Conduction cooling type superconducting coil, superconducting magnet device, and method for manufacturing conduction cooling type superconducting coil
The conduction-cooled superconducting coil design addresses high contact and thermal resistance issues by using a multilayer solenoid structure with low-melting point metal connections and insulation, achieving rapid stabilization and efficient cooling of high-temperature superconducting coils.
Patent Information
- Application Number
- JP2023079998
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-27
AI Technical Summary
Conventional superconducting coils face challenges with high contact resistance and thermal resistance between wires, leading to excessive Joule heat generation, strain resistance issues, and prolonged stabilization times due to circulating currents, especially when using high-temperature superconductors like MgB2.
A conduction-cooled superconducting coil design featuring a multilayer solenoid structure with superconducting wires wound around a bobbin, using a low-melting point metal to connect and insulate the wires, and a porous metal material for thermal conduction, reducing contact resistance and thermal resistance while allowing efficient cooling.
The design stabilizes magnetic fields quickly, suppresses circulating currents, prevents wire burnout, and enhances cooling efficiency, enabling stable operation without liquid helium.
Smart Images

Figure 2024164491000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a conduction-cooled superconducting coil in which a coil winding is cooled by thermal conduction using a refrigerator, a superconducting magnet device, and a method for manufacturing a conduction-cooled superconducting coil. [Background technology]
[0002] Superconducting coils can pass current with a current density several tens to several hundreds of times higher than that of normal conducting coils, and can generate a strong magnetic field. In addition, because current can pass through them with zero electrical resistance, energy loss can be kept to a minimum. For this reason, superconducting coils are used in MRI (Magnetic Resonance Imaging) devices, NMR (Nuclear Magnetic Resonance) devices, accelerators, single crystal silicon pulling devices, and the like.
[0003] Conventional superconducting coils are mainly made of low-temperature superconductors, and liquid helium and other coolants have been used to cool them below their transition temperature. A typical low-temperature superconductor is niobium titanium (NbTi), which has a transition temperature of about 10 K. Low-temperature superconductors have generally been maintained at an extremely low temperature of about 4 K by using liquid helium in combination with a refrigerator.
[0004] However, in recent years, helium has become scarce and expensive due to factors such as the depletion of helium in natural gas fields that have traditionally been used, delays in the development of new helium supply sources due to social instability, etc. Under these circumstances, in order to reduce the amount of liquid helium used, efforts are being made to commercialize high-temperature superconductors that can maintain a superconducting state using only refrigerators, and to commercialize superconducting coils that use high-temperature superconductors.
[0005] High-temperature superconductors include REBCO such as REBa2Cu3O and Bi2Sr2Ca2Cu3O 10Examples of such superconductors include BSCCO, such as YBa2Cu3O7, and YBCO, such as YBa2Cu3O7. Magnesium diboride (MgB2) is also known as a material that transitions at a higher temperature than low-temperature superconductors. MgB2 has a high transition temperature of approximately 39K, and is made from abundant elements, so it is expected to be put to practical use and become widespread.
[0006] Although high-temperature superconductors and MgB2 can be operated without using liquid helium, they have the disadvantage of being inferior in strain resistance compared to conventional low-temperature superconductors. In general, superconductors are prone to strain during processes such as applying insulating coating to superconducting wires and bending superconducting wires. When high-temperature superconductors or MgB2 are made into long wires or when the wires are bent into coils, they are damaged by strain, making it difficult to obtain the required superconducting properties, such as critical current density, over the entire length.
[0007] In addition, high-temperature superconductors and MgB2 have the characteristic that hot spots, which are a phenomenon of localized normal conductive transition, are more likely to occur than conventional low-temperature superconductors. The specific heat of a superconductor is more than 10 times that of conventional 4K at high temperatures of about 15K or higher. In high-temperature regions where high-temperature superconductors and MgB2 are used, temperature changes are less likely to occur, so if a quench occurs due to some disturbance, the normal conductive region will not propagate. The normal conductive transition only progresses locally, and superconducting current flows into a small normal conductive region. There is a problem that the superconducting wire will burn out due to excessive Joule heat generated locally.
[0008] Conventionally, non-insulated coils have been proposed as a measure to avoid the occurrence of hot spots. Non-insulated coils are formed of non-insulated wires whose outer circumferential surface is not covered with an insulating layer. Furthermore, no insulating material is interposed between the non-insulated wires wound in a coil shape, and normal conductors such as stabilizing materials are arranged. For example, Patent Document 1 describes a superconducting coil in which non-insulated regions are provided between superconducting wires where no insulating material is provided (see paragraphs 0067 to 0072).
[0009] In a non-insulated coil, adjacent superconducting wires are connected via normal conductors. Therefore, even if a quench occurs in one of the superconducting wires, the supercurrent transported through the superconducting wire can bypass the region where normal transition has occurred and escape to the surrounding superconducting region. This prevents excessive Joule heat from being generated in the region where normal transition has occurred, and therefore prevents the superconducting wire from burning out, causing disconnection, or burning of components. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2020-025014 A Summary of the Invention [Problem to be solved by the invention]
[0011] The use of non-insulated coils may be able to avoid problems caused by hot spots. However, large currents of up to several hundred amperes may flow through superconducting coils. When large currents flow through a superconducting coil, a structure with extremely low contact resistance between the superconducting wires is required to prevent the generation of excessive Joule heat.
[0012] Conventionally, structures with low contact resistance between superconducting wires were limited to cases where a sufficient contact area between the superconducting wires could be secured. In cases where superconducting wires with rectangular cross sections, such as rectangular wires, are used, the contact area between the superconducting wires could not be sufficiently large unless the sides of the superconducting wires were in surface contact with each other.
[0013] Even if the contact area between superconducting wires can be secured, when conducting cooling, it is necessary to reduce not only the electrical contact resistance between the superconducting wires but also the thermal contact resistance between the superconducting wires. In order to reduce the thermal contact resistance, it is necessary to apply a certain amount of surface pressure to the sides of the superconducting wires so that they come into contact with each other. However, when using high-temperature superconductors or MgB2, it is difficult to apply sufficient surface pressure because of their poor strain resistance.
[0014] Furthermore, when a structure with low contact resistance between superconducting wires, such as a non-insulated coil, is adopted, it becomes possible to release the superconducting current from the region where the normal transition has occurred, but there is a problem that an induced current flows between the superconducting wires when the superconducting current is swept. When a superconducting current is swept through a superconducting coil, an induced current is generated in the base material of the superconducting wire, etc. The circulating current that flows between the superconducting wires due to induction is characterized by a large time constant. This causes a problem in that it takes a long time for the generated magnetic field to stabilize after the rated current value is reached. In addition, Joule heat and energy loss due to the circulating current become problems.
[0015] Therefore, an object of the present invention is to provide a conduction-cooled superconducting coil, a superconducting magnet device, and a method for manufacturing a conduction-cooled superconducting coil, which are capable of forming a stable magnetic field in a short period of time by achieving both suppression of circulating current flowing between superconducting wires and efficient conduction cooling of the superconducting wire in a coil winding in which the superconducting wire is wound. [Means for solving the problem]
[0016] In order to solve the above problems, the present invention provides a conduction-cooled superconducting coil having a coil winding in which a superconducting wire is wound around a bobbin in a multi-layered solenoid shape, the coil winding being cooled by thermal conduction by a refrigerator, the coil winding having a plurality of rows of the superconducting wire arranged in the axial direction of the bobbin and a plurality of layers of the superconducting wire stacked in the radial direction of the bobbin, the rows of the superconducting wire are electrically and thermally connected to each other by a low-melting-point metal having a melting point of 300° C. or less, and the layers of the superconducting wire are electrically insulated from each other by an insulating material. Also, a superconducting magnet device includes the conduction-cooled superconducting coil.
[0017] A method for producing a conduction-cooled superconducting coil according to the present invention has a coil winding in which a superconducting wire is wound around a bobbin in a multi-layered solenoid shape, and the coil winding is cooled by thermal conduction by a refrigerator, and includes the steps of: winding the superconducting wire around the bobbin in a solenoid shape to form a layer of the superconducting wire in which a plurality of rows of the superconducting wire are arranged in the axial direction of the bobbin; attaching a low-melting-point metal having a melting point of 300° C. or less around the superconducting wire; and attaching a low-melting-point metal to the outside of the low-melting-point metal. The method includes the steps of: arranging an insulating material; winding the superconducting wire in a solenoid shape around the insulating material to form a next layer of the superconducting wire in which a plurality of rows of the superconducting wire are arranged in the axial direction of the bobbin; and performing the process of depositing the low-melting point metal and arranging the insulating material once or a plurality of times to form the coil winding.; and heat-treating the coil winding to melt and solidify the low-melting point metal to electrically and thermally connect the rows of superconducting wire together via the low-melting point metal. Effect of the Invention
[0018] According to the present invention, it is possible to provide a conduction-cooled superconducting coil, a superconducting magnet device, and a method for manufacturing a conduction-cooled superconducting coil, which are capable of forming a stable magnetic field in a short period of time by suppressing the circulating current flowing between the superconducting wires and efficiently conducting cooling the superconducting wire in a coil winding in which the superconducting wire is wound. [Brief description of the drawings]
[0019] [Figure 1] 1 is a cross-sectional view showing a schematic diagram of a superconducting coil according to an embodiment of the present invention. [Diagram 2] 1 is a diagram showing an example of a main part of a superconducting coil according to an embodiment of the present invention; [Diagram 3] 5A to 5C are diagrams illustrating an example of a method for manufacturing a superconducting coil according to an embodiment of the present invention. [Figure 4A] 1A to 1C are diagrams showing examples of the shape of a porous metal material used in a superconducting coil. [Figure 4B]1A to 1C are diagrams showing examples of the shape of a porous metal material used in a superconducting coil. [Figure 4C] 1A to 1C are diagrams showing examples of the shape of a porous metal material used in a superconducting coil. [Diagram 5] 1 is a diagram showing an example of a main part of a superconducting coil according to an embodiment of the present invention; [Figure 6] 5A to 5C are diagrams illustrating an example of a method for manufacturing a superconducting coil according to an embodiment of the present invention. [Figure 7] 1 is a diagram showing an example of a main part of a superconducting coil according to an embodiment of the present invention; [Figure 8] FIG. 2 is a development view showing a connection portion of a superconducting coil according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, a conduction-cooled superconducting coil, a superconducting magnet device, and a method for manufacturing a conduction-cooled superconducting coil according to an embodiment of the present invention will be described with reference to the drawings. In the following drawings, common components are designated by the same reference numerals, and duplicated descriptions will be omitted.
[0021] FIG. 1 is a cross-sectional view that shows a schematic diagram of a superconducting coil according to an embodiment of the present invention. FIG. 2 is a diagram showing an example of a main part of a superconducting coil according to an embodiment of the present invention. FIG. 1 shows only one side of a cross section of a conduction-cooled superconducting coil according to this embodiment, with respect to the central axis of the coil. The dashed line in FIG. 1 indicates the central axis of the coil and the bobbin. The arrow in FIG. 1 indicates an example of the winding direction. FIG. 2 shows an enlarged view of region A surrounded by a dashed line in FIG. 1.
[0022] As shown in Figures 1 and 2, the superconducting coil 1 of this embodiment includes a bobbin 2, a coil winding 3 wound with a superconducting wire 10, a cooling plate 4, a coil insulation material 5, a porous metal material 6, an interlayer insulation material 7, a low-melting point metal layer 8, and a resin layer 9.
[0023] The superconducting coil 1 is a conduction-cooled superconducting coil in which the coil winding 3 around which the superconducting wire 10 is wound is cooled by thermal conduction using a refrigerator. The superconducting coil 1 is stored in a cryostat (not shown) and is thermally connected to the refrigerator. The superconducting coil 1 can be used as a superconducting magnet device by cooling the coil winding 3 to a temperature below the superconducting transition temperature using the refrigerator and passing a superconducting current through the coil winding 3.
[0024] A superconducting magnet device using the superconducting coil 1 can be provided in an open-type or tunnel-type MRI device, an NMR device, an accelerator equipped with a deflection magnet, a focusing magnet, etc., a magnet-type pulling device for single crystal silicon, etc. Since the superconducting coil 1 is of a conduction cooling type, it can be operated without using a coolant such as liquid helium or with reduced usage of the coolant.
[0025] In this specification, "thermally connecting" means that target components are brought into direct or indirect contact with each other without substantially any space between them to form a structure that allows efficient heat transfer by thermal conduction within the components or heat transfer between the components. When the components are brought into indirect contact with each other, one or more highly thermally conductive components with high thermal conductivity can be sandwiched between the target components.
[0026] The bobbin 2 is a cylinder for holding the coil winding 3. The bobbin 2 can be made of a copper material such as oxygen-free copper. In FIG. 1, the bobbin 2 has a cylindrical main body and a flange portion having a larger diameter than the main body. The flange portion is provided on one axial end side of the main body. A cooling plate 4 is disposed on the other axial end side of the main body.
[0027] The coil winding 3 is formed by winding the superconducting wire 10 in a multi-layer solenoid shape around the bobbin 2. The superconducting wire 10 can be wound, for example, in an aligned manner around the outer circumferential surface of the main body of the bobbin 2. The coil winding 3 around which the superconducting wire 10 is wound is disposed so as to be sandwiched between the flange portion of the bobbin 2 and the cooling plate 4, and is thermally connected to the flange portion of the bobbin 2 and the cooling plate 4.
[0028] In the example of Fig. 1, eight layers of superconducting wire 10 are shown. If the diameter of superconducting wire 10 is one pitch, then in Fig. 1, the odd-numbered layers (first layer, third layer, fifth layer, etc.) and the even-numbered layers (second layer, fourth layer, sixth layer) are laminated in the radial direction at the same pitch (same phase), but the odd-numbered layers and the even-numbered layers may be laminated in an aligned winding with a pitch (phase) shifted by 1 / 2 pitch. When the pitch is shifted by 1 / 2 pitch, the radial dimension can be reduced.
[0029] The cooling plate 4 thermally connects the coil winding 3 and the refrigerator. The cooling plate 4 can be made of a copper material such as oxygen-free copper, an aluminum material, or the like. In FIG. 1, the cooling plate 4 is provided in a disk shape similar to the flange portion of the bobbin 2. The cooling plate 4 is provided on one axial side of the main body portion of the bobbin 2 and outside one axial end of the bobbin 2 of the coil winding 3 so as to face the flange portion of the bobbin 2. The refrigerator can be thermally connected to the outer circumferential surface or top surface of the cooling plate 4.
[0030] The coil insulation material 5 is an insulating material for electrically insulating the coil winding 3 from other members. In Fig. 1, the coil insulation material 5 is interposed in layers between the coil winding 3 and the flange portion of the bobbin 2, between the coil winding 3 and the main body portion of the bobbin 2, and between the coil winding 3 and the cooling plate 4.
[0031] The coil insulation material 5 is made of an insulating material with high electrical resistivity and is formed to a thickness that does not impede heat transfer between components. The coil insulation material 5 may be a resin film, a resin sheet, a glass fiber sheet formed from molded glass fiber, or a glass cloth formed from woven glass braid. The resin may be an insulating resin such as polyimide or heat-resistant epoxy resin.
[0032] 1 and 2, the superconducting wire 10 is provided as a round wire. The round wire may be a wire having a circular cross section or an elliptical cross section. The round wire may have any roundness or flatness. The coil winding 3 is preferably provided as a round wire over the entire length, but a part of the coil winding 3 may have a cross section other than a round wire.
[0033] Generally, round wires have a shape in which the sides of the superconducting wires are in line contact when adjacent to each other. Therefore, round wires have a large contact electrical resistance and contact thermal resistance between the superconducting wires compared to rectangular wires and tape wires, whose sides are in surface contact with each other. Although the circulating current circulating between the superconducting wires is suppressed, it is disadvantageous in terms of heat transfer between the superconducting wires and in terms of escaping the superconducting current in the event of a partial quench.
[0034] In contrast, in the superconducting coil 1 according to this embodiment, the use of a low melting point metal reduces the electrical contact resistance and thermal contact resistance between the superconducting wires, and therefore it is possible to employ a round superconducting wire 10. The use of a round superconducting wire 10 can be advantageous in that it reduces the number of manufacturing steps and manufacturing costs, reduces anisotropy, and allows manufacturing by wire drawing such as extrusion and drawing.
[0035] As shown in Fig. 1, the coil winding 3 has a plurality of rows of superconducting wires 10 arranged in the axial direction of the bobbin 2 and a plurality of layers of superconducting wires 10 stacked in the radial direction of the bobbin 2 by winding the superconducting wire 10 in a multi-layered solenoid shape. Each row of the superconducting wires 10 extends along the radial direction of the bobbin 2. Each layer of the superconducting wires 10 extends along the axial direction of the bobbin 2. In Fig. 1, a total of 12 rows and 8 layers of the coil winding 3 are formed.
[0036] The superconducting wire 10 can be wound in the following procedure, as shown by the arrows in Fig. 1. First, the superconducting wire 10 is wound in a solenoid shape around the bobbin 2 from the upper end to the lower end in the axial direction of the bobbin 2. When the superconducting wire 10 reaches the lower end in the axial direction of the bobbin 2, the winding diameter is expanded and the wire is wound around the superconducting wire 10 at the lower end. After that, the wire is turned back in the opposite direction and wound in a solenoid shape around the superconducting wire 10 of the previous layer that has already been wound, from the lower end to the upper end in the axial direction of the bobbin 2.
[0037] Similarly, when it reaches the upper end of the bobbin 2 in the axial direction, the winding diameter is enlarged and it is wound around the superconducting wire 10 at the upper end. Then, it turns back in the opposite direction and is wound in a solenoid shape around the superconducting wire of the previous layer that has already been wound, from the upper end to the lower end in the axial direction of the bobbin 2. By repeating such winding, it is possible to form the coil winding 3 in which the superconducting wire 10 is wound in a multi-layer solenoid shape.
[0038] The superconducting wire 10 may be wound starting from either one end side or the other end side in the axial direction of the bobbin 2. Although the coil winding 3 is formed of a single long superconducting wire 10, the coil winding 3 may be formed of a single superconducting wire 10 or a plurality of superconducting wires 10. The coil winding 3 may be provided in any number of rows or layers. The number of rows of the coil winding 3 may be changed for each layer.
[0039] 2, the coil winding 3 is formed by combining a porous metal material 6, an interlayer insulating material 7, a low melting point metal layer 8, and a resin layer 9 with a superconducting wire 10. The porous metal material 6 and the interlayer insulating material 7 are disposed between the layers of the superconducting wire 10. The low melting point metal layer 8 and the resin layer 9 fill the space around the superconducting wire 10 in each layer sandwiched between the interlayer insulating material 7 and the porous metal material 6.
[0040] The superconducting wire 10 is formed of superconducting filaments 11 and a base material 12. In Fig. 2, the superconducting wire 10 is provided in a multi-core wire structure including a plurality of superconducting filaments 11. The multi-core wire structure provides stabilization and reduction of AC loss through redundancy. However, the superconducting wire 10 may be provided in a single-core wire structure. The superconducting filaments 11 can be provided in any number and in any arrangement as long as they are surrounded by the base material 12.
[0041] The superconducting filament 11 is formed of a superconductor capable of undergoing a superconducting transition at or below a predetermined transition temperature. The superconducting filament 11 may contain impurities for magnetic flux pinning in addition to the superconductor capable of undergoing a superconducting transition. The material of the superconducting filament 11 may be magnesium diboride (MgB2) or a high-temperature superconductor such as REBCO, BSCCO, or YBCO.
[0042] The base material 12 is formed of a normal conductor that is a good conductor. The base material 12 not only forms a matrix that supports the superconducting wire 10, but may also have functions such as a stabilizing material, a buffer material, and a barrier material. Materials that can be used for the base material 12 include copper, aluminum, iron, niobium, silver, nickel, and alloys thereof. If the base material 12 is a good conductor, when a quench occurs, the superconducting current flowing through the superconducting filaments 11 can be easily released to the surrounding superconducting filaments 11 and the surrounding superconducting wire 10.
[0043] As shown in Fig. 2, the superconducting wire 10 is provided as an uninsulated wire whose outer circumferential surface is not covered with an insulating layer. Conventional superconducting wires have an insulating material such as enamel applied to their outer circumferential surface, and are provided with an insulated structure in which the outer circumferential surface is covered with an insulating layer. In contrast, when the superconducting wire 10 is an uninsulated wire, the contact electrical resistance between the superconducting wires 10 is small, so that when a quench occurs, the superconducting current flowing through the superconducting filaments 11 can escape to the surroundings.
[0044] 1 and 2, the entire superconducting wire 10 forming the coil winding 3 is provided as an uninsulated wire, but only a part of the superconducting wire 10 forming the coil winding 3 may be provided as an uninsulated wire. The superconducting wire 10 whose outer circumferential surface is not covered with an insulating layer may be disposed in only a part of the coil winding 3, such as an area where hot spots are likely to occur.
[0045] Areas where hot spots are likely to occur include the radially inner area of the bobbin 2 where the bending radius of the coil winding 3 is small, and areas on one or the other axial end sides of the bobbin 2 where the superconducting wire 10 transitions to the next layer where magnetic flux is likely to concentrate. By making only a portion of the wire an uninsulated wire, it is possible to efficiently suppress the occurrence of hot spots while reducing losses due to circulating currents circulating between the superconducting wires 10.
[0046] In general, MgB2 and high-temperature superconductors undergo a superconducting transition at a higher temperature than conventional superconductors, and therefore are used with a higher specific heat than conventional superconductors. If the specific heat is large, when a quench occurs due to the application of a disturbance such as strain to the superconductor, the normal conducting region generated by the normal conducting transition does not easily propagate to the surroundings, and hot spots are more likely to occur.
[0047] A hot spot is a phenomenon in which a part of a superconductor undergoes a localized normal conducting transition, resulting in a localized normal conducting region within a superconducting region. When a hot spot occurs in a superconducting wire, supercurrent flows into the localized normal conducting region, generating a large amount of Joule heat. The locally generated excessive Joule heat can cause the superconducting wire to burn out, resulting in a break in the wire or burning of surrounding components.
[0048] If the contact electrical resistance between the sides of a superconducting wire is small, the superconducting current that has flowed into the normal conducting region can escape, preventing problems caused by hot spots. However, even if the superconducting wire is an uninsulated wire, if the superconducting wire is a round wire, it is difficult to ensure a sufficient contact area between the sides of the superconducting wire, making it difficult to sufficiently reduce the contact electrical resistance between the sides, and the superconducting current of several hundred amperes cannot be allowed to bypass the normal conducting region and escape to the surrounding superconducting region.
[0049] On the other hand, if the contact area between the sides of the superconducting wires is secured and the contact electrical resistance between the sides is reduced, problems such as a long relaxation time of the generated magnetic field and energy loss arise. If the contact electrical resistance between the superconducting wires is small, an induced current is generated in the base material of the superconducting wire when the superconducting current is swept, and a circulating current that circulates between the superconducting wires is likely to occur. Circulating currents are characterized by a large time constant. Therefore, the relaxation time until the generated magnetic field stabilizes after the rated current value is reached becomes long, and there is a problem that it takes several hours to start stable operation. In addition, Joule heat and energy loss due to the circulating current become problems.
[0050] Even if the contact area between the side surfaces of the superconducting wire 10 is ensured and the contact electrical resistance between the side surfaces is reduced, the contact thermal resistance between the side surfaces may not be sufficiently reduced. When the coil winding 3 is conductively cooled, it is necessary to reduce the contact thermal resistance between the side surfaces. However, in order to reduce the contact thermal resistance, contact with a certain degree of surface pressure is required. When MgB2 or a high-temperature superconductor is used, there is a problem that the appropriate surface pressure cannot be ensured because of their poor strain resistance.
[0051] Therefore, in the superconducting coil 1, a low melting point metal is filled between the rows of the superconducting wires 10 to provide a low melting point metal layer 8. When a low melting point metal is filled between the rows of the superconducting wires 10, adjacent superconducting wires 10 can be integrated together with the low melting point metal to electrically and thermally connect the superconducting wires 10 to each other and to the surrounding members. Therefore, the contact electrical resistance and contact thermal resistance between the superconducting wires 10 can be reduced more than ever before.
[0052] Providing the low melting point metal layer 8 reduces the contact electrical resistance between the superconducting wires 10, so that when a quench occurs, the superconducting current flowing through the coil winding 3 can be released to the surrounding superconducting regions, bypassing the normal conductive region. Since a conductive path for releasing the superconducting current is formed, the occurrence of hot spots is suppressed, and the generation of excessive Joule heat caused by the superconducting current flowing through the normal conductive region is prevented. Therefore, burning of the superconducting wire 10 can be avoided. In addition, since the contact thermal resistance between the superconducting wires 10 is reduced, the coil winding 3 can be efficiently cooled by conduction while suppressing distortion of the superconducting wire 10.
[0053] Furthermore, when low-melting point metal layer 8 is provided, a circulating current that circulates between superconducting wires 10 is likely to occur, but the lengthening of the relaxation time of the generated magnetic field due to the circulating current and the Joule heat and energy loss due to the circulating current can be suppressed by disposing interlayer insulating material 7 between the layers of superconducting wire 10. Low-melting point metal layer 8 and interlayer insulating material 7 can provide both a measure against hot spots and a measure against circulating currents.
[0054] The porous metal material 6 thermally connects the rows of superconducting wires 10 to each other and between the rows of superconducting wires 10 and the cooling plate 4. The porous metal material 6 is arranged in layers along the axial direction of the bobbin 2 between the layers of superconducting wires 10. The porous metal material 6 is arranged between each layer of superconducting wires 10, radially outward of the inner layer of superconducting wires 10 and radially inward of the interlayer insulating material 7.
[0055] The porous metal material 6 is provided in a sheet shape, and a large number of through holes are formed penetrating the main surface in the thickness direction. The porous metal material 6 is made conductive by using a conductive material with high electrical conductivity. As the porous metal material 6, punching metal, expanded metal, mesh metal, etc. can be used. As the material of the porous metal material 6, copper, copper alloy, aluminum, aluminum alloy, etc. can be used.
[0056] The porous metal material 6 is preferably in contact with and thermally connected to the cooling plate 4 and the flange portion of the bobbin 2. The porous metal material 6 and the cooling plate 4 and the flange portion of the bobbin 2 are preferably in contact with each other by applying a surface pressure of a predetermined level or more. By applying a surface pressure in a compressive direction between the porous metal material 6 and the surrounding members and using a conductive material with high electrical conductivity as the porous metal material 6, it becomes possible to efficiently cool the superconducting wire 10 by utilizing the thermal conduction through the porous metal material 6.
[0057] By providing the porous metal material 6, the rows of superconducting wires 10 are thermally connected to each other and to the cooling plate 4, so that the superconducting wires 10 can be efficiently conductively cooled. Even if Schur heat is generated in the superconducting wires 10 when a quench occurs, the heat can be efficiently dissipated toward the cooling plate 4, so that a temperature rise in the superconducting coil 1 can be suppressed. The porous metal material 6 also has a function of retaining the low-melting point metal in a molten state when the low-melting point metal layer 8 is formed.
[0058] The interlayer insulating material 7 electrically insulates the layers of the superconducting wire 10 from one another. The interlayer insulating material 7 can suppress a circulating current circulating between the layers of the superconducting wire 10. The interlayer insulating material 7 is arranged in layers between the layers of the superconducting wire 10 along the axial direction of the bobbin 2. The interlayer insulating material 7 is arranged between each layer of the superconducting wire 10, radially outward of the porous metal material 6 from the bobbin 2 and radially inward of the outer layer of the superconducting wire 10 from the bobbin 2.
[0059] The interlayer insulating material 7 is made of an insulating material with high electrical resistivity. Examples of the interlayer insulating material 7 that can be used include a resin film, a resin sheet, a glass fiber sheet made of molded glass fiber, and a glass cloth made of woven glass. Examples of the resin that can be used include insulating resins such as polyimide and heat-resistant epoxy resin.
[0060] By providing the interlayer insulating material 7, the layers of the superconducting wire 10 are electrically insulated from each other, so that the cross-sectional area of the conductive path can be reduced and the electrical resistance between the layers of the superconducting wire 10 can be increased. This makes it possible to reduce the time constant of the circulating current circulating between the superconducting wires 10. This shortens the relaxation time until the generated magnetic field stabilizes after the rated current value is reached, and the superconducting coil 1 can be started in a short time. In addition, it is possible to suppress Joule heat and energy loss due to the circulating current while forming a conductive path that allows the superconducting current to escape during a quench.
[0061] The low-melting point metal layer 8 electrically and thermally connects the rows of superconducting wires 10 to each other and to surrounding members. The low-melting point metal layer 8 is formed of a low-melting point metal having a melting point of 300° C. or less. The low-melting point metal layer 8 is formed by attaching a low-melting point metal to the periphery of the layer of superconducting wire 10 while winding the superconducting wire 10, melting the low-melting point metal to fill the space around the superconducting wire 10, and then solidifying the molten low-melting point metal.
[0062] 2, the low-melting point metal layer 8 is disposed between each layer of the superconducting wire 10, radially outward of the outer circumferential surface of the superconducting wire 10 and radially inward of the bobbin 2 relative to the porous metal material 6. The low-melting point metal layer 8 as shown in FIG. 2 can be formed by applying a fluid material such as a solder paste containing a low-melting point metal only to the outer surface of each layer of the superconducting wire 10.
[0063] 2, the low-melting point metal layer 8 is filled in the space around the superconducting wire 10 and is formed at least on the radial outside of the bobbin 2 between the rows of the superconducting wire 10. When the low-melting point metal is filled between the rows of the superconducting wire 10, the rows of the superconducting wire 10 can be electrically and thermally connected to each other by the low-melting point metal layer 8 while the layers of the superconducting wire 10 are insulated from each other by the interlayer insulating material 7. Nearby sections of the superconducting wire 10 constituting the same row are electrically and thermally connected to each other, so that measures against hot spots and circulating currents can be efficiently achieved at the same time.
[0064] The low-melting-point metal layer 8 can be formed of a low-melting-point metal that has a melting point of 300°C or less and is a good conductor with high electrical conductivity. If the melting point is 300°C or less, it can be melted at a relatively low temperature and filled into the space around the superconducting wire 10. Therefore, it can be electrically and thermally connected to the surrounding members without any gaps, and the surrounding members, particularly the coil insulating material 5 and the interlayer insulating material 7, can be prevented from being thermally decomposed or burned due to high temperatures. In addition, when MgB2 is used, it is possible to avoid an unintended reaction of generating MgB2 that occurs at high temperatures of 500°C or more.
[0065] Examples of the material for the low melting point metal 8 include tin, indium, and multi-element alloys such as a tin alloy, an indium alloy, a lead alloy, and a gold alloy, each of which contains at least one of tin, indium, lead, gold, silver, copper, nickel, antimony, and bismuth. Specific examples of the alloy include a tin-lead alloy, a tin-antimony alloy, a tin-bismuth alloy, a tin-copper alloy, a tin-indium alloy, a tin-silver alloy, a tin-gold alloy, a lead-silver alloy, a tin-lead-antimony alloy, a tin-lead-bismuth alloy, a tin-lead-copper alloy, a tin-lead-silver alloy, a tin-silver-copper alloy, and a gold-lead alloy.
[0066] The resin layer 9 thermally connects the superconducting wires 10 to each other and to the surrounding members. The resin layer 9 is made of a resin material such as an epoxy resin. The resin layer 9 can be formed by impregnating the superconducting coil 1 on which the low melting point metal layer 8 is formed with resin, filling the space around the superconducting wires 10 and the low melting point metal layer 8 with the resin, and then curing the resin. By filling with a thermosetting resin, it is possible to harden it by heat treatment.
[0067] 2, the resin layer 9 is disposed between each layer of the superconducting wire 10, radially outward of the interlayer insulating material 7 and radially inward of the outer peripheral surface of the superconducting wire 10. The resin layer 9 can fill not only the space around the superconducting wire 10 but also voids inside the superconducting coil 1, such as a gap between the bobbin 2 and other members and a gap between the cooling plate 4 and other members.
[0068] By providing the resin layer 9, the space around the superconducting wire 10 is filled with resin, reducing voids inside the coil winding 3, thereby improving the thermal conductivity of the coil winding 3. Furthermore, the superconducting wire 10 is fixed by the resin layer 9, reducing distortion of the superconducting wire 10 that may cause quenching. Furthermore, by using a resin with high electrical resistivity, the circulating current circulating between the superconducting wires 10 can be suppressed.
[0069] In such a superconducting coil 1, the rows of the superconducting wires 10 are electrically and thermally connected to each other by the low melting point metal, and the layers of the superconducting wires 10 are electrically insulated from each other by the insulating material, so that the occurrence of hot spots can be suppressed and the circulating current circulating between the superconducting wires can be suppressed. Therefore, it is possible to prevent the superconducting wires 10 from burning due to hot spots, to lengthen the relaxation time of the magnetic field generated by the circulating current, and to reduce Joule heat and energy loss due to the circulating current. In addition, the low melting point metal and the porous metal material can improve the heat removal performance in the axial direction of the bobbin 2. In addition, the contact electrical resistance and contact thermal resistance between the rows of the superconducting wires 10 are reduced, so that it is possible to adopt a round wire as the superconducting wire 10.
[0070] Therefore, according to such a superconducting coil 1, in the coil winding in which the superconducting wire is wound, it is possible to provide a conduction-cooled superconducting coil that is unlikely to burn out the superconducting wire and can form a stable magnetic field in a short period of time by achieving both suppression of the circulating current flowing between the superconducting wires and efficient conduction cooling of the superconducting wire, regardless of the cross-sectional shape of the superconducting wire.
[0071] FIG. 3 is a diagram showing an example of a method for manufacturing a superconducting coil according to an embodiment of the present invention. As shown in Figure 3, the superconducting coil 1 shown in Figures 1 and 2 can be manufactured by using a solder paste containing a low-melting point metal that forms the low-melting point metal layer 8, a metal sheet that is the porous metal material 6, and an insulating material that is the interlayer insulating material 7, and by melting the low-melting point metal by heat treatment to fill the space.
[0072] When forming the superconducting coil 1, first, the superconducting wire 10 is wound around the bobbin 2 in a solenoid shape to form one layer of the superconducting wire 10 (step S10). By winding the superconducting wire 10 around the bobbin 2 along the axial direction of the bobbin 2, one layer of the superconducting wire 10 is wound.
[0073] Next, a low-melting metal having a melting point of 300° C. or less is applied to the surface of the layer of superconducting wire 10 (step S11). The process of applying the low-melting metal can be performed by applying a solder paste containing the low-melting metal. The low-melting metal is applied to at least the radially outer surface of the layer of superconducting wire 10 of bobbin 2.
[0074] The solder paste may be a semi-liquid material in a slurry or cream form that contains a particulate low melting point metal and any type of flux. As the flux, various materials may be used, such as resin materials such as rosin, epoxy resin, polyimide resin, polyamide resin, acrylic resin, and polyester resin, and rubber materials such as isoprene rubber and styrene butadiene rubber. The flux may contain any type of solvent or activator.
[0075] Next, a metal sheet, which is a porous metal material 6, is arranged around the low melting point metal attached to the superconducting wire 10 (step S12). A flexible sheet material, a plate material previously formed into a curved or cylindrical shape, or the like can be used as the porous metal material 6. Such a porous metal material 6 can be arranged or wound so as to cover the outer surface of the low melting point metal attached to the superconducting wire 10.
[0076] By arranging the porous metal material 6, when the low melting point metal is melted, the low melting point metal can be held by the pores. If the bobbin 2 is placed vertically, there is a risk that the low melting point metal attached to the periphery of the superconducting wire 10 will flow down due to gravity. In contrast, if the porous metal material 6 is arranged so as to cover the low melting point metal, the paste can be held in and around the through holes by surface tension or the like, even if the bobbin 2 is placed vertically.
[0077] Next, an insulating material that will become the interlayer insulating material 7 is arranged around the metal sheet that is the porous metal material 6 (step S13). A flexible film material, sheet material, or the like can be used as the interlayer insulating material 7. Such interlayer insulating material 7 can be arranged or wound so as to cover the outer surface of the porous metal material 6 in the radial direction of the bobbin 2.
[0078] Next, it is determined whether the number of layers of the superconducting wire 10 wound around the bobbin 2 has reached a preset number of layers (step S14). The number of layers of the superconducting wire 10 to be wound around the bobbin 2 can be set in advance to an arbitrary value depending on the number of rows of the superconducting wire 10, the upper limit of the current density of the superconducting wire 10, the required strength of the magnetic field to be generated, etc.
[0079] If the result of the determination is that the number of layers has not reached the preset number (step S14; NO), the process returns to step S10. In the subsequent steps, the superconducting wire 10 is wound in a solenoid shape around the insulating material arranged outside the already wound layer of the superconducting wire 10 to form the next layer of the superconducting wire 10. Then, steps S11 to S14 are repeated.
[0080] On the other hand, when the result of the determination indicates that the preset number of layers has been reached (step S14; YES), the process proceeds to step S15. Until it is determined that the preset number of layers has been reached, the process of forming the next layer of superconducting wire 10, the process of attaching low melting point metal, the process of arranging a metal sheet, and the process of arranging an insulating material are performed once or multiple times to form coil winding 3 around bobbin 2.
[0081] Next, the bobbin 2 and the coil winding 3 are heat-treated (step S15). The heat treatment melts the low-melting point metal, and the low-melting point metal fills the spaces between the rows of the superconducting wires 10 and between the rows of the superconducting wires 10 and the surrounding members. The low-melting point metal is then solidified by forced cooling or natural cooling to form the low-melting point metal layer 8.
[0082] The coil winding 3 is heat-treated at a temperature equal to or higher than the melting point of the low-melting-point metal. The heat treatment temperature is preferably 300°C or lower, and is preferably equal to or lower than the heat resistance temperature of the surrounding members such as the insulating material. By suppressing the heat treatment temperature, it is possible to prevent thermal decomposition and scorching of the coil insulating material 5 and the interlayer insulating material 7 when using insulating materials made of general resin materials.
[0083] Next, the bobbin 2 and the coil winding 3 are impregnated with resin (step S16). The resin impregnation can be performed by, for example, a vacuum infusion process (VIP). When the atmosphere is evacuated while the coil winding 3 wound around the bobbin 2 is being impregnated with resin, the voids around the superconducting wire 10 are degassed and the resin permeates the voids. When the permeated thermosetting resin or the like is cured, the superconducting coil 1 having the resin layer 9 formed thereon is obtained.
[0084] According to this manufacturing method, since the solder paste containing the low melting point metal is used, the viscosity of the paste allows the low melting point metal to be attached with high uniformity. Since the low melting point metal layer 8 with high uniformity in thickness can be easily formed, the contact electrical resistance and contact thermal resistance between the rows of the superconducting wires 10 can be stably reduced. Furthermore, since the metal sheet that is the porous metal material 6 is used, the solder paste that may flow down due to gravity can be held in the through holes or around the through holes by surface tension or the like. Since the low melting point metal layer 8 with high uniformity in thickness can be formed regardless of the orientation of the bobbin 2, the contact electrical resistance and contact thermal resistance between the rows of the superconducting wires 10 can be more reliably reduced. Furthermore, since the insulating material such as a film material or sheet material that becomes the interlayer insulating material 7 is used, the layers of the superconducting wires 10 can be more reliably insulated from each other.
[0085] 4A, 4B, and 4C are diagrams showing examples of the form of a porous metal material used in a superconducting coil according to an embodiment of the present invention. In Fig. 4A, 4B, and 4C, the main surface of a porous metal material 6 is enlarged and typically shown. Fig. 4A shows an example of a punched metal. Fig. 4B shows an example of an expanded metal. Fig. 4C shows an example of a mesh metal.
[0086] As shown in Fig. 4A, punched metal 6A as porous metal material 6 is provided in a shape with many through holes punched therein. As shown in Fig. 4B, expanded metal 6B as porous metal material 6 is provided in a shape in which many parallel slits are machined in a staggered pattern in a metal plate and extended in the direction in which the slits open. As shown in Fig. 4C, mesh metal 6C as porous metal material 6 is provided in a shape in which metal wires are formed in a lattice pattern.
[0087] The porous metal material 6 can be provided in any suitable form with a large number of through holes, but it is preferable to use punched metal, expanded metal, mesh metal, etc., in terms of low electrical resistance between both ends, compared to metal fiber sheets, etc. The porous metal material 6 can be provided with any suitable thickness, size of through holes, and number of through holes, as long as it is capable of holding the solder paste and forming a conductive path. The thickness of the porous metal material 6 can be set to, for example, 0.5 mm or more and 2 mm or less.
[0088] Fig. 5 is an enlarged view showing an example of a main part of a superconducting coil according to an embodiment of the present invention, in which a region A surrounded by a dashed line in Fig. 1 is shown in a different form from that in Fig. 2. As shown in FIG. 5, the superconducting coil 1 according to this embodiment can also be provided in a form in which the space around the superconducting wire 10 is filled with only the low-melting point metal layer 8.
[0089] In Figure 5, the low-melting point metal layer 8 is arranged between each layer of the superconducting wire 10, both radially outward of the bobbin 2 from the interlayer insulating material 7 and radially inward of the outer peripheral surface of the superconducting wire 10, and also radially outward of the bobbin 2 from the outer peripheral surface of the superconducting wire 10 and radially inward of the bobbin 2 from the porous metal material 6.
[0090] In this embodiment, a resin layer 9 may or may not be formed between the layers of the superconducting wire 10. For example, only the low melting point metal layer 8 may be filled between the layers of the superconducting wire 10, and the resulting bobbin 2 and coil winding 3 may be impregnated with resin to form the resin layer 9 only in the gaps between the bobbin 2 and other members, the gaps between the cooling plate 4 and other members, and the like.
[0091] According to this embodiment, the contact electrical resistance and contact thermal resistance around the superconducting wire 10 can be reduced by the conduction path provided by the low-melting-point metal layer 8. The low-melting-point metal layer 8 made of a low-melting-point metal is more likely to have high thermal conductivity and electrical conductivity than the resin layer 9 made of a resin. It is also possible to omit or shorten the process of impregnating the bobbin 2 and the coil winding 3 with resin. The resin layer 9 has inferior radiation resistance compared to the low-melting-point metal layer 8, making it advantageous for accelerator applications and the like.
[0092] FIG. 6 is a diagram showing an example of a method for manufacturing a superconducting coil according to an embodiment of the present invention. As shown in FIG. 6, the superconducting coil 1 shown in FIG. 5 can be manufactured by applying a solder paste containing a low melting point metal that forms the low melting point metal layer 8 to both side surfaces of each layer of the superconducting wire 10.
[0093] When forming the superconducting coil 1, similarly to step S10 described above, the superconducting wire 10 is wound around the bobbin 2 in a solenoid shape to form one layer of the superconducting wire 10 (step S20).
[0094] Next, a low-melting-point metal having a melting point of 300° C. or less is applied to the surface of the layer of superconducting wire 10 (step S11). The process of applying the low-melting-point metal can be performed by applying a solder paste containing the low-melting-point metal. The low-melting-point metal is applied to the surface of the layer of superconducting wire 10 on both sides in the radial direction of bobbin 2.
[0095] For example, for the first layer, the low melting point metal can be applied to the outer peripheral surface of the bobbin 2 and the inner surface of the superconducting wire 10 wound around the outer peripheral surface, in addition to the outer peripheral surface of the bobbin 2 in the radial direction of the layer of superconducting wire 10. For the second and subsequent layers, the low melting point metal can be applied to the outer peripheral surface of the insulating material already placed and the inner surface of the superconducting wire 10 wound around the outer peripheral surface, in addition to the outer peripheral surface of the bobbin 2 in the radial direction of the layer of superconducting wire 10.
[0096] Next, similarly to steps S12 to S15 described above, the metal sheet which is the porous metal material 6 is arranged (step S22), the insulating material which becomes the interlayer insulating material 7 is arranged (step S23), it is determined whether or not the preset number of layers has been reached (step S24), and the bobbin 2 and the coil winding 3 are heat-treated (step S25). The low-melting point metal is melted by the heat treatment and then solidified, thereby obtaining the superconducting coil 1 on which the low-melting point metal layer 8 is formed.
[0097] In such a manufacturing method, the process of impregnating the bobbin 2 and the coil winding 3 with resin after the heat treatment (step S25) can be omitted. Alternatively, if necessary, the process of impregnating with resin can be performed by shortening the treatment time, etc.
[0098] According to this manufacturing method, the low-melting point metal layer 8 is formed on both sides of the layer of the superconducting wire 10 in the radial direction of the bobbin 2, so that the electrical contact resistance and the thermal contact resistance around the superconducting wire 10 can be reduced and the resin impregnation process can be omitted or shortened. This simplifies the manufacturing process of the superconducting coil 1. In addition, the heat treatment and the wettability of the low-melting point metal make it possible to manufacture the superconducting coil 1 with reduced voids in a short time without sufficient degassing.
[0099] In addition, between each layer of the superconducting wire 10, a resin layer 9 is arranged in FIG. 2 on the radially outer side of the bobbin 2 than the interlayer insulating material 7 and on the radially inner side of the outer peripheral surface of the superconducting wire 10, and a low melting point metal layer 8 is arranged in FIG. 5, but this space can be a gap that is not filled with resin or low melting point metal. The low melting point metal layer 8 on one side reduces the contact thermal resistance between the rows of the superconducting wire 10, so good heat transfer can be obtained even with a gap. In such a case, the process of impregnating the bobbin 2 and the coil winding 3 with resin and the application of the low melting point metal to both sides can be omitted.
[0100] Fig. 7 is a diagram showing an example of a main part of a superconducting coil according to an embodiment of the present invention, in which a region A surrounded by a dashed line in Fig. 1 is shown in a different form from that in Fig. 2. As shown in FIG. 7, the superconducting coil 1 according to this embodiment can also be configured in such a manner that the coil winding 3 is formed by a plurality of superconducting wires 10, and the superconducting wires 10 are joined together via a low-melting point metal layer 8.
[0101] 7, the coil winding 3 is formed by serially connecting a plurality of superconducting wires 10. The superconducting wires 10 constituting the coil winding 3 are connected to each other at their sides only via a low-melting-point metal layer 8 made of a low-melting-point metal, without using an independent solder.
[0102] When the coil winding 3 is formed by a plurality of superconducting wires 10, the connection portion connecting the superconducting wires 10 can have a structure in which the superconducting wire 10 arranged radially inside the bobbin 2 and the superconducting wire 10 of the next layer arranged radially outside the bobbin 2 relative to the superconducting wire 10 are electrically connected by a low-melting point metal.
[0103] In general, since it is difficult to manufacture a large superconducting coil using a single superconducting wire, it is manufactured by connecting multiple superconducting wires in series by soldering. At the joints that connect the superconducting wires, Joule heat is likely to be generated due to electrical resistance. For this reason, it is common to overlap the superconducting wires by about 20 to 100 mm and solder the sides of the superconducting wires together.
[0104] However, in the conventional method of soldering the sides of overlapping superconducting wires together, it was necessary to secure a structure and space different from other sections of the coil winding in order to perform appropriate soldering. Conventionally, the superconducting wire was surrounded by a gap, and solder was formed only in a certain area. Therefore, the spacing between the wound superconducting wires and the size of the space around the superconducting wire were different between the connection section where the sides of the superconducting wires are arranged so as to be in close contact with each other and the section other than the connection section.
[0105] In contrast, when the superconducting wires 10 are connected via the low-melting metal layer 8, the low-melting metal layer 8 filling the space around the superconducting wires 10 can connect the sides of the superconducting wires 10 together, and therefore, unlike conventional soldering, a connection part that is a continuous structure or space from other sections can be formed. Since multiple superconducting wires 10 can be connected together without excessively changing the spacing between the superconducting wires 10 or the size of the space around the superconducting wires 10, it is possible to suppress an increase in contact resistance, distortion of the superconducting wires 10 that can cause quenching, and friction that generates heat.
[0106] As shown in Fig. 7, the joints for connecting a plurality of superconducting wires 10 together are preferably provided between layers of the superconducting wires 10. When the joints are provided between layers of the superconducting wires 10, the side of another superconducting wire 10 can be connected by a low-melting point metal applied to the radially outer surface of the bobbin 2 of the layer of the superconducting wire 10. Since the formation of the low-melting point metal layer 8 and the connection of the superconducting wires 10 can be combined, a continuous coil winding 3 with small positional deviation can be formed.
[0107] Moreover, it is preferable that the connection portion for connecting the multiple superconducting wires 10 together is provided at either one end or the other end in the axial direction of the bobbin 2. In Fig. 7, the connection portion is provided at the upper end of the bobbin 2. As shown in Fig. 7, at the axial end of the bobbin 2, the axial length of the bobbin 2 of the porous metal material 6 and the interlayer insulating material 7 is shortened and the intervening porous metal material 6 and the interlayer insulating material 7 are removed, so that the sides of the superconducting wires 10 can be easily brought into contact with each other.
[0108] Fig. 8 is a development view showing a connection part of a superconducting coil according to an embodiment of the present invention. Fig. 8 shows a connection part connecting a plurality of superconducting wires 10 shown in Fig. 7 developed from a coil shape, and a part of the development view is extracted. In Fig. 8, reference numeral 10A indicates a superconducting wire 10 located on the radially inner side of the bobbin 2. Reference numeral 10B indicates a superconducting wire 10 located on the radially outer side of the bobbin 2. Reference numeral OL indicates an overlap between the superconducting wire 10A located on the inner side and the superconducting wire 10B located on the outer side.
[0109] As shown in Fig. 8, a connection portion for connecting superconducting wire 10A located inside and superconducting wire 10B located outside is preferably provided at, for example, the upper end in the axial direction of bobbin 2. Fig. 8 mainly illustrates one layer of superconducting wire 10A, superconducting wire 10B connected to this layer, and a part of low-melting point metal layer 8 filled therearound.
[0110] Superconducting wire 10A located on the inside and superconducting wire 10B located on the outside can be connected in an overlap OL where superconducting wire 10A and superconducting wire 10B are partially parallel to each other so as to allow movement between the layers, by integrating their side surfaces with low-melting point metal layer 8. In the overlap OL, the side surface of superconducting wire 10A and the side surface of superconducting wire 10B can be electrically connected only via low-melting point metal layer 8.
[0111] In the overlap OL, the low-melting point metal layer 8 is disposed between each layer of the superconducting wire 10, both radially outward of the interlayer insulating material 7 and radially inward of the outer peripheral surface of the superconducting wire 10, and also radially outward of the bobbin 2 and radially inward of the porous metal material 6. The thickness of the low-melting point metal layer 8 in the overlap OL is preferably equal to the thickness of the low-melting point metal layer 8 in other sections of the coil winding 3.
[0112] The connection of the plurality of superconducting wires 10 to each other via the low-melting point metal layer 8 can be performed by applying a solder paste or the like containing a low-melting point metal to the side surfaces of the superconducting wires 10A and 10B in the overlap OL to adhere the low-melting point metal, and then heat-treating the coil winding 3 to melt and solidify the low-melting point metal. When connection is performed via the low-melting point metal layer 8, the soldering of the superconducting wires 10 to each other can be omitted.
[0113] According to such a connection method, it is not necessary to excessively change the distance between the superconducting wires 10 or the size of the space around the superconducting wires 10, and additional processing of the bobbin 2 and the cooling plate 4 can be omitted. Since the space for connecting the superconducting wires 10 can be easily secured inside the coil winding 3, it is possible to improve the manufacturing efficiency of the large superconducting coil 1 by connecting a plurality of superconducting wires 10 together.
[0114] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible within the scope of the present invention. For example, the present invention is not necessarily limited to having all the configurations of the above embodiment. It is possible to replace a part of the configuration of an embodiment with another configuration, add a part of the configuration of an embodiment to another form, or omit a part of the configuration of an embodiment. [Explanation of symbols]
[0115] 1 Superconducting coil 2 Bobbin 3 Coil Winding 4 Cooling plate 5 Coil insulation 6 Porous metal material 7 Interlayer insulation 8 Low melting point metal layer 9 Resin layer 10 Superconducting wire 11 Superconducting filament 12 Base material
Claims
1. A conduction-cooled superconducting coil having a coil winding in which a superconducting wire is wound around a bobbin in a multi-layer solenoid shape, the coil winding being cooled by thermal conduction using a refrigerator, the coil winding has a plurality of rows of the superconducting wires arranged in an axial direction of the bobbin and a plurality of layers of the superconducting wires stacked in a radial direction of the bobbin, The rows of superconducting wires are electrically and thermally connected to each other by a low-melting-point metal having a melting point of 300° C. or less, A conduction-cooled superconducting coil in which the layers of the superconducting wire are electrically insulated from each other by an insulating material.
2. 2. The conduction-cooled superconducting coil according to claim 1, A conduction-cooled superconducting coil, wherein the cross-sectional shape of the superconducting wire is circular or elliptical.
3. 2. The conduction-cooled superconducting coil according to claim 1, A conduction-cooled superconducting coil in which a part or all of the superconducting wire is an uninsulated wire that is not covered with an insulating layer.
4. 2. The conduction-cooled superconducting coil according to claim 1, A conduction-cooled superconducting coil, wherein the low-melting-point metal is tin, a tin alloy, indium, an indium alloy, a lead alloy, or a gold alloy.
5. 2. The conduction-cooled superconducting coil according to claim 1, A conduction-cooled superconducting coil, wherein the insulating material is a resin film, a resin sheet, a glass fiber sheet, or a braided glass cloth.
6. 2. The conduction-cooled superconducting coil according to claim 1, A conduction-cooled superconducting coil, in which a conductive porous metal material having a large number of through holes is disposed radially outside the bobbin relative to the layer of superconducting wire and radially inside the bobbin relative to the insulating material.
7. 7. The conduction-cooled superconducting coil according to claim 6, A conduction-cooled superconducting coil, wherein the porous metal material is a punched metal, an expanded metal, or a mesh metal.
8. 2. The conduction-cooled superconducting coil according to claim 1, A conduction-cooled superconducting coil in which the superconducting wire and the low-melting-point metal are surrounded by a resin.
9. 2. The conduction-cooled superconducting coil according to claim 1, The coil winding is formed of a plurality of superconducting wires, A conduction-cooled superconducting coil in which a superconducting wire arranged radially inside the bobbin and a superconducting wire of a next layer arranged radially outside the bobbin with respect to the superconducting wire are electrically connected by the low-melting point metal.
10. 2. The conduction-cooled superconducting coil according to claim 1, a conductive porous metal material having pores formed therein is disposed on the outer side of the superconducting wire layer in the radial direction of the bobbin and on the inner side of the insulating material in the radial direction of the bobbin; a cooling plate cooled by the refrigerator is disposed outside one axial end of the bobbin of the coil winding, A conduction-cooled superconducting coil in which the porous metal material and the cooling plate are in contact with each other and thermally connected.
11. A superconducting magnet device comprising the conduction-cooled superconducting coil according to any one of claims 1 to 10.
12. A method for manufacturing a conduction-cooled superconducting coil, the method comprising the steps of: winding a superconducting wire around a bobbin in a multi-layer solenoid shape; and cooling the coil winding by thermal conduction using a refrigerator, the method comprising the steps of: a step of winding the superconducting wire around the bobbin in a solenoid shape to form a layer of the superconducting wire in which a plurality of rows of the superconducting wire are arranged in an axial direction of the bobbin; a step of attaching a low melting point metal having a melting point of 300° C. or less around the superconducting wire; disposing an insulating material on the outside of the low melting point metal; a step of winding the superconducting wire in a solenoid shape around the insulating material to form a next layer of the superconducting wire in which a plurality of rows of the superconducting wire are arranged in the axial direction of the bobbin, and performing the process of depositing the low melting point metal and disposing the insulating material once or a plurality of times to form the coil winding; and heat-treating the coil winding to melt and solidify the low-melting point metal to electrically and thermally connect the rows of superconducting wires together via the low-melting point metal.
Citation Information
Patent Citations
High-temperature superconducting coil and superconducting magnet device
JP2020025014A