Ultraviolet transmission suppression material containing lignocellulose nanofiber
The use of lignocellulose nanofibers with a filler in UV transmission suppressing materials addresses toxicity and environmental concerns, providing effective UV suppression and maintaining mechanical integrity in resin compositions.
Patent Information
- Application Number
- JP2023079877
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing ultraviolet transmission suppressing materials, such as those containing polyolefin resins with talc, hindered amine stabilizers, and ultraviolet absorbers, may be toxic and have a significant environmental impact, while materials using nanocellulose fibers do not effectively suppress UV transmission.
A UV transmission suppressing material is developed using lignocellulose nanofibers (LCNF) with a filler, where the mass ratio of filler to LCNF is between 0.3/1 to 12/1, and the fibers are treated with fatty acids to enhance dispersion and bonding, resulting in a non-toxic and environmentally friendly composition.
The material effectively suppresses UV transmission, maintains mechanical properties, and reduces environmental impact by using lignocellulose nanofibers with a filler, ensuring uniform dispersion and integration with resin materials.
Smart Images

Figure 2024164419000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an ultraviolet ray transmission suppression material containing lignocellulose nanofibers. [Background technology]
[0002] In recent years, cellulose has been used as a renewable resource. Nanocellulose fibers obtained by pulverizing cellulose have been blended with resins and the like for the purpose of improving mechanical strength, etc. Examples of nanocellulose fibers include cellulose nanofibers (CNF) with long fiber length, and cellulose nanocrystals (CNC) with short fiber length and needle-shaped crystals. Bacterial cellulose nanofibers produced by cellulose-producing bacteria such as acetic acid bacteria, and chitin nanofibers and chitosan nanofibers, which are different from cellulose, are also known. Methods for obtaining nanocellulose fibers include chemical defibration treatment, mechanical defibration treatment, and a combination of these for defibration of cellulose obtained from wood, and a method of synthesis using cellulose-producing bacteria such as acetic acid bacteria. Examples of chemical defibration treatments include the TEMPO oxidation method, the phosphoric acid esterification method, and the enzyme hydrolysis method, and examples of mechanical defibration treatments include the high-pressure homogenizer method, the microfluidizer method, the grinder grinding method, the freeze-pulverization method, the high-shear kneading method, and the ball mill grinding method.
[0003] Patent Document 1 describes a method for producing a resin material reinforcement material, which includes a step of mixing water, micro cellulose fibers containing nanocellulose fibers, and a filler surface-treated with fatty acids while applying a shear force, a step of drying the mixture, and a step of pulverizing the solid content after drying. According to this, it is possible to easily produce a resin material reinforcement material by preventing the micro cellulose fibers from agglomerating during the process of drying the micro cellulose fibers, and it is said that when the resin material reinforcement material is mixed into a resin material, the strength of the resin material can be greatly improved compared to conventional methods. However, there has been no report on the ability to effectively suppress ultraviolet light transmission.
[0004] On the other hand, Patent Document 2 describes a polyolefin resin composition obtained by adding (B) talc surface-treated with an organic silane compound, (C) a hindered amine stabilizer, and (D) an ultraviolet absorber to (A) a polyolefin. According to this, it is said that a polyolefin resin composition having excellent weather resistance can be provided by using talc surface-treated with an organic silane compound, a hindered amine stabilizer, and an ultraviolet absorber in combination. However, the ultraviolet absorbers used may be toxic or may need to be neutralized to reduce the environmental load when disposed of, and therefore a safe ultraviolet absorber has been desired. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-144614 A [Patent Document 2] Japanese Patent Application Publication No. 6-220261 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide an ultraviolet ray transmission inhibitor containing lignocellulose nanofibers that has a high ultraviolet ray transmission inhibitory effect, is non-toxic, and has a low environmental impact. [Means for solving the problem]
[0007] The above problem is solved by providing an ultraviolet transmission inhibitor containing lignocellulose nanofibers (LCNF).
[0008] In this case, it is preferable that the composition further contains a filler, and the mass ratio of the filler to the LCNF (filler / LCNF) is 0.3 / 1 to 12 / 1.
[0009] A resin composition containing the ultraviolet transmission suppressor is a preferred embodiment, a resin pellet containing the ultraviolet transmission suppressor is a preferred embodiment, a coating material containing the ultraviolet transmission suppressor is a preferred embodiment, and a paint containing the ultraviolet transmission suppressor is also a preferred embodiment. Effect of the Invention
[0010] The present invention can provide an ultraviolet ray transmission inhibitor containing lignocellulose nanofibers that has a high ultraviolet ray transmission inhibitory effect, is non-toxic, and has a low environmental impact. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the results of measuring the light transmittance of the polypropylene sheets obtained in Example 1 and Comparative Examples 1 and 2. [Diagram 2] FIG. 2 is a graph showing the results of measuring the light transmittance of the polypropylene sheets obtained in Examples 1 to 5. [Diagram 3] FIG. 2 is a graph showing the results of a tensile test carried out after a weather resistance test using the polypropylene pellets obtained in Example 1 and Comparative Example 2. [Figure 4] FIG. 1 shows the results of a tensile test carried out after a weather resistance test using the polypropylene pellets obtained in Example 6 and Comparative Example 3. [Diagram 5] FIG. 1 shows the results of measuring the light transmittance of LCNF-containing varnish and varnish alone. [Figure 6] FIG. 1 shows areas A to F of a circular iron plate coated with red paint in a metal halide test. [Figure 7] FIG. 2 is a diagram showing the results of observation with a polarizing microscope in the evaluation of dispersibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The ultraviolet transmission suppressor of the present invention is characterized by containing lignocellulose nanofibers (hereinafter, sometimes abbreviated as "LCNF"). As nanocellulose fibers, in addition to LCNF, cellulose nanofibers (CNF), cellulose nanocrystals (CNC), bacterial cellulose nanofibers, and chitin nanofibers and chitosan nanofibers, which are different from cellulose, are known. As a result of the intensive research conducted by the present inventors, it has become clear that an ultraviolet transmission suppressor having a high ultraviolet transmission suppression effect can be obtained by containing LCNF. From the comparison between the examples and the comparative examples in the ultraviolet acceleration test described below, it can be seen that the polypropylene pellets of Comparative Example 2 containing no LCNF and the polypropylene pellets of Comparative Example 1 containing CNF have a lower number average molecular weight Mn after the ultraviolet acceleration test, and the ratio of the weight average molecular weight Mw to the number average molecular weight Mn, Mw / Mn (dispersity), is larger than that of the blank PP, indicating that the molecular weight distribution is broad. In other words, it is considered that the polypropylene was decomposed by the ultraviolet acceleration test to produce low molecular weight polypropylene. In contrast, the polypropylene pellets of Example 1 containing LCNF did not show a decrease in molecular weight after the ultraviolet accelerated test, and the Mw / Mn (dispersity) showed almost no change compared to the blank PP, demonstrating a high ultraviolet transmission suppression effect. With regard to this, the inventors have clarified that by adding the ultraviolet transmission suppressor of the present invention to a resin, etc., the penetration of ultraviolet light into the resin, etc. was suppressed, and thus ultraviolet degradation of the resin, etc. (decomposition and deterioration of mechanical properties) was suppressed.
[0013] The LCNF used in the present invention may be one obtained by a known method such as a high-pressure homogenizer method, a microfluidizer method, a grinder grinding method, a freeze crushing method, a high shear kneading method, a ball mill grinding method, or a water jet method. The LCNF contains a certain amount of lignin, and in this respect is distinguished from CNF that does not contain lignin. The amount of lignin contained in the LCNF is preferably 1 to 80 mass%, more preferably 2 to 70 mass%, and even more preferably 3 to 60 mass%. The LCNF used in the present invention contains cellulose and hemicellulose in addition to lignin, and the amount of cellulose contained in the LCNF is preferably 15 to 80 mass%, more preferably 20 to 70 mass%, and even more preferably 30 to 60 mass%. In addition, the amount of hemicellulose contained in the LCNF is preferably 5 to 40 mass%, more preferably 8 to 35 mass%, and even more preferably 12 to 30 mass%. The LCNF used in the present invention may further contain a certain amount of ash and organic solvent soluble matter. The ash content of the LCNF is preferably 0.01 to 3 mass%, more preferably 0.05 to 2 mass%, and even more preferably 0.1 to 1.5 mass%. The organic solvent soluble content of the LCNF is preferably 0.1 to 10 mass%, more preferably 0.5 to 8 mass%, and even more preferably 1 to 5 mass%.
[0014] The fiber width (fiber thickness) of the LCNF used in the present invention is preferably 2 nm to 50 μm, more preferably 5 nm to 30 μm, even more preferably 10 nm to 10 μm, and particularly preferably 15 nm to 1 μm. The fiber length of the LCNF used in the present invention is preferably 10 nm to 5 mm, more preferably 50 nm to 2 mm, even more preferably 100 nm to 1 mm, and particularly preferably 500 nm to 500 μm.
[0015] In a preferred embodiment, the ultraviolet ray transmission suppressor of the present invention further contains a filler, and the mass ratio of the filler to the LCNF (filler / LCNF) is 0.3 / 1 to 12 / 1. Having the mass ratio (filler / LCNF) in this range has the advantage of preventing the LCNF from agglomerating, and of obtaining a uniform composition when the ultraviolet ray transmission suppressor is mixed with a resin or the like. The mass ratio (filler / LCNF) is more preferably 0.5 / 1 to 10 / 1, even more preferably 0.8 / 1 to 8 / 1, particularly preferably 1 / 1 to 6 / 1, and most preferably 1.2 / 1 to 4 / 1.
[0016] As the filler, fillers to be mixed in molded bodies of synthetic resin materials such as rubber or plastic, or fillers to be mixed in synthetic resin compositions such as paints can be used. Examples of the filler include calcium carbonate, talc, silica, clay, wollastonite, potassium titanate, zonolite, titanium oxide, and magnesium oxide. Among them, fillers surface-treated with fatty acid and / or fatty acid salt are preferably used. For example, a slurry obtained by mixing a filler with water is stirred while being heated to about 50 to 70°C, and fatty acid and / or fatty acid salt are added thereto and further stirred. This is pressed, dehydrated, and then dried, and can be used. The filler may be treated with other components in addition to fatty acid and / or fatty acid salt. Examples of other components include silane coupling agents.
[0017] The fatty acid may be either saturated or unsaturated, but it is preferable to use saturated fatty acids because unsaturated fatty acids are easily oxidized and deteriorated. If the number of carbon atoms in the fatty acid is small, the odor will be strong. For this reason, the number of carbon atoms in the fatty acid is preferably 6 or more, more preferably 10 or more. If the number of carbon atoms is large, the melting point will be high, so the number of carbon atoms is preferably 30 or less, more preferably 24 or less. Examples of fatty acids include caproic acid, decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, lignoceric acid, and oleic acid. Examples of fatty acid salts include sodium salts of the above fatty acids and potassium salts of the above fatty acids.
[0018] By making the particle size of the filler approximately the same as the fiber width of the LCNF, it becomes possible to mix the filler and the LCNF uniformly in the mixing process. This makes it possible to obtain a uniform composition when blended with a resin material or the like. The average particle size of the filler is preferably 2 to 100 μm, and more preferably 2 to 50 μm. The average particle size of the filler refers to the particle size at 50% of the cumulative value in the particle size distribution determined by the laser diffraction / scattering method.
[0019] When the ultraviolet ray transmission suppressor of the present invention further contains a filler, a preferred embodiment is to wet mix the paste-like LCNF and the filler while applying a shear force to obtain a mixture. When dry-mixed, the LCNF may diffuse into the air. Wet mixing can prevent the LCNF from diffusing into the air and reducing the yield. The application of shear force allows the LCNF and the filler to be mixed uniformly. It is presumed that the application of shear force causes the LCNF and the filler to be physically bonded to each other and integrated. To mix while applying a shear force, a mixer, a ball mill, a stone mill-type mill such as a mass colloider, a homogenizer, or the like may be used.
[0020] In a preferred embodiment, after obtaining the mixture, a drying step is performed to reduce the moisture content of the mixture to obtain a dried product. The drying method is not particularly limited, and for example, the mixture is placed in an arbitrary container and the container is stored in a hot air dryer. A vacuum dryer may be used instead of the hot air dryer. If a vacuum dryer is used, the boiling point can be lowered to reduce the moisture content in a shorter time.
[0021] After obtaining the dried product, a pulverization process is carried out to suitably obtain the ultraviolet ray transmission suppressor of the present invention. The pulverization method is not particularly limited, and for example, it is possible to simply pulverize using a device such as a mixer, a pin mill, a roller mill, or a hammer mill. By pulverizing using any method, it is possible to easily obtain the ultraviolet ray transmission suppressor of the present invention in powder form.
[0022] The ultraviolet transmission suppressor of the present invention can be blended with various materials. For example, the ultraviolet transmission suppressor of the present invention can be blended with polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polyamide resins such as nylon; polystyrene resins; epoxy resins; acetal resins; fluorine-based resins, etc., to produce resin compositions or resin pellets. Therefore, a resin composition blended with the ultraviolet transmission suppressor is a preferred embodiment, and a resin pellet blended with the ultraviolet transmission suppressor is also a preferred embodiment.
[0023] The ultraviolet ray transmission suppressor of the present invention can also be blended with rubbers such as natural rubber, isoprene rubber, butadiene rubber, chloroprene rubber, acrylonitrile-butadiene copolymer rubber, ethylene-propylene-diene terpolymer rubber, urethane rubber, silicone rubber, fluorine rubber, etc., and can also be blended with thermoplastic elastomers such as styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers, urethane-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, etc. Therefore, rubbers blended with an ultraviolet ray transmission suppressor are a preferred embodiment, and thermoplastic elastomers blended with an ultraviolet ray transmission suppressor are also preferred embodiments.
[0024] Furthermore, the ultraviolet transmission suppressor of the present invention can be blended into a paint. In the present invention, the paint includes a coating material used as a top coat. Therefore, a paint containing an ultraviolet transmission suppressor is a preferred embodiment, and a coating material containing an ultraviolet transmission suppressor is also a preferred embodiment. The paint may contain a resin, a solvent, or the like, as necessary. Examples of the resin include vinyl acetate resin, urethane resin, acrylic resin, polyester resin, epoxy resin, polyvinyl alcohol resin, and polyurea resin. Examples of the solvent include water or an aqueous solvent mainly composed of water; alcohol solvents such as methanol, ethanol, propanol, isopropanol, and butanol; polyhydric alcohol solvents such as ethylene glycol, diethylene glycol, thiodiethylene glycol, triethylene glycol, tetraethylene glycol, and polyethylene glycol; aromatic hydrocarbon solvents such as toluene and xylene; ether solvents such as dimethyl ether, ethyl methyl ether, diethyl ether, tetrahydrofuran, and 1,4-dioxane; and nitrile solvents such as acetonitrile, propionitrile, and benzonitrile. The paint may be a paint containing a color pigment, or a clear paint not containing a color pigment, such as varnish. Among them, a water-based paint containing a color pigment is a preferred embodiment, and a water-based clear paint used as a top coat is also a preferred embodiment. In addition, additives such as plasticizers, dispersants, anti-settling agents, emulsifiers, thickeners, defoamers, anti-mold agents, preservatives, anti-skinning agents, and anti-sagging agents may be added within a range that does not impair the effects of the present invention.
[0025] As described above, the ultraviolet transmission suppressor of the present invention can be blended with various materials, and therefore can be suitably used in various applications that may be deteriorated by ultraviolet rays, such as agricultural resin sheets; automotive resin parts; daily necessities such as clothespins and resin ropes; paints (including coating materials) for automobiles, building materials, stationery, etc.; sealants used on the exterior walls of houses; lubricants; and adhesives. When blending the ultraviolet transmission suppressor of the present invention with various materials, it may be poorly dispersed within a range that does not impair the ultraviolet transmission suppression effect. When used in applications where good appearance is desired, it is preferable that the dispersion state is good. EXAMPLES
[0026] The present invention will now be described in more detail with reference to the following examples. The raw materials used in the following examples are as follows. [Raw materials] Lignocellulose nanofibers (LCNF; ash content 0.3 mass%, organic solvent soluble content 2.9 mass%, lignin 34 mass%, cellulose 47 mass%, hemicellulose 15 mass%) were used, Cellfim L100 manufactured by Mori Machinery Co., Ltd. The fiber width was 30 to 300 nm, and the fiber length was 100 μm or less. The cellulose nanofibers (CNF; lignin 0 mass%, cellulose 90 mass%, hemicellulose 10 mass%) used were Cellfim C500 manufactured by Mori Machinery Co., Ltd. The fiber width was 20 to 200 nm, and the fiber length was 500 μm or less. The filler that was surface-treated with fatty acid was Shiraishi Kogyo Co., Ltd.'s Hakuenka CC. This filler is calcium carbonate that has been surface-treated with fatty acid, and the average particle size measured by the laser diffraction / scattering method is 21.1 μm. The filler is in the form of secondary agglomerates, so the particle size is larger than the catalog value. The varnish (solid content 52.8%) used was a water-based urethane varnish manufactured by Washin Paint Co., Ltd.
[0027] Example 1 [Ultraviolet transmission suppressing material] A paste-like LCNF with a water content of 90% by mass was mixed with a filler surface-treated with a fatty acid in a weight ratio of 40:60 using a mixer (Kawata Co., Ltd. "Super Mixer: Model SMV-20"). The mixture obtained by mixing was dried with hot air using a hot air dryer (Matsui Mfg. Co., Ltd. "Box Dryer") and pulverized at a rotation speed of 3600 rpm using a mixer (Kawata Co., Ltd. "Super Mixer: Model SMV-20") to obtain a powdered ultraviolet transmission suppressor.
[0028] [Preparation of polypropylene pellets] The raw polypropylene pellets were put into a kneader, heated and kneaded to melt, and then 1 part by weight of maleic anhydride-modified polypropylene (Kayabrid 006PP, Kayaku Akzo Co., Ltd.) was added as a compatibilizer for 100 parts by weight of polypropylene, followed by the ultraviolet ray transmission suppressor obtained in the example. The ultraviolet ray transmission suppressor was added in such an amount that the LCNF was 4% by mass relative to the total weight including the polypropylene, maleic anhydride-modified polypropylene, and ultraviolet ray transmission suppressor. The mixture was then further kneaded to produce LCNF-containing polypropylene pellets.
[0029] [Preparation of polypropylene sheet] The obtained pellets were set in a press and pressed at 180° C. and 15 MPa for 2 minutes, and then immediately cooled to prepare a polypropylene sheet.
[0030] Examples 2 to 5 In Example 1, LCNF-containing polypropylene pellets were prepared so that the LCNF contents were 0.4 mass%, 1.2 mass%, 2 mass%, and 2.8 mass%, respectively, and polypropylene sheets were prepared using the pellets.
[0031] Example 6 LCNF-containing polyamide pellets were prepared in the same manner as in Example 1, except that raw material pellets of polyamide (nylon 6) were used instead of raw material pellets of polypropylene.
[0032] Comparative Example 1 A powder was obtained in the same manner as in Example 1, except that CNF was used instead of LCNF, and CNF-containing polypropylene pellets and a polypropylene sheet were produced.
[0033] Comparative Example 2 Polypropylene pellets and a polypropylene sheet were prepared in the same manner as in Example 1, except that no ultraviolet transmission suppressant was used.
[0034] Comparative Example 3 Polyamide pellets were prepared in the same manner as in Example 1, except that raw material pellets of polyamide (nylon 6) were used instead of raw material pellets of polypropylene, and no ultraviolet transmission suppressant was used.
[0035] [Transmittance measurement of polypropylene sheet] The light transmittance was measured for the polypropylene sheets of Examples 1 to 5 and Comparative Examples 1 and 2 using an ultraviolet-visible-near infrared spectrophotometer equipped with an integrating sphere ("V-750" manufactured by JASCO Corporation). The results are shown in FIGS.
[0036] [UV acceleration test using a xenon weather meter] Using the polypropylene pellets obtained in Example 1, Comparative Examples 1 and 2, injection molding was performed at 210°C to obtain each molded body (size: 60mm x 80mm x 5mm). The molded body was subjected to a 400-hour ultraviolet accelerated test using a xenon weather meter. The change in molecular weight after the accelerated test was measured using a high-temperature GPC device (HLC-8321GPC / HT, detector RI). 1,2,4-trichlorobenzene was used as the eluent. The measurement sample was dissolved in 1,2,4-trichlorobenzene and insoluble matter was removed. The results are shown in Table 1. As can be seen from Table 1, the molded body using the polypropylene pellets (without LCNF) of Comparative Example 2 had a reduced molecular weight after the ultraviolet accelerated test. Since the Mw / Mn (dispersity) is larger than that of the blank PP, it can be seen that the molecular weight distribution is broad. In other words, it is considered that the polypropylene was decomposed by the ultraviolet accelerated test to produce low molecular weight polypropylene. In addition, the molded body using the polypropylene pellets (containing CNF) of Comparative Example 1 had a slightly reduced molecular weight after the ultraviolet accelerated test. On the other hand, the molecular weight of the molded article using the polypropylene pellets (containing LCNF) of Example 1 did not decrease after the ultraviolet accelerated test. Therefore, it was found that the inclusion of LCNF exerts an ultraviolet ray transmission suppression effect.
[0037] [Table 1]
[0038] [Tensile test after weather resistance test] Using the polypropylene pellets obtained in Example 1 and Comparative Example 2, and the polyamide pellets obtained in Example 6 and Comparative Example 3, test pieces (thickness 4 mm, width 10 mm) were prepared in accordance with JIS K7161-2:2014, and outdoor exposure tests (0 weeks, 7 weeks, 21 weeks, 35 weeks, 49 weeks, and 63 weeks) were performed. In accordance with JIS K7161-1:2014, a tensile test was performed at a test speed of 2 mm / min using a tensile compression tester (Shimadzu Corporation "AGS-5KNG") to determine the stress, elastic modulus, and elongation. The results are shown in Tables 2, 3, 3, and 4.
[0039] [Table 2]
[0040] [Table 3]
[0041] [Transmittance measurement after dispersion in varnish] Only the varnish was applied onto a polypropylene plate, and the varnish was peeled off after drying. LCNF was added to the varnish so that the LCNF was 0.5 mass% relative to the total amount of varnish, and the mixture was stirred with a brush to prepare an LCNF-containing varnish. This LCNF-containing varnish was applied onto a polypropylene plate, and the LCNF-containing varnish was peeled off after drying. The light transmittance was measured using an ultraviolet-visible-near infrared spectrophotometer equipped with an integrating sphere ("V-750" manufactured by JASCO Corporation). The results are shown in Figure 5.
[0042] [Color change after metal halide test] Varnishes containing 0.25 mass%, 0.5 mass%, 1 mass% and 1.5 mass% LCNF were prepared. As shown in Fig. 6, a circular iron plate coated with red paint was divided into regions A to F. Regions E and F were topcoated with varnish containing LCNF, regions C and D were topcoated with varnish only, and regions A and B were not topcoated. Then, only regions B, C and E were exposed to ultraviolet ray irradiance of 150 mW / cm2. 2 A metal halide test was performed by irradiating the sample with light at 4000 K for 24 hours, and the color of the surfaces of areas A to F was measured using a color reader ("CR-10" manufactured by Konica Minolta, Inc.). The results are shown in Table 4.
[0043] [Table 4]
[0044] [Evaluation of dispersibility] In Example 1, the powder after drying with hot air was pulverized at a rotation speed of 1800 rpm to obtain an insufficiently pulverized ultraviolet transmission suppressor as a powder. The powder was used to prepare polypropylene pellets so that the LCNF content was 4 mass%, and the pellets were used to prepare a poorly dispersed polypropylene sheet. Observation was performed using a polarizing microscope (Nikon Corporation's "ECLIPSE Ci-POL"). The observation was performed without using a polarizing plate. The polypropylene sheets of Example 1 and Comparative Example 2 were also observed in the same manner. The obtained results are shown in FIG. 7. In the poorly dispersed polypropylene sheet, aggregates of about 100 to 300 μm were observed. On the other hand, in the polypropylene sheet of Example 1, aggregates of about 10 to 30 μm were observed. In the polypropylene sheet of Comparative Example 2 that did not contain LCNF, no aggregates were observed.
Claims
1. An ultraviolet light transmission inhibitor containing lignocellulose nanofiber (LCNF).
2. 2. The ultraviolet ray transmission suppressor according to claim 1, further comprising a filler, the mass ratio of the filler to the LCNF (filler / LCNF) being 0.3 / 1 to 12 / 1.
3. A resin composition comprising the ultraviolet ray transmission suppressor according to claim 1 or 2.
4. A resin pellet containing the ultraviolet ray transmission suppressor according to claim 1 or 2.
5. A coating material comprising the ultraviolet ray transmission inhibitor according to claim 1 or 2.
6. A paint comprising the ultraviolet ray transmission inhibitor according to claim 1 or 2 blended therein.
Citation Information
Patent Citations
Ultraviolet light absorbing lignocellulosic film
JP1992033986A
UV absorbing film and preparation thereof
JP1997241571A
Composition having infrared light-absorbing property and its production
JP1997241615A
Coating method of forming coating containing ultraviolet shielding agent and infrared shielding agent