Method for producing low-molecular-weight polytetrafluoroethylene
By controlling the dose rate ratio during the irradiation of high molecular weight PTFE, the method achieves uniform molecular weight distribution in low molecular weight PTFE, addressing the variability issue and improving its performance as an additive in various applications.
Patent Information
- Application Number
- JP2023080864
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing low molecular weight polytetrafluoroethylene (PTFE) result in significant variations in molecular weight due to uneven radiation absorption during the irradiation process.
The method involves irradiating high molecular weight PTFE in a batch manner with a controlled dose rate ratio (maximum dose rate/minimum dose rate) of 2.00 or less, using electron beams or gamma rays, and maintaining specific irradiation conditions to achieve a melt viscosity of 1.0×10^2 Pa·s to 7.0×10^5 Pa·s, ensuring uniform molecular weight distribution.
This approach produces low molecular weight PTFE with minimal variation in molecular weight, enhancing its applicability as an additive in coatings, inks, cosmetics, and greases by improving slipperiness and texture.
Smart Images

Figure 2024165044000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing low molecular weight polytetrafluoroethylene. [Background technology]
[0002] Low-molecular-weight polytetrafluoroethylene (also called "polytetrafluoroethylene wax" or "polytetrafluoroethylene micropowder"), which has a molecular weight of several thousand to several hundred thousand, has excellent chemical stability, extremely low surface energy, and is not prone to fibrillation, and is therefore used as an additive to improve the slipperiness and texture of coating surfaces in the production of plastics, inks, cosmetics, paints, greases, and the like (see, for example, Patent Document 1).
[0003] Known methods for producing low-molecular-weight polytetrafluoroethylene include a polymerization method, a radiolysis method, a thermal decomposition method, etc. Patent Document 2 describes a method for producing low-molecular-weight polytetrafluoroethylene by a radiolysis method.
[0004] Patent Documents 3 and 4 describe a method in which polytetrafluoroethylene is continuously irradiated with electron beams while being stirred in a container. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-147617 [Patent Document 2] International Publication No. 2020 / 013336 [Patent Document 3] U.S. Pat. No. 4,777,192 [Patent Document 4] U.S. Patent No. 6,486,481 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present disclosure is to provide a method for producing low molecular weight polytetrafluoroethylene (PTFE) with small variation in molecular weight. [Means for solving the problem]
[0007] The present disclosure (1) relates to a method for producing a high molecular weight polytetrafluoroethylene having a melt viscosity of 1.0×10 at 380° C. by irradiating the high molecular weight polytetrafluoroethylene with radiation in a batch system so that the ratio of the maximum dose rate to the minimum dose rate (maximum dose rate / minimum dose rate) is 2.00 or less. 2 Pa·s or more, 7.0×10 5 A method for producing low-molecular-weight polytetrafluoroethylene, comprising the step (1) of obtaining low-molecular-weight polytetrafluoroethylene having a molecular weight of not more than Pa·s.
[0008] The present disclosure (2) is the manufacturing method of the present disclosure (1), in which the minimum absorbed dose of the radiation is 50 kGy or more and less than 200 kGy.
[0009] The present disclosure (3) is the production method of the present disclosure (1) or (2), in which the irradiation is carried out in the presence of oxygen.
[0010] The present disclosure (4) is a manufacturing method of any combination with any of the present disclosures (1) to (3) in which the radiation is an electron beam, a gamma ray, or an X-ray.
[0011] The present disclosure (5) is a manufacturing method for any combination with any of the present disclosures (1) to (4), in which the irradiation is carried out at a distance of 10 m or less from the source of the radiation to the furthest part of the high molecular weight polytetrafluoroethylene.
[0012] The present disclosure (6) is a manufacturing method for any combination with any of the present disclosures (1) to (5), in which the irradiation is carried out with the distance from the radiation source to the closest part of the high molecular weight polytetrafluoroethylene being 5 cm or more.
[0013] The present disclosure (7) is a manufacturing method for any combination with any of the present disclosures (1) to (6), in which the high molecular weight polytetrafluoroethylene is placed in a position facing the effective area of the radiation source, the irradiation is performed, and the effective area is an area whose distance from the center of the radiation source is 95% or less of the distance from the center to an end of the radiation source.
[0014] The present disclosure (8) is a manufacturing method for any combination with any of the present disclosures (1) to (7), in which the irradiation is performed on the high molecular weight polytetrafluoroethylene filled in an irradiation container composed of at least one material selected from the group consisting of metals, glasses, ceramics, and organic materials.
[0015] The present disclosure (9) is the manufacturing method of the present disclosure (8), wherein the irradiation container is cylindrical or prismatic.
[0016] The present disclosure (10) is a manufacturing method according to the present disclosure (8) or (9), wherein the irradiation container has at least one surface selected from the group consisting of a plate-like surface, a mesh-like surface, and a surface having a slit-like opening.
[0017] The present disclosure (11) is a manufacturing method for performing the above-mentioned irradiation by arranging a plurality of irradiation containers filled with the above-mentioned high molecular weight polytetrafluoroethylene in a row and performing the above-mentioned irradiation in any combination with any of the present disclosures (1) to (10).
[0018] The present disclosure (12) is a method for producing an arbitrary combination of the high molecular weight polytetrafluoroethylene with any one of the present disclosures (1) to (11) in which the standard specific gravity of the high molecular weight polytetrafluoroethylene is 2.130 or more and 2.230 or less.
[0019] The present disclosure (13) is a method for producing an arbitrary combination of the high-molecular-weight polytetrafluoroethylene and the low-molecular-weight polytetrafluoroethylene, both of which are powders, with any of the present disclosures (1) to (12).
[0020] The present disclosure (14) further includes, before the step (1), a step (2) of obtaining a molded article by heating the high molecular weight polytetrafluoroethylene to a temperature equal to or higher than its primary melting point, and the molded article has a specific gravity of 1.0 g / cm 3 This is a method for producing any combination of any of the above-mentioned disclosures (1) to (13). Effect of the Invention
[0021] According to the present disclosure, it is possible to provide a method for producing low-molecular-weight PTFE with small variation in molecular weight. [Brief description of the drawings]
[0022] [Figure 1] FIG. 2 is a diagram showing an example of a mode of radiation irradiation. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of an irradiation container filled with high molecular weight PTFE. [Diagram 3] FIG. 11 is a cross-sectional view showing another example of an irradiation container filled with high molecular weight PTFE. [Figure 4] FIG. 13 is a diagram showing an example of the arrangement of irradiation containers. [Diagram 5] FIG. 2 is a diagram showing the positional relationship between a radiation source and an irradiation target, and sampling points in Examples 1 and 2 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Conventionally, when high molecular weight PTFE is irradiated with radiation, there is a problem in that the absorbed dose of radiation varies greatly depending on the position in the irradiation container, resulting in large variations in the molecular weight of the obtained low molecular weight PTFE. The present inventors have found that by irradiating radiation so that the ratio of the maximum dose rate to the minimum dose rate falls within a specific range, the variation in molecular weight of the resulting low-molecular-weight PTFE can be suppressed, and have completed the manufacturing method of the present disclosure. The present disclosure will now be described in detail.
[0024] In this specification, there are some places where the expression "~" is used to indicate a numerical range from a lower limit value to an upper limit value, but the numerical range in this description is a numerical range specified as being equal to or greater than the lower limit value and equal to or less than the upper limit value, including the lower limit value and the upper limit value.
[0025] The present disclosure relates to a method for producing a high molecular weight PTFE having a melt viscosity of 1.0×10 at 380° C. by irradiating the high molecular weight PTFE with radiation in a batch system so that the ratio of the maximum dose rate to the minimum dose rate (maximum dose rate / minimum dose rate) is 2.00 or less. 2 Pa·s or more, 7.0×10 5 The present invention relates to a method for producing a low-molecular-weight PTFE, comprising the step (1) of obtaining a low-molecular-weight PTFE having a molecular weight of not more than Pa·s.
[0026] In step (1), the high molecular weight PTFE is irradiated with radiation in a batch manner so that the ratio of the maximum dose rate to the minimum dose rate (hereinafter also referred to as the dose rate ratio) is 2.00 or less. By keeping the dose rate ratio within the above range, a low molecular weight PTFE with small molecular weight variation can be obtained. The dose rate ratio is preferably 1.90 or less, more preferably 1.70 or less, even more preferably 1.50 or less, and particularly preferably 1.30 or less. The dose rate ratio may also be 1.00 or more, 1.10 or more, or greater than 1.55.
[0027] The dose rate ratio is calculated as a ratio between the maximum and minimum absorbed dose rates obtained at multiple locations in an irradiation container containing a sample. The absorbed dose rates are calculated at least at a location where the dose value is expected to be the smallest (e.g., the center of the irradiation container or the inner surface of the irradiation container farthest from the radiation source) and a location where the dose value is expected to be the highest (e.g., the inner surface of the irradiation container closest to the radiation source). The absorbed dose rate can be measured by two methods: actual measurement using a chemical dosimeter and calculation simulation using the Monte Carlo simulation code "PHITS" (Journal of Nuclear Science and Technology, 2018, Vol. 55, No. 6, p. 684-690). Alanine dosimeters and PMMA dosimeters can be used as chemical dosimeters. Three alanine dosimeters are installed in the area where the dose value is expected to be the smallest. Additionally, five PMMA dosimeters, which are used for radiation process management, are installed per surface area in the area where the dose value is expected to be the highest. When an alanine dosimeter is used, the dose is calculated using a calibration curve prepared from an alanine dosimeter standard sample based on the ESR spectrum measured by electron spin resonance (microwave frequency set to 9.8 GHz, resonance magnetic field set to 350 mT) specifically for the alanine-derived radical in the crystal, in accordance with ISO / ASTM51607 and JIS standards (JIS Z4571). When using a PMMA dosimeter, RadixW (manufactured by Radie Industrial Co., Ltd.) is used as the dosimeter, and after irradiation in accordance with ISO / ASTM51276 and JIS standards (JIS Z4572), the absorbance at 320 nm or 280 nm is measured using a spectrophotometer, and the dose is calculated from the calibration curve. In the simulation using PHITS, the actual size, number, and irradiation time of the cobalt radiation source, the size, material, and shape of the irradiation container, as well as the size, material, and actual arrangement of the walls and floor in the irradiation chamber that affect the transmission and scattering of radiation, are simulated, and a Monte Carlo simulation is performed in accordance with ISO / ASTM52303 and JIS standards (JIS Z4574). The simulation allows for a more detailed evaluation of the dose distribution inside the irradiation container. Among the multiple evaluation points obtained by the PHITS simulation, the dose rate evaluation results at the same locations as the actual measurement points using a chemical dosimeter were compared with the actual measurements, and the validity of the simulation results was confirmed.
[0028] When irradiating samples in a plurality of irradiation containers, the dose rate ratio between the containers is preferably within the above-mentioned range. In this case, the dose rate ratio calculated from the maximum and minimum absorbed dose rates of the samples in the plurality of containers may be adjusted to within the above-mentioned range, or the dose ratio calculated from the minimum absorbed dose of the samples in the entirety and the maximum absorbed dose in each container may be adjusted to within the above-mentioned range.
[0029] The above-mentioned radiation is not particularly limited as long as it is ionizing radiation, and examples thereof include electron beams, gamma rays, X-rays, neutron beams, and high-energy ions. From the viewpoint of industrial use, however, electron beams, gamma rays, or X-rays are preferred, and electron beams or gamma rays are more preferred. The electron beam can be generated, for example, from an electron accelerator. Gamma rays can be produced, for example, from radioisotopes. X-rays can be generated, for example, by irradiating a target such as a metal with a particle beam from a particle accelerator. Quasi-monochromatic X-rays can also be generated by inverse Compton scattering (laser Compton scattering) when a high-energy electron beam is collided with a laser beam. Furthermore, X-rays can be generated by synchrotron radiation, and X-rays can also be generated by installing an undulator or wiggler at the lower stage of a particle accelerator.
[0030] As the gamma ray source, a cobalt 60 source is preferred because it is widely used in industrial applications. Examples of the radiation source include rod-shaped or plate-shaped sources, with plate-shaped sources being preferred. Examples of the plate-shaped radiation source include rod-shaped radiation source pencils arranged on a flat plate.
[0031] The radiation is applied in batches. In this disclosure, irradiation in a batch mode means that the irradiation is carried out without feeding (addition) and draining (removal) of the contents (high molecular weight PTFE) of the irradiation vessel. Therefore, the batch-type irradiation in the present disclosure does not include a mode in which irradiation is performed while the contents are being supplied or discharged, but does include a mode in which irradiation is performed while the container is being moved on a conveyor or the like. It is preferable that the batch-type irradiation in the present disclosure does not involve substantial movement of the contents (high molecular weight PTFE) in the irradiation container. Here, substantial movement of the contents means that the position of the contents in the container is intentionally changed, and includes not only the above-mentioned supply (addition) and discharge (removal), but also stirring of the contents. Batch irradiation does not require dedicated irradiation equipment as in the continuous type, and existing irradiation containers and irradiation equipment can be used, which reduces costs. In addition, even small amounts of high molecular weight PTFE can be processed. Furthermore, it is easy to change the high molecular weight PTFE and irradiation conditions (irradiation amount, etc.) for processing. The radiation may be irradiated continuously until the desired absorbed dose is reached, or may be irradiated intermittently and repeatedly until the desired cumulative absorbed dose is reached.
[0032] The average absorbed dose of the radiation may be, for example, 10 kGy or more, preferably 30 kGy or more, more preferably 40 kGy or more, even more preferably 50 kGy or more, even more preferably 60 kGy or more, particularly preferably 70 kGy or more, and most preferably 80 kGy or more. The average absorbed dose may be 1000 kGy or less, preferably 750 kGy or less, more preferably 600 kGy or less, even more preferably 500 kGy or less, even more preferably 350 kGy or less, and particularly preferably less than 200 kGy. The average absorbed dose is calculated as the average value of the absorbed doses measured by dosimeters installed at multiple points on the surface of the irradiation container facing the radiation source. The dosimeter (chemical dosimeter) is as described above.
[0033] The average absorbed dose rate during irradiation with the above-mentioned radiation is not particularly limited, but for example, in the case of gamma rays emitted from cobalt 60 or the like, it is preferably 0.1 kGy / h or more, more preferably 1 kGy / h or more, and even more preferably 2 kGy / h or more. In the case of an electron beam from an electron accelerator, 0.1 kGy / s or more is preferable, 1 kGy / s or more is more preferable, and 10 kGy / s or more is even more preferable. In the case of irradiating a sample while moving it on a conveyor or the like, 0.1 kGy / pass or more is preferable, 1 kGy / pass or more is more preferable, and 10 kGy / pass or more is even more preferable. In the case of X-rays generated by irradiating a particle beam from a particle accelerator, particularly an electron beam from an electron accelerator, on a target for X-ray generation, the dose is preferably 5 Gy / s or more, more preferably 50 Gy / s or more, even more preferably 0.1 kGy / s or more, even more preferably 0.5 kGy / s or more, particularly preferably 1 kGy / s or more, and most preferably 10 kGy / s or more. When irradiating a sample while moving it on a conveyor or the like, the dose is preferably 0.1 kGy / pass or more, more preferably 1 kGy / pass or more, and even more preferably 10 kGy / pass or more. The average absorbed dose rate is calculated as the average value of the absorbed dose rates measured by dosimeters installed at multiple points on the surface of the irradiation container. The dosimeter (chemical dosimeter) is as described above. It can also be calculated by the PHITS calculation simulation described above. The dosimeter and the calculation simulation may be used in combination.
[0034] The minimum absorbed dose of the radiation may be, for example, 10 kGy or more, preferably 30 kGy or more, more preferably 40 kGy or more, even more preferably 50 kGy or more, even more preferably 60 kGy or more, particularly preferably 70 kGy or more, and most preferably 80 kGy or more. The minimum absorbed dose may be 1000 kGy or less, preferably 750 kGy or less, more preferably 600 kGy or less, even more preferably 500 kGy or less, even more preferably 350 kGy or less, and particularly preferably less than 200 kGy. The minimum absorbed dose is determined as the absorbed dose measured by a dosimeter installed at a location where the dose value is expected to be the smallest (for example, the center of the irradiation container or the inner surface of the irradiation container farthest from the radiation source). The dosimeter (chemical dosimeter) is as described above.
[0035] The radiation irradiation temperature is not particularly limited as long as it is equal to or higher than the gamma dispersion temperature near -80°C and equal to or lower than the melting point of the high molecular weight PTFE. It is also known that molecular chains of high molecular weight PTFE crosslink near the melting point, and in order to suppress crosslinking, the temperature is preferably 320°C or lower, more preferably 310°C or lower, and even more preferably 300°C or lower. From an economical perspective, it is preferable to irradiate at a temperature range from room temperature to about 50°C, but the temperature may be raised in order to increase the efficiency of decomposition by radiation. The above irradiation temperature is the temperature of the sample (high molecular weight PTFE) during irradiation. Additionally, the sample temperature may be changed between -80°C and 320°C during radiation irradiation.
[0036] The irradiation may be carried out in any atmosphere, for example in air, in an inert gas, in vacuum, etc. It is also preferred to carry out the irradiation in the presence of oxygen. In this specification, "in the presence of oxygen" means that the oxygen concentration in the atmosphere in which the step is carried out is 2.0% by volume or more. The oxygen concentration may be 3.0% by volume or more, 5.0% by volume or more, 10% by volume or more, 15% by volume or more, or 20% by volume or more. In this case, the main component gas may be an inert gas, such as nitrogen gas, argon gas, helium gas, or a mixture thereof. The oxygen concentration can be easily measured by a method of analyzing the atmosphere in which the process is carried out, for example, the gas phase portion in a container in which the high molecular weight PTFE is placed, by gas chromatography, a method using an oxygen concentration measuring device, or a method of examining the color tone of an oxygen detector placed in the container.
[0037] The environment in which step (1) is carried out may be any of pressurized, atmospheric, and reduced pressure environments. The reduced pressure environment means an environment in which the pressure is reduced to a vacuum of 100 Pa or less using a vacuum pump such as a diaphragm pump, an oil rotary pump, or a scroll pump.
[0038] The irradiation in step (1) may be performed by fixing the high molecular weight PTFE in front of the radiation source, or may be performed while moving the high molecular weight PTFE so as to pass in front of the radiation source using a conveyor, etc. It is preferable to perform the irradiation while moving the high molecular weight PTFE, since this allows easy production of low molecular weight PTFE with small molecular weight variation.
[0039] FIG. 1 is a diagram showing an example of radiation irradiation. In the embodiment of FIG. 1, an irradiation container 11 filled with high-molecular-weight PTFE powder is placed on an irradiation table 12, and the high-molecular-weight PTFE is irradiated with radiation from a radiation source 10. When the irradiation table is a transport device such as a conveyor, irradiation is performed while moving the irradiation container so as to pass in front of the radiation source 10 (in the x-axis direction in the drawing). In each figure, the x-axis represents the width direction of radiation source 10, the y-axis represents the direction perpendicular to the radiation emission surface, and the z-axis represents the height direction of radiation source 10.
[0040] In the above irradiation, the distance from the radiation source to the closest part of the high-molecular-weight PTFE is not particularly limited, but it is preferably 5 cm or more for the safety of the apparatus. Furthermore, the distance from the source of the radiation to the furthest part of the high-molecular-weight PTFE may be 10 m or less, 5 m or less, or 2 m or less. This makes it easy to bring the dose rate ratio within the above-mentioned range. The distance from the radiation source refers to the distance from the radiation emission surface.
[0041] FIG. 2 is a cross-sectional view showing an example of an irradiation container filled with high molecular weight PTFE. In FIG. 2, the distance from the radiation source 10 to the farthest part of the high molecular weight PTFE powder 100 filled in the irradiation container 11 is a, and the distance from the radiation source 10 to the nearest part of the high molecular weight PTFE powder 100 is b.
[0042] In the above irradiation, the high-molecular-weight PTFE is preferably disposed at a position facing the effective area of the radiation source described below. The effective area may be an area on the radiation emission surface. (effective area) A region whose distance from the center of the radiation source is 95% or less, preferably 90% or less, of the distance from the center to the edge of the radiation source. When the radiation source is rod-shaped or plate-shaped, a sufficient absorbed dose may not be obtained from its ends, for example, near the upper and lower ends. By arranging the high molecular weight PTFE at a position facing the effective area of the radiation source as described above, a sufficient absorbed dose can be obtained from the entire high molecular weight PTFE, and the dose rate ratio can be easily set within the above-mentioned range. When irradiation is performed while moving the high molecular weight PTFE, it is preferable to move the high molecular weight PTFE so that each portion of the high molecular weight PTFE passes through the range at least once. When the irradiation is performed while moving the high molecular weight PTFE, the end of the radiation source in the definition of the effective region may be the end in the direction perpendicular to the moving direction of the high molecular weight PTFE. For example, when the high molecular weight PTFE is moved in the x-axis direction in FIG. 1, the end of the radiation source in the definition of the effective region may be the end (upper end, lower end) in the z-axis direction.
[0043] FIG. 3 is a cross-sectional view showing another example of an irradiation container filled with high molecular weight PTFE. In FIG. 3, the high molecular weight PTFE powder 100 is disposed a distance c below a position corresponding to the upper end of the radiation source 10 and a distance d above a position corresponding to the lower end of the radiation source 10 so as to face the effective area of the radiation source 10.
[0044] The above-mentioned irradiation is usually carried out on the above-mentioned high molecular weight PTFE filled in an irradiation container. The irradiation container is preferably made of at least one material selected from the group consisting of metal, glass, ceramics, and organic materials, and is more preferably made of metal in that it is less susceptible to deterioration due to radiation. Examples of the metal include stainless steel, copper, iron, titanium, and aluminum, and from the viewpoint of versatility, stainless steel is preferred, and highly corrosion-resistant stainless steel is more preferred. Examples of the organic material include paper, rubber, FRP (fiber reinforced plastic), and thermoplastic organic materials. As the irradiation container, a paper irradiation container is preferable from the viewpoint of disposability, and an FRP or aluminum irradiation container is preferable from the viewpoint of weight reduction. A fiber drum that is a combination of these is more preferable.
[0045] The irradiation container is preferably a sealed container.
[0046] The irradiation container has a density of 0.3 g / cm 3 It is preferable that the concentration is 1.0 g / cm or more. 3 More preferably, it is 3.0 g / cm or more. 3 More preferably, it is 19.3 g / cm or more. 3 It is preferable that the density is 8.9 g / cm or less. 3 More preferably, it is 8.0 g / cm or less. 3 It is even more preferable that: By setting the density of the irradiation container within the above range, the dose rate ratio can be easily set within the above range. The density is measured as an average density by a conventional density measuring method.
[0047] The shape of the irradiation container is not particularly limited and may be a cylindrical shape, a prismatic shape, or the like. A cylindrical shape is preferable from the viewpoint of uniform irradiation. Moreover, a prismatic shape is preferable, and a quadrangular prism shape is more preferable, from the viewpoint of reducing dead space in the installation location, facilitating installation of a dosimeter, facilitating container replacement and transportation, and the like. The irradiation container may be a container having a variable internal volume, such as a bag. A container having a variable internal volume and a container having a non-variable internal volume may be used in combination.
[0048] The surface constituting the irradiation container may be plate-shaped, but from the viewpoint of practical weight reduction, it may be, for example, mesh-shaped or may have slit-shaped openings. The irradiation container preferably has at least one type of surface selected from the group consisting of a plate-like surface, a mesh-like surface, and a surface having slit-like openings.
[0049] The size of the irradiation container is preferably such that the distance between the radiation source and the high-molecular-weight PTFE can be set within the above-mentioned range. For example, when the irradiation container is cylindrical, the diameter is preferably 5 to 110 cm, more preferably 10 cm or more, and more preferably 55 cm or less. When the irradiation container is in the shape of a prismatic column, the length of at least one side of the bottom surface is preferably 5 to 110 cm, more preferably 10 cm or more, and more preferably 55 cm or less. The height (depth) of the irradiation container can be determined according to, for example, the amount of high-molecular-weight PTFE to be filled and the size of the radiation source.
[0050] The thickness of the irradiation container, preferably the thickness of the side surface of the irradiation container, is preferably 0.1 to 10 mm, more preferably 1 mm or more, and more preferably 3 mm or less. By setting the thickness of the irradiation container within the above range, the dose rate ratio can be easily set within the above range.
[0051] The irradiation is preferably performed by arranging a plurality of irradiation containers filled with the high molecular weight PTFE in a row. The radiation is scattered by the irradiation table on which the irradiation containers are arranged, and the scattered radiation may wrap around the side of the irradiation container, resulting in a large difference in the dose between the center and the end of the container. By arranging a plurality of irradiation containers in a row, the wraparound of the scattered radiation is blocked by the adjacent irradiation containers, enabling more uniform irradiation. The above aspect is particularly suitable when the radiation source is plate-shaped. It is preferable that the irradiation containers are arranged in a line in a width direction of the radiation source. The plurality of irradiation containers may or may not be in contact with each other, but in terms of increasing the shielding effect against scattered radiation, it is preferable to arrange them as close as possible.
[0052] FIG. 4 is a diagram showing an example of the arrangement of irradiation containers. In FIG. 4, a plurality of irradiation containers 11 are arranged side by side in the width direction of the radiation source 10 (the x-axis direction in the figure).
[0053] The irradiation may be performed by stacking a plurality of irradiation containers filled with the high molecular weight PTFE in the height direction.
[0054] The irradiation is preferably performed from a plurality of different directions with respect to the high molecular weight PTFE, which allows for more uniform irradiation. Irradiation from a plurality of different directions does not necessarily have to be performed simultaneously, but may be performed sequentially by changing the direction of the high molecular weight PTFE (or irradiation container). In the above embodiment, irradiation may be performed from two or more directions, but the more directions the more uniform the irradiation can be. It is preferable to perform irradiation from at least one direction and the opposite direction.
[0055] The manufacturing method of the present disclosure may further include, prior to step (1), a step (2) of obtaining a molded article by heating the high-molecular-weight PTFE to a temperature equal to or higher than its primary melting point. In this case, the molded article obtained in step (2), cutting chips generated when the molded article is cut, or the molded article pulverized (coarse particles, powder, etc.) can be used as the high-molecular-weight PTFE in step (1). The primary melting point is preferably 300° C. or higher, more preferably 310° C. or higher, and even more preferably 320° C. or higher. The primary melting point means the maximum peak temperature of the endothermic curve appearing on the crystal melting curve when unsintered high molecular weight PTFE is measured by a differential scanning calorimeter. The endothermic curve was obtained by heating the material at a heating rate of 10°C / min using a differential scanning calorimeter.
[0056] The molded product in step (2) has a specific gravity of 1.0 g / cm 3 It is preferable that the content is 1.5 g / cm or more. 3 More preferably, it is 2.5 g / cm or more. 3 When the specific gravity of the molded article is within the above range, the pores and irregularities on the surface are small, and as a result, a low molecular weight PTFE having a small specific surface area can be obtained. The specific gravity can be measured by a water displacement method. The manufacturing method of the present disclosure may further include a step of pulverizing the molded article after step (2). The molded article may be coarsely pulverized and then further pulverized into smaller pieces.
[0057] The manufacturing method of the present disclosure may further include, after step (1), a step of pulverizing the low-molecular-weight PTFE to obtain a powder of the low-molecular-weight PTFE.
[0058] The pulverization method is not particularly limited, but may be a method of pulverization using a pulverizer, which may be an impact type such as a planetary mill, hammer mill, pin mill, or jet mill, or a friction type such as a cutter mill that pulverizes the material by shearing force caused by unevenness between a rotating blade and an outer stator.
[0059] The grinding temperature is preferably -200°C or higher and lower than 50°C. In freeze-grinding, the temperature is usually -200 to -100°C, but grinding may be performed at a temperature close to room temperature (10 to 30°C). Liquid nitrogen is generally used in freeze-grinding, but this requires large-scale equipment and increases the grinding costs. In terms of simplifying the process and reducing grinding costs, grinding at 10°C or higher and lower than 50°C is more preferable, grinding at 10 to 40°C is even more preferable, and grinding at 10 to 30°C is particularly preferable.
[0060] After the above pulverization, fine particles and fibrous particles may be removed by air classification, and then coarse particles may be removed by further classification.
[0061] In air classification, the crushed particles are sent to a cylindrical classification chamber by reduced pressure air, dispersed by the swirling air current in the chamber, and the fine particles are classified by centrifugal force. The fine particles are collected from the center into a cyclone and a bag filter. Rotating bodies such as cones and rotors are installed in the classification chamber to ensure uniform swirling motion of the crushed particles and air.
[0062] When using a classifying cone, the classification point is adjusted by adjusting the secondary air volume and the gap between the classifying cones. When using a rotor, the air volume in the classifying chamber is adjusted by the rotor rotation speed.
[0063] Methods for removing coarse particles include air classification using a mesh, a vibrating sieve, an ultrasonic sieve, etc., with air classification being preferred.
[0064] Next, the high-molecular-weight PTFE to be irradiated in step (1) of the production method of the present disclosure and the low-molecular-weight PTFE obtained after carrying out step (1) will be described.
[0065] The low molecular weight PTFE obtained after carrying out step (1) has a melt viscosity of 1.0×10 at 380° C. 2 Pa·s or more, 7.0×10 5In the present disclosure, "low molecular weight" means that the melt viscosity is within the above range. The melt viscosity is 1.0×10 3 Pa s or more is preferable, and 1.5×10 3 More preferably, it is 1.0×10 4 It is more preferable that the viscosity is 3.0×10 Pa s or more. 5 It is preferable that the density is less than 1.0×10 Pa s. 5 It is more preferable that it is less than Pa·s.
[0066] The melt viscosity was measured in accordance with ASTM D 1238 using a flow tester (manufactured by Shimadzu Corporation) and a 2φ-8L die, with a 2 g sample preheated at 380° C. for 5 minutes and maintained at the above temperature under a load of 0.7 MPa.
[0067] The high molecular weight PTFE to be irradiated with radiation preferably has a standard specific gravity (SSG) of 2.130 to 2.230. The standard specific gravity (SSG) is a value measured in accordance with ASTM D 4895.
[0068] The high molecular weight PTFE has a melt viscosity much higher than that of the low molecular weight PTFE, and it is difficult to measure the melt viscosity accurately. On the other hand, although the melt viscosity of the low molecular weight PTFE can be measured, it is difficult to obtain a molded product that can be used to measure the standard specific gravity from the low molecular weight PTFE, and it is difficult to measure the standard specific gravity accurately. Therefore, in the present disclosure, the standard specific gravity is adopted as an index of the molecular weight of the high molecular weight PTFE, and the melt viscosity is adopted as an index of the molecular weight of the low molecular weight PTFE. Note that there is no known measurement method that can directly specify the molecular weight of either the high molecular weight PTFE or the low molecular weight PTFE.
[0069] The low-molecular-weight PTFE preferably has a melting point of 320 to 340°C, and more preferably 324 to 336°C.
[0070] The above melting point is measured using a differential scanning calorimeter (DSC). After temperature calibration in advance using indium and lead as standard samples, about 3 mg of low molecular weight PTFE is placed in an aluminum pan (crimp container), and the temperature is raised at 10°C / min in the temperature range of 250 to 380°C under an air flow of 200 ml / min. The minimum point of the heat of fusion in the above range is taken as the melting point.
[0071] In the manufacturing method of the present disclosure, the shape of the high molecular weight PTFE is not particularly limited, and may be a powder (fine powder, molding powder, etc.), a molded product of the high molecular weight PTFE, cutting chips generated when a molded product of the high molecular weight PTFE is cut, or a pulverized product of the high molecular weight PTFE (coarse particles, powder, etc.). When the high molecular weight PTFE is a powder, the powder of the low molecular weight PTFE can be easily obtained. The high molecular weight PTFE may be crosslinked.
[0072] Furthermore, the shape of the low-molecular-weight PTFE obtained by the production method of the present disclosure is not particularly limited, but is preferably a powder.
[0073] When the low-molecular-weight PTFE obtained by the production method of the present disclosure is in the form of powder, the specific surface area is preferably 0.5 to 25 m 2 It is preferable that the molecular weight is 1 / g. As a low molecular weight PTFE powder, the specific surface area is 0.5 m 2 / g or more, 7.0m 2 / g, and a type with a specific surface area of 7.0 m 2 / g or more, 25m 2 There is a demand for types with a high specific surface area of less than 1 / g. Low-molecular-weight PTFE powders of the type having a low specific surface area have the advantage of being easily dispersed in matrix materials such as paints, but the dispersed particle size in the matrix material is large, making them inferior for fine dispersion. The specific surface area of low molecular weight PTFE powder with a low specific surface area is 1.0 m 2 / g or more is preferable, and 5.0m 2 / g or less is preferable, and 3.0m2 / g or less is more preferable. As the matrix material, in addition to plastics and inks, paints and the like are also suitably used. When a type of low molecular weight PTFE powder with a high specific surface area is dispersed in a matrix material such as paint, the dispersed particle size in the matrix material is small, and the effect of modifying the surface, such as improving the texture of the coating surface, is high, and the oil absorption amount is also large. However, there is a risk that it will not disperse easily, for example, it will take a long time to disperse in the matrix material, and there is also a risk that the viscosity of the paint, etc. will increase. The specific surface area of the high-specific-surface-area type low molecular weight PTFE powder is 8.0 m 2 / g or more is preferable, and 20m 2 / g or less is preferable. As the matrix material, oil, grease, paint, plastic, etc. are also preferably used.
[0074] The specific surface area is measured by the BET method using a surface analyzer (product name: BELSORP-miniII, manufactured by Microtrack-Bell Co., Ltd.) and a mixed gas of 30% nitrogen and 70% helium as the carrier gas and liquid nitrogen for cooling.
[0075] When the low-molecular-weight PTFE obtained by the manufacturing method of the present disclosure is in the form of a powder, the average particle size is preferably 0.5 to 200 μm, more preferably 50 μm or less, even more preferably 25 μm or less, and particularly preferably 10 μm or less. In this way, since the powder has a relatively small average particle size, a coating film having superior surface smoothness can be formed when used as an additive for paint, for example.
[0076] The above average particle size is measured using a laser diffraction particle size distribution analyzer (HELOS&RODOS) manufactured by JEOL Ltd. without using a cascade and at a dispersion pressure of 3.0 bar, and is equal to the particle size corresponding to 50% of the integrated particle size distribution.
[0077] The low-molecular-weight PTFE may have a carboxyl group at the molecular chain terminal. The number of carboxyl groups is 10. 6There may be 5 or less per piece, more than 5, or 30 or more. When the irradiation is carried out substantially in the absence of oxygen, the number of carboxyl groups can be 5 or less. The number of carboxyl groups is a value measured by the following method, the detection limit of which is 0.5. (Measurement method) The following measurements are carried out in accordance with the method for analyzing terminal groups described in JP-A-4-20507. The low molecular weight PTFE powder is preformed by hand press to produce a film with a thickness of 0.1 to 1.0 mm. The produced film is subjected to infrared absorption spectroscopy. The infrared absorption spectroscopy of PTFE, which is produced by contacting PTFE with fluorine gas and completely fluorinated at the ends, is also performed, and the number of terminal carboxyl groups is calculated from the difference spectrum between the two using the following formula. Number of terminal carboxyl groups (10 carbon atoms) 6 (per piece) = (l × K) / t l: Absorbance K: Correction coefficient t: film thickness (mm) The absorption frequency of the carboxyl group is 3560 cm -1 The correction factor for front and rear is 440.
[0078] The molecular chain terminals of the low molecular weight PTFE may have unstable terminal groups derived from the chemical structure of the polymerization initiator or chain transfer agent used in the polymerization reaction of the high molecular weight PTFE. The unstable terminal groups are not particularly limited, and examples thereof include -CH2OH, -COOH, -COOCH3, etc.
[0079] The low-molecular-weight PTFE may be one that has been stabilized for unstable terminal groups. The method for stabilizing the unstable terminal groups is not particularly limited, and examples thereof include a method of exposing the terminals to a fluorine-containing gas to change them to trifluoromethyl groups [-CF3].
[0080] The low-molecular-weight PTFE may also be terminally amidated. The method for terminal amidation is not particularly limited, and examples thereof include a method of exposing the PTFE to a fluorine-containing gas, for example, and contacting the resulting fluorocarbonyl group [-COF] with ammonia gas, as disclosed in JP-A-4-20507.
[0081] When the above-mentioned low-molecular-weight PTFE is one in which the above-mentioned unstable terminal group has been stabilized or the terminals have been amidated, it is easily compatible with the counterpart material and can have improved dispersibility when used as an additive to the counterpart material such as paint, grease, cosmetics, plating solution, toner, plastics, etc.
[0082] The high molecular weight PTFE to be irradiated may be a homo-PTFE consisting of only tetrafluoroethylene (TFE) units, or may be a modified PTFE containing TFE units and modified monomer units based on a modified monomer copolymerizable with TFE. In the manufacturing method of the present disclosure, the composition of the polymer does not change, so the low molecular weight PTFE has the same composition as the high molecular weight PTFE to be irradiated.
[0083] In the modified PTFE, the content of the modified monomer unit is preferably 0.001 to 1% by mass of the total monomer units, more preferably 0.01% by mass or more, more preferably 0.5% by mass or less, and even more preferably 0.1% by mass or less. In this specification, the modified monomer unit means a part of the molecular structure of the modified PTFE that is derived from the modified monomer, and the total monomer units means a part derived from all monomers in the molecular structure of the modified PTFE. The content of the modified monomer unit can be determined by a known method such as Fourier transform infrared spectroscopy (FT-IR).
[0084] The above-mentioned modified monomer is not particularly limited as long as it is copolymerizable with TFE, and examples thereof include perfluoroolefins such as hexafluoropropylene [HFP], chlorofluoroolefins such as chlorotrifluoroethylene [CTFE], hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride [VDF], perfluorovinyl ethers, perfluoroalkylethylenes, ethylene, etc. The modified monomer used may be one type or multiple types.
[0085] The perfluorovinyl ether is not particularly limited, and may be, for example, a perfluorovinyl ether represented by the following general formula (1): CF2=CF-ORf (1) (wherein Rf represents a perfluoro organic group). In this specification, the "perfluoro organic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms. The perfluoro organic group may have an ether oxygen.
[0086] An example of the perfluorovinyl ether is perfluoro(alkyl vinyl ether) [PAVE], where Rf in the general formula (1) represents a perfluoroalkyl group having 1 to 10 carbon atoms. The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5.
[0087] Examples of the perfluoroalkyl group in the above PAVE include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group. Perfluoro(propyl vinyl ether) [PPVE] in which the perfluoroalkyl group is a perfluoropropyl group is preferred.
[0088] The perfluorovinyl ether further includes those represented by the above general formula (1), in which Rf is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms, and those represented by the following formula:
[0089] [ka]
[0090] (wherein m represents 0 or an integer of 1 to 4), Rf is a group represented by the following formula:
[0091] [ka]
[0092] (wherein n represents an integer of 1 to 4).
[0093] The perfluoroalkylethylene is not particularly limited, and examples thereof include (perfluorobutyl)ethylene (PFBE), (perfluorohexyl)ethylene, and (perfluorooctyl)ethylene.
[0094] The modifying monomer in the modified PTFE is preferably at least one selected from the group consisting of HFP, CTFE, VDF, PPVE, PFBE and ethylene, and more preferably at least one selected from the group consisting of HFP and CTFE.
[0095] The low molecular weight PTFE can be suitably used as a molding material, ink, cosmetics, paint, grease, office automation equipment member, additive for modifying toner, organic photoreceptor material for copying machine, additive for plating solution, etc. Examples of the molding material include engineering plastics such as polyoxybenzoyl polyester, polyimide, polyamide, polyamideimide, polyacetal, polycarbonate, polyphenylene sulfide, etc. The low molecular weight PTFE is particularly suitable as a thickening agent for grease.
[0096] The low-molecular-weight PTFE can be suitably used as an additive to molding materials, for example, for improving the non-stickiness and sliding properties of copy rolls, for improving the texture of engineering plastic molded products such as surface sheets for furniture, automobile dashboards, and covers for home appliances, for improving the slipperiness and abrasion resistance of machine parts that generate mechanical friction such as light-load bearings, gears, cams, push-button phone buttons, projectors, camera parts, and sliding materials, and as a processing aid for engineering plastics.
[0097] The low molecular weight PTFE can be used as an additive for paints to improve the slipperiness of varnishes and paints.The low molecular weight PTFE can be used as an additive for cosmetics to improve the slipperiness of cosmetics such as foundations.
[0098] The low molecular weight PTFE is also suitable for use in improving the oil repellency or water repellency of wax, etc., and for use in improving the slipperiness of grease or toner.
[0099] The low molecular weight PTFE can also be used as an electrode binder for secondary batteries or fuel cells, a hardness adjuster for electrode binders, a water repellent treatment agent for electrode surfaces, and the like.
[0100] The low molecular weight PTFE and lubricating oil can also be used to prepare a grease. The grease is characterized by containing the low molecular weight PTFE and lubricating oil, and therefore the low molecular weight PTFE is uniformly and stably dispersed in the lubricating oil, and has excellent properties such as load resistance, electrical insulation, and low moisture absorption.
[0101] The lubricating oil (base oil) may be a mineral oil or a synthetic oil. Examples of the lubricating oil (base oil) include paraffinic or naphthenic mineral oils, synthetic hydrocarbon oils, ester oils, fluorine oils, and synthetic oils such as silicone oils. From the viewpoint of heat resistance, fluorine oils are preferred, and examples of the fluorine oils include perfluoropolyether oils and low polymers of trifluorochloroethylene. The low polymers of trifluorochloroethylene may have a weight average molecular weight of 500 to 1200.
[0102] The grease may further contain a thickener. Examples of the thickener include metal soaps, composite metal soaps, bentonite, phthalocyanine, silica gel, urea compounds, urea-urethane compounds, urethane compounds, and imide compounds. Examples of the metal soaps include sodium soaps, calcium soaps, aluminum soaps, and lithium soaps. Examples of the urea compounds, urea-urethane compounds, and urethane compounds include diurea compounds, triurea compounds, tetraurea compounds, other polyurea compounds, urea-urethane compounds, diurethane compounds, and mixtures thereof.
[0103] The grease preferably contains 0.1 to 60% by mass of the low molecular weight PTFE, more preferably 0.5% by mass or more, even more preferably 5% by mass or more, and even more preferably 50% by mass or less. If the amount of the low molecular weight PTFE is too large, the grease may become too hard and may not exhibit sufficient lubrication, and if the amount of the low molecular weight PTFE is too small, the grease may not exhibit sufficient sealing properties.
[0104] The grease may also contain solid lubricants, extreme pressure agents, antioxidants, oiliness agents, rust inhibitors, viscosity index improvers, detergents and dispersants, and the like.
[0105] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES
[0106] The present disclosure will now be described in more detail with reference to examples, but the present disclosure is not limited to these examples.
[0107] Various physical properties were measured by the following methods.
[0108] (Melt Viscosity) The sampled low molecular weight PTFE powder samples were measured in accordance with ASTM D 1238 using a flow tester (manufactured by Shimadzu Corporation) and a 2φ-8L die, with 2 g of the sample preheated at 380°C for 5 minutes, and maintained at the above temperature under a load of 0.7 MPa.
[0109] (Absorbed Dose Rate) The actual measurements were made by the method using the chemical dosimeter described above.
[0110] (dose rate ratio) It is calculated as the ratio between the maximum and minimum absorbed dose rates obtained at multiple sampling locations.
[0111] The "Overall Judgment" column in the table is based on the following criteria. ○: PTFE melt viscosity was 1.0×10 at all sampling points 4 Pa·s or more, 1.0×10 5 Within the range of Pa s or less ×:Other than the above
[0112] Example 1 8.0 kg of high molecular weight PTFE fine powder (1) (standard specific gravity 2.171, homogenous body, measured in accordance with ASTM D 4895) was weighed with a weighing balance, placed in a 50 L aluminum airtight bag (inner bag polyethylene, with a cock) and sealed. The airtight bag was placed in a fiber drum (material: cardboard) with a size of Φ300 mm × 350 mmH and the lid was closed. The fiber drum was placed parallel to the gamma ray source. The irradiation temperature was 30 ° C. After 1.5 h of irradiation, the irradiation was stopped once and the fiber drum was rotated 90 °. Irradiation was started again, and after another 1.5 h of irradiation, the irradiation was stopped again. The fiber drum was further rotated 90 °. By repeating this, irradiation was performed for 1.5 h each on four sides for a total of 6 h, and a low molecular weight PTFE powder was obtained. The airtight bag was opened, and sampling was performed from three points using a pencil-shaped powder sampler (manufactured by Tsutsui Rikagaku Kikai Co., Ltd.). The positional relationship between the radiation source and the object to be irradiated as viewed from above and the sampling points are shown in Figure 5. The melt viscosity of the obtained low molecular weight PTFE was measured. The results are shown in Table 1. At all sampling points, the melt viscosity was 1.0×10 4 Pa·s or more, 1.0×10 5 It is clear that the variation in molecular weight of the low-molecular-weight PTFE is small.
[0113] Example 2 For comparison, irradiation was stopped once after 3 hours of irradiation, and the fiber drum was rotated 180°. Irradiation was restarted and stopped after 3 hours of irradiation, for a total of 6 hours of irradiation. Other than that, the same operations as in Example 1 were performed. The results are shown in Table 1. At all sampling points, the melt viscosity was 1.0×10 4 Pa·s or more, 1.0×10 5 It is clear that the variation in molecular weight of the low-molecular-weight PTFE is small.
[0114] Comparative Example 1 For comparison, irradiation was continued for 6 hours without rotating the fiber drum during the irradiation. Other than that, the same operation as in Example 1 was performed. The results are shown in Table 1. At the sampling points A and B, the melt viscosity was 1.0×10 4 Pa·s or more, 1.0×10 5 However, at sampling point C, it deviates from the above range, indicating that there is large variation in the molecular weight of the low molecular weight PTFE.
[0115] [Table 1] [Explanation of symbols]
[0116] 10: Source 11: Irradiation container 12: Irradiation table 100: High molecular weight PTFE powder
Claims
1. High molecular weight polytetrafluoroethylene was irradiated with radiation in a batch system so that the ratio of the maximum dose rate to the minimum dose rate (maximum dose rate / minimum dose rate) was 2.00 or less, and the melt viscosity at 380° C. was 1.0×10 2 Pa・s or more, 7.0×10 5 A method for producing low-molecular-weight polytetrafluoroethylene, comprising: (1) obtaining low-molecular-weight polytetrafluoroethylene having a viscosity of Pa·s or less.
2. The method according to claim 1, wherein the minimum absorbed dose of the radiation is 50 kGy or more and less than 200 kGy.
3. The method according to claim 1 or 2, wherein the irradiation is carried out in the presence of oxygen.
4. 3. The method according to claim 1, wherein the radiation is an electron beam, a gamma ray or an X-ray.
5. 3. The method according to claim 1, wherein the irradiation is performed at a distance of 10 m or less from a source of the radiation to the furthest portion of the high-molecular-weight polytetrafluoroethylene.
6. 3. The method according to claim 1, wherein the irradiation is carried out with the distance from the source of the radiation to the closest portion of the high molecular weight polytetrafluoroethylene being 5 cm or more.
7. 3. The manufacturing method according to claim 1, wherein the high-molecular-weight polytetrafluoroethylene is disposed in a position facing an effective area of a source of the radiation, and the irradiation is performed, and the effective area is an area whose distance from the center of the radiation source is 95% or less of the distance from the center to an end of the radiation source.
8. 3. The manufacturing method according to claim 1, wherein the irradiation is performed on the high-molecular-weight polytetrafluoroethylene filled in an irradiation container made of at least one material selected from the group consisting of metals, glasses, ceramics, and organic materials.
9. The method according to claim 8 , wherein the irradiation container is cylindrical or prismatic.
10. The method according to claim 8 , wherein the irradiation container has at least one surface selected from the group consisting of a plate-like surface, a mesh-like surface, and a surface having slit-like openings.
11. The method according to claim 1 or 2, wherein the irradiation is performed by arranging a plurality of irradiation containers filled with the high molecular weight polytetrafluoroethylene in parallel.
12. 3. The method according to claim 1, wherein the high molecular weight polytetrafluoroethylene has a standard specific gravity of 2.130 or more and 2.230 or less.
13. 3. The method according to claim 1, wherein the high molecular weight polytetrafluoroethylene and the low molecular weight polytetrafluoroethylene are both in the form of powder.
14. The method further includes, before the step (1), a step (2) of obtaining a molded article by heating the high molecular weight polytetrafluoroethylene to a temperature equal to or higher than its primary melting point, and the molded article has a specific gravity of 1.0 g / cm 3 The method according to claim 1 or 2, wherein
Citation Information
Patent Citations
Polytetrafluoroethylene powder and its production
JP1998147617A
Apparatus and method for radiation processing of materials
US4777192A
Vibratory table apparatus and associated equipment and methods for radiation treatment of polymeric materials
US6486481B1
Method for producing low-molecular-weight polytetrafluoroethylene
WO2020013336A1