Manufacturing method of rail covering structure

The use of a fiber-reinforced prepreg sheet with a curable resin for rail covering structures addresses the challenges of abrasion resistance and workability in existing methods, offering a quick and effective solution for rail corrosion prevention.

JP2024164803APending Publication Date: 2024-11-27SEKISUI CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024030417
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-02-29
Publication Date
2024-11-27

AI Technical Summary

Technical Problem

Existing methods for preventing rail corrosion, such as the tape and aramid fiber construction methods, face issues with abrasion resistance and workability, and require complex processes that are time-consuming and require skilled labor.

Method used

A method for manufacturing a rail covering structure using a fiber-reinforced prepreg sheet with a curable resin, involving steps of applying adhesive, pasting the prepreg sheet, and curing the resin to form a covering layer, with a focus on shortening construction time and improving workability.

Benefits of technology

The method provides a corrosion-resistant and durable rail covering structure that can be easily applied to complex rail shapes within a short time frame, enhancing corrosion prevention and reducing construction time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164803000001_ABST
    Figure 2024164803000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a rail covering structure which is excellent in the effect of preventing rail corrosion and is easy to operate.SOLUTION: A manufacturing method of a rail covering structure 30, which includes a rail 10 and a covering layer 20 that covers a portion of the rail 10, in which the covering layer 20 includes a cured product of a fiber-reinforced prepreg that has a reinforcing member and curable resin, includes: an adhesive application process to apply an adhesive to a work surface of the rail 10; an attachment process to attach a prepreg sheet including the fiber-reinforced prepreg onto the adhesive before the adhesive applied to the construction surface cures; an adhesive curing process in which the adhesive cures after the attachment process; and a covering layer curing process in which the curable resin cures after the attachment process to form the covering layer 20.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a rail covering structure. [Background technology]

[0002] Electricity, which powers trains, flows through the rails. This makes the rails susceptible to corrosion. Even a small amount of rail corrosion can cause the rail to break. For this reason, methods for preventing rail corrosion include, for example, a tape method in which tape is wrapped around the bottom of the rail to prevent the progression of corrosion, and an aramid fiber method in which aramid fiber is wrapped around the bottom of the rail and then impregnated with resin to prevent the progression of corrosion (see Patent Document 1). However, the tape method has a problem in that it has low abrasion resistance, and when the tape is used on-site, the tape deteriorates and the rail corrodes. The aramid fiber method involves impregnating aramid fibers with resin on-site, and so has problems with workability. The aramid fiber method includes a base scraping process, a primer application process, an epoxy resin application process, an aramid fiber attachment process, an epoxy resin topcoat application process, an aramid fiber impregnation process with the resin, and a resin curing process, making the process complicated and requiring the operator to have resin impregnation techniques. As a method for solving the problem of workability, for example, the prepreg sheet method is known. The prepreg sheet method is a method in which a prepreg sheet, in which reinforcing fibers are impregnated with resin, is attached to an object. The prepreg sheet method includes a base surface scraping step, a primer application step, an adhesive application step, a prepreg sheet attachment step, and a resin curing step. The fiber-reinforced prepreg sheet method is used for steel structures such as steel pipes and pedestrian bridges. It is a construction method. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-108768 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in order to apply prepreg sheets to rail corrosion, it is necessary to make the fiber-reinforced prepreg conform to the complex shape of a rail and attach it to that complex shape. In addition, reinforcement and repair of installed rails must be completed in a short period of time. Therefore, an object of the present invention is to provide a method for manufacturing a rail covering structure which is excellent in the effect of preventing corrosion of rails and is easy to operate. [Means for solving the problem]

[0005] The present invention has the following aspects. <1> A method for manufacturing a rail covering structure, comprising: a rail; and a covering layer covering a portion of the rail, the covering layer including a cured product of a fiber-reinforced prepreg having a reinforcing member and a curable resin, the method comprising: A bonding step of bonding a prepreg sheet including the fiber reinforced prepreg to a construction surface of the rail; A method for manufacturing a rail covering structure, comprising: a covering layer curing step of curing the curable resin to form the covering layer after the attaching step. <2> A method for manufacturing a rail covering structure, comprising: a rail; and a covering layer covering a portion of the rail, the covering layer including a cured product of a fiber-reinforced prepreg having a reinforcing member and a curable resin, the method comprising: an adhesive application step of applying an adhesive to the construction surface of the rail; A bonding step of bonding a prepreg sheet including the fiber reinforced prepreg onto the adhesive applied to the application surface before the adhesive hardens; an adhesive curing step of curing the adhesive after the attaching step; A method for manufacturing a rail covering structure, comprising: a covering layer curing step of curing the curable resin to form the covering layer after the attaching step. <3> A method for manufacturing a rail covering structure, comprising: a rail; and a covering layer covering a portion of the rail, the covering layer including a cured product of a fiber-reinforced prepreg having a reinforcing member and a curable resin, the method comprising: An adhesive application step of applying an adhesive to one surface of a prepreg sheet including the fiber reinforced prepreg; an attachment step of applying the adhesive to the construction surface of the rail before the adhesive applied to the prepreg sheet hardens, and attaching the prepreg sheet to the construction surface of the rail; an adhesive curing step of curing the adhesive after the attaching step; A method for manufacturing a rail covering structure, comprising: a covering layer curing step of curing the curable resin to form the covering layer after the attaching step. <4> The time from applying the adhesive to starting to attach the prepreg sheet is 60 minutes or less. <2> or <3> A method for manufacturing a covering structure for a rail according to claim 1. <5> The attaching step includes a degassing operation of pressing the prepreg sheet against the rail to remove air present between the adhesive and the prepreg sheet or between the adhesive and the rail. <2> ~ <4> A method for manufacturing a rail covering structure according to any one of the preceding claims. <6> Further comprising a primer application step of applying a primer to the application surface; <1> ~ <5> A method for manufacturing a rail covering structure according to any one of the preceding claims. Effect of the Invention

[0006] According to the method for manufacturing a rail covering structure of the present invention, construction time can be shortened. [Brief description of the drawings]

[0007] [Figure 1] 1 is a cross-sectional view showing a rail covering structure according to one embodiment of the present invention; [Diagram 2] FIG. 2 is an enlarged view of region s in FIG. [Diagram 3] FIG. 2 is a perspective view showing a flammability test of a coating layer of a rail coating structure according to one embodiment of the present invention. [Figure 4] 1 is a perspective view showing a method for manufacturing a rail covering structure according to one embodiment of the present invention; [Diagram 5] 4A to 4C are cross-sectional views showing a method for manufacturing a rail covering structure according to one embodiment of the present invention. [Figure 6] 4A to 4C are cross-sectional views showing a method for manufacturing a rail covering structure according to one embodiment of the present invention. [Figure 7] FIG. 2 is a cross-sectional view showing an energy ray irradiation device used in a coating layer curing step. [Figure 8] FIG. 2 is a schematic diagram illustrating a measurement method for a fatigue test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will now be described with reference to the drawings. (Rail covering structure) FIG. 1 is a cross-sectional view showing a rail covering structure according to one embodiment of the present invention. In addition, the drawings used in the following explanation may show characteristic parts in an enlarged manner for the sake of convenience in order to make the features easier to understand, and the dimensional ratios of each component may differ from the actual ones.

[0009] As shown in FIG. 1, a rail covering structure 30 includes a rail 10 and a covering layer 20 covering a portion of the rail 10 . The rail 10 has a head portion 11, a web portion 12, and a bottom portion 13. The rail 10 has the bottom portion 13, the web portion 12, and the head portion 11, which are successively arranged vertically from below to above. The cross section of the bottom portion 13 is substantially triangular. The bottom portion 13 has a bottom surface 13a that contacts the installation surface such as the surface of the sleeper, and one bottom upper surface 13b and the other bottom upper surface 13c that are continuous with the bottom surface 13a and rise from one end 13d and the other end 13e of the bottom portion 13. The abdomen 12 has a generally rectangular cross-sectional shape. The abdomen 12 has both side surfaces (one abdomen side surface 12a and the other abdomen side surface 12b) that are continuous with one bottom upper surface 13b and the other bottom upper surface 13c of the bottom 13. The head 11 has a substantially rectangular cross-sectional shape.

[0010] In this embodiment, the coating layer 20 covers the bottom surface 13a, the ends 13d and 13e, the bottom upper surfaces 13b and 13c, and parts of the rail web portions 12a and 12b. That is, the coating layer 20 covers the bottom portion 13 and parts of the web portion 12. In the present invention, the coating layer 20 only needs to cover the bottom surface 13a and not the head portion 11, and may not cover all or part of the web portion side surfaces 12a and 12b, or all or part of the bottom upper surfaces 13b and 13c. However, from the viewpoint of further enhancing the corrosion prevention effect, it is preferable that the coating layer 20 covers all or part of the bottom portion 13 and the web portion. The covering layer 20 may cover not only the rail 10 but also any portion where corrosion due to electricity (galvanic corrosion) is expected to occur.

[0011] 2, the adhesive layer 18 is located between the rail 10 and the covering layer 20. By having the adhesive layer 18, the covering layer 20 can be adhered to the rail 10 more firmly. The rail 10 and the covering layer 20 may be in direct contact with each other without the adhesive layer 18 therebetween.

[0012] In this embodiment, the covering layer 20 has no space between it and the rail 10. In the present invention, the covering layer 20 may have a space between a part of it and the rail 10. However, in order to more effectively prevent the intrusion of water or air between the rail 10 and the covering layer 20, it is preferable that the covering layer 20 has no space between it and the rail 10.

[0013] The covering layer 20 is a cured product of a prepreg sheet. The prepreg sheet has a fiber-reinforced prepreg. That is, the covering layer 20 is formed by curing a curable resin of the fiber-reinforced prepreg. The prepreg sheet is adhered to the rail 10 and hardens, blocking contact with air and water and preventing corrosion of the rail 10. At the same time, the hardened prepreg sheet and the rail 10 are integrated, reinforcing the strength of the rail 10.

[0014] The coating layer 20 is preferably transparent. If the coating layer 20 is transparent, the remaining air can be visually confirmed during the deaeration operation, and the state of corrosion on the surface of the rail 10 can be easily visually confirmed. Here, being transparent means that visible light passes through to such an extent that the surface of the rail 10 can be seen, for example, 20% or more of visible light passes through.

[0015] The coating layer 20 has a basis weight of 1500 g / m 2 More than 3500g / m 2 Less than 2000 g / m is preferable. 2 More than 3000g / m 2 The following is more preferable. When the basis weight is equal to or more than the above lower limit, the corrosion resistance can be further improved. When the basis weight is equal to or less than the above upper limit, the flexibility of the prepreg sheet constituting the covering layer 20 is increased, and the covering layer 20 can more easily conform to the construction surface (the area where the covering layer is provided).

[0016] The thickness t20 of the covering layer 20 is preferably 3.0 mm or less, more preferably 2.0 mm or less. When the thickness t20 is equal to or less than the above upper limit, the flexibility of the prepreg sheet constituting the covering layer 20 is increased, and the covering layer 20 can more easily conform to the construction surface. The thickness t20 of the coating layer 20 is preferably 1.0 mm or more, and more preferably 1.5 mm or more. When the thickness t20 is equal to or more than the above lower limit, the corrosion resistance can be further improved.

[0017] The covering layer 20 may be a single continuous sheet, or a combination of two or more sheets. In order to simplify the process of attaching the covering layer 20 to the rail 10, it is preferable that the covering layer 20 be a single continuous sheet.

[0018] The covering layer 20 (that is, the cured product of the prepreg sheet) preferably has flame retardancy as determined by a flammability test for railway vehicles, and more preferably is non-flammable. During maintenance and inspection, the rail head is scraped with a grinding vehicle, and the fiber reinforced prepreg is exposed to sparks. Therefore, the coating layer 20 needs to be flame retardant or higher (it does not burn when the source of fire is far away) when attached to the iron (rail).

[0019] The flammability test for railway vehicles will now be explained. Flammability tests for railway vehicles are conducted in accordance with the methods described in "Guide to Flammability Tests of Materials for Railway Vehicles - Flammability Tests - JRMA (Japan Railway Rolling Stock and Machinery Association)." The combustion test (non-metallic materials for railway vehicles) method is as shown in Figure 3, in which a B5 test material (182 mm x 257 mm) 110 is held at a 45° incline and placed on a stand 130 made of a material with low thermal conductivity such as cork so that the center of the bottom of the fuel container 120 is 25.4 mm (1 inch) vertically below the center of the underside (burning surface) of the test material 110, 0.5 mL of pure ethyl alcohol is poured into the fuel container 120 and ignited, and the pure ethyl alcohol is left to burn out. The combustion judgment is made separately during and after the combustion of the pure ethyl alcohol. During the combustion of the pure ethyl alcohol, the ignition, flame, smoke generation, flame state, etc. of the test material 110 are observed. After the combustion of the pure ethyl alcohol, the residual flame, residual dust, carbonization, and deformation state are investigated. When the test material 110 is a hygroscopic material, the pre-test treatment of the test material 110 is as follows: cut to a specified size, place it in a well-ventilated room away from direct sunlight, at least 1 m away from the floor, and leave it for at least 5 days. The conditions in the test room are temperature: 15℃~30℃, humidity: 60%~75%, and no air movement.

[0020] The resistance value (DC insulation resistance value) measured by the DC insulation resistance test (under the following measurement conditions) of JIS E 1203:2007 in the coating layer 20 (i.e., in the state in which the resin of the fiber-reinforced prepreg is cured) is 5×10 6 Ω or more, 5×10 8Ω or more is preferable, 5×10 10 Ω or more is more preferable. If the DC insulation resistance value is equal to or greater than the above lower limit, it is possible to prevent current from passing from the rail 10 to the ground, and to prevent corrosion of the rail 10 due to current. There is no particular limit to the upper limit of the DC insulation resistance value. The DC insulation resistance value is adjusted by a combination of the types of curable resin and reinforcing members of the prepreg sheet, the thickness of the covering layer 20, and the like.

[0021] <Measurement conditions> Applied voltage: 500V DC x 1 min. Conditioning: 20℃ x 48 hours. Test equipment: High Resistance Meter 4339B (Agilent Technologies). Test specimen: Width 20mm x Length 40mm x Thickness 1.5mm.

[0022] The voltage (AC breakdown voltage) measured in the covering layer 20 by the AC breakdown voltage test of JIS C 2110-1:2016 (measurement conditions below) is preferably 20 kV or more, more preferably 30 kV or more, and even more preferably 40 kV or more. When the AC breakdown voltage is equal to or more than the lower limit, it is possible to prevent current flow from the rail 10 to the ground and prevent corrosion of the rail 10 due to current. The upper limit of the AC breakdown voltage is not particularly limited. The AC insulation resistance value is adjusted by a combination of the types of the curable resin and reinforcing member of the prepreg sheet, the thickness of the covering layer 20, and the like.

[0023] <Measurement conditions> (conditions) Test atmosphere: in oil. Temperature: 23℃. Test equipment: AC / DC insulation breakdown tester, YST-243AT-100 type. Boost speed: 3kV / sec.

[0024] The voltage (DC breakdown voltage) measured in the covering layer 20 by the DC breakdown voltage test of JIS C 2110-2:2016 (measurement conditions below) is preferably 15 kV or more, more preferably 30 kV or more, and even more preferably 40 kV or more. If the DC breakdown voltage is equal to or more than the lower limit, the passage of electricity from the rail 10 to the ground can be prevented, and corrosion of the rail 10 due to the current can be better prevented. The upper limit of the DC breakdown voltage is not particularly limited. The DC breakdown voltage is adjusted by a combination of the types of the curable resin and reinforcing member of the prepreg sheet, the thickness of the covering layer 20, and the like.

[0025] <Measurement conditions> Test atmosphere: in oil. Temperature: 23℃. Test equipment: AC / DC insulation breakdown tester, YST-243AT-100 type. Boost speed: 5kV / sec.

[0026] The coating layer 20 has a water permeability of preferably 0.15 g or less, more preferably 0.10 g or less, and even more preferably 0.05 g or less, as measured by the water permeability test for anticorrosive coating layers in Appendix F of JIS A 7502-2:2015. If the water permeability is equal to or greater than the lower limit, the contact of water with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be better prevented. The lower limit of the water permeability is not particularly limited. This water permeability is adjusted by a combination of the types of curable resin and reinforcing members of the prepreg sheet, the thickness of the coating layer 20, and the like.

[0027] To determine the water permeability of the coating layer 20 as specified in Appendix F of JIS A 7502-2, a test specimen is prepared according to the method described in "a) In the case of the applied lining method" in "F3.2 Preparation of test specimen" of Appendix F. Specifically, the test specimen was a flexible plate (a regular octagon inscribed in a circle with a thickness of 6 mm and a diameter of 150 mm) specified in JIS A 5430, on which the coating layer 20 was laminated.

[0028] Using this test specimen, a water permeability test is performed at a water pressure of 0.29 MPa for 1 hour in accordance with "7.6 (water permeability test)" of JIS A 1404. The mass difference (p2-p1) between the mass p1 of the flexible plate before the water permeability test and the mass p2 of the flexible plate after the water permeability test is wiped off is defined as the water permeability of the coating layer 20.

[0029] The coating layer 20 has a chloride ion blocking ability of 1.0×10 as measured by the quality standard for surface protection work, "medium corrosion protection type C." -3 mg / cm 2 ·days or less is preferable, 0.9×10 -3 mg / cm 2 Days or less is preferable, and 0.8×10 -3 mg / cm 2 When the chloride ion blocking property is equal to or less than the above upper limit, the contact of salt with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be prevented more effectively. The lower limit of the chloride ion blocking property is not particularly limited, but is substantially 0.7×10 -3 mg / cm 2 The chloride ion blocking property is adjusted by combining the types of curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, and the like. The "Quality standard for surface protection work, Medium corrosion protection type C" is the quality standard for surface protection work, "Medium corrosion protection type C" in Part 2 Concrete structures, Volume 2 Surface protection guidelines for concrete structures, Hanshin Expressway Co., Ltd., "Guidelines for repairing road structures," (July 2018).

[0030] The coating layer 20 has an oxygen barrier property of 1.00 mol / m as measured by the quality standard for surface protection work, "medium corrosion protection type C." 2 · years or less is preferable, 0.10 mol / m 2 Less than 0.05 mol / m is preferable. 2 It is even more preferable that the oxygen barrier property is equal to or less than one year. When the oxygen barrier property is equal to or less than the above upper limit, contact of oxygen with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be prevented more effectively. The lower limit of the oxygen barrier property is not particularly limited. The oxygen barrier property is adjusted by a combination of the types of the curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, etc.

[0031] In the covering layer 20, the amount of wear measured under the following measurement conditions using an apparatus described in JIS A 1452:2015 is preferably smaller than the amount of wear of a mortar plate. Such an amount of wear can further increase the durability of the covering layer 20. This amount of wear is adjusted by a combination of the types of curable resin and reinforcing member of the prepreg sheet, the thickness of the covering layer 20, and the like.

[0032] <Measurement conditions> -Specimen size: 50mm x 50mm. Number of samples: n=3 each. Abrasive material: Silicon carbide abrasive 2C as specified in JIS R 6111, 4.1.2, Table 6. Fall height: 65cm Total fall weight: 10kg.

[0033] The main wear amount of the coating layer 20 is preferably 30% by mass or less of the wear amount of the mortar plate, more preferably 20% by mass or less, and further preferably 10% by mass or less. The smaller the amount of wear of the coating layer 20, the more the deterioration of the coating layer 20 caused by wear between the coating layer 20 and flying pebbles and sand is suppressed.

[0034] In the coating layer 20, the amount of wear in the JIS K 7204 wear test is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0.1% by mass or less. When the amount of wear is equal to or less than the upper limit, durability can be further improved. The lower limit of the amount of wear is not particularly limited. This amount of wear is adjusted by a combination of the types of curable resin and reinforcing member of the sheet for preventing rail corrosion, the thickness of the coating layer 20, and the like.

[0035] It is preferable that the coating layer 20 has no abnormalities on the impact surface measured under the following conditions in accordance with the bending and impact test methods for building boards of JIS A 1408:2017.

[0036] <Measurement conditions> - Method of specimen placement: S1: Full support on sand. Weight classification: spherical weight: W2-1000. Weight fall height: 50cm.

[0037] The adhesive layer 18 is a cured product of an adhesive. When the covering layer 20 is transparent, it is preferable that the adhesive layer 18 is transparent. If the adhesive layer 18 is transparent, the remaining air can be visually confirmed during the degassing operation, and the corrosion state of the surface of the rail 10 can be easily visually confirmed.

[0038] The thickness t18 of the adhesive layer 18 (i.e., the distance from the surface of the rail 10 to the covering layer 20) is determined taking into consideration the type of adhesive, etc., and is, for example, preferably 0.1 to 1.5 mm, more preferably 0.1 to 0.5 mm. When the thickness t18 is equal to or greater than the above lower limit, the covering layer 20 can be more firmly adhered to the rail 10. When the thickness t18 is equal to or less than the above upper limit, the adhesive can be hardened more quickly, thereby shortening the construction time.

[0039] The resistance value (DC insulation resistance value) measured in the DC insulation resistance test (measurement conditions below) of the adhesive layer 18 (cured product of the adhesive) according to JIS E 1203:2007 is 5×10 6 Ω or more is preferable, 5×10 8 Ω or more is preferable, 5×10 10 Ω or more is more preferable. When the ends of two prepreg sheets are butted together to form a joint of the covering layer 20, a part of the adhesive layer 18 may leak at this joint. If the DC insulation resistance value of the adhesive layer 18 is equal to or greater than the above lower limit, even if the adhesive layer 18 is exposed, it is possible to prevent current from passing from the rail 10 to the ground, and to more effectively prevent corrosion of the rail 10 due to current. There is no particular limit to the upper limit of the DC insulation resistance value of the adhesive layer 18. The DC insulation resistance value is adjusted by the type of adhesive of the adhesive layer 18. <Measurement conditions> ·Applied voltage: 500V DC x 1min. Conditioning: 20℃ x 48 hours. Test equipment: High Resistance Meter 4339B (Agilent Technologies). The adhesive was cured to create a 5mm thick plate, which was then cut to create a test specimen measuring 20mm wide x 40mm long x 5mm thick. Two φ5mm holes were drilled in the centre of the test specimen before measurements were taken.

[0040] The voltage (AC breakdown voltage) measured in the adhesive layer 18 by the AC breakdown voltage test of JIS C 2110-1:2016 (measurement conditions below) is preferably 20 kV or more, more preferably 30 kV or more, and even more preferably 40 kV or more. If the AC breakdown voltage is equal to or greater than the lower limit, even if the adhesive layer 18 is exposed, it is possible to prevent current flow from the rail 10 to the ground and prevent corrosion of the rail 10 due to current. The upper limit of the AC breakdown voltage is not particularly limited. The DC insulation resistance value is adjusted by a combination of the type of adhesive of the adhesive layer 18, the thickness t18 of the adhesive layer 18, and the like.

[0041] The voltage (DC breakdown voltage) of the adhesive layer 18 measured by the DC breakdown voltage test of JIS C 2110-2:2016 is preferably 15 kV or more, more preferably 30 kV or more, and even more preferably 40 kV or more. If the DC breakdown voltage is equal to or more than the lower limit, even if the adhesive layer 18 is exposed, the passage of electricity from the rail 10 to the ground can be prevented, and corrosion of the rail 10 due to the current can be better prevented. The upper limit of the DC breakdown voltage is not particularly limited. The AC breakdown voltage is adjusted by a combination of the type of adhesive of the adhesive layer 18, the thickness t18 of the adhesive layer 18, and the like.

[0042] The adhesive layer 18 has a water permeability of preferably 0.15 g or less, more preferably 0.10 g or less, and even more preferably 0.05 g or less, as measured by the water permeability test for anticorrosive coating layers in Appendix F of JIS A 7502-2:2015. If the water permeability is equal to or greater than the lower limit, even if the adhesive layer 18 is exposed, contact of water with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be better prevented. The lower limit of the water permeability is not particularly limited. This water permeability is adjusted by a combination of the type of adhesive of the adhesive layer 18, the thickness t18 of the adhesive layer 18, and the like.

[0043] The adhesive layer 18 has a chloride ion blocking property of 1.0×10 -3 mg / cm 2 ·days or less is preferable, 0.9×10 -3 mg / cm 2 Days or less is preferable, and 0.8×10 -3 mg / cm 2 When the chloride ion blocking property is equal to or less than the above upper limit, the contact of salt with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be prevented more effectively. The lower limit of the chloride ion blocking property is not particularly limited, but is substantially 0.7×10 -3 mg / cm 2 The chloride ion blocking property is adjusted by a combination of the type of adhesive in the adhesive layer 18, the thickness t18 of the adhesive layer 18, and the like.

[0044] The adhesive layer 18 has an oxygen barrier property of 1.00 mol / m as measured by the quality standard for surface protection work, "medium corrosion protection type C." 2 · years or less is preferable, 0.10 mol / m 2 Less than 0.05 mol / m is preferable. 2 It is even more preferable that the oxygen barrier property is equal to or less than 1 year. When the oxygen barrier property is equal to or less than the above upper limit, even if the adhesive layer 18 is exposed, the contact of oxygen with the surface of the rail 10 can be prevented, and corrosion of the rail 10 can be prevented more effectively. The lower limit of the oxygen barrier property is not particularly limited. The oxygen barrier property is adjusted by a combination of the type of adhesive of the adhesive layer 18, the thickness t18 of the adhesive layer 18, etc.

[0045] A primer layer may be provided between the adhesive layer 18 and the rail 10. By providing the primer layer, the adhesive layer 18 and the rail 10 can be bonded more firmly. The adhesive layer 18 may not be provided, and only a primer layer may be provided between the rail 10 and the covering layer 20. By providing the primer layer, stronger adhesion can be achieved compared to the case where only the covering layer 20 is provided.

[0046] (Method of manufacturing rail covering structure) The method for manufacturing the rail covering structure of this embodiment involves attaching a prepreg sheet to a rail via an adhesive, curing the attached prepreg sheet to form the covering layer 20, and curing the adhesive to form an adhesive layer.

[0047] The prepreg sheet is an uncured resin sheet that includes a reinforcing member and a curable resin. In the prepreg sheet, the curable resin impregnates the reinforcing member. The prepreg sheet may be made of only fiber-reinforced prepreg, or may have a layer (optional layer) other than the fiber-reinforced prepreg. The optional layers include a primer layer, an adhesive layer, a paint layer, and the like.

[0048] Examples of the reinforcing member include inorganic fibers such as glass fibers, organic fibers such as vinylon fibers, and metal fibers such as carbon fibers and steel fibers. Among these, glass fibers are preferred as the reinforcing member from the viewpoint of improving insulation properties.

[0049] The form of the fiber is not particularly limited, and examples thereof include a form in which fibers such as tow, cloth, chopped fiber, and continuous fiber are aligned in one direction; a form in which continuous fibers are woven in the warp and weft directions; a form in which the direction of the tow is aligned in one direction and held by auxiliary weft threads; a form in which a plurality of fiber sheets in which the direction of the fibers is aligned in one direction are overlapped and stitched together with auxiliary threads so that the directions of the fibers are different; and a form in which the fibers are nonwoven. Among these, nonwoven fabrics are preferred from the viewpoint of isotropic arrangement of the fibers.

[0050] Among them, a chopped strand mat of glass fiber is suitable as the reinforcing member, since the use of the chopped strand mat as the reinforcing member can improve the insulation property and the flexibility.

[0051] The content of the reinforcing member is preferably 10 to 35 mass%, more preferably 15 to 30 mass%, and even more preferably 18 to 23 mass%, based on the total mass of the fiber-reinforced prepreg. When the content of the reinforcing member is equal to or more than the lower limit, the strength and durability of the prepreg sheet can be further increased. When the content of the reinforcing member is equal to or less than the upper limit, the flexibility of the prepreg sheet can be further increased.

[0052] Examples of the curable resin include photocurable resins, thermosetting resins, etc. Among them, from the viewpoint of facilitating application, photocurable resins are preferred as the curable resin. Examples of the photocurable resin include photocurable vinyl ester resin, photocurable unsaturated polyester resin, photocurable epoxy resin, etc. Among these, photocurable vinyl ester resin is preferred from the viewpoint of corrosion resistance.

[0053] The content of the curable resin is preferably 65 to 90 mass%, more preferably 70 to 85 mass%, and even more preferably 77 to 82 mass%, based on the total mass of the fiber reinforced prepreg. When the content of the curable resin is equal to or more than the lower limit, the flexibility of the prepreg sheet can be further increased. When the content of the curable resin is equal to or less than the upper limit, the content of the reinforcing member can be increased, and the strength and durability of the prepreg sheet can be further increased.

[0054] The weight of the prepreg sheet is 1500g / m 2 More than 3500g / m 2 Less than 2000 g / m is preferable. 2 More than 3000g / m 2 The following is more preferable. When the basis weight is equal to or more than the above lower limit, the corrosion resistance can be further improved. When the basis weight is equal to or less than the above upper limit, the flexibility of the prepreg sheet is increased, and the sheet can more easily conform to the construction surface.

[0055] The thickness of the prepreg sheet is preferably 3.0 mm or less, more preferably 2.0 mm or less. When the thickness is equal to or less than the upper limit value, the flexibility of the prepreg sheet is increased, and the prepreg sheet can more easily conform to the construction surface. The thickness of the prepreg sheet is preferably 1.0 mm or more, and more preferably 1.5 mm or more. When the thickness of the prepreg sheet is equal to or more than the above lower limit, the corrosion resistance can be further improved.

[0056] Next, an example of a method for manufacturing a rail covering structure will be described. The manufacturing method for the rail covering structure of this embodiment includes a step of applying a primer to the construction surface of the rail (hereinafter referred to as "step A1"), a step of applying an adhesive to the construction surface via the primer (hereinafter referred to as "step B1"), a step of attaching a prepreg sheet to the construction surface to which the adhesive has been applied (hereinafter referred to as "step C1"), a step of curing the curable resin of the prepreg sheet to form a covering layer (hereinafter referred to as "step D1"), and a step of curing the adhesive (hereinafter referred to as "step E1").

[0057] The adhesive is preferably a two-liquid adhesive. Examples of two-liquid adhesives include epoxy resin adhesives, vinyl ester resin adhesives, and unsaturated polyester resin putty containing glass fiber. Among these, vinyl ester resin adhesives are preferred from the viewpoints of corrosion resistance and shortening the curing time.

[0058] In the manufacturing method of the rail covering structure of the present embodiment, it is preferable to carry out surface preparation (surface treatment) on the surface of the rail 10, particularly the surface to be worked on, to remove rust prior to step A1.

[0059] Examples of the method for preparing the base include scraping with a grinder or sandpaper. Regardless of whether the rail is new or existing, scraping types 1 to 4 may be appropriately selected according to the condition of the rail. From the viewpoint of adhesion, scraping types 1 or 2 may be used.

[0060] "Process A1" Step A1 is a primer application step. In step A1, a primer is applied to the construction surface of the rail 10. In detail, the primer is applied to both side surfaces (one side surface 12a and the other side surface 12b) of the abdominal portion 12 of the rail 10, one boundary 12c and the other boundary 12d between the abdominal portion 12 and the bottom portion 13, the bottom surface 13a of the bottom portion 13 of the rail 10, one bottom upper surface 13b and the other bottom upper surface 13c of the bottom portion 13 of the rail 10, and one end 13d and the other end 13e of the bottom portion 13 of the rail 10. Note that the "construction surface" may include at least the bottom surface 13a.

[0061] The method for applying the primer to the surface to be applied is not particularly limited, but for example, a brush application method, a roller application method, a spray application method, etc. can be used.

[0062] The amount of primer applied is 0.05 kg / m per unit area of ​​the application surface. 2 More than 0.25kg / m 2 Less than 0.1 kg / m is preferable. 2 More than 0.2kg / m 2 The following is more preferable. If the amount of primer applied is equal to or greater than the above lower limit, the adhesion between the rail 10 and the adhesive can be improved. If the amount of primer applied is equal to or less than the above upper limit, the primer can be applied more uniformly to the object.

[0063] Examples of the primer include an epoxy resin-based primer, a urethane resin-based primer, a polyester resin-based primer, a polypropylene resin-based primer, etc. Among these, the urethane resin-based primer is preferred from the viewpoint of workability. The primer may be of the wet curing type or the room temperature curing type, but from the viewpoint of workability on site, the wet curing type is preferable. After applying the primer, leave it to cure until it is no longer tacky.

[0064] "Process B1" Step B1 is an adhesive application step. In step B1, adhesive is applied to the construction surface via the primer applied in step A1. In this embodiment, adhesive is applied via the primer to both side surfaces (one side surface 12a and the other side surface 12b) of the inner portion 12 of the rail 10, the bottom surface 13a of the bottom portion 13 of the rail 10, and one bottom upper surface 13b and the other bottom upper surface 13c of the bottom portion 13 of the rail 10.

[0065] The method for applying the adhesive to the application surface is not particularly limited, but for example, a brush application method, a spray application method, etc. can be used.

[0066] The amount of adhesive applied is 0.05 kg / m per unit area of ​​the application surface. 2 More than 0.25kg / m 2 Less than 0.1 kg / m is preferable. 2 More than 0.2kg / m 2 The following is more preferable. If the amount of adhesive applied is equal to or more than the above lower limit, the surface of the rail 10 and the covering layer 20 can be more firmly bonded. If the amount of adhesive applied is equal to or less than the above upper limit, workability is improved.

[0067] "Process C1" Step C1 is an attachment step. In step C1, a prepreg sheet is attached onto the adhesive applied to the application surface before the adhesive hardens. In step C1, first, a prepreg sheet is attached to one of the abdominal side surfaces 12a of the rail 10 to which the adhesive is applied. Next, the prepreg sheet is folded at the boundary 12c between the abdominal portion 12 and the bottom portion 13, and attached to one of the bottom upper surfaces 13b of the bottom portion 13 of the rail 10. Next, the prepreg sheet is folded at one end 13d of the bottom portion 13 of the rail 10, and attached to the bottom surface 13a of the bottom portion 13 of the rail 10. Next, the prepreg sheet is folded at the other end 13e of the bottom portion 13 of the rail 10, and attached to the other bottom upper surface 13c of the bottom portion 13 of the rail 10. Next, the prepreg sheet is folded at the boundary 12d between the abdominal portion 12 and the bottom portion 13, and attached to the other abdominal side surface 12b of the rail 10. At this time, it is preferable to squeeze the prepreg sheet with a spatula or the like to remove air between the adhesive and the prepreg sheet (degassing operation).

[0068] After the adhesive is applied to the rail 10, the time from placing the prepreg sheet on the adhesive to starting to attach it to the rail 10 (attachment start time) is preferably 60 minutes or less, more preferably 45 minutes or less, and even more preferably 20 minutes or less. If the attachment start time is less than the above upper limit, the adhesive has not hardened, so that the deaeration operation can be performed more effectively and the construction time can be further shortened. From the viewpoint of shortening the time to start attachment, step B1 and step C1 may be performed in parallel. "Performed in parallel" means that while applying adhesive to the rail 10, the prepreg sheet is attached in such a way as to spread the applied adhesive. When "performed in parallel", the time to start attachment is preferably 60 seconds or less, and more preferably 30 seconds or less.

[0069] In step C1, a plurality of prepreg sheets may be used, and the plurality of prepreg sheets may be overlapped with each other in the longitudinal direction of the rail 10. Alternatively, the longitudinal end faces of the plurality of prepreg sheets may be butted against each other so that the plurality of prepreg sheets do not overlap each other. When the adhesive layer has low insulation and it is necessary to secure insulation with the covering layer, it is preferable to overlap the prepreg sheets in order to ensure insulation. By overlapping the prepreg sheets, the covering layer 20 formed is less likely to peel off, so that the barrier between the external environment and the rail 10 can be maintained. It is preferable to butt the rail corrosion prevention sheets together in order to prevent steps from occurring due to overlapping of the sheets. However, the most preferable method is to use a single sheet of rail corrosion prevention sheet attached over the entire length of the rail.

[0070] For example, a case where a first prepreg sheet 21 and a second prepreg sheet 22 are used as prepreg sheets as shown in Figures 4 and 5 will be described. For example, a case where the first prepreg sheet 21 and the second prepreg sheet 22 are attached to one bottom upper surface 13b of the bottom portion 13 of the rail 10, the other end 13e of the bottom portion 13, and the bottom surface 13a of the bottom portion 13 will be described. A primer 40 is applied to one bottom upper surface 13b of the bottom 13 of the rail 10, the other end 13e of the bottom 13, and the bottom surface 13a of the bottom 13. Next, adhesive 50 is applied via primer 40 to one bottom upper surface 13b of bottom 13 of rail 10, the other end 13e of bottom 13, and bottom surface 13a of bottom 13. Next, the first prepreg sheet 21 is attached to one bottom upper surface 13b of the bottom portion 13 of the rail 10, the other end 13e of the bottom portion 13, and the bottom surface 13a of the bottom portion 13 via the adhesive 50. Next, the second prepreg sheet 22 is attached to one bottom upper surface 13b of the bottom 13 of the rail 10, the other end 13e of the bottom 13, and the bottom surface 13a of the bottom 13 via an adhesive 50. At this time, one end 22a of the second prepreg sheet 22 in the longitudinal direction of the rail 10 is overlapped on one end 21a of the first prepreg sheet 21 in the longitudinal direction of the rail 10. In this case, it is preferable that the one end 21a of the first prepreg sheet 21 and the one end 22a of the second prepreg sheet 22 are bonded to each other via, for example, a primer and an adhesive applied to the one end 21a of the first prepreg sheet 21. In this way, after the prepreg sheets 21, 22 are attached to the rail 10, it is possible to maintain the insulation between both side surfaces of the abdominal portion 12 of the rail 10 (one abdominal side surface 12a and the other abdominal side surface 12b), one boundary 12c and the other boundary 12d between the abdominal portion 12 and the bottom portion 13, the bottom surface 13a of the bottom portion 13 of the rail 10, one bottom upper surface 13b and the other bottom upper surface 13c of the bottom portion 13 of the rail 10, and one end 13d and the other end 13e of the bottom portion 13 of the rail 10 and the external environment. The overlap length between one end 21a of the first prepreg sheet 21 and one end 22a of the second prepreg sheet 22 (W shown in FIG. 4) may be 0 mm or more, or 10 mm or more.

[0071] 6, the end face 21b of the first prepreg sheet 21 and the end face 22b of the second prepreg sheet 22 may be butted against each other, and the first prepreg sheet 21 and the second prepreg sheet 22 may be attached to the rail 10 with an adhesive 50. In this embodiment, the prepreg sheets do not overlap each other near the boundary 23 between the first prepreg sheet 21 and the second prepreg sheet 22, so that the thickness of the covering layer can be made uniform. When the end face 21b of the first prepreg sheet 21 and the end face 22b of the second prepreg sheet 22 are butted together and the prepreg sheets are attached to the rail 10, it is preferable that the adhesive used in step B1, in a cured state (i.e., in the state of the adhesive layer 18), has any of the above-mentioned DC insulation resistance value, AC insulation breakdown voltage, DC insulation breakdown voltage, water permeation amount, chloride ion blocking property and oxygen blocking property (collectively referred to as "various characteristics") within a preferred range, and it is more preferable that at least any of the DC insulation resistance value, water permeation amount and chloride ion blocking property are within a preferred range.

[0072] "Process D1" Step D1 is a coating layer curing step in which the curable resin of the fiber-reinforced prepreg of the prepreg sheet is cured to make the prepreg sheet into a coating layer. In step D1, the curable resin of the prepreg sheet is cured by energy ray irradiation to form the covering layer 20. The type of energy ray is appropriately determined depending on the type of curable resin, and examples thereof include ultraviolet rays, electromagnetic waves, heat, and the like. In step D1, the amount of energy radiation applied is not particularly limited and is adjusted appropriately depending on the type and amount of the curable resin in the prepreg sheet. The method of irradiating the energy beam is not particularly limited. As an example of a preferred irradiation method, the rail 10 to which the prepreg sheet is attached is raised with a ring or the like, and in this state, an energy ray irradiator is fixed to the rail 10 with a fixing member, and the prepreg sheet is irradiated with energy rays from the energy ray irradiator. With this method, it is not necessary to hold the energy ray irradiator by hand, and the manpower required for the curing work can be reduced. FIG. 7 is a cross-sectional view showing a schematic configuration of an energy ray irradiation device 60 used in this method. The energy ray irradiation device 60 includes a wheel 61, a pair of anti-tipping plates 62 located on both sides of the wheel 61 and attached to the axis of the wheel 61, a fixing member 63, and three energy ray irradiators 64a, 64b, and 64c fixed to one surface of the fixing member 63. The width of the wheel 61 is approximately the same as the width of the head 11 of the rail 10, and the pair of anti-tipping plates 62 protrude below the wheel 61. In this example, the fixing member 63 is made of steel, and both ends are attached to the pair of anti-tipping plates 62, respectively, with the surface on the energy ray irradiators 64a, 64b, and 64c side facing inward, forming a ring shape with a substantially pentagonal cross section. The fixing member may be made of a material other than steel as long as it can be used to attach the energy ray irradiators. As shown in Fig. 7, when the rail 10 with the prepreg sheet 21 attached thereto is raised and a wheel 61 is placed on the head 11, the rail 10 is surrounded by the wheel 61, a pair of anti-tip plates 62, and a fixing member 63. At this time, the pair of anti-tip plates 62 clamp the head 11 to prevent the wheel 61 from tipping over. The three energy ray irradiators 64a, 64b, and 64c are located below the bottom 13 of the rail 10 and on the left and right sides of the abdomen 12, respectively. By irradiating energy rays from the energy ray irradiators 64a, 64b, and 64c toward the bottom 13 and abdomen 12 of the rail 10, the curable resin of the prepreg sheet 21 is cured to form the coating layer 20.

[0073] "Process E1" Step E1 is an adhesive curing step for curing the adhesive to form an adhesive layer 18. The method of curing the adhesive includes, for example, leaving the adhesive to stand for a desired period of time. The time for curing the adhesive (curing time) is appropriately determined depending on the type of adhesive, etc., and is, for example, preferably within 60 minutes, more preferably 10 to 60 minutes, and even more preferably 20 to 40 minutes. If the curing time is equal to or greater than the above lower limit, the adhesive and the rail 10 or the covering layer 20 can be more firmly bonded. If the curing time is equal to or less than the above upper limit, the construction time can be further shortened. In step E1, the adhesive may or may not be heated.

[0074] In this embodiment, step D1 and step E1 may be performed sequentially or simultaneously. When step D1 and step E1 are performed sequentially, step D1 may be performed first, or step E1 may be performed first. However, from the viewpoint of further shortening the construction time, it is preferable to carry out step D1 and step E1 simultaneously.

[0075] Through the above steps, the bottom 13 of the rail 10 is covered with the covering layer 20, and both side surfaces of the web portion 12 of the rail 10 that are continuous with the bottom 13 of the rail 10 are covered with the covering layer 20, thereby forming a rail covering structure 30.

[0076] According to the rail covering structure of this embodiment, the bottom of the rail and both side surfaces of the rail body are covered with a covering layer. The covering layer has a specific range of resistance measured in a DC insulation resistance test, and therefore can block leakage current from contact points between the rail fixing jig and the rail, the bottom of the rail, etc., and prevent electrolytic corrosion of the rail.

[0077] According to the method for manufacturing a rail covering structure of this embodiment, since a flexible prepreg sheet is attached to the rail, the prepreg sheet can conform to the complex shape of the rail. In addition, according to the method for manufacturing a rail covering structure of this embodiment, since the adhesive is cured after the prepreg sheet is attached to the rail, the time required for curing the adhesive can be shortened, thereby shortening the construction time.

[0078] (Other embodiments) It should be noted that the present invention is not limited to the above-described embodiment. The manufacturing method for the rail covering structure of this embodiment includes the steps of applying a primer to the construction surface of the rail (hereinafter referred to as "step A1"), applying an adhesive to the prepreg sheet (hereinafter referred to as "step B2"), attaching the adhesive-coated surface of the prepreg sheet to the construction surface via the primer before the adhesive hardens (hereinafter referred to as "step C2"), hardening the prepreg sheet by irradiating it with energy rays (hereinafter referred to as "step D1"), and hardening the adhesive (hereinafter referred to as "step E1"). That is, the manufacturing method of the rail covering structure of this embodiment differs from the manufacturing method of the above-described embodiment in that step B2 is used instead of step B1, and step C2 is used instead of step C1.

[0079] In the method for preventing corrosion of a rail according to the present embodiment, it is also preferable to carry out surface preparation (surface treatment) on the surface of the rail 10 to remove rust prior to step A2.

[0080] "Process A1" In step A1, a primer is applied to the surface of the rail 10 to be installed.

[0081] "Process B2" Step B2 is an adhesive application step in which an adhesive is applied to one surface of the prepreg sheet. In step B2, an adhesive is applied to the prepreg sheet. The method for applying the adhesive to the prepreg sheet is not particularly limited, but may be, for example, a brush coating method, a spray coating method, a dipping method, or the like. The adhesive is the same as that used in the above-mentioned step B1.

[0082] The amount of adhesive applied is 0.5 kg / m per unit area of ​​the surface of the prepreg sheet. 2 More than 2.0kg / m 2 Less than 0.7kg / m is preferable. 2 More than 1.2kg / m 2The following is more preferable. When the amount of adhesive applied is equal to or more than the above-mentioned lower limit, the rail 10 and the prepreg sheet can be bonded more firmly. When the amount of adhesive applied is equal to or less than the above-mentioned upper limit, workability is improved. The prepreg sheet may be a single continuous sheet, or a combination of two or more sheets. In order to simplify the process of attaching the prepreg sheet to the rail 10, it is preferable that the prepreg sheet is a single continuous sheet.

[0083] "Process C2" Step C2 is an attachment step in which the adhesive applied to the prepreg sheet is applied to the application surface of the rail before the adhesive hardens, and the prepreg sheet is attached to the application surface of the rail. In step C2, the surface of the prepreg sheet on which the adhesive has been applied is attached to the rail 10 via a primer, similar to step C1 described above. At this time, it is preferable to squeeze the prepreg sheet with a spatula or the like to remove air between the adhesive and the prepreg sheet or between the adhesive and the rail 10 (degassing operation). The start time of attachment in step C2 is the same as the start time of attachment in step C1.

[0084] The time from applying the adhesive to the prepreg sheet and applying the adhesive of the prepreg sheet to the rail 10 until the start of attaching the prepreg sheet to the rail 10 (attachment start time) is preferably 60 minutes or less, more preferably 45 minutes or less, and even more preferably 20 minutes or less. If the attachment start time is less than the above upper limit, the adhesive has not hardened, and the deaeration operation can be performed more effectively and the construction time can be further shortened. From the viewpoint of shortening the time to start attachment, step B2 and step C2 may be performed in parallel. "Performed in parallel" means that while applying adhesive to the prepreg sheet, the prepreg sheet is attached to the rail 10 in a manner that spreads the applied adhesive. When "performed in parallel", the time to start attachment is preferably 60 seconds or less, and more preferably 30 seconds or less.

[0085] "Process D1" In step D1, the curable resin of the prepreg sheet is cured by energy ray irradiation.

[0086] "Process E1" In step E1, the adhesive is cured to form an adhesive layer 18, which bonds the rail 10 and the covering layer 20 or the prepreg sheet.

[0087] Through the above steps, the covering layer 20 is provided on a portion of the rail 10, forming a rail covering structure 30.

[0088] According to the method for manufacturing a rail covering structure of this embodiment, the application time can be reduced by utilizing the time it takes for the primer to harden to apply adhesive to the attachment surface of the prepreg sheet.

[0089] In the above embodiment, the step A1 of applying a primer to the rail is included before the step B1 or B2, but the present invention is not limited to this. Depending on the type of adhesive used in the step B1 or B2, the step A1 may not be included. In the above-described embodiment, there is a step B1 of applying an adhesive to the application surface via a primer or a step B2 of applying an adhesive to the prepreg sheet, but the present invention is not limited to this. For example, if the prepreg sheet has adhesiveness, it can be applied without using an adhesive, so the prepreg sheet may be directly attached to the rail 10. Alternatively, the prepreg sheet may be attached via a primer.

[0090] Although the embodiment of the present invention has been described in detail above with reference to the drawings, the embodiment is merely an example of the present invention. Therefore, the present invention is not limited to the configuration of the embodiment, and it goes without saying that even if there are design changes within the scope of the present invention, they are included in the present invention. In addition, for example, when multiple configurations are included in each embodiment, it goes without saying that possible combinations of these configurations are included even if not specifically stated. In addition, when multiple examples or modified examples are disclosed as the present invention, it goes without saying that possible combinations of configurations across these are included even if not specifically stated. In addition, it goes without saying that the configurations depicted in the drawings are included even if not specifically stated. Furthermore, when the term "etc." is used, it is used to mean that equivalents are included. EXAMPLES

[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0092] (Materials used) <Prepreg sheet> Sheet 1: Reinforcement material = glass chopped strand mat, hardening resin = vinyl ester, basis weight: 2580g / m 2 Dimensions: Thickness 1.5 mm, length 400 mm, width 400 mm, DC insulation resistance value after curing = 4.6 x 10 14 Ω, AC breakdown voltage after curing = 20 kV, DC breakdown voltage after curing = 15 kV, water permeability after curing = 0.15 g, chloride ion blocking property after curing = 0.7 × 10 -3 mg / cm 2 -day, oxygen barrier after curing = 0.01 mol / m 2 ·year. Sheet 2: Reinforcement material = glass chopped strand mat, hardening resin = polyester, basis weight: 2580g / m 2 Dimensions: Thickness 1.5 mm, length 400 mm, width 400 mm, DC insulation resistance value after curing = 4.6 x 10 14Ω, AC breakdown voltage after curing = 20 kV, DC breakdown voltage after curing = 15 kV, water permeability after curing = 0.15 g, chloride ion blocking property after curing = 0.7 × 10 -3 mg / cm 2 -day, oxygen barrier after curing = 0.01 mol / m 2 ·year.

[0093] <Primer> - Urethane primer: Thinkbond Primer U-100 (product name), manufactured by Sekisui Chemical Co., Ltd. <Adhesive> Base material: Vinyl ester adhesive, Pasting Primer V200 (product name), manufactured by Sekisui Chemical Co., Ltd. Hardener: Mepox D (product name), manufactured by Sekisui Chemical Co., Ltd. The DC insulation resistance of the cured adhesive, which was a mixture of the base agent and the curing agent, was measured using the method described above. It was 1.3 × 10 16 It was Omega.

[0094] (Evaluation method) <Fatigue test> As shown in Fig. 7, a sleeper 220, a track pad 210, and a rail covering structure 30 were placed in this order on an H-beam 230. The rail covering structure 30 was fixed to the sleeper 220 with a rail fastening jig 200. Then, a load test was performed 10 million times on the center of the rail with a load of 5 to 100 kN applied vertically downward. Then, the appearance of the rail covering structure (bottom: surface in contact with the track pad 210, fastening part: surface in contact with the rail fastening jig 200 and its vicinity) was observed and evaluated according to the following criteria.

[0095] ≪Judgment criteria≫ ◎: No visible change in appearance. ○: Whitening was confirmed by visual inspection. ×: Lifting, peeling, or cracking was visually confirmed.

[0096] (Examples 1-1 to 1-6) Both sides of the rail web, the bottom surface of the rail base, and the top surface of the rail base were prepared with sandpaper to remove rust from these surfaces. Next, the fine rust particles on the surface of the rail were wiped off with a cloth soaked in acetone. Next, a urethane primer was applied to the bottom and the web of the rail and allowed to cure until no tack (stickiness) remained. Next, an adhesive made of a mixture of a base agent and a hardener was applied to the bottom and the abdomen of the rail via a urethane primer. After the adhesive was applied, Sheet 1 was attached to the surface to which the adhesive was applied at the attachment start time in Table 1. At this time, the prepreg sheet was pressed against the rail to push out the adhesive between the rail and Sheet 1 together with any air bubbles, so that no air bubbles remained between the rail and Sheet 1. The state of the adhesive when Sheet 1 was attached is also shown in the table. After the sheet 1 was attached to the rail, natural light was irradiated (for 20 minutes) in an environment of 23° C. to cure the prepreg and the adhesive, thereby obtaining a rail covering structure for each example. The resulting rail covering structure was subjected to a fatigue test, the results of which are shown in the table.

[0097] [Table 1]

[0098] As shown in Table 1, in Examples 1-1 to 1-6 in which the present invention was applied, the results of the fatigue test (sole) were "A", and the results of the fatigue test (fastening portion) were "O". These results show that a rail covering structure with sufficient durability can be obtained even if the adhesion start time is shortened.

[0099] (Examples 2-1 to 2-4, Reference Examples) The test was conducted based on the salt spray test method of JIS Z 2371. The base material used was a 70mm square piece of SS400, and the surface was treated by attaching 3M's CNS Bevel Black for power tools #120 to a scraping device to polish the surface. Next, a primer was applied to the polished surface by a brush coating method. Next, the adhesive was applied by a brush coating method, and immediately thereafter, the prepreg sheet in Table 2 was attached while squeezing the adhesive out. Any excess adhesive from the prepreg sheet was lightly wiped off, and five test pieces were prepared. The test pieces were arranged in a salt spray device (CYP-90a: manufactured by Suga Test Instruments), and a salt solution (sodium chloride, concentration 5±0.5%, specific gravity: 1.029-1.036, pH: 6.5-7.2) prepared based on the neutral salt spray test method described in JIS Z 2371 4.2.1 was placed in the salt solution supply tank, after which salt spray was performed (spray: 35±1°C, spray rate: 1.5±0.5mL / hr). The adhesive strength was evaluated using a Sanko Techno Technotester RT-3000LDII Construction Research Institute-type tensile tester to evaluate the adhesive strength up to 1000 hours after the salt water spray, with the time before the salt water spray being set as 0 hours, and the average value of N=5 was calculated. The results are shown in the table.

[0100] [Table 2]

[0101] Examples 2-1, 2-2 and Reference Example are examples in which the prepreg sheets were attached to the uncured adhesive, whereas Examples 2-3 and 2-4 are examples in which the prepreg sheets were attached to the cured adhesive. As shown in Table 2, in Examples 2-1 and 2-2 in which the prepreg sheet was attached to the uncured adhesive, the tensile test results after 1000 hours of salt spray were 1.7 to 1.9 MPa. In Examples 2-3 and 2-4, in which the prepreg sheet was attached after the adhesive had hardened, the tensile test results after 1000 hours of salt spray were 1.2 to 1.4 MPa. [Explanation of symbols]

[0102] 10 Rail 18 Adhesive layer 20 Covering layer 21, 22 Prepreg sheet 30 Rail Covering Structure 40 Primer 50 Adhesive 60 Energy Ray Irradiation Device 61 wheels 62 Fall prevention board 63 Fixing member 64a, 64b, 64c Energy ray irradiator

Claims

1. A method for manufacturing a rail covering structure, comprising: a rail; and a covering layer covering a portion of the rail, the covering layer including a cured product of a fiber-reinforced prepreg having a reinforcing member and a curable resin, the method comprising: A bonding step of bonding a prepreg sheet including the fiber reinforced prepreg to a construction surface of the rail; A method for manufacturing a rail covering structure, comprising: a covering layer curing step of curing the curable resin to form the covering layer after the attaching step.

2. A method for manufacturing a rail covering structure, comprising: a rail; and a covering layer covering a portion of the rail, the covering layer including a cured product of a fiber-reinforced prepreg having a reinforcing member and a curable resin, the method comprising: an adhesive application step of applying an adhesive to the construction surface of the rail; A bonding step of bonding a prepreg sheet including the fiber reinforced prepreg onto the adhesive applied to the application surface before the adhesive hardens; an adhesive curing step of curing the adhesive after the attaching step; A method for manufacturing a rail covering structure, comprising: a covering layer curing step of curing the curable resin to form the covering layer after the attaching step.

3. A method for manufacturing a rail covering structure, comprising: a rail; and a covering layer covering a portion of the rail, the covering layer including a cured product of a fiber-reinforced prepreg having a reinforcing member and a curable resin, the method comprising: An adhesive application step of applying an adhesive to one surface of a prepreg sheet including the fiber reinforced prepreg; an attachment step of applying the adhesive to the construction surface of the rail before the adhesive applied to the prepreg sheet hardens, and attaching the prepreg sheet to the construction surface of the rail; an adhesive curing step of curing the adhesive after the attaching step; A method for manufacturing a rail covering structure, comprising: a covering layer curing step of curing the curable resin to form the covering layer after the attaching step.

4. 4. The method for manufacturing a rail covering structure according to claim 2 or 3, wherein the time from applying the adhesive to starting to attach the prepreg sheet is 60 minutes or less.

5. 4. The method for manufacturing a rail covering structure according to claim 2 or 3, wherein the attaching step includes a degassing operation of pressing the prepreg sheet against the rail to degas air present between the adhesive and the prepreg sheet or between the adhesive and the rail.

6. The method for manufacturing a rail covering structure according to any one of claims 1 to 3, further comprising a primer application step of applying a primer to the application surface.

Citation Information

Patent Citations

  • Joint reinforcement method

    JP2019108768A