Manufacturing method of semiconductor member
The PEC etching method forms a fully depleted gate portion in semiconductor members, addressing the challenge of precise structure formation in fin FETs, enhancing yield and performance by controlling gate width and reducing crystal damage.
Patent Information
- Application Number
- JP2023080631
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for manufacturing semiconductor members, such as fin field effect transistors, struggle to form precise structures that affect the operating characteristics of the device, particularly in controlling the width of the gate portion for accurate switching and current control.
A novel method involving photoelectrochemical etching (PEC) is employed, where a wafer is etched using a mask and light irradiation to form a convex gate portion, with etching automatically stopping when the depletion layer is fully depleted, allowing precise control of the gate width.
This method enables precise control of the gate width, improving the yield and reducing damage to the semiconductor crystal, resulting in a fully depleted and normally-off type fin FET with enhanced performance.
Smart Images

Figure 2024164910000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a semiconductor article. [Background technology]
[0002] Semiconductor members in which structures are formed in semiconductor materials are widely used in semiconductor elements, etc. For example, a fin field effect transistor in which a fin structure is formed as a gate portion is known (see, for example, Patent Document 1). For example, structures used in semiconductor elements are preferably formed with a precise shape because they affect the operating characteristics of the element. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 047286 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a novel method for producing a semiconductor member used in a semiconductor element or the like. [Means for solving the problem]
[0005] According to one aspect of the present invention, Preparing a processing object including a wafer made of a conductive semiconductor and a mask disposed on an upper surface of the wafer; a step of immersing the processing object in an etching solution and irradiating the upper surface side of the wafer with light to photoelectrochemically etch the wafer; having The step of photoelectrochemically etching the wafer comprises: Etching a portion of the wafer outside the mask to form a protrusion below the mask; etching the first side surface and the second side surface until a full width between the first side surface and the second side surface of the protrusion facing each other is depleted, thereby automatically stopping the etching of the first side surface and the second side surface; Manufacturing method of semiconductor member is provided. Effect of the Invention
[0006] A novel method for producing a semiconductor member used in a semiconductor element or the like is provided. [Brief description of the drawings]
[0007] [Figure 1] 1(a) and 1(b) are respectively a cross-sectional view and a top view that diagrammatically show a FET 100 according to an embodiment of the present invention. [Diagram 2] FIG. 2(a) is a cross-sectional view that typically illustrates a processing target 150 in PEC etching according to the embodiment, and FIG. 2(b) is a cross-sectional view that typically illustrates a PEC etching apparatus 200 according to the embodiment. [Diagram 3] 3(a) to 3(c) are schematic cross-sectional views showing the wafer 10a and the semiconductor member 10 in the vicinity of the mask 160 in PEC etching according to the embodiment. [Figure 4] 4(a) and 4(b) are a cross-sectional view and a top view, respectively, that diagrammatically show a FET 100 according to a first modified example. [Diagram 5] FIG. 5 is a top view diagrammatically illustrating a FET 100 according to a second modification. [Figure 6] Fig. 6(a) is a table showing the dependence of twice the depletion layer width W D at each carrier concentration n on the applied voltage V when the Schottky barrier Φ B is 1 eV. Fig. 6(b) is a table showing the tolerance of the width W D of the gate protrusion 16 when the threshold tolerance is ±50 mV and ±100 mV. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] A method for manufacturing a semiconductor member according to an embodiment of the present invention will be described. Here, a field effect transistor (FET), which is a semiconductor element, will be given as an example of the semiconductor member according to the embodiment. The semiconductor member according to the embodiment may have only a semiconductor member, or may have a semiconductor member and other members such as electrodes, as in this example. Furthermore, the use of the semiconductor member manufactured by the manufacturing method according to the embodiment does not have to be limited to FETs.
[0009] The structure and operation of a FET 100 according to an embodiment will be illustratively described. Figures 1(a) and 1(b) are a cross-sectional view and a top view, respectively, that typically show the FET 100 according to the embodiment. The FET 100 has a semiconductor member 10, a gate electrode 20, a source electrode 30, and a drain electrode 40. The FET 100 may have other members, such as an insulating film, as necessary.
[0010] The semiconductor member 10 is made of a semiconductor material that has conductivity by containing a predetermined concentration of n-type conductive impurities (hereinafter also simply referred to as impurities). As the semiconductor material constituting the semiconductor member 10, a material that can be etched by photoelectrochemical (PEC) etching can be appropriately used, for example, gallium nitride (GaN), silicon carbide (SiC), etc. are used. Note that the semiconductor material is not limited to wide-gap semiconductors such as GaN, and conventional compound semiconductors such as gallium arsenide (GaAs), indium phosphide (InP), etc. may also be used. Here, the explanation will be given taking GaN containing n-type impurities such as silicon (Si) as an example of the semiconductor material constituting the semiconductor member 10.
[0011] The semiconductor member 10 used in the FET 100 of this example has a substrate 11 and a layer 12 (hereinafter referred to as a drift layer 12) epitaxially grown on the substrate 11. A protrusion 16 (hereinafter referred to as a gate protrusion 16) is formed in the drift layer 12 by a manufacturing method (processing method) according to the embodiment, specifically, PEC etching. The gate protrusion 16 has a width W (see FIG. 3(c)). As will be described in detail later, the width W of the gate protrusion 16 is determined by the carrier concentration of the drift layer 12. In other words, the carrier concentration of the drift layer 12, that is, the impurity concentration added to the drift layer 12, is set so as to obtain a predetermined width W.
[0012] For example, the carrier concentration of the drift layer 12 is set to 1×10 16 / cm 3 By setting the carrier concentration of the drift layer 12 at about 600 nm, the width W of the gate protrusion 16 can be set to 600 nm (see FIG. 6(a)). By lowering the carrier concentration of the drift layer 12, the width W of the gate protrusion 16 can be increased, and by increasing the carrier concentration of the drift layer 12, the width W of the gate protrusion 16 can be decreased (see FIG. 6(a)). The width W of the gate protrusion 16 (more specifically, the width W of the narrowest part of the gate protrusion 16) is preferably 200 nm or more and 2000 nm or less. The carrier concentration of the drift layer 12 is set so that the width W of the gate protrusion 16 is in such a range. Note that the relationship between the carrier concentration of the drift layer 12 and the width W of the gate protrusion 16 can vary to some extent depending on the semiconductor material used (since the width of the depletion layer depends on the dielectric constant of the semiconductor material). The precise relationship between the carrier concentration of the drift layer 12 and the width W of the gate protrusion 16 in the semiconductor material used may be determined, for example, by a preliminary experiment, and the carrier concentration of the drift layer 12 may be set based on the determined precise relationship.
[0013] A gate protrusion 16 is formed on the upper surface of the semiconductor member 10, i.e., the upper surface of the drift layer 12, and a recess 15 (hereinafter referred to as gate recess 15) is formed on the outer portion of the gate protrusion 16 (in a plan view).
[0014] The gate protrusion 16 functions as a gate of the FET 100. In this example, the FET 100 is a fin FET, and as shown in FIG 1(b), the gate protrusion 16 (hatched portion slanting upward to the right) has a fin-like (linear) shape.
[0015] The height of the gate protrusion 16 (i.e., the depth of the gate recess 15) may be set appropriately, for example, to about 1 μm. Note that the height of the gate protrusion 16 is the thickness of the gate portion in the direction of current flow, and if it is too thin (too low), it is not preferable from the viewpoint of current control. For this reason, the height of the gate protrusion 16, that is, the depth of the PEC etching when forming the gate protrusion 16, is preferably, for example, 500 nm or more.
[0016] A gate electrode 20 is disposed on the inner surface of the gate recess 15, at least on the side surface of the gate protrusion 16. The gate electrode 20 is disposed on one side surface of the gate protrusion 16 and on the other side surface opposing the side surface, so as to sandwich the side portion of the gate protrusion 16 from both sides. The gate electrode 20 is connected to a gate pad 21 disposed on the upper surface of the semiconductor member 10, and is connected to an external circuit via the gate pad 21.
[0017] A gate voltage is applied to the side surface of the gate protrusion 16 by the gate electrode 20. By controlling the gate voltage, the carrier distribution in the gate protrusion 16 can be changed to switch the FET 100 between the on state and the off state. As will be described in detail later, the gate protrusion 16 formed by the manufacturing method of the embodiment is totally depleted, so that the FET 100 is of a normally-off type. In other words, by performing an on operation in which a predetermined positive voltage is applied to the gate electrode 20, the number of electrons in the gate protrusion 16 can be increased, and the FET 100 can be turned on.
[0018] Although FIGS. 1(a) and 1(b) show an example of a Schottky type gate electrode structure in which the gate electrode 20 is disposed directly on the side surface of the gate protrusion 16, a MOS type gate electrode structure in which the gate electrode 20 is disposed on the side surface of the gate protrusion 16 via a gate insulating film may also be used, if necessary.
[0019] A source electrode 30 is disposed on the upper surface of the gate protrusion 16 (on one side in the up-down direction of the gate protrusion 16). The source electrode 30 is connected to a source pad 31 disposed on the upper surface of the semiconductor member 10, and is connected to an external circuit via the source pad 31. A drain electrode 40 is disposed on the lower surface of the semiconductor member 10, i.e., on the lower surface of the substrate 11 (on the other side in the up-down direction of the gate protrusion 16).
[0020] With a predetermined voltage applied between the source electrode 30 and the drain electrode 40, a gate voltage can be applied to the gate electrode 20 to turn on the FET 100, thereby operating the FET 100 so that a drain current flows in the thickness direction (vertical direction) of the semiconductor material 10.
[0021] A method for manufacturing the FET 100 will be described by way of example. A gate protrusion 16 is formed on the upper surface (upper surface of the drift layer 12) of a flat semiconductor member 10a (hereinafter referred to as the wafer 10a) on which the gate protrusion 16 has not yet been formed. By forming the gate protrusion 16 on the wafer 10a, the semiconductor member 10 is obtained. The method for manufacturing the FET 100 according to the embodiment has a feature in that the gate protrusion 16 is formed by PEC etching, as will be described in detail below.
[0022] Thereafter, a gate electrode 20, a source electrode 30, a drain electrode 40, and other components such as an insulating film are formed on the semiconductor component 10 using known techniques for patterning a metal film, known techniques for patterning an insulating film, etc., as appropriate, thereby manufacturing the FET 100.
[0023] The process of forming the gate protrusion 16 by PEC etching will be described in detail. FIG. 2(a) is a cross-sectional view that shows a schematic diagram of a processing object 150 in PEC etching according to an embodiment. The processing object 150 has a wafer 10a and a mask 160. As described above, the wafer 10a has a substrate 11 and a drift layer 12. The mask 160 is disposed on the upper surface of the wafer 10a (the upper surface of the drift layer 12) on a region where the gate protrusion 16 is to be formed. As the mask 160, a resist mask, a hard mask, or the like may be appropriately used. The mask 160 is preferably light-shielding so as not to transmit light 231 irradiated in the PEC etching described later.
[0024] FIG. 2(b) is a cross-sectional view showing a schematic diagram of a PEC etching apparatus 200 according to an embodiment. An etching solution (electrolytic solution) 220 is contained in a container 210, and a processing object 150 is immersed in the etching solution 220. An object-side electrode 241 is disposed on the lower surface of the wafer 10a (on the lower surface of the substrate 11), and the processing object 150 is immersed in the etching solution 220 in a state in which the object-side electrode 241 and the lower surface and side surface of the wafer 10a are covered with a coating member 244 such as a resist so as not to be exposed to the etching solution 220 (so as not to be in electrical contact with the etching solution 220). As a result, the opening region of the mask 160 on the upper surface of the wafer 10a (on the upper surface of the drift layer 12) is selectively exposed to the etching solution 220.
[0025] The etching solution 220 may be any suitable etching solution capable of PEC etching the semiconductor material constituting the wafer 10a (more specifically, the semiconductor material constituting the drift layer 12) (such as an aqueous potassium hydroxide solution or an aqueous phosphoric acid solution). The etching solution 220 may be alkaline or acidic as required. As described below, the pH of the etching solution 220 is appropriately adjusted according to the width W of the gate protrusion 16, and an etching solution 220 corresponding to a suitable pH is used.
[0026] One end of a (insulating-coated) wire 242 is connected to the processing object side electrode 241. The etchant side electrode 243 is attached to the other end of the wire 242, and the etchant side electrode 243 is immersed in the etchant 220. A voltage source 240 is disposed midway along the wire 242. The voltage source 240 applies a predetermined etching voltage for performing PEC etching between the processing object side electrode 241 and the etchant side electrode 243, i.e., between the wafer 10a and the etchant 220.
[0027] With an etching voltage applied between the wafer 10a and the etching solution 220, light 231 for performing PEC etching is irradiated from the light source 230 onto the upper surface of the wafer 10a, that is, the upper surface of the drift layer 12 which is the surface to be etched. In this manner, PEC etching is performed on the wafer 10a.
[0028] 3(a) to 3(c) are schematic cross-sectional views showing the wafer 10a and the semiconductor member 10 near the mask 160 in PEC etching according to an embodiment. See FIG. 3(a). An etching voltage is applied such that the wafer 10a side is positive and the etching solution 220 side is negative. Light 231 is irradiated having a wavelength corresponding to energy greater than the band gap of the semiconductor material constituting the upper surface of the wafer 10a, which is the region to be etched.
[0029] A depletion layer 10D (hatched area with an upward slanting angle to the right) is formed on the upper surface of the wafer 10a. Photoexcitation caused by irradiation of the upper surface of the wafer 10a with light 231 generates pairs of electrons and holes in the surface layer of the upper surface. A negative voltage applied to the etching solution 220 induces the holes to the upper surface side (etching solution 220 side) of the wafer 10a. The holes oxidize the semiconductor material, and the oxides are dissolved in the etching solution, so that etching progresses. In an example in which the wafer 10a is made of GaN, the holes decompose the GaN into gallium (Ga) and nitrogen (N), and the gallium is oxidized by oxygen contained in the etching solution 220 to generate gallium oxide, which is dissolved in the acidic or alkaline etching solution 220, so that etching progresses. The electrons generated in pairs with the holes are induced to the lower surface side of the wafer 10a.
[0030] 3(b), the outer portion of the mask 160 (in a plan view) of the wafer 10a is etched to form the gate recess 15, thereby forming the gate protrusion 16 below the mask 160 (leaving the gate protrusion 16 below the mask 160). As the etching of the bottom surface of the gate recess 15 progresses (the gate recess 15 becomes deeper), the etching of the side surface of the gate protrusion 16, which is the side surface of the gate recess 15, also progresses. In other words, the etching of the mutually opposing side surfaces 16a and 16b of the gate protrusion 16 progresses, and the width of the gate protrusion 16 becomes narrower.
[0031] It is preferable that the light 231 has a light component that is obliquely incident on the upper surface of the wafer 10a so that the light 231 can be easily irradiated onto the side surfaces 16a and 16b of the gate convex portion 16. Furthermore, due to etching of the side surfaces 16a and 16b, the width of the gate convex portion 16 becomes narrower than the width of the mask 160. For this reason, it is preferable to form the mask 160 to be slightly wider than the width W of the gate convex portion 16 that is ultimately desired.
[0032] The holes move by diffusing in the non-depleted region of the wafer 10a. When the width of the gate protrusion 16 is sufficiently wide, specifically, when a non-depleted region remains between the depletion layer 10D formed on the side surface 16a and the depletion layer 10D formed on the side surface 16b of the gate protrusion 16, the holes move through this region, and the etching of the side surface 16a and the side surface 16b progresses.
[0033] 3(c), when the width of the gate protrusion 16 narrows to a width W such that the entire width of the gate protrusion 16 becomes the depletion layer 10D, holes cannot move and the etching of the side surface 16a and the side surface 16b automatically stops.
[0034] After the width of the gate protrusion 16 reaches width W and etching of the side surfaces 16a and 16b stops, etching proceeds until the depth of the gate recess 15 reaches a predetermined depth, and then irradiation of the light 231 is stopped to terminate the PEC etching.
[0035] In this example, the FET 100 is a FinFET, and the mask 160 includes a linear portion (in a plan view). In the PEC etching step, a gate protrusion 16 is formed that includes a linear portion having a narrowest width W (in a plan view) of 200 nm or more and 2000 nm or less.
[0036] As described above, the process of forming the gate convex portion 16 by PEC etching (the manufacturing method of the semiconductor material 10 according to the embodiment) includes the steps of preparing the processing object 150, and PEC etching the wafer 10a by immersing the processing object 150 in the etching solution 220 and irradiating the wafer 10a with light 231 from the top side of the wafer 10a.
[0037] In the process of PEC etching the wafer 10a, an outer portion of the mask 160 of the wafer 10a is etched to form a gate protrusion 16 below the mask 160, and the side 16a and the side 16b are etched until the entire width between the opposing side 16a and the side 16b of the gate protrusion 16 is depleted, whereby the etching of the side 16a and the side 16b is automatically stopped.
[0038] The width W of the gate protrusion 16 formed in the embodiment is determined by the width of the depletion layer 10D. As described below, the width of the depletion layer 10D is determined by the carrier concentration of the semiconductor member 10, more specifically, the portion where the gate protrusion 16 is to be formed (the drift layer 12 in this example), and the pH of the etching solution 220. Therefore, even if there is an error in the size of the mask 160, the width W of the gate protrusion 16 can be precisely controlled by the carrier concentration and the pH of the etching solution 220.
[0039] In a FinFET power device, the threshold voltage for switching on and off is determined by the width W of the gate protrusion 16, which is the gate portion. For this reason, it is preferable that the width W be precisely controlled. The preferable width W is estimated as follows.
[0040] The embodiment shows a Schottky gate electrode structure in which the semiconductor member 10 is made of GaN and the gate electrode 20 is made of gold (Au). D teeth,
number
[0041] Built-in potential Φ bi teeth,
number
[0042] Depletion layer width W D By forming the width W of the gate protrusion 16 to be twice as large as the Schottky barrier Φ when a voltage V is applied to the gate electrode 20, the entire width of the gate protrusion 16 is depleted. B When is 1 eV, the depletion layer width W at each carrier concentration n D 13 is a table showing the dependency of the double value of the width W of the gate protrusion 16 that is fully depleted on the applied voltage V.
[0043] The carrier concentration n is 5×10 15 / cm 3 , 8×10 15 / cm 3 , 1×10 16 / cm 3 , and 2×10 16 / cm 3 The applied voltage V is changed from +0.2V to -0.35V in increments of 0.05V (50mV). The width W is shown in nm. When the carrier concentration n is 5×10 15 / cm 3 2.5kV withstand voltage, 1×10 16 / cm 3 This makes it possible to realize GaN power devices with a voltage rating of 1.5 kV.
[0044] For a specific carrier concentration n, when the width W of the gate protrusion 16 is a value in this table, the FinFET just reaches the off state at the applied voltage V. In other words, this applied voltage V becomes the threshold. For example, when the carrier concentration n is 1×10 16 / cm 3 When the width W is 600 nm, the entire width W is depleted when the applied voltage V is 0, and the FinFET is turned off.
[0045] Consider the case of a design in which the device is exactly in the off state (pinch-off) when the applied voltage V is 0. FIG. 6(b) is a table showing the tolerance of the width W of the gate protrusion 16 when the threshold voltage tolerance is ±50 mV and ±100 mV. When the threshold voltage tolerance is ±50-100 mV, the tolerance of the width W of the gate protrusion 16 is ±10-50 nm. It is very difficult to suppress the tolerance of the width W of the gate protrusion 16 to such a low level using conventional lithography.
[0046] In the embodiment, as described above, the gate protrusion 16 is formed by PEC etching. The barrier height of the semiconductor member 10 in contact with the etching solution 220 is controlled by the pH of the etching solution 220. Therefore, the depletion layer width W D That is, the width W of the gate protrusion 16 to be formed is controlled by the pH of the etching solution 220.
[0047] More specifically, the Schottky barrier Φ in the fabricated Schottky electrode structure B By adjusting the pH of the etching solution 220 so that the depletion layer width W D is the depletion layer width W when the applied voltage V=0 in the Schottky electrode structure. D In this manner, it is possible to form the gate protrusion 16 having a width W such that the gate is in an off state when the applied voltage V is 0 when the Schottky electrode structure is formed.
[0048] As described above, the width W of the gate protrusion 16 according to the embodiment can be precisely controlled by the carrier concentration n and the pH of the etching solution 220. With current growth technology, it is possible to keep the variation in the carrier concentration n within the wafer surface to about ±2% on average. For example, when the carrier concentration n is 1×10 16 / cm 3 In the case of ±2%, the error in width W within the wafer surface is ±6 nm, which can be reduced to ±10 nm or less.
[0049] For example, in a comparative example in which the gate protrusion 16 is formed by a combination of ultraviolet lithography using a stepper and dry etching, the yield of the device is only about 50%. In contrast, in the gate protrusion 16 formed by PEC etching in the embodiment as described above, the error in width W can be suppressed to ±10 nm or less, thereby improving the yield.
[0050] In the comparative embodiment using dry etching, there is a concern about damage to the semiconductor crystal due to dry etching. In contrast, in the embodiment, the gate protrusion 16 is formed by PEC etching, which is wet etching, so that damage to the semiconductor crystal is suppressed. Also, in the embodiment, the width W can be determined by automatically stopping etching in the width direction of the gate protrusion 16. Furthermore, in the embodiment, a fully depleted gate protrusion 16 can be formed, so that the obtained FET 100 can be a normally-off type.
[0051] Next, a description will be given of a FET 100 according to a modification of the above-mentioned embodiment. Figures 4(a) and 4(b) are a cross-sectional view and a top view, respectively, that diagrammatically show a FET 100 according to a first modification.
[0052] In the above embodiment, the FET 100 having a Schottky type (or MOS type) gate electrode structure is exemplified. The gate electrode structure is not limited to this. As a first modification, the FET 100 having a pn type gate electrode structure is exemplified.
[0053] In the first modification, the gate recess 15 is filled with a semiconductor layer 13 (hatched portion slanting upward to the left) of a conductivity type (i.e., p-type) opposite to that of the drift layer 12. The gate electrode 20 is formed on the semiconductor layer 13. A gate voltage is applied to a pn junction formed by the semiconductor layer 13 and the gate protrusion 16 via the semiconductor layer 13.
[0054] The manufacturing method of the FET 100 according to the first modification is the same as that of the above-described embodiment up to the step of forming the gate protrusion 16. After the gate protrusion 16 is formed, the semiconductor layer 13 is formed, for example, by regrowth. If necessary, polishing may be performed to flatten the upper surface of the semiconductor member 10 on which the semiconductor layer 13 has been grown. Thereafter, the gate electrode 20, the source electrode 30, the drain electrode 40, and other members such as an insulating film are formed on the semiconductor member 10, thereby manufacturing the FET 100 according to the first modification.
[0055] 5 is a top view diagrammatically illustrating a FET 100 according to a second modified example. In the above-described embodiment, a FET 100 having a fin-shaped (linear) gate protrusion 16 is exemplified. The shape of the gate protrusion 16 is not limited to this. As a second modified example, a FET 100 (nanorod transistor) having a rod-shaped (island-shaped) gate protrusion 16 is exemplified. In the nanorod transistor, a gate electrode 20 is formed so as to surround the entire periphery (in a plan view) of the gate protrusion 16.
[0056] In the method for manufacturing the FET 100 according to the second modification, the process for forming the gate protrusion 16 is different from that of the above-described embodiment. In this example, the mask 160 includes an island-shaped portion (in a plan view). In the PEC etching process, the gate protrusion 16 including the island-shaped portion having a width W of the narrowest portion (in a plan view) of 200 nm or more and 2000 nm or less is formed. After the gate protrusion 16 is formed, the gate electrode 20, the source electrode 30, the drain electrode 40, and other members such as an insulating film are formed on the semiconductor member 10, thereby manufacturing the FET 100 according to the second modification.
[0057] The FET 100 according to the first and second modifications has the same advantages as the above-described embodiment, such as the ability to precisely control the width W by forming the fully depleted gate protrusion 16 by PEC etching.
[0058] <Preferred embodiment of the present invention> Preferred aspects of the present invention will be described below.
[0059] (Appendix 1) Preparing a processing object including a wafer made of a conductive semiconductor and a mask disposed on an upper surface of the wafer; a step of immersing the processing object in an etching solution and irradiating the upper surface side of the wafer with light to photoelectrochemically etch the wafer; having The step of photoelectrochemically etching the wafer comprises: Etching a portion of the wafer outside the mask to form a protrusion below the mask; etching the first side surface and the second side surface until a full width between the first side surface and the second side surface of the protrusion facing each other is depleted, thereby automatically stopping the etching of the first side surface and the second side surface; A method for manufacturing a semiconductor component.
[0060] (Appendix 2) the mask includes a linear portion, In the step of photoelectrochemically etching the wafer, the convex portion is formed to include a linear portion having a narrowest portion width of 200 nm or more and 2000 nm or less. A method for producing a semiconductor member according to appendix 1.
[0061] (Appendix 3) the mask includes islands; In the step of photoelectrochemically etching the wafer, the convex portion is formed to include an island-shaped portion having a narrowest portion width of 200 nm or more and 2000 nm or less. A method for producing a semiconductor member according to appendix 1.
[0062] (Appendix 4) forming a gate electrode for applying a gate voltage to a side surface of the protrusion, a source electrode disposed on one side in a vertical direction of the protrusion, and a drain electrode disposed on the other side in a vertical direction of the protrusion; The method for producing a semiconductor article according to any one of Appendices 1 to 3, further comprising: [Explanation of symbols]
[0063] 10...semiconductor member, 10a...wafer, 10D...depletion layer, 11...substrate, 12...drift layer, 13...semiconductor layer, 15...gate recess, 16...gate protrusion, 16a...side, 16b...side, 20...gate electrode, 21...gate pad, 30...source electrode, 31...source pad, 40...drain electrode, 100...FET, 150...processing object, 160...mask, 200...PEC etching device, 210...container, 220...etching liquid, 230...light source, 231...light, 240...voltage source, 241...processing object side electrode, 242...wiring, 243...etching liquid side electrode, 244...covering member
Claims
1. Preparing a processing object including a wafer made of a conductive semiconductor and a mask disposed on an upper surface of the wafer; a step of immersing the processing object in an etching solution and irradiating the upper surface side of the wafer with light to photoelectrochemically etch the wafer; having The step of photoelectrochemically etching the wafer comprises: Etching a portion of the wafer outside the mask to form a protrusion below the mask; etching the first side surface and the second side surface until a full width between the first side surface and the second side surface of the protrusion facing each other is depleted, thereby automatically stopping the etching of the first side surface and the second side surface; A method for manufacturing a semiconductor component.
2. the mask includes a linear portion, In the step of photoelectrochemically etching the wafer, the convex portion is formed to include a linear portion having a narrowest portion width of 200 nm or more and 2000 nm or less. The method for producing a semiconductor article according to claim 1 .
3. the mask includes islands; In the step of photoelectrochemically etching the wafer, the convex portion is formed to include an island-shaped portion having a narrowest portion width of 200 nm or more and 2000 nm or less. The method for producing a semiconductor article according to claim 1 .
4. forming a gate electrode for applying a gate voltage to a side surface of the protrusion, a source electrode disposed on one side in a vertical direction of the protrusion, and a drain electrode disposed on the other side in a vertical direction of the protrusion; The method for producing a semiconductor article according to any one of claims 1 to 3, further comprising:
Citation Information
Patent Citations
Semiconductor laser device and manufacturing method of nitride semiconductor device
JP2008282836A
Structures and intermediate structures
JP2020013837A
Vertical field effect transistor and method for forming same