Non-aqueous PTFE dispersion solution for secondary battery

JP2024164942APending Publication Date: 2024-11-28MITSUBISHI PENCIL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023080689
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Benefits of technology

【0008】 本発明によれば、分散安定性及び活物質との混合性が良好な、新規な二次電池用非水系PTFE分散液を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164942000001
    Figure 2024164942000001
Patent Text Reader

Abstract

To provide a novel non-aqueous PTFE dispersion solution for a secondary battery which exhibit an excellent dispersion stability and an excellent mixing property with an active material.SOLUTION: The non-aqueous PTFE dispersion solution for a secondary battery of the present invention includes polytetrafluoroethylene particles, a non-aqueous solvent, and a dispersant. In the particle size distribution of the polytetrafluoroethylene particles measured by a laser diffraction technique, D10 is at least 2.0 μm, D90 is 50 μm at largest, and the rate of increase measured in accordance with ASTM D4895 of the polytetrafluoroethylene particles is in the range of 380-1000%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a non-aqueous PTFE dispersion for a secondary battery. [Background technology]

[0002] Polytetrafluoroethylene (PTFE) is a material that has excellent heat resistance, electrical insulation, low dielectric properties, low friction properties, non-adhesiveness, weather resistance, etc., and is used in various applications. In addition, powdered PTFE has the property of fibrillating when shear force is applied, and this property is utilized to fibrillate powdered PTFE to bind active materials used in secondary batteries. For this purpose, a non-aqueous dispersion of PTFE particles has been proposed.

[0003] Patent Document 1 discloses a non-aqueous dispersion of polytetrafluoroethylene micropowder, which contains at least 5 to 60 mass % of polytetrafluoroethylene micropowder and 0.1 to 15 mass % of polyvinyl butyral relative to the mass of the polytetrafluoroethylene micropowder, and is characterized in that the water content of the entire dispersion, as measured by the Karl Fischer method, is 8000 ppm or less.

[0004] Patent Document 2 discloses a binder for batteries that is composed of an aqueous or non-aqueous dispersion or powder containing core-shell composite microparticles with an average particle size of 0.05 to 1 μm, the core of which is made of fibril-forming polytetrafluoroethylene and the shell of which is a non-fibril-forming polymer, and the weight ratio of the core to the shell of the composite microparticles is 98:2 to 50:50. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-066327 A [Patent Document 2] International Publication No. 96 / 012764 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention provides a novel non-aqueous PTFE dispersion for secondary batteries, which has good dispersion stability, miscibility with an active material, and film-formability when mixed with an active material. [Means for solving the problem]

[0007] As a result of intensive research, the present inventors have found that the above problems can be solved by the following means, and have completed the present invention. That is, the present invention is as follows: <Aspect 1> Contains polytetrafluoroethylene particles, a non-aqueous solvent, and a dispersant, In the particle size distribution of the polytetrafluoroethylene particles measured by a laser diffraction method, D10 is 2.0 μm or more and D90 is 50 μm or less, and The nonaqueous PTFE dispersion for secondary batteries, wherein the polytetrafluoroethylene particles have an elongation of 380 to 1000% as measured in accordance with ASTM D4895. <Aspect 2> The nonaqueous PTFE dispersion for a secondary battery according to aspect 1, wherein the polytetrafluoroethylene particles have an average primary particle diameter of 100 nm to 500 nm as measured by a scanning electron microscope. <Aspect 3> The nonaqueous PTFE dispersion for a secondary battery according to aspect 1 or 2, wherein in the particle size distribution, D50 is 12 μm to 45 μm. <Aspect 4> The nonaqueous PTFE dispersion for a secondary battery according to any one of Aspects 1 to 3, having a water content of 8000 ppm or less. <Aspect 5> The nonaqueous PTFE dispersion for secondary batteries according to any one of Aspects 1 to 4, wherein the content of the polytetrafluoroethylene particles is 5% by mass to 60% by mass with respect to the mass of the nonaqueous PTFE dispersion for secondary batteries. <Aspect 6> The nonaqueous PTFE dispersion for a secondary battery according to any one of Aspects 1 to 5, wherein a ratio of the mass of the dispersant to the mass of the polytetrafluoroethylene particles is 0.001 to 0.15. <Aspect 7> The nonaqueous PTFE dispersion for a secondary battery according to any one of Aspects 1 to 6, wherein the dispersant is at least one selected from the group consisting of polyvinyl alcohol-based, butyral-based, acrylic, and urethane-based dispersants. <Aspect 8> The nonaqueous PTFE dispersion for a secondary battery according to any one of Aspects 1 to 7, wherein the nonaqueous solvent is at least one selected from the group consisting of aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, aromatic polar solvents, alcohols, polyhydric alcohols, glycol ethers, esters, and aprotic polar solvents. <Aspect 9> A method for producing a slurry for a secondary battery, comprising mixing the nonaqueous PTFE dispersion for a secondary battery according to any one of Aspects 1 to 8 and a battery material. Effect of the Invention

[0008] According to the present invention, it is possible to provide a novel non-aqueous PTFE dispersion for secondary batteries, which has good dispersion stability and good mixability with active materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] 《Non-aqueous PTFE dispersion liquid for secondary batteries》 The non-aqueous PTFE dispersion for a secondary battery of the present invention is It contains polytetrafluoroethylene particles, a non-aqueous solvent, and a dispersant, In the particle size distribution of the polytetrafluoroethylene particles measured by a laser diffraction method, D10 is 2.0 μm or more and D90 is 50 μm or less, and The polytetrafluoroethylene particles have an elongation of 380 to 1000% as measured in accordance with ASTM D4895.

[0010] The inventors have found that the above-mentioned configuration, particularly the relatively narrow particle size distribution and relatively large elongation of the polytetrafluoroethylene particles, makes it possible to obtain dispersion stability, good mixability with active materials, and film-formability when mixed with an active material.

[0011] Here, the particle size distribution is measured by the laser diffraction method on a volume basis, and D10, D90, and D50 (median diameter) mean the diameters of particles when the cumulative distribution of the population is 10%, 90%, and 50%, respectively. Measurement by the laser diffraction method can be performed, for example, using a particle size distribution measuring device MT3300II (Microtrack Bell Co., Ltd.).

[0012] In the above particle size distribution, D10 is 2.0 μm or more, 2.2 μm or more, or 2.5 μm or more, so that the amount of polytetrafluoroethylene particles added can be reduced, thereby improving the battery characteristics. This D10 may be 30.0 μm or less, 27.0 μm or less, 25.0 μm or less, 22.0 μm or less, 20.0 μm or less, 17.0 μm or less, 15.0 μm or less, 12.0 μm or less, 10.0 μm or less, 9.0 μm or less, 8.0 μm or less, 7.0 μm or less, 6.0 μm or less, 5.0 μm or less, 4.0 μm or less, or 3.5 μm or less.

[0013] In the above particle size distribution, D90 of 50 μm or less, 45 μm or less, 40 μm or less, 37 μm or less, or 35 μm or less can improve film formability, particularly when mixed with an active material. This D90 may be 15 μm or more, 17 μm or more, 20 μm or more, 25 μm or more, 28 μm or more, 30 μm or more, 33 μm or more, 35 μm or more, 38 μm or more, 40 μm or more, 45 μm or more, or 47 μm or more.

[0014] In the above particle size distribution, D50 may be 11 μm or more, or 12 μm or more, and may be 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, or 25 μm or less. In particular, when D50 is within the above range, the nonaqueous PTFE dispersion for secondary batteries of the present invention can have good mixability with the active material.

[0015] The non-aqueous PTFE dispersion for secondary batteries of the present invention can be prepared by various dispersion methods. Examples of the dispersion method include a method using a disperser, a ball mill, a bead mill, etc. The shear force applied during dispersion may be adjusted appropriately so that the polytetrafluoroethylene particles in the non-aqueous PTFE dispersion for secondary batteries are not fibrillated.

[0016] From the viewpoint of enhancing the effect of the present invention, it is preferable that the non-aqueous PTFE dispersion for secondary batteries of the present invention does not contain coarse particles, for example, polytetrafluoroethylene particles having a particle diameter of 500 μm or more. These coarse particles can be removed, for example, by a known classification means such as mesh filtration after the dispersion treatment.

[0017] The water content of the nonaqueous PTFE dispersion for secondary batteries of the present invention is preferably 9000 ppm or less, 8800 ppm or less, 8500 ppm or less, 8300 ppm or less, 8000 ppm or less, or 7700 ppm or less, from the viewpoint of improving the battery characteristics of the obtained secondary battery. This water content may be 0 ppm or more, 1000 ppm or more, 2000 ppm or more, 3000 ppm or more, or 4000 ppm or more.

[0018] In the present invention (including the Examples described later), the measurement of the water content by the Karl Fischer method conforms to JIS K 0068:2001 and was performed using MCU-610 (manufactured by Kyoto Electronics Manufacturing Co., Ltd.) Specifically, the nonaqueous PTFE dispersion for secondary batteries is dissolved in an alcohol-based solvent, which is reacted with a KF reagent, and the water content of the nonaqueous PTFE dispersion for secondary batteries can be calculated from the volume consumed by the KF reagent.

[0019] In addition to the amount of moisture contained in the non-aqueous solvent, other possible causes include moisture contained in the materials themselves, such as polytetrafluoroethylene micropowder and dispersant, and external moisture contamination during the manufacturing process in which polytetrafluoroethylene micropowder is dispersed in the non-aqueous solvent (moisture in the air, condensation on the equipment walls, etc.). However, by ultimately keeping the moisture content of the non-aqueous dispersion of polytetrafluoroethylene micropowder to 8000 ppm or less, it is possible to obtain a non-aqueous dispersion of polytetrafluoroethylene micropowder with better storage stability.

[0020] In order to reduce the moisture content of the non-aqueous solvent and the non-aqueous dispersion of polytetrafluoroethylene micropowder to 8000 ppm or less, a commonly used method for dehydrating non-aqueous solvents can be used, for example, molecular sieves can be used. In addition, the polytetrafluoroethylene micropowder and dispersant can be used in a state where the moisture content has been sufficiently reduced by dehydrating them by heating or reducing pressure.

[0021] Furthermore, after preparing a non-aqueous dispersion of polytetrafluoroethylene micropowder, it is possible to remove moisture using molecular sieves or membrane separation methods, but methods other than those mentioned above can also be used without any particular limitation as long as they can reduce the moisture content of the non-aqueous dispersion.

[0022] Each component of the present invention will now be described.

[0023] <Polytetrafluoroethylene particles> The polytetrafluoroethylene particles used in the present invention are polytetrafluoroethylene particles having an elongation of 380 to 1000% as measured in accordance with ASTM D4895.

[0024] The polytetrafluoroethylene particles used in the present invention may be subjected to dry pulverization, wet pulverization, or electron beam treatment before being mixed and stirred with the non-aqueous solvent and dispersant.

[0025] The average primary particle diameter of the polytetrafluoroethylene particles of the present invention is preferably 100nm or more, 120nm or more, 150nm or more, 180nm or more, 200nm or more, or 230nm or more from the viewpoint of improving the film-forming property when the non-aqueous PTFE dispersion for secondary batteries is applied. This average primary particle diameter may be 500nm or less, 450nm or less, 430nm or less, 400nm or less, 380nm or less, 350nm or less, 330nm or less, 300nm or less, or 280nm or less. This average primary particle diameter was calculated using the major axis diameter of the primary particles observed with a scanning electron microscope (SEM).

[0026] The polytetrafluoroethylene particles of the present invention have an elongation of 380% or more, 400% or more, 420% or more, 450% or more, 480% or more, 500% or more, 530% or more, or 550% or more, so that the film formability can be improved when the non-aqueous PTFE dispersion for secondary batteries is applied. This elongation may also be 1000% or less, 900% or less, 800% or less, 700% or less, or 650% or less.

[0027] The elongation was measured in accordance with ASTM D4895, and more specifically, was measured by the following procedure. 1. Polytetrafluoroethylene particles are formed into a disk-shaped sheet, and a pressure of 34.5 MPa is applied and maintained for 3 minutes. 2. The disk-shaped sheet is placed in an environment with an initial temperature of 290°C, heated at 120°C / h, held at 380°C for 30 minutes, cooled at 60°C / h, held at 290°C for 24 minutes, and sintered at room temperature for 30 minutes. 3. The sintered disk-shaped sheet is punched out into a dumbbell shape to prepare a test sheet. 4. Set the gauge length L0 and then place it in the jig. 5. After resetting the displacement and stress to zero, pull the specimen at a tensile speed of 50 mm / min until it breaks, measure the stress F and length L1 at break, and calculate the breaking elongation using the following formula. Breaking elongation EL = (L1-L0) / L0 x 100%

[0028] The content of polytetrafluoroethylene particles in the nonaqueous PTFE dispersion for secondary batteries of the present invention is preferably 5 mass% or more, 10 mass% or more, 15 mass% or more, 20 mass% or more, 25 mass% or more, or 28 mass% or more, relative to the mass of the nonaqueous PTFE dispersion for secondary batteries, from the viewpoint of improving film-formability, and is preferably 60 mass% or less, 55 mass% or less, 50 mass% or less, 45 mass% or less, 40 mass% or less, 35 mass% or less, or 33 mass% or less, from the viewpoint of obtaining dispersion stability.

[0029] <Non-aqueous solvent> The non-aqueous solvent generally refers to a solvent other than water, and examples of the solvent that can be used include hydrocarbon solvents, aromatic hydrocarbon solvents, aromatic polar solvents, alcohols, polyhydric alcohols, glycol ethers, esters, aprotic polar solvents, etc. These solvents may be used alone or in combination.

[0030] The content of the non-aqueous solvent may be 50 mass% or more, 55 mass% or more, 60 mass% or more, or 65 mass% or more, and may be 85 mass% or less, 80 mass% or less, 75 mass% or less, or 70 mass% or less, based on the mass of the non-aqueous PTFE dispersion for secondary batteries.

[0031] As the hydrocarbon solvent, an aliphatic hydrocarbon solvent, an aromatic hydrocarbon solvent, etc. can be used. These solvents have low water solubility, and therefore may be preferable from the viewpoint of suppressing the capture of water vapor in the air, thereby suppressing an increase in the moisture content. These solvents may be used alone or in combination.

[0032] Examples of the aliphatic hydrocarbon solvent that can be used include hexane, heptane, octane, cyclohexane, methylcyclohexane, ethylcyclohexane, and tetrachloromethane.

[0033] As the aromatic hydrocarbon solvent, for example, benzene, chlorobenzene, toluene, xylene, cymene, mesitylene, etc. can be used.

[0034] Examples of aromatic polar solvents that can be used include benzyl alcohol, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, propylene glycol monophenyl ether, diethylene glycol monophenyl ether, alkylsulfonic acid phenyl ester, butyl phthalate, ethylhexyl phthalate, tridecyl phthalate, ethylhexyl trimellitate, diethylene glycol dibenzoate, and dipropylene glycol dibenzoate.

[0035] Examples of the alcohol that can be used include ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butyl alcohol, 1-pentanol, isoamyl alcohol, sec-amyl alcohol, 3-pentanol, tert-amyl alcohol, n-hexanol, methylamyl alcohol, 2-ethylbutanol, n-heptanol, 2-heptanol, 3-heptanol, n-octanol, 2-octanol, 2-ethylhexanol, 3,5,5-trimethylhexanol, nonanol, n-decanol, undecanol, n-decanol, trimethylnonyl alcohol, tetradecanol, heptadecanol, cyclohexanol, and 2-methylcyclohexanol.

[0036] Examples of polyhydric alcohols that can be used include ethylene glycol, diethylene glycol, 3-methyl-1,3-butanediol, triethylene glycol, dipropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,5-pentanediol, hexylene glycol, and octylene glycol.

[0037] Examples of glycol ethers that can be used include methyl isopropyl ether, ethyl ether, ethyl propyl ether, ethyl butyl ether, isopropyl ether, butyl ether, hexyl ether, 2-ethylhexyl ether, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylbutyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, tetraethylene glycol monobutyl ether, 3-methyl-3-methoxy-1-butanol, 3-methoxy-1-butanol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol tertiary butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monobutyl ether, and tetrapropylene glycol monobutyl ether.

[0038] Examples of the ester include propylene glycol methyl ether acetate, propylene glycol diacetate, 3-methyl-3-methoxybutyl acetate, propylene glycol ethyl ether acetate, ethylene glycol ethyl ether acetate, butyl formate, isobutyl formate, isoamyl formate, ethyl acetate, propyl acetate, butyl acetate, isopropyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, propyl propionate, isobutyl propionate, isoamyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, methyl isobutyrate, ethyl isobutyrate, isobutyric acid, Propyl valerate, methyl valerate, ethyl valerate, propyl valerate, methyl isovalerate, ethyl isovalerate, propyl isovalerate, methyl trimethylacetate, ethyl trimethylacetate, propyl trimethylacetate, methyl caproate, ethyl caproate, propyl caproate, methyl caprylate, ethyl caprylate, propyl caprylate, methyl laurate, ethyl laurate, methyl oleate, ethyl oleate, caprylic acid triglyceride, tributyl acetate citrate, octyl oxystearate, propylene glycol monoricinoleate, methyl 2-hydroxyisobutyrate, 3-methoxybutyl acetate, and the like can be used.

[0039] Aprotic polar solvents are generally solvents that do not contain acidic hydrogen. Examples of aprotic polar liquid media that can be used include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone.

[0040] <Dispersant> The dispersant may be any dispersant that dissolves in a non-aqueous solvent and disperses polytetrafluoroethylene, and may be any known dispersant. For example, commercially available dispersants may be used as wetting dispersants. Examples of such dispersants include polyester dispersants, acrylic dispersants, polyethyleneimine dispersants, phosphate ester dispersants, urethane dispersants, and fluorine dispersants. From the viewpoint of suppressing side reactions when the battery is made, it is particularly preferable to use polyvinyl alcohol, butyral, or acrylic / urethane dispersants. These dispersants may be used alone or in combination.

[0041] The content of the dispersant may be 0.1% by mass or more, 0.3% by mass or more, 0.5% by mass or more, 0.7% by mass or more, 0.9% by mass or more, 1.0% by mass or more, 1.3% by mass or more, 1.5% by mass or more, 1.7% by mass or more, 1.9% by mass or more, 2.0% by mass or more, 2.1% by mass or more, 2.3% by mass or more, 2.5% by mass or more, 2.7% by mass or more, or 2.9% by mass or more, and may be 5.0% by mass or less, 4.7% by mass or less, 4.5% by mass or less, 4.3% by mass or less, 4.0% by mass or less, 3.7% by mass or less, 3.5% by mass or less, 3.3% by mass or less, or 3.1% by mass or less.

[0042] The ratio of the mass of the dispersant to the mass of the polytetrafluoroethylene particles is preferably 0.001 or more, 0.005 or more, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, or 0.09 or more from the viewpoint of dispersion stability, and is preferably 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, or 0.11 or less from the viewpoint of improving film-formability when mixed with the active material.

[0043] <<Method for producing slurry for secondary battery>> The slurry for secondary batteries can be produced by mixing the non-aqueous PTFE dispersion for secondary batteries and a battery material, particularly a particulate battery material. The conditions for producing the slurry for secondary batteries are not particularly limited. For example, the slurry for secondary electrodes can be produced by a method including a step of preparing the non-aqueous dispersion, then adding an active material, a conductive material, etc. as a battery material constituting the slurry for secondary batteries, and mixing while stirring as necessary, or a method including a step of adding an active material, a conductive material, etc. at the same time as preparing the non-aqueous dispersion. In addition to the solvent contained in the non-aqueous dispersion, other solvents may be added.

[0044] When the above-mentioned non-aqueous PTFE dispersion for secondary batteries is mixed with an active material, the polytetrafluoroethylene particles of the non-aqueous PTFE dispersion for secondary batteries fibrillate and enter between the particles of the active material, and the fibrillated polytetrafluoroethylene particles surround the active material, thereby binding the active material.

[0045] The mixing can be carried out using a known mixing means, for example, a stirring and mixing means such as a planetary mixer.

[0046] The battery materials may include a positive electrode active material, a negative electrode active material, a conductive material, and a solid electrolyte. That is, the slurry for the secondary battery may be a slurry for a positive electrode of a secondary battery, a slurry for a positive electrode of a secondary battery, or a slurry for a solid electrolyte.

[0047] (Cathode active material) As the positive electrode active material, for example, metal compounds such as metal oxides and metal sulfides capable of doping or intercalating lithium ions, and conductive polymers can be used. Examples include oxides of transition metals such as Fe, Co, Ni, and Mn, composite oxides with lithium, and inorganic compounds such as transition metal sulfides. Specifically, MnO, VO, VO 13, transition metal oxide powders such as TiO2, layered lithium nickelate, lithium cobaltate, lithium manganate, spinel-structured lithium manganate, ternary (NCM) lithium materials, for example LiNi 0.8 Co 0.1 Mn 0.1 Composite oxide powders of lithium and transition metals such as O2, lithium iron phosphate-based materials which are olivine-structured phosphate compounds, transition metal sulfide powders such as TiS2 and FeS, etc. can be mentioned. Also, conductive polymers such as polyaniline, polyacetylene, polypyrrole, and polythiophene can be used. Further, the above inorganic compounds and organic compounds may be mixed and used.

[0048] (Anode active material) As the anode active material, graphite materials such as graphite (natural graphite, artificial graphite, etc.), coke, and carbon fiber; elements capable of forming an alloy with lithium, that is, for example, elements such as silicon-based compounds, Al, Sn, Ag, Bi, Mg, Zn, In, Ge, Pb, and Ti; compounds containing elements capable of forming an alloy with lithium; composites of elements capable of forming an alloy with lithium and the above compounds with carbon and / or the above graphite materials, or nitrides containing lithium, etc. can be exemplified. Among these, graphite materials and silicon-based compounds are preferable, and as graphite and silicon-based compounds, silicon particles or silicon oxide particles are more preferable.

[0049] In addition, the silicon oxide in the present invention is represented by SiO x (0 < x ≤ 2). Also, in the present invention, as the anode active material, a silicon compound alone may be used, or a composite of a silicon-based compound and a graphite material may be used.

[0050] For example, titanium oxide can be used as the metal oxide-based negative electrode active material particles. The titanium oxide is not particularly limited as long as it can absorb and release lithium, but for example, spinel-type lithium titanate, ramsdellite-type lithium titanate, titanium-containing metal composite oxide, titanium dioxide (TiO2(B)) having a monoclinic crystal structure, and anatase-type titanium dioxide can be used.

[0051] Spinel-type lithium titanate includes Li 4+x Ti5O 12 (x varies in the range of -1≦x≦3 depending on the charge / discharge reaction). Ramsdellite-type lithium titanate includes Li 2+y Ti3O7 (where y varies in the range of -1≦y≦3 depending on the charge / discharge reaction). TiO2(B) and anatase-type titanium dioxide include Li 1+z TiO2 (z changes in the range of -1≦z≦0 depending on the charge / discharge reaction).

[0052] Examples of titanium-containing metal composite oxides include metal composite oxides containing Ti and at least one element selected from the group consisting of P, V, Sn, Cu, Ni, and Fe. Examples of metal composite oxides containing Ti and at least one element selected from the group consisting of P, V, Sn, Cu, Ni, and Fe include TiO2-P2O5, TiO2-V2O5, TiO2-P2O5-SnO2, and TiO2-P2O5-MeO (Me is at least one element selected from the group consisting of Cu, Ni, and Fe).

[0053] Such a metal composite oxide preferably has a microstructure with low crystallinity, in which a crystalline phase and an amorphous phase coexist, or in which an amorphous phase exists alone, which can further improve cycle performance.

[0054] The content of the active material may be 40 mass% or more, 45 mass% or more, 50 mass% or more, 55 mass% or more, 60 mass% or more, or 65 mass% or more, and may be 80 mass% or less, 75 mass% or less, or 70 mass% or less, relative to the mass of the slurry for secondary batteries.

[0055] (solid electrolyte) As the solid electrolyte, a known solid electrolyte can be used, and examples of the solid electrolyte include an organic solid electrolyte and an inorganic solid electrolyte.

[0056] Examples of the organic solid electrolyte include polymer electrolytes such as polyethylene oxide (PEO) and organic electrolyte salts such as lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0057] Examples of inorganic solid electrolytes include (i) sulfide-based inorganic solid electrolytes, (ii) oxide-based inorganic solid electrolytes, (iii) halide-based inorganic solid electrolytes, and (iv) hydride-based inorganic solid electrolytes. Among these, sulfide-based inorganic solid electrolytes are preferred from the viewpoint of forming a better interface between the active material and the inorganic solid electrolyte.

[0058] (i) The sulfide-based inorganic solid electrolyte preferably contains sulfur atoms, has the ionic conductivity of a metal belonging to Group 1 or 2 of the periodic table, and has electronic insulation. The sulfide-based inorganic solid electrolyte preferably contains at least Li, S, and P as elements and has lithium ion conductivity, but may contain elements other than Li, S, and P depending on the purpose or case.

[0059] An example of the sulfide-based inorganic solid electrolyte is a lithium ion conductive inorganic solid electrolyte that satisfies the composition represented by the following formula (S1). L a1 M b1 P c1 S d1 A e1 (S1) In the formula, L represents an element selected from Li, Na, and K, and Li is preferred. M represents an element selected from B, Zn, Sn, Si, Cu, Ga, Sb, Al, and Ge. A represents an element selected from I, Br, Cl, and F. a1 to e1 represent the composition ratio of each element, and a1:b1:c1:d1:e1 satisfies 1-12:0-5:1:2-12:0-10. a1 is preferably 1.0 or more, 1.5 or more, or 2.0 or more, and 9.0 or less, 8.5 or less, or 7.5 or less. b1 is more preferably 0 or more, and 3.0 or less, 2.0 or less, or 1.0 or less. d1 is preferably 2.5 or more, or 3.0 or more, and 10.0 or less, 9.0 or less, or 8.5 or less. e1 is preferably 0 or more, and 5.0 or less, 4.0 or less, or 3.0 or less.

[0060] The composition ratio of each element can be controlled by adjusting the blending amounts of the raw material compounds when producing the sulfide-based inorganic solid electrolyte, as described below.

[0061] The sulfide-based inorganic solid electrolyte may be amorphous (glass) or crystallized (glass ceramic), or may be partially crystallized. For example, Li-PS-based glass containing Li, P, and S, or Li-PS-based glass ceramic containing Li, P, and S can be used.

[0062] The sulfide-based inorganic solid electrolyte can be produced by reacting at least two or more raw materials selected from the group consisting of lithium sulfide (LiS), phosphorus sulfide (e.g., diphosphorus pentasulfide (PS)), elemental phosphorus, elemental sulfur, sodium sulfide, hydrogen sulfide, lithium halides (e.g., LiI, LiBr, LiCl), and sulfides of elements represented by M above (e.g., SiS, SnS, GeS).

[0063] In the Li-PS glass and Li-PS glass ceramics, the ratio of Li2S to P2S5 is preferably 60:40 to 90:10, more preferably 68:32 to 78:22, in terms of the molar ratio of Li2S:P2S5. By setting the ratio of Li2S to P2S5 within this range, the lithium ion conductivity can be made high. Specifically, the lithium ion conductivity is preferably set to 1×10 -4 S / cm or more, 3×10 -4 S / cm or more, 5×10 -4 S / cm or more, 7×10 -4 S / cm or more, or 1×10 -3 S / cm or more. There is no upper limit, but it is 1×10 -1 It is practical to have a value of less than S / cm.

[0064] As specific examples of sulfide-based inorganic solid electrolytes, examples of combinations of raw materials are shown below. For example, Li2S-P2S5, Li2S-P2S5-LiCl, Li2S-P2S5-H2S, Li2S-P2S5-H2S-LiCl, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SiS2-LiCl, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3 , Li2S-GeS2, Li2S-GeS2-ZnS, Li2S-Ga2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2S-SiS2, L i2S-Al2S3, Li2S-SiS2-Al2S3, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-LiI, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, Li 10Examples include GeP2S12. However, the mixing ratio of each raw material is not limited. As a method for synthesizing a sulfide-based inorganic solid electrolyte material using such a raw material composition, for example, an amorphization method can be mentioned. Examples of the amorphization method include a mechanical milling method, a solution method, and a melt quenching method. According to these methods, processing at room temperature becomes possible, and simplification of the manufacturing process can be achieved.

[0065] (ii) The oxide-based inorganic solid electrolyte preferably contains oxygen atoms, has ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and has electron insulation. The ionic conductivity of the oxide-based inorganic solid electrolyte is preferably 1×10 -6 S / cm or more, 3×10 -6 S / cm or more, 5×10 -6 S / cm or more, 7×10 -6 S / cm or more, or 1×10 -5 S / cm or more. The upper limit is not particularly limited, but it is practical that it is 1×10 -1 S / cm or less.

[0066] Specific compound examples include, for example, Li xa La ya TiO3 (xa satisfies 0.3 ≤ xa ≤ 0.7, and ya satisfies 0.3 ≤ ya ≤ 0.7.) (LLT); Li xb La yb Zr zb Mbb mb O nb (Mbb is one or more elements selected from Al, Mg, Ca, Sr, V, Nb, Ta, Ti, Ge, In, and Sn. xb satisfies 5 ≤ xb ≤ 10, yb satisfies 1 ≤ yb ≤ 4, zb satisfies 1 ≤ zb ≤ 4, mb satisfies 0 ≤ mb ≤ 2, and nb satisfies 5 ≤ nb ≤ 20.); Li xc B yc Mcc zc O nc (Mcc is one or more elements selected from C, S, Al, Si, Ga, Ge, In, and Sn. xc satisfies 0 < xc ≤ 5, yc satisfies 0 < yc ≤ 1, zc satisfies 0 < zc ≤ 1, and nc satisfies 0 < nc ≤ 6.); Lixd (Al, Ga) yd (Ti, Ge) zd Si ad P md O nd (xd satisfies 1 ≤ xd ≤ 3, yd satisfies 0 ≤ yd ≤ 1, zd satisfies 0 ≤ zd ≤ 2, ad satisfies 0 ≤ ad ≤ 1, md satisfies 1 ≤ md ≤ 7, nd satisfies 3 ≤ nd ≤ 13); Li (3-2xe) Mee xe DeeO (xe represents a number from 0 or more to 0.1 or less, Mee represents a divalent metal atom. Dee represents a halogen atom or a combination of two or more halogen atoms.); Li xf Si yf O zf (xf satisfies 1 ≤ xf ≤ 5, yf satisfies 0 < yf ≤ 3, zf satisfies 1 ≤ zf ≤ 10); Li xg S yg O zg (xg satisfies 1 ≤ xg ≤ 3, yg satisfies 0 < yg ≤ 2, zg satisfies 1 ≤ zg ≤ 10); Li3BO3; Li3BO3 - Li2SO4; Li2O - B2O3 - P2O5; Li2O - SiO2; Li6BaLa2Ta2O12; Li3PO(4 - 3 / 2w)Nw (w is w < 1); Li having a LISICON (Lithium super ionic conductor) type crystal structure 3.5 Zn 0.25 GeO4; La having a perovskite type crystal structure 0.55 Li 0.35 TiO3; LiTi2P3O12 having a NASICON (Natrium super ionic conductor) type crystal structure; Li 1+xh+yh (Al, Ga) xh (Ti, Ge) 2-xh Si yh P 3-yh O 12 (xh satisfies 0 ≤ xh ≤ 1, yh satisfies 0 ≤ yh ≤ 1); Li7La3Zr2O having a garnet type crystal structure 12(LLZ), etc. Also preferred are phosphorus compounds containing Li, P and O. Examples include lithium phosphate (Li3PO4); LiPON in which part of the oxygen element of lithium phosphate is replaced with nitrogen element; LiPOD1 (D1 is preferably one or more elements selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Ag, Ta, W, Pt and Au), etc. Furthermore, LiAlON (A1 is one or more elements selected from Si, B, Ge, Al, C and Ga), etc. can also be preferably used.

[0067] (iii) The halide-based inorganic solid electrolyte is preferably a compound that contains a halogen atom, has ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and has electronic insulation. The halide-based inorganic solid electrolyte is not particularly limited, but examples thereof include compounds such as LiCl, LiBr, LiI, Li3YBr6, and Li3YCl6 described in ADVANCED MATERIALS, 2018, 30, 1803075. Among these, Li3YBr6 and Li3YCl6 are preferred.

[0068] (iv) The hydride-based inorganic solid electrolyte is preferably a compound that contains hydrogen atoms, has the ionic conductivity of a metal belonging to Group 1 or 2 of the periodic table, and has electronic insulation. The hydride-based inorganic solid electrolyte is not particularly limited, but examples thereof include LiBH4, Li4(BH4)3I, and 3LiBH4-LiCl.

[0069] (Conductive material) The conductive material may be, for example, a carbon-based conductive material, which may be carbon fibers, carbon nanotubes (CNTs), and / or carbon particles.

[0070] Carbon fibers include, but are not limited to, milled fibers, chopped fibers, etc. These may be used alone or in combination.

[0071] The average length of the carbon fibers can be 1 μm or more, 3 μm or more, 5 μm or more, 10 μm or more, or 15 μm or more, and can be 100 μm or less, 70 μm or less, 50 μm or less, or 30 μm or less.

[0072] Examples of carbon particles include graphene, graphite, and carbon black such as acetylene black and ketjen black, etc. These may be used alone or in combination.

[0073] The shape of the carbon particles is not particularly limited, and may be, for example, flat, array-like, spherical, or the like.

[0074] The average particle size of the carbon particles can be 100 nm or more, 200 nm or more, 300 nm or more, 500 nm or more, 700 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and can be 20 μm or less, 15 μm or less, 10 μm or less, or 7 μm or less. Here, the average particle size adopted in this specification is appropriately selected depending on the size of the target carbon particles, and in the case of particles less than about 1 μm, it is the value of the histogram average particle size (D50) based on the scattering intensity distribution measured by the dynamic light scattering method, and in the case of particles of 1 μm or more, it is the value of the median size (D50) calculated on a volume basis in the laser diffraction method. Measurement by the dynamic light scattering method can be performed using, for example, DelsaMax CORE (Beckman Coulter, Inc.). Measurement by the laser diffraction method can be performed using, for example, a particle size distribution measuring device MT3300II (Microtrack Bell, Inc.).

[0075] The content of the carbonaceous conductive material in the electrode layer-forming non-aqueous dispersion liquid may be 1.0 mass % or more, 1.5 mass % or more, 2.0 mass % or more, or 2.5 mass % or more, and may be 15.0 mass % or less, 12.0 mass % or less, 10.0 mass % or less, 8.0 mass % or less, 6.0 mass % or less, 5.0 mass %, 4.5 mass % or less, 4.0 mass % or less, 3.5 mass % or less, or 3.0 mass % or less, based on the total mass of the electrode layer-forming non-aqueous dispersion liquid.

[0076] <Other solvents> The other solvent may be the non-aqueous solvent mentioned in relation to the non-aqueous PTFE dispersion for secondary batteries. The other solvent may be the same as or different from the solvent contained in the non-aqueous dispersion. It is preferable to mix the non-aqueous dispersion so that the polytetrafluoroethylene solid content is 5% by mass or less, 4% by mass or less, 3% by mass or less, 2% by mass or less, or 1% by mass or less relative to 100% by mass of the slurry for secondary batteries. EXAMPLES

[0077] The present invention will be specifically described with reference to examples and comparative examples, but the present invention is not limited to these.

[0078] <<Preparation of non-aqueous PTFE dispersion for secondary batteries>> Example 1 3 parts by mass of a urethane-based wetting dispersant (DISPERBYK-162, BYK) was dissolved in 67 parts by mass of xylene as a non-aqueous solvent. Then, 30 parts by mass of polytetrafluoroethylene (PTFE) particles were added thereto and stirred and mixed using a disperser. As the PTFE particles, PTFE particles A (F-106, Daikin Industries, Ltd., average particle size 550 μm, apparent density 500 g / L, elongation rate 600%, average primary particle size 250 nm, melting point 327°C) were used. Then, the mixture was passed through a circulation bead mill nine times to carry out dispersion. Then, the mixture was subjected to mesh filtration to remove coarse particles of 500 μm or more, and a non-aqueous PTFE dispersion for secondary batteries of Example 1 was prepared.

[0079] The number of bead mill treatments in Table 1 is counted as one treatment in which the PTFE particles pass through the bead-packed section of the mill.

[0080] The particle size distribution of the obtained non-aqueous PTFE dispersion for secondary batteries was measured by a laser diffraction method to obtain D10, D50 (average particle size), and D90 on a volume basis. The measurement was performed at 25°C in an ethanol solvent using an LA-960 manufactured by Horiba, Ltd.

[0081] Moreover, the water content of the obtained nonaqueous PTFE dispersion for secondary batteries was measured by the Karl Fischer method.

[0082] Examples 2 to 5 and Comparative Examples 1 to 4 Non-aqueous PTFE dispersions for secondary batteries of Examples 2 to 5 and Comparative Examples 1 to 4 were prepared in the same manner as in Example 1, except that the PTFE particles shown in Table 1 were used. Details of the PTFE particles shown in Table 1 are as follows. PTFE particle B: F-104, Daikin Industries, Ltd., average particle size 500 μm, apparent density 460 g / L, elongation rate 400%, average primary particle size 250 nm, melting point 327°C PTFE particles C: F-208, Daikin Industries, Ltd., average particle size 610 μm, apparent density 490 g / L, elongation rate 560%, average primary particle size 250 nm, melting point 325°C PTFE particle D: TLP10F-1, Mitsui Chemours Fluoro Products Co., Ltd., elongation 350%, average primary particle size 300 nm, melting point 329°C Butyral dispersant: S-LEC BL-5Z (Sekisui Chemical Co., Ltd.) Acrylic dispersant: Disperbyk-2000 (BYK)

[0083] In addition, only in Comparative Example 3, the above-mentioned mesh filtration was not carried out.

[0084] <Evaluation of PTFE dispersion> <Dispersion stability> The non-aqueous PTFE dispersion for secondary batteries thus prepared was left to stand for 24 hours, and then the D90 value was measured on a volume basis using a laser diffraction method to evaluate the dispersion stability of each of the aqueous dispersions for forming an electrode layer in Examples 1 to 9, Comparative Examples 1 to 7, and Reference Example. The evaluation criteria were as follows: A: The D90 value after standing was 50 μm or less. B: The D90 value after standing was greater than 50 μm and less than 100 μm. C: The D90 value after standing was more than 100 μm.

[0085] <Evaluation of slurry for secondary batteries (positive electrodes)> <Mixability with active materials> 10 parts by mass of the above non-aqueous PTFE dispersion for secondary batteries, 0.4 parts by mass of acetylene black as a conductive material, 74.6 parts by mass of lithium nickel-cobalt-manganese oxide (NCM) as an active material, and 15 parts by mass of xylene as a solvent were dispersed using a planetary mixer to prepare 100 parts by mass of slurry for secondary battery positive electrodes.

[0086] The appearance of the obtained slurry for secondary battery positive electrodes was visually confirmed and the evaluation criteria were as follows: A: PTFE particle fibrils and active material were uniformly mixed. B: PTFE particle fibrils and active material were unevenly distributed.

[0087] <<Creation of coating film>> The obtained slurry for secondary battery positive electrodes was applied to an aluminum foil with a wet film thickness of 100 μm to a length of 10 m using a comma coater with a coating width of 200 mm. The following evaluations were carried out on this coating film.

[0088] <Film forming property> The appearance of the resulting coating film was visually observed to evaluate the film formability, and the evaluation criteria were as follows: A: A uniform and flat coating was formed. B: Although some unevenness was observed on the surface, a uniform coating film was formed. C: A uniform coating film was not formed, and the surface of the aluminum foil was exposed.

[0089] Table 1 shows the configurations and evaluation results of the examples and comparative examples.

[0090] [Table 1]

[0091] From Table 1, it can be seen that the nonaqueous PTFE dispersions for secondary batteries of Examples 1 to 5, which contain PTFE particles having a D10 of 2.0 μm or more, a D90 of 50 μm or less, and an elongation of 380 to 1000% measured in accordance with ASTM D4895, have good dispersion stability and miscibility with active materials.

Claims

1. It contains polytetrafluoroethylene particles, a non-aqueous solvent, and a dispersant, In the particle size distribution of the polytetrafluoroethylene particles measured by a laser diffraction method, D10 is 2.0 μm or more and D90 is 50 μm or less, and The polytetrafluoroethylene particles have an elongation of 380 to 1000% as measured in accordance with ASTM D4895. Non-aqueous PTFE dispersion liquid for secondary batteries.

2. 2. The nonaqueous PTFE dispersion for secondary batteries according to claim 1, wherein the polytetrafluoroethylene particles have an average primary particle diameter of 100 nm to 500 nm as measured by a scanning electron microscope.

3. 3. The non-aqueous PTFE dispersion for secondary batteries according to claim 1, wherein in the particle size distribution, D50 is 12 μm to 45 μm.

4. 3. The nonaqueous PTFE dispersion for a secondary battery according to claim 1, wherein the water content is 8000 ppm or less.

5. 3. The non-aqueous PTFE dispersion for secondary batteries according to claim 1, wherein the content of the polytetrafluoroethylene particles is 5% by mass to 60% by mass relative to the mass of the non-aqueous PTFE dispersion for secondary batteries.

6. 3. The non-aqueous PTFE dispersion for secondary batteries according to claim 1, wherein the ratio of the mass of the dispersant to the mass of the polytetrafluoroethylene particles is 0.001 to 0.

15.

7. 3. The non-aqueous PTFE dispersion for a secondary battery according to claim 1, wherein the dispersant is at least one selected from the group consisting of polyvinyl alcohol-based, butyral-based, acrylic-based, and urethane-based dispersants.

8. The non-aqueous PTFE dispersion for secondary batteries according to claim 1 or 2, wherein the non-aqueous solvent is at least one selected from the group consisting of aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, aromatic polar solvents, alcohols, polyhydric alcohols, glycol ethers, esters, and aprotic polar solvents.

9. A method for producing a slurry for a secondary battery, comprising mixing the nonaqueous PTFE dispersion for a secondary battery according to claim 1 or 2 and a battery material.

Citation Information

Patent Citations

  • Non-aqueous dispersion of polytetrafluoroethylene micropowder

    JP2017066327A

  • Binder for cell and composition for electrode and cell prepared therefrom

    WO1996012764A1