visual inspection that checks for the presence or absence of surface scratches on the solder resist layer.
[0027] In the present invention, the "surface area / area" of the uneven surface of the cured photosensitive film is preferably 1.022 or more, more preferably 1.025 or more, and is preferably 1.400 or less, from the viewpoint of the balance between the surface whitening caused by light scattering on the uneven surface of the photosensitive film and the improvement of the yield in appearance inspection.
[0028] In the present invention, from the viewpoint of a balance between the blackness of the uneven surface of the cured photosensitive film and an improvement in yield in appearance inspection, the arithmetic mean surface roughness Ra of the uneven surface of the cured photosensitive film is more than 0.1 μm, preferably 0.15 μm or more, and more preferably 0.2 μm or more, and is less than 0.5 μm, preferably 0.45 μm or less, and more preferably 0.4 μm or less.
[0029] In the present invention, in order to form a low-gloss solder resist layer, the uneven surface of the cured photosensitive film preferably has a 60° gloss of 50 or less, more preferably 45 or less, and even more preferably 40 or less. Note that the 60° gloss in the present invention refers to a measured value on (the uneven surface of) a cured photosensitive film having a film thickness of 20 to 30 μm after curing, and the measuring equipment and measuring conditions are as described in the Examples.
[0030] In the present invention, in order to form a solder resist layer having a high blackness that provides excellent visibility of the marking ink, the L* value in the L*a*b* color space of the uneven surface of the cured photosensitive film is preferably 25 or less, more preferably 23 or less, and more preferably 20 or less. Note that the L* value in the present invention refers to the measured value of (the uneven surface of) the cured photosensitive film having a film thickness of 20 to 30 μm after curing, and the measuring equipment and measuring conditions are as described in the Examples.
[0031] The photosensitive film having an uneven surface with the above-mentioned "surface area / area" being more than 1.025 and less than 1.400, and the arithmetic mean surface roughness Ra being more than 1 μm and less than 0.5 μm, is patterned by exposure and development to become a cured film provided on a circuit board. The cured film is preferably a solder resist layer. Such a photosensitive film can be formed using a photosensitive resin composition, and the photosensitive resin composition can be any conventionally known solder resist ink or the like without any restrictions, but an example of a photosensitive resin composition that can be preferably used for the photosensitive film according to the present invention will be described below.
[0032] <Photosensitive resin composition> The photosensitive resin composition for forming the photosensitive film preferably contains a carboxyl group-containing photosensitive resin, a photopolymerization initiator, and a colorant. Each component of the photosensitive resin composition will be described in detail below.
[0033] [Carboxyl group-containing photosensitive resin] In the photosensitive resin composition, various conventionally known resins having a carboxyl group in the molecule can be used as the carboxyl group-containing photosensitive resin. By including a carboxyl group-containing resin in the photosensitive resin composition, it is possible to impart alkaline developability to the photosensitive resin composition. In particular, a carboxyl group-containing photosensitive resin having an ethylenically unsaturated double bond in the molecule is preferred from the viewpoint of photocurability and development resistance. The ethylenically unsaturated double bond is preferably derived from acrylic acid or methacrylic acid or a derivative thereof. In addition, a carboxyl group-containing resin having no ethylenically unsaturated double bond may be used in combination with the carboxyl group-containing photosensitive resin. Specific examples of the carboxyl group-containing photosensitive resin include the following compounds (which may be either oligomers or polymers): The carboxyl group-containing photosensitive resin may be used alone or in combination of two or more kinds.
[0034] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.
[0035] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0036] (3) Carboxylic acid-containing photosensitive urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds and diol compounds.
[0037] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).
[0038] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).
[0039] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl groups present in the side chains.
[0040] (7) A carboxyl group-containing photosensitive resin obtained by reacting a multifunctional epoxy resin with the hydroxyl groups of a bifunctional (solid) epoxy resin further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0041] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.
[0042] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.
[0043] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0044] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0045] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).
[0046] In this specification, (meth)acrylate is a term that collectively refers to acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.
[0047] The acid value of the carboxyl group-containing photosensitive resin is preferably 40 to 150 mgKOH / g. By making the acid value of the carboxyl group-containing photosensitive resin 40 mgKOH / g or more, alkaline development becomes good. Also, by making the acid value 150 mgKOH / g or less, it becomes easy to draw a good resist pattern. More preferably, it is 50 to 130 mgKOH / g.
[0048] The weight-average molecular weight of the carboxyl group-containing photosensitive resin varies depending on the resin skeleton, but is generally preferably 2,000 to 150,000. By making the weight-average molecular weight 2,000 or more, it is possible to improve tack-free performance and resolution. In addition, by making the weight-average molecular weight 150,000 or less, it is possible to improve developability and storage stability. It is more preferably 5,000 to 100,000.
[0049] The amount of the carboxyl group-containing photosensitive resin in the photosensitive resin composition is preferably 20% by mass or more and 60% by mass or less, calculated as solid content. By making it 20% by mass or more, the strength of the cured coating film can be improved. Also, by making it 60% by mass or less, the viscosity becomes appropriate and the printability is improved. More preferably, it is 30% by mass or more and 50% by mass or less.
[0050] [Photopolymerization initiator] The photopolymerization initiator contained in the photosensitive resin composition is for reacting the above-mentioned carboxyl group-containing photosensitive resin and the photopolymerizable monomer described below by exposure to light. Any known photopolymerization initiator can be used. The photopolymerization initiator may be used alone or in combination of two or more.
[0051] Specific examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentane. Bisacylphosphine oxides such as 2,6-dimethoxybenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloyl monoacylphosphine oxides such as phenylphosphinic acid isopropyl ester and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; ethyl phenyl(2,4,6-trimethylbenzoyl)phosphinate, 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether, and other benzoins; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, and other benzophenones;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1-butanone acetophenones such as acetophenone, N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, Anthraquinones such as 2-aminoanthraquinone; ketals such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyl oxime esters such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium, and other titanocenes; phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, tetramethylthiuram disulfide, and the like.
[0052] Commercially available α-aminoacetophenone photopolymerization initiators include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins. Commercially available acylphosphine oxide photopolymerization initiators include Omnirad 819 manufactured by IGM Resins. Commercially available oxime ester photopolymerization initiators include Irgacure OXE01 and OXE02 manufactured by BASF Japan Ltd., N-1919 manufactured by ADEKA Corporation, Adeka Arcles NCI-831 and NCI-831E, and TR-PBG-304 manufactured by Changzhou Strong Electronic New Materials Co., Ltd.
[0053] The amount of the photopolymerization initiator is, in terms of solid content, preferably 0.1 to 20 parts by mass, more preferably 0.5 to 18 parts by mass, and even more preferably 1 to 15 parts by mass, relative to 100 parts by mass of the carboxyl group-containing photosensitive resin. When the amount is 0.01 part by mass or more, the photocurability of the resin composition is good, and the film properties such as chemical resistance are also good, while when the amount is 20 parts by mass or less, the light absorption at the surface of the resist film (cured film) is good, and the deep curability is less likely to decrease.
[0054] A photoinitiator assistant or a sensitizer may be used in combination with the above-mentioned photopolymerization initiator. Examples of the photoinitiator assistant or sensitizer include benzoin compounds, anthraquinone compounds, thioxanthone compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds. In particular, it is preferable to use thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2-isopropylthioxanthone, and 4-isopropylthioxanthone. By including a thioxanthone compound, it is possible to improve the deep curing property. Although these compounds may be used as photopolymerization initiators, it is preferable to use them in combination with a photopolymerization initiator. In addition, the photoinitiator assistant or sensitizer may be used alone or in combination of two or more kinds.
[0055] In addition, since these photopolymerization initiators, photoinitiator assistants, and sensitizers absorb specific wavelengths, in some cases the sensitivity is reduced and they may function as ultraviolet absorbers. However, they are not used only for the purpose of improving the sensitivity of the resin composition. If necessary, they can absorb light of a specific wavelength to increase the photoreactivity of the surface, change the line shape and opening of the resist pattern to a vertical, tapered, or reverse tapered shape, and improve the accuracy of the line width and opening diameter.
[0056] [Coloring agent] The photosensitive resin composition preferably contains a colorant to adjust the 60° gloss of the uneven surface of the photosensitive film and the L* value in the L*a*b* color space to a desired range. Known colorants such as red, blue, green, yellow, and black can be used as the colorant, and any of pigments, dyes, and coloring matters can be used, but from the viewpoint of reducing the environmental load and having little effect on the human body, a colorant that does not contain halogen is preferable.
[0057] Red colorants include monoazos, disazos, azo lakes, benzimidazolone, perylene, diketopyrrolopyrrole, condensed azos, anthraquinones, and quinacridones. Specific examples of red colorants include those having the following Color Index (CI; published by The Society of Dyers and Colourists) numbers:
[0095] Examples of monoazo red colorants include Pigment Red 1, 2, 3, 4, 5, 6, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 112, 114, 146, 147, 151, 170, 184, 187, 188, 193, 210, 245, 253, 258, 266, 267, 268, and 269. Examples of disazo red colorants include Pigment Red 37, 38, and 41. Examples of monoazo lake-based red colorants include Pigment Red 48:1, 48:2, 48:3, 48:4, 49:1, 49:2, 50:1, 52:1, 52:2, 53:1, 53:2, 57:1, 58:4, 63:1, 63:2, 64:1, and 68. Examples of benzimidazolone-based red colorants include Pigment Red 171, 175, 176, 185, and 208. Examples of perylene-based red colorants include Solvent Red 135, 179, Pigment Red 123, 149, 166, 178, 179, 190, 194, and 224. Examples of diketopyrrolopyrrole red colorants include Pigment Red 254, 255, 264, 270, and 272. Examples of condensed azo red colorants include Pigment Red 220, 144, 166, 214, 220, 221, and 242. Examples of anthraquinone red colorants include Pigment Red 168, 177, and 216, Solvent Red 52, 149, 150, and 207. Examples of quinacridone red colorants include Pigment Red 122, 202, 206, 207, and 209.
[0058] Blue colorants include phthalocyanine and anthraquinone types, and pigment types include compounds classified as pigments, such as Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, and 60. Dye types include Solvent Blue 35, 63, 67, 68, 70, 83, 87, 94, 97, 122, and 136. In addition to the above, metal-substituted or unsubstituted phthalocyanine compounds can also be used.
[0059] Examples of yellow colorants include monoazo, disazo, condensed azo, benzimidazolone, isoindolinone, and anthraquinone. For example, anthraquinone yellow colorants include Solvent Yellow 163, Pigment Yellow 24, 108, 193, 147, 199, and 202. Examples of isoindolinone yellow colorants include Pigment Yellow 110, 109, 139, 179, and 185. Examples of condensed azo yellow colorants include Pigment Yellow 93, 94, 95, 128, 155, 166, and 180. Examples of benzimidazolone yellow colorants include Pigment Yellow 120, 151, 154, 156, 175, and 181. Examples of monoazo yellow colorants include Pigment Yellow 1, 2, 3, 4, 5, 6, 9, 10, 12, 61, 62, 62:1, 65, 73, 74, 75, 97, 100, 104, 105, 111, 116, 167, 168, 169, 182, and 183. Examples of disazo yellow colorants include Pigment Yellow 12, 13, 14, 16, 17, 55, 63, 81, 83, 87, 126, 127, 152, 170, 172, 174, 176, 188, and 198.
[0060] Examples of black colorants include carbon black, Pigment Black 1, 6, 7, 8, 9, 10, 11, 12, 13, 18, 20, 25, 26, 28, 29, 30, 31, and 32.
[0061] Other colorants such as purple, orange, brown, and white may be added. Specific examples include Pigment Violet 19, 23, 29, 32, 36, 38, and 42, Solvent Violet 13 and 36, CI Pigment Orange 1, 5, 13, 14, 16, 17, 24, 34, 36, 38, 40, 43, 46, 49, 51, 61, 63, 64, 71, and 73, Pigment Brown 23 and 25, and titanium oxide.
[0062] The amount of the colorant in the photosensitive resin composition is not particularly limited, but is preferably 0.1 to 5% by mass based on the total amount of the photosensitive resin composition.
[0063] [Photopolymerizable monomer] The photosensitive resin composition of the present invention can contain a photopolymerizable monomer. The photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. Examples of such photopolymerizable monomers include commonly known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, and epoxy (meth)acrylates. Specifically, alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; mono- or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-methylolacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, and trishydroxyethyl isocyanurate. Polyhydric alcohols such as polyhydric alcohols or their alkylene oxide adducts or ε-caprolactone adducts; phenols such as phenoxy acrylate and bisphenol A diacrylate or their alkylene oxide adducts; glycidyl ether acrylates such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate; and acrylates obtained by directly acrylate or urethane acrylate of polyols such as polyether polyols, polycarbonate diols, hydroxyl group-terminated polybutadiene, and polyester polyols, as well as melamine acrylates and at least one of the methacrylates corresponding to the acrylates, can be appropriately selected and used. Such photopolymerizable monomers can also be used as reactive diluents.The photopolymerizable monomers may be used alone or in combination of two or more.
[0064] [Thermosetting component] The photosensitive resin composition of the present invention may contain a thermosetting component. By containing a thermosetting component in the photosensitive resin composition, the heat resistance of the cured coating can be improved. As the thermosetting component, for example, known thermosetting components such as amino resins such as melamine resins, benzoguanamine resins, melamine derivatives, and benzoguanamine derivatives, isocyanate compounds, blocked isocyanate compounds, cyclocarbonate compounds, epoxy compounds, oxetane compounds, episulfide resins, bismaleimides, and carbodiimide resins can be used. Particularly preferred is a thermosetting component having a plurality of cyclic ether groups or cyclic thioether groups (hereinafter abbreviated as cyclic (thio)ether groups) in the molecule. The thermosetting component can be used alone or in combination of two or more types.
[0065] The thermosetting component having multiple cyclic (thio)ether groups in the molecule is a compound having multiple 3-, 4-, or 5-membered cyclic (thio)ether groups in the molecule, and examples thereof include compounds having multiple epoxy groups in the molecule, i.e., polyfunctional epoxy compounds, compounds having multiple oxetanyl groups in the molecule, i.e., polyfunctional oxetane compounds, and compounds having multiple thioether groups in the molecule, i.e., episulfide resins.
[0066] Examples of such epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, biphenyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, triphenylmethane type epoxy resins, and the like.
[0067] Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Corporation; YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by Nippon Steel Chemical & Material Co., Ltd.; EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation; and RE-306 manufactured by Nippon Kayaku Co., Ltd.
[0068] Examples of the polyfunctional oxetane compound include bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, and (3-ethyl-3-oxetanyl)methyl acrylate. Examples of the oxetanes include polyfunctional oxetanes such as acrylate, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and their oligomers or copolymers, as well as ethers of oxetane alcohols and novolac resins, poly(p-hydroxystyrene), cardo-type bisphenols, calixarenes, calixresorcinarenes, or resins having hydroxyl groups such as silsesquioxane. Other examples include copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates.
[0069] Examples of compounds having multiple cyclic thioether groups in the molecule include bisphenol A episulfide resins, etc. Using a similar synthesis method, episulfide resins in which the oxygen atoms of the epoxy groups of novolac epoxy resins are replaced with sulfur atoms can also be used.
[0070] Examples of amino resins such as melamine derivatives and benzoguanamine derivatives include methylolmelamine compounds, methylolbenzoguanamine compounds, methylolglycoluril compounds, and methylolurea compounds.
[0071] As the isocyanate compound, a polyisocyanate compound can be blended. Examples of the polyisocyanate compound include aromatic polyisocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate, o-xylylene diisocyanate, m-xylylene diisocyanate, and 2,4-tolylene dimer; tetramethylene diisocyanate; Examples of the isocyanate include aliphatic polyisocyanates such as isocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), and isophorone diisocyanate; alicyclic polyisocyanates such as bicycloheptane triisocyanate; and adducts, biurets, and isocyanurates of the above-mentioned isocyanate compounds.
[0072] The blocked isocyanate compound may be an addition reaction product of an isocyanate compound and an isocyanate blocking agent. Examples of isocyanate compounds that can react with an isocyanate blocking agent include the polyisocyanate compounds described above. Examples of isocyanate blocking agents include phenol-based blocking agents, lactam-based blocking agents, active methylene-based blocking agents, alcohol-based blocking agents, oxime-based blocking agents, mercaptan-based blocking agents, acid amide-based blocking agents, imide-based blocking agents, amine-based blocking agents, imidazole-based blocking agents, and imine-based blocking agents.
[0073] The amount of the thermosetting component is preferably 0.5 to 2.5 mol, more preferably 0.8 to 2.0 mol, of functional groups of the thermosetting component that reacts with 1 mol of carboxyl groups contained in the carboxyl group-containing photosensitive resin, calculated as solid content.
[0074] [Thermosetting catalyst] In addition to the above-mentioned thermosetting component, the photosensitive resin composition can also contain a thermosetting catalyst. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. In addition, examples of commercially available products include 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, and 2P4MHZ (all trade names of imidazole-based compounds) manufactured by Shikoku Chemical Industry Co., Ltd., and U-CAT 3513N (a trade name of a dimethylamine-based compound), DBU, DBN, and U-CAT SA 102 (all bicyclic amidine compounds and their salts) manufactured by San-Apro Co., Ltd. In particular, the present invention is not limited to these, and any material that promotes the reaction of at least one of an epoxy resin or oxetane compound with a carboxyl group and at least one of an epoxy group and an oxetanyl group with a carboxyl group may be used alone or in combination of two or more types.
[0075] [Filler] In the present invention, in order to improve the physical strength of the cured coating obtained by using the photosensitive film laminate and to adjust the uneven surface of the cured photosensitive film, a filler can be blended into the photosensitive resin composition as necessary. As the filler, known inorganic or organic fillers can be used, and barium sulfate, spherical silica, hydrotalcite, and talc are particularly preferably used. In addition, metal oxides and metal hydroxides such as aluminum hydroxide can be used as extender pigment fillers to obtain flame retardancy.
[0076] The amount of the filler to be blended is not particularly limited, but from the viewpoints of viscosity, coatability, moldability, etc., it is preferably 25 to 80 mass % in terms of solid content based on the total amount of the photosensitive resin composition.
[0077] The above-mentioned filler may be surface-treated to enhance dispersibility in the photosensitive resin composition. By using a surface-treated filler, aggregation can be suppressed. The surface treatment method is not particularly limited, and a known and commonly used method may be used, but it is preferable to treat the surface of the inorganic filler with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group.
[0078] As the coupling agent, silane-based, titanate-based, aluminate-based, zircoaluminate-based, and other coupling agents can be used. Among them, silane-based coupling agents are preferred. Examples of such silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane, which can be used alone or in combination. It is preferable that these silane-based coupling agents are immobilized on the surface of the filler in advance by adsorption or reaction. Here, the amount of the coupling agent to be treated with respect to 100 parts by mass of the spherical silica is preferably 0.5 to 10 parts by mass.
[0079] [Organic solvents] The photosensitive resin composition may contain an organic solvent from the viewpoint of ease of preparation of the composition and coating properties. Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. These organic solvents can be used alone or in combination of two or more.
[0080] [Other added ingredients] The photosensitive resin composition may further contain, as necessary, components such as elastomers, mercapto compounds, urethanization catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper inhibitors, antioxidants, rust inhibitors, thickeners such as organic bentonite and montmorillonite, at least one of silicone-based, fluorine-based, and polymer-based defoamers and leveling agents, and flame retardants such as phosphorus compounds such as phosphinates, phosphate ester derivatives, and phosphazene compounds. These may be known in the field of electronic materials.
[0081] [First film] The first film supports the above-mentioned photosensitive film (i.e., a resin layer made of a photosensitive resin composition) and has a role of imparting a predetermined surface form to the surface of the photosensitive film that contacts the first film during exposure and development of the photosensitive film, and refers to a film that is at least adhered to the photosensitive film when the photosensitive film side of the photosensitive film laminate is laminated by heating or the like so as to contact a base material such as a substrate and integrally molded. The first film may be peeled off from the photosensitive film laminate in a process after lamination. In particular, in the present invention, it is preferable that the first film is peeled off from the photosensitive film laminate in a process after exposure. In addition, in the present invention, it is preferable to use a first film such that 1.025<"surface area / area"<1.400. It is more preferable to use a first film such that 0.1 μm<"arithmetic mean surface roughness Ra"<0.5 μm on the surface side that contacts the photosensitive film. Use of a first film having such a surface morphology makes it easier to form a photosensitive film having a surface ratio of 1.025<"surface area / area"<1.400, and further makes it easier to form a photosensitive film having a surface ratio of 0.1 μm<"arithmetic mean surface roughness Ra"<0.5 μm. In other words, the predetermined surface morphology of the first film is imprinted on the surface of the photosensitive film, which is effective in making it easier to form a photosensitive film that can improve the blackness of the cured coating that is formed later and can improve the yield in appearance inspection.
[0082] The first film can be any film having the above-mentioned surface configuration, and can be suitably used, for example, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyimide films, polyamideimide films, polypropylene films, polystyrene films, and other films made of thermoplastic resins, among which polyester films can be suitably used from the viewpoints of heat resistance, mechanical strength, ease of handling, etc. The first film may be a single layer, or may be a laminate of two or more layers.
[0083] In addition, it is preferable to use the above-mentioned thermoplastic resin film which has been uniaxially or biaxially stretched in order to improve its strength.
[0084] When a thermoplastic resin film is used as the first film, the surface can be formed into the above-mentioned predetermined shape by adding a filler to the resin when forming the film (kneading treatment), matte coating (coating treatment), blasting the film surface such as sandblasting, or hairline processing or chemical etching. For example, when a filler is added to the resin, the "surface area / area" and "arithmetic mean surface roughness Ra" can be controlled by adjusting the particle size and amount of the filler. In addition, when the surface of the first film is coated, the "surface area / area" and "arithmetic mean surface roughness Ra" can be controlled by adjusting the type and amount of the coating agent. In addition, when a blasting treatment is performed, the "surface area / area" and "arithmetic mean surface roughness Ra" can be controlled by adjusting the processing conditions such as the blasting material and blasting pressure.
[0085] The surface of the first film on which the photosensitive film is to be provided may be subjected to a release treatment. For example, a release agent such as wax, silicone wax, alkyd resin, urethane resin, melamine resin, silicone resin, etc. may be dissolved or dispersed in a suitable solvent to prepare a coating liquid, which is then applied to the surface of the first film by a known method such as a coating method such as roll coating or spray coating, gravure printing, or screen printing, and then dried, to perform the release treatment.
[0086] The thickness of the first film is not particularly limited, but is appropriately selected from the range of about 10 to 150 μm depending on the application.
[0087] [Second film] The photosensitive film laminate of the present invention may have a second film on the other side of the photosensitive film (the side opposite to the first film) for the purpose of preventing adhesion of dust and the like to the surface of the above-mentioned photosensitive film and improving handling. The second film in the present invention refers to a film that is peeled off from the photosensitive film laminate before lamination when the photosensitive film side of the photosensitive film laminate is laminated by heating or the like so as to be in contact with a base material such as a substrate and integrally molded.
[0088] The second film may be, for example, a polyester film, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, or surface-treated paper, but it is preferable to select a material such that the adhesive strength between the second film and the photosensitive film is smaller than the adhesive strength between the first film and the photosensitive film. In addition, in order to make it easier to peel off the second film when using the photosensitive film laminate, the surface of the second film that comes into contact with the photosensitive film may be subjected to the above-mentioned release treatment.
[0089] The thickness of the second film is not particularly limited, but is appropriately selected from the range of about 10 to 150 μm depending on the application.
[0090] [Method of manufacturing the cured product and the printed wiring board] A cured product is formed using the photosensitive film or photosensitive film laminate of the present invention. A method for forming such a cured product and a method for manufacturing a printed wiring board provided with the above-mentioned cured product (cured coating) on a substrate on which a circuit pattern is formed will be described. As an example, a method for manufacturing a printed wiring board using a photosensitive film laminate provided with a second film will be described. First, i) the second film is peeled off from the above-mentioned photosensitive film laminate to expose the photosensitive film, ii) the photosensitive film of the photosensitive film laminate is attached to the substrate on which the circuit pattern is formed, iii) exposure is performed from the first film of the photosensitive film laminate, iv) the first film is peeled off from the photosensitive film laminate and development is performed to form a patterned photosensitive film on the substrate, and v) the patterned photosensitive film is cured by light irradiation or heat to form a cured coating, thereby forming a printed wiring board. It goes without saying that when a photosensitive film laminate without a second film is used, the peeling step (i step) of the second film is unnecessary. Each step will be described below.
[0091] First, the second film is peeled off from the photosensitive film laminate to expose the photosensitive film, and the photosensitive film of the photosensitive film laminate is laminated on a substrate on which a circuit pattern is formed. Examples of substrates on which a circuit pattern is formed include printed wiring boards and flexible printed wiring boards on which circuits are formed in advance, as well as copper-clad laminates of all grades (such as FR-4) made of materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven cloth epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, copper-clad laminates for high-frequency circuits made of fluororesin, polyethylene, polyphenylene ether, polyphenylene oxide, cyanate ester, etc., as well as polyimide films, PET films, glass substrates, ceramic substrates, wafer plates, etc.
[0092] In order to laminate the photosensitive film of the photosensitive film laminate on the circuit board, it is preferable to laminate the film under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, even if the circuit board surface has irregularities, the photosensitive resin composition layer adheres to the circuit board, so that no air bubbles are mixed in, and the filling of the recesses on the board surface is improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.
[0093] Next, exposure (irradiation with active energy rays) is performed from above the first film of the photosensitive film laminate. This process hardens only the exposed photosensitive film. The exposure process is not particularly limited, and for example, it may be selectively exposed to active energy rays through a photomask having a desired pattern formed thereon by a contact (or non-contact) method, or the desired pattern may be exposed to active energy rays by a direct imaging device.
[0094] The exposure machine used for the active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm. In addition, a direct imaging machine (for example, a laser direct imaging machine that draws an image directly with a laser based on CAD data from a computer) may also be used. The laser light source of the direct imaging machine may be either a gas laser or a solid laser, so long as it uses a laser beam with a maximum wavelength in the range of 350 to 410 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 20 to 800 mJ / cm. 2 , preferably 20 to 600 mJ / cm 2 The range may be:
[0095] After the exposure, the first film is peeled off from the photosensitive film laminate and development is performed to form a patterned photosensitive film on the substrate. When the first film is peeled off, the surface of the exposed and cured photosensitive film is imprinted with the shape of the first film surface.
[0096] The developing step is not particularly limited, and may be a dipping method, a shower method, a spray method, a brush method, etc. As the developing solution, an alkaline aqueous solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, etc. may be used.
[0097] Next, the patterned photosensitive film is cured by irradiation with active energy rays (light) or heat to form a cured product (cured coating). This process is called main curing or additional curing, and promotes polymerization of unreacted monomers in the photosensitive film, and furthermore, the amount of remaining carboxyl groups can be reduced by thermally curing the carboxyl group-containing photosensitive resin and the epoxy resin. The active energy ray irradiation can be performed in the same manner as the above-mentioned exposure, but it is preferable to perform it under conditions of stronger irradiation energy than that during exposure. For example, 500 to 3000 mJ / cm 2 The heat curing can be carried out under heating conditions of 100 to 200°C for about 20 to 90 minutes. It is preferable that the main curing is carried out by performing heat curing after photocuring. By carrying out photocuring first, the flow of the resin is suppressed even during heat curing, and the shaped surface may be maintained.
[0098] In the manner described above, it is possible to impart a suitable unevenness to the surface of the cured product, which results in a high degree of blackness while improving the yield in visual inspection due to the suitable unevenness of the surface of the cured product. EXAMPLES
[0099] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0100] <Preparation of Photosensitive Resin Composition> The components shown in Table 1 below were mixed in the amounts (solid content) shown in the table, pre-mixed with a mixer, and then kneaded with a three-roll mill to prepare the following photosensitive resin compositions A and B. Details of each component in Table 1 are as follows. Carboxyl-containing photosensitive resin: UE9210 manufactured by DIC Corporation Epoxy resin: EPICLON N-770 manufactured by DIC Corporation Colorant A: A black appearance pigment made by mixing 35% by mass of a blue colorant (CI Pigment Blue 15:3), 15% by mass of a yellow colorant (CI Pigment Yellow 147), and 50% by mass of a red colorant (BASF Japan Ltd., Paliogen Red K3580). Colorant B: MA100 (carbon black) manufactured by Mitsubishi Chemical Corporation Photopolymerization initiator: Irgacure OXE02 (ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(0-acetyloxime)) manufactured by BASF Japan Ltd. Inorganic filler: B-30 (barium sulfate) manufactured by Sakai Chemical Industry Co., Ltd.
[0101] [Table 1]
[0102] [Example 1] <Preparation of Photosensitive Film Laminate> Iso-butylated melamine resin (Amidair L-125-60, solids 60%, manufactured by DIC Corporation) and acrylic resin for melamine baking (Acrydic A-405, solids 50%, manufactured by DIC Corporation) were mixed in a ratio of 25:75 (solids equivalent) by mass and pre-mixed with a mixer to obtain an acrylic melamine resin. The obtained acrylic melamine resin was then diluted with methyl ethyl ketone to prepare a resin solution with a solids concentration of 35% by mass. Methyl ethyl ketone was further added to this resin solution to obtain an appropriate solids concentration depending on the thickness of the coating film, and then it was mixed with a silicone resin (Simac US-270, manufactured by Toa Gosei Co., Ltd.) and a resin with a maximum particle size of 2 μm. A filler (SO-C2, spherical silica, manufactured by Admatechs Co., Ltd.) adjusted to the desired thickness was added so that the blending ratio of the acrylic melamine resin, silicone resin, and filler was 59.7:0.3:20 by mass, and the mixture was thoroughly stirred at room temperature to obtain a uniform coating liquid. The obtained coating liquid was applied to a polyethylene terephthalate film (E5041, manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm, and dried at 130° C. for 20 seconds to produce a first film 1 (uneven PET1) including an intermediate layer. The value of “area / surface area” of the coated surface (uneven surface) of the obtained first film 1 was 1.041, and the arithmetic average surface roughness Ra was 0.246 nm.
[0103] A shape measuring laser microscope (VK-X100, manufactured by Keyence Corporation) was used to measure the arithmetic mean surface roughness Ra. After starting the shape measuring laser microscope (VK-X100) main body (control unit) and the VK observation application (VK-H1VX, manufactured by Keyence Corporation), the sample (first film) to be measured was placed on the xy stage with the surface having the protruding part of the first film facing up. The lens revolver of the microscope unit (VK-X110, manufactured by Keyence Corporation) was turned to select a 10x objective lens, and the focus and brightness were roughly adjusted in the image observation mode of the VK observation application (VK-H1VX). The xy stage was operated to adjust so that the approximate center of the sample surface was at the center of the screen. The 10x objective lens was replaced with a 50x magnification, and the focus was adjusted to the surface of the sample using the autofocus function of the image observation mode of the VK observation application (VK-H1VX). Select the simple mode of the shape measurement tab of the VK observation application (VK-H1VX), press the measurement start button, measure the surface shape of the sample, and obtain a surface image file. Start the VK analysis application (VK-H1XA manufactured by Keyence Corporation) and display the obtained surface image file, then perform tilt correction and adjust the display area to 55965 μm 2 The Ra values of the range were measured.
[0104] In the "surface area / area" measurement, the observation measurement range (area) in measuring the surface shape of the sample is 55965 μm 2 An analysis application (Keyence Corporation VK-H1XA) was used. Select [Volume / Area] from the measurement analysis menu on the display screen to display the [Volume / Area] window, and set the display area to 55965 μm for the [Full Area] measurement in the [Volume / Area] window. 2 The values of [volume·area] were measured.
[0105] Next, the photosensitive resin composition A obtained as described above was applied to the uneven surface of the first film 1 described above and dried at a temperature of 80°C for 15 minutes to form a photosensitive film with a thickness of 30 μm, thereby obtaining a photosensitive film laminate comprising the photosensitive film and the first film.
[0106] <Preparation of test substrate> The surface of a Cu solid substrate (150 mm x 95 mm x 0.89 mmt) was chemically polished using CZ8101 manufactured by MEC Co., Ltd. Then, the surface of the photosensitive film of the photosensitive film laminate obtained by the above method was laminated on the chemically polished surface of the Cu solid substrate using a vacuum laminator CVP-300 (manufactured by Nikko Materials Co., Ltd.) to obtain a structure. This structure was subjected to pattern exposure according to the evaluation items so that the number of hardening steps was 15 steps using a Stouffer 41-step step tablet using a DXP-3580 (manufactured by Oak Manufacturing Co., Ltd., ultra-high pressure mercury lamp DI exposure machine). 10 minutes after the start of exposure, the first film was peeled off, and development was performed with a 1 mass % sodium carbonate aqueous solution at 30 ° C for a development time 2 to 3 times the break point (shortest development time). The substrate was then exposed to 1000 mJ using a UV conveyor (metal halide lamp, manufactured by Oak Manufacturing Co., Ltd.) and cured in a heat circulation box furnace at 150°C for 60 minutes to obtain a test substrate 1 having a cured product (solder resist layer) of the photosensitive film on the substrate. The film thickness of the cured product (solder resist layer) was reduced by 20% from the film thickness (30 μm) of the photosensitive film after drying.
[0107] [Example 2] Test substrate 2 was produced in the same manner as in Example 1, except that photosensitive resin composition B was used instead of photosensitive resin composition A in Example 1.
[0108] [Example 3] A test substrate 3 was prepared in the same manner as in Example 1, except that a first film 2 (textured PET 2) was used in which the blending ratio of acrylic melamine resin, silicone resin, and filler in Example 1 was changed to 59.7:0.3:15 by mass.
[0109] [Comparative Example 1] A test substrate 4 was prepared in the same manner as in Example 1, except that a first film 3 (textured PET 3) was used in which the blending ratio of acrylic melamine resin, silicone resin, and filler in Example 1 was changed to 59.7:0.3:108 by mass.
[0110] [Comparative Example 2] Test substrate 5 was produced in the same manner as in Comparative Example 1, except that photosensitive resin composition B was used instead of photosensitive resin composition A in Comparative Example 1.
[0111] [Comparative Example 3] A test substrate 6 was prepared in the same manner as in Example 1, except that the first film 1 in Example 1 was changed to a first film 4 (PET4, manufactured by Nisshin Chemical Industry Co., Ltd., T100) having a [surface area / area] value of 1.011 and an arithmetic mean surface roughness Ra of 0.040 μm.
[0112] <Evaluation items> Next, the evaluation items and evaluation procedures for each of the examples and comparative examples are as follows.
[0113] <Measurement of surface parameters> The arithmetic mean surface roughness Ra and "surface area / area" were measured in the same manner as above for the surface of the solder resist layer of each of the test substrates prepared as described above in Examples 1 to 3 and Comparative Examples 1 to 3. The evaluation results are shown in Table 2 below.
[0114] <Evaluation of scratch visibility> A pencil lead having a hardness of 2H was pressed against the surface of the cured coating in the exposed area of each test substrate of Examples 1 to 3 and Comparative Examples 1 to 3 prepared as described above at an angle of 45° with a load of 4.9 N, and moved at a speed of 1 mm per second, and the visibility of scratches on the surface of the cured coating was visually evaluated according to the following criteria. The evaluation results are shown in Table 3 below. [Evaluation Criteria] ◯: No scratches were observed on the surface of the cured coating in the exposed area. ×: Scratches were observed on the surface of the cured coating in the exposed area.
[0115] <Evaluation of Blackness> After curing, the L value of the test substrate was measured using a color difference meter (CM-2600d, manufactured by Konica Minolta, Inc.) in SCE mode including specular reflection light, and the blackness was evaluated according to the following criteria. The evaluation results are shown in Table 3 below. [Evaluation Criteria] ◯: The L* value in the L*a*b* color space was 25 or less. ×: The L* value in the L*a*b* color space was more than 25.
[0116] <Gloss evaluation> A digital variable angle gloss meter (BYK-micro-TRI-gloss) was used to measure the gloss. After calibration with a standard plate, the gloss of the Gs (60°) on the uneven surface of the photosensitive film was measured and evaluated according to the following criteria. The evaluation results are shown in Table 3 below. [Evaluation Criteria] ◯: 60° gloss level was 50 or less. ×: The 60° gloss was more than 50.
[0117] Comparing Examples 1 to 3 with Comparative Examples 1 and 2, when the [surface area / area] of the solder resist layer is 1,400 or more, the inconspicuousness of scratches is rated as ◯, but the blackness is rated as ×, indicating that the visibility of the marking ink is reduced.
[0118] Comparing Examples 1 to 3 with Comparative Example 3, when the [surface area / area] of the solder resist layer is 1.025 or less, the blackness is rated as ◯, but the inconspicuousness of scratches is rated as ×, indicating that scratches are easily noticeable.
[0119] Although the embodiment of the present invention has been specifically described above, the present invention is not limited to this embodiment, and various modifications are possible without departing from the spirit and scope of the present invention.
[0120] [Table 2]
[0121]
Table 3
Claims
1. A photosensitive film laminate comprising a photosensitive film and a first film provided on one surface of the photosensitive film, the photosensitive film has a textured surface in contact with the first film; The textured surface of the cured photosensitive film has the following parameters: (A) 1.025<surface area / area<1.400 (B) 0.1 μm<arithmetic mean surface roughness Ra<0.5 μm A photosensitive film laminate, characterized in that:
2. 2. The photosensitive film laminate according to claim 1, wherein the uneven surface of the cured photosensitive film has a 60° gloss of 50 or less.
3. 3. The photosensitive film laminate according to claim 1, wherein the uneven surface of the cured photosensitive film has an L* value of 25 or less in the L*a*b* color space.
4. The photosensitive film laminate according to any one of claims 1 to 3, wherein the photosensitive resin composition forming the photosensitive film comprises a carboxyl group-containing photosensitive resin, a photopolymerization initiator, and a colorant.
5. A cured product formed using the photosensitive film laminate according to any one of claims 1 to 4.
6. A printed wiring board comprising the cured product according to claim 5.
Citation Information
Patent Citations
Energy beam curable resin composition
JP2002097239A
Photosensitive resin composition, dry film, cured product, and printed wiring board
JP2015206992A