Method for controlling battery system

JP2024165830AActive Publication Date: 2024-11-28PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023082362
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28
Estimated Expiration
2043-05-18

Smart Images

  • Figure 2024165830000001_ABST
    Figure 2024165830000001_ABST
Patent Text Reader

Abstract

To suppress degradation of a non-aqueous electrolyte secondary battery.SOLUTION: The present invention relates to a method for controlling a battery system 100 having a non-aqueous electrolyte secondary battery 1, the non-aqueous electrolyte secondary battery 1 including a positive electrode active material and a negative electrode active material. The positive electrode active material is changed in the phase by charge or discharge of the non-aqueous electrolyte secondary battery 1 and charging or discharging is restricted so that the positive electrode active material is prevented from charging or discharging in a charge depth region P in which a phase change happens after a specific condition is satisfied.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a control method for a battery system. [Background technology]

[0002] Japanese Patent Application Laid-Open No. 2013-196805 discloses a lithium-ion secondary battery system that, when the start SOC or end SOC of a charge / discharge cycle of a lithium-ion secondary battery is detected or estimated to be a characteristic point appearing on a Q-dV / dQ curve, sets the start SOC or end SOC to an SOC that avoids the characteristic point appearing on the Q-dV / dQ curve. The lithium-ion secondary battery system disclosed in this publication is said to be able to improve the cycle characteristics of the lithium-ion secondary battery. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-196805 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors wish to suppress the deterioration of non-aqueous electrolyte secondary batteries. [Means for solving the problem]

[0005] The method for controlling a battery system disclosed herein is a method for controlling a battery system including a non-aqueous electrolyte secondary battery. The non-aqueous electrolyte secondary battery includes a positive electrode active material and a negative electrode active material, and the positive electrode active material undergoes a phase change due to charging and discharging of the non-aqueous electrolyte secondary battery. After a specific condition is reached, charging and discharging are prevented or limited in a charge depth region where the phase change occurs. With such a battery system, deterioration of the non-aqueous electrolyte secondary battery is suppressed. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a schematic diagram showing a battery system 100. As shown in FIG. [Diagram 2] FIG. 2 is a vertical cross-sectional view that illustrates a schematic internal structure of the nonaqueous electrolyte secondary battery 1. As shown in FIG. [Diagram 3] FIG. 3 is a perspective view that diagrammatically illustrates the electrode assembly 20 of the nonaqueous electrolyte secondary battery 1. As shown in FIG. [Figure 4] FIG. 4 is a flowchart showing a flow executed by the control device 70. [Diagram 5] FIG. 5 is a graph showing a Q-dV / dQ curve. [Figure 6] FIG. 6 is a graph showing an SOC-dV / dSOC curve. [Figure 7] FIG. 7 is a graph showing the relationship between the number of cycles and the capacity retention rate. [Figure 8] FIG. 8 is a graph showing the relationship between the number of cycles and the capacity retention rate. [Figure 9] FIG. 9 is a graph showing the relationship between the number of cycles and the rate of increase in resistance. [Figure 10] FIG. 10 is a graph showing the relationship between the number of cycles and the rate of increase in resistance. [Figure 11] FIG. 11 is a graph showing the relationship between the number of cycles and the capacity retention rate. [Figure 12] FIG. 12 is a graph showing the relationship between the number of cycles and the capacity retention rate. [Figure 13] FIG. 13 is a graph showing the relationship between the number of cycles and the capacity retention rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Hereinafter, an embodiment of the technology disclosed herein will be described with reference to the drawings. The embodiment described herein is, of course, not intended to limit the present invention in particular. Each drawing is drawn typically and does not necessarily reflect the actual product. Furthermore, the same reference numerals are appropriately used for members and parts that perform the same function, and duplicated descriptions are appropriately omitted.

[0008] <Battery System 100> FIG. 1 is a schematic diagram showing a battery system 100. As shown in FIG. 1, the battery system 100 includes a nonaqueous electrolyte secondary battery 1 and a control device 70. The nonaqueous electrolyte secondary battery 1 may be multiple or may be a single battery. From the viewpoint of adjusting the battery capacity, operating voltage, etc. in accordance with an external load, it is preferable that the battery system 100 uses multiple nonaqueous electrolyte secondary batteries 1. The multiple nonaqueous electrolyte secondary batteries 1 may be connected in series, in parallel, or in a combination of series and parallel.

[0009] <Nonaqueous electrolyte secondary battery 1> The nonaqueous electrolyte secondary battery 1 includes a positive electrode active material and a negative electrode active material. In this embodiment, a lithium ion secondary battery is used as the nonaqueous electrolyte secondary battery 1. An example of the nonaqueous electrolyte secondary battery 1 will be described below.

[0010] Fig. 2 is a vertical cross-sectional view that typically shows the internal structure of the nonaqueous electrolyte secondary battery 1. Fig. 3 is a perspective view that typically shows an electrode assembly 20 of the nonaqueous electrolyte secondary battery 1. As shown in Fig. 2, the battery includes a case 10, the electrode assembly 20, and a nonaqueous electrolyte (not shown).

[0011] The case 10 is a box-shaped container. In this embodiment, a rectangular case 10 is used. An electrode body 20 and a non-aqueous electrolyte are housed inside the case 10. For example, a metal material (such as aluminum) having a certain strength is used for the case 10. A positive electrode terminal 12 and a negative electrode terminal 14 are attached to the case 10. The positive electrode terminal 12 and the negative electrode terminal 14 are connected to the electrode body 20 inside the case 10. Specifically, the positive electrode terminal 12 is connected to the positive electrode plate 30 (see FIG. 3) of the electrode body 20. Aluminum or the like is used for the positive electrode terminal 12. On the other hand, the negative electrode terminal 14 is connected to the negative electrode plate 40 (see FIG. 3) of the electrode body 20. Copper or the like is used for the negative electrode terminal 14.

[0012] The electrode body 20 is a power generating element of the nonaqueous electrolyte secondary battery 1. As shown in FIG. 3, the electrode body 20 includes a positive electrode plate 30, a negative electrode plate 40, and a separator 50. In this embodiment, the electrode body 20 is a wound electrode body. The wound electrode body is produced by stacking and winding the positive electrode plate 30, the negative electrode plate 40, and the separator 50. The structure of the electrode body 20 is not particularly limited, and may be any other conventionally known structure (such as a stacked electrode body).

[0013] The positive electrode plate 30 includes a positive electrode core 32, which is a metal foil having electrical conductivity, and a positive electrode active material layer 34 formed on the surface of the positive electrode core 32. The positive electrode core 32 is made of aluminum or the like. The positive electrode active material layer 34 contains a positive electrode active material, a conductive material, a binder, and the like. The conductive material may be a carbon material such as acetylene black or graphite. The binder may be a resin material such as polyvinylidene fluoride (PVdF).

[0014] In this embodiment, the positive electrode active material layer 34 contains a lithium composite oxide having a nickel content of 70 mol % or more relative to metal atoms other than lithium (hereinafter, also referred to as a "high Ni-containing lithium composite oxide") as a positive electrode active material. By using a high Ni-containing lithium composite oxide as the positive electrode active material, the capacity of the nonaqueous electrolyte secondary battery 1 can be increased.

[0015] As the high Ni-containing lithium composite oxide, a lithium nickel cobalt manganese composite oxide is preferable. In the lithium nickel cobalt manganese composite oxide, the Ni content relative to the metal atoms other than Li is 70 mol % or more as described above. In the lithium nickel cobalt manganese composite oxide, the Ni content relative to the metal atoms other than Li is preferably 80 mol % or more.

[0016] The type of high Ni-containing lithium composite oxide is not particularly limited as long as the Ni content relative to metal atoms other than lithium is 70 mol% or more. Examples of high Ni-containing lithium composite oxides include lithium nickel cobalt manganese composite oxides and lithium nickel cobalt aluminum composite oxides. Examples of high Ni-containing lithium composite oxides include lithium transition metal composite oxides represented by the following formula (I). Li a Ni 1-b A b O 2 (I)

[0017] Here, a is preferably 0.8 or more and 1.2 or less, and b is preferably less than 0.2. A is an element other than Ni, and preferably contains at least one of Co and Mn. In addition, the molar ratio of the total of the Co content (moles) and the Mn content (moles) to the A content (moles) is preferably 0.8 or more. At least one element selected from the group consisting of Al, Zr, B, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Sr, Ca, W, Mo, Nb, Ti, and Si may be contained.

[0018] The positive electrode active material layer 34 may contain a surfactant. The surfactant may be a known surfactant that has been conventionally used in positive electrode active material layers or a surfactant having properties equal to or greater than those of the known surfactant. Specifically, the surfactant may be a cationic surfactant, an anionic surfactant, an amphoteric surfactant, a nonionic surfactant, or the like. These may be used alone or in combination of two or more.

[0019] The negative electrode plate 40 includes a negative electrode core 42, which is a metal foil having electrical conductivity, and a negative electrode active material layer 44 applied to the surface of the negative electrode core 42. The negative electrode core 42 is made of copper or the like. The negative electrode active material layer 44 contains a negative electrode active material, a binder, a thickener, and the like. Examples of the negative electrode active material include carbon materials such as graphite, hard carbon, and soft carbon. Examples of the binder include resin materials such as styrene butadiene rubber (SBR). Examples of the thickener include resin materials such as carboxymethyl cellulose (CMC).

[0020] The separator 50 is an insulating sheet interposed between the positive electrode plate 30 and the negative electrode plate 40. For example, resin materials such as polyethylene (PE), polypropylene (PP), polyester, cellulose, and polyamide can be used as the separator 50. A heat-resistant layer containing an inorganic filler may be formed on the surface of the separator 50. As the inorganic filler, inorganic oxides such as aluminum oxide, magnesium oxide, silicon oxide, and titanium oxide, nitrides such as aluminum nitride and silicon nitride, metal hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide, and clay minerals such as mica, talc, boehmite, zeolite, apatite, and kaolin can be used. The separator 50 may contain a binder for fixing the heat-resistant layer to the surface. As the binder, resin binders such as polyvinylidene fluoride (PVdF) and acrylic resins can be used.

[0021] The non-aqueous electrolyte typically contains a non-aqueous solvent and an electrolyte salt (in other words, a supporting salt). As the non-aqueous solvent, various organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones that are used in electrolytes of general lithium ion secondary batteries can be used without any particular limitation. Among them, carbonates are preferable, and specific examples thereof include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such non-aqueous solvents can be used alone or in appropriate combination of two or more. As the electrolyte salt, for example, LiPF 6 , LiBF 4 Lithium salts such as lithium bis(fluorosulfonyl)imide (LiFSI) can be used. Among them, LiPF 6 The non-aqueous electrolyte may contain various additives such as, for example, an oxalate complex, a film-forming agent such as vinylene carbonate (VC), a gas generating agent such as biphenyl (BP) or cyclohexylbenzene (CHB), a thickener, etc.

[0022] However, the capacity of a nonaqueous electrolyte secondary battery may decrease due to repeated charging and discharging of the nonaqueous electrolyte secondary battery. The decrease in capacity of a nonaqueous electrolyte secondary battery due to charging and discharging is also called cycle deterioration. Cycle deterioration may progress due to a chemical reaction occurring between a positive electrode, a negative electrode, and a nonaqueous electrolyte during charging and discharging. For example, the positive electrode active material contained in the positive electrode active material layer may undergo a phase change due to charging and discharging of the nonaqueous electrolyte secondary battery. The phase change of the positive electrode active material may occur when lithium is absorbed or released into the positive electrode active material during charging and discharging. The phase change does not progress at a constant rate during charging and discharging. For example, the ease of phase change may vary depending on the state of charge (SOC) during charging and discharging of the nonaqueous electrolyte secondary battery. When the state of charge of the nonaqueous electrolyte secondary battery is charged and discharged in a state of charge region where a phase change occurs (hereinafter also referred to as a "phase change region"), the phase change of the positive electrode active material is likely to progress. In addition, the depth of charge at which a phase change is likely to occur may differ depending on the type of positive electrode active material. By controlling the charge and discharge of the nonaqueous electrolyte secondary battery so that the depth of charge does not reach the depth of charge at which a phase change is likely to occur, it is possible to suppress a decrease in the capacity of the nonaqueous electrolyte secondary battery.

[0023] The charge / discharge control can be executed after a specific condition is reached. The specific condition can be set based on data acquired during charging / discharging of the nonaqueous electrolyte secondary battery 1. In this embodiment, the condition is set by calculating and evaluating damage caused by a phase change in the positive electrode active material based on data acquired during charging / discharging. Here, the charge / discharge of the nonaqueous electrolyte secondary battery 1 is controlled by a control device 70. A method for controlling the charge / discharge of the nonaqueous electrolyte secondary battery 1 will be described below together with the configuration of the control device 70.

[0024] FIG. 4 is a flowchart showing a flow executed by the control device 70 (see FIG. 1). The control device 70 controls the upper limit of SOC during charging and discharging. In this embodiment, the upper limit SOC in the initial state is set to 100%. As shown in FIG. 4, the control device 70 is configured to execute a process S10 for detecting a charging and discharging capacity Q, a process S20 for detecting a charging depth region P where a phase change occurs, a process S30 for determining whether or not charging and discharging have occurred across the charging depth region P where a phase change occurs, a process S40 for calculating and storing a damage amount D, a process S50 for comparing the damage amount D with a threshold value Th, and a process S60 for changing the upper limit SOC.

[0025] <Control device 70> The control device 70 controls the charging and discharging of the nonaqueous electrolyte secondary battery 1. As shown in FIG. 1, the control device 70 controls the range of the SOC (depth of charge) when the nonaqueous electrolyte secondary battery 1 is charged and discharged. The control device 70 is, for example, a microcomputer. The control device 70 includes, for example, an I / F, a CPU, a ROM, and a RAM. The control device 70 may be composed of a single computer or may be composed of multiple computers.

[0026] The control device 70 includes a sensor 71. The sensor 71 includes a voltage sensor 71a, a current sensor 71b, and a temperature sensor 71c. The voltage sensor 71a detects the battery voltage of the nonaqueous electrolyte secondary battery 1. The current sensor 71b detects the charge / discharge current of the nonaqueous electrolyte secondary battery 1. The temperature sensor 71c detects the battery temperature of the nonaqueous electrolyte secondary battery 1. As the temperature sensor 71c, various elements (e.g., a thermistor, etc.) that detect temperature can be used. The battery voltage, the charge / discharge current, and the battery temperature are acquired at predetermined intervals. The intervals at which the battery voltage, the charge / discharge current, and the battery temperature are acquired can be set, for example, every 1 second to every 100 seconds. In this embodiment, the intervals at which the battery voltage, the charge / discharge current, and the battery temperature are acquired are set to every 10 seconds. The intervals at which the battery voltage, the charge / discharge current, and the battery temperature are acquired may be set appropriately depending on the ROM and RAM capacity of the control device 70.

[0027] The control device 70 includes a charge / discharge capacity detection unit 72 and an SOC detection unit 73. In the charge / discharge capacity detection unit 72 and the SOC detection unit 73, values ​​acquired by the voltage sensor 71a, the current sensor 71b, and the temperature sensor 71c are associated with time and used to estimate the charge / discharge capacity Q and the SOC.

[0028] The control device 70 includes a detection unit 74, a determination unit 75, a calculation unit 76, a storage unit 77, a comparison unit 78, and a control unit 79. Each of the units 72 to 79 included in the control device 70 may be realized by one or a plurality of processors, or may be incorporated into a circuit.

[0029] <Process S10 for detecting charge / discharge capacity Q> In process S10 (see FIG. 4), the charge / discharge capacity detection unit 72 detects the charge / discharge capacity Q by integrating the current detected by the current sensor 71b. The SOC may be detected in conjunction with the detection of the charge / discharge capacity Q. The SOC detection unit 73 estimates the SOC based on, for example, a pre-stored full charge capacity and the charge / discharge capacity Q. The SOC is calculated by the charge / discharge capacity Q relative to the full charge capacity (charge / discharge capacity Q / full charge capacity). The SOC detection unit 73 may calculate from a pre-stored relationship between the battery voltage and the SOC. After the charge / discharge capacity Q is detected, the voltage change amount dV / dQ relative to the charge / discharge capacity is then calculated.

[0030] <Process S20 for detecting the charging depth region P where a phase change occurs> In process S20 (see FIG. 4), the detection unit 74 detects a charge depth region (phase change region) P where a phase change occurs. In this embodiment, the detection unit 74 detects a voltage change amount dV / dQ with respect to the charge / discharge capacity Q. The charge depth region P where a phase change occurs is detected based on the voltage change amount dV / dQ with respect to the charge / discharge capacity Q. In this embodiment, the detection unit 74 detects the phase change region P based on a Q-dV / dQ curve that indicates the relationship between the charge / discharge capacity Q and the voltage change amount dV / dQ with respect to the charge / discharge capacity (hereinafter also simply referred to as "dV / dQ").

[0031] According to the inventor's findings, when a high Ni-containing lithium composite oxide is used as the positive electrode active material, a phase change may occur near the full charge capacity (for example, a charge depth of 70% or more, and may be 80% or more). The occurrence of a phase change in the positive electrode active material during charging and discharging is detected based on the battery voltage and battery current detected by the sensor 71. According to the inventor's findings, a phase change occurring in the positive electrode active material can be detected based on the Q-dV / dQ curve. When a phase change occurs in the positive electrode active material near the full charge capacity during charging, dV / dQ becomes small. When a phase change occurs in the positive electrode active material, dV / dQ becomes maximum near the full charge capacity during charging. In addition, an inflection point appears where the change in dV / dQ with respect to the charge / discharge capacity Q becomes large. For example, by detecting the charge / discharge capacity Q when dV / dQ becomes equal to or less than the maximum value, a charge depth region where a phase change occurs in the positive electrode active material can be detected.

[0032] FIG. 5 is a graph showing a Q-dV / dQ curve. In FIG. 5, the Q-dV / dQ curves of the lithium ion secondary batteries of Examples 1 to 3 described later are shown together with the potential curves. As shown in FIG. 5, the full charge capacity of the nonaqueous electrolyte secondary battery 1 is about 200 Ah. In this embodiment, dV / dQ reaches a maximum when the charge / discharge capacity Q is about 170 Ah. dV / dQ reaches a minimum when the charge / discharge capacity Q is about 180 Ah. dV / dQ reaches the maximum (dV / dQ when the charge / discharge capacity Q is about 170 Ah) or less when the charge / discharge capacity Q is about 190 Ah. At this time, the phase change region P is a region where the charge / discharge capacity Q is 170 Ah or more and 190 Ah or less (charging depth 85% or more and 95% or less). The electrodes are easily damaged when charging and discharging in the charging depth region P. In this way, the detection unit 74 detects the phase change region P based on the relationship of dV / dQ with respect to the charge / discharge capacity Q. When the charge depth region P is detected, it is determined whether or not charging / discharging has occurred across the charge depth region P. Note that "charging / discharging across the charge depth region P" is not limited to the case where the charge / discharge capacity Q is charged from below the lower limit of the phase change region P to above the upper limit, or discharged from above the upper limit of the phase change region P to below the lower limit, but also includes the case where charging or discharging has occurred without passing through the phase change region P.

[0033] When the charge / discharge current I is large, it may be difficult to accurately detect the charge depth region P due to the influence of overvoltage. The detection unit 74 may detect the charge depth region P based on a parameter other than the voltage change amount dV / dQ. For example, the charge depth region P may be detected based on dV / dSOC.

[0034] FIG. 6 is a graph showing an SOC-dV / dSOC curve. dV / dSOC is the amount of voltage change relative to SOC. The detection unit 74 may detect the phase change region P based on the SOC-dV / dSOC curve (see FIG. 6) showing the relationship between SOC and dV / dSOC, similar to the Q-dV / dQ curve. According to the knowledge of the present inventor, when the charge / discharge current I is large, the detection accuracy can be improved by detecting the charge depth region P based on the SOC-dV / dSOC curve. The detection of the amount of voltage change dV / dQ may be performed when the current value is equal to or less than a certain current value, and dV / dSOC may be substituted for the current value above that. For example, the detection unit 74 may detect the Q-dV / dQ curve when the charge / discharge current is less than 0.1 C, and detect the SOC-dV / dSOC curve when the charge / discharge current I is 0.1 C or more.

[0035] The depth of charge at which a phase change occurs can be known in advance by testing or the like. In this case, the detection of the depth of charge region P by the detection unit 74 is not necessarily performed. However, the phase change region P may vary with deterioration of the battery. In this case, the control device 70 may store data on the phase change region P according to deterioration of the battery (e.g., a decrease in capacity maintenance rate, etc.). The control device 70 may be configured to be able to read data on the phase change region P according to deterioration of the battery.

[0036] <Process S30 for determining whether charging / discharging has been performed in the charging depth region P where a phase change occurs> In process S30 (see FIG. 4), the determination unit 75 determines whether or not charging / discharging has occurred in the charge depth region P where a phase change occurs. If the charge / discharge capacity Q detected by the charge / discharge capacity detection unit 72 is within the charge depth region P detected by the detection unit 74 (Yes), the process proceeds to process S40 (see FIG. 4), where the damage amount D is calculated. If the charge / discharge capacity Q is not within the charge depth region P (No), the process ends, and the upper limit of the SOC during charging / discharging is not changed.

[0037] <Process S40 for calculating and storing the amount of damage D> In process S40, calculation unit 76 calculates the amount of damage D. Storage unit 77 stores the amount of damage D. Here, the amount of damage D is a numerical value of the damage caused by charging and discharging in the above-mentioned region of depth of charge P. Damage to the positive electrode active material can accumulate as the phase change of the positive electrode active material progresses during charging and discharging in the region of depth of charge P.

[0038] In this embodiment, the calculation unit 76 performs calculations based on the charge / discharge current I and the battery temperature T when charging / discharging in the charge depth region P. The calculation unit 76 calculates the damage amount D based on a pre-stored map. The map is set so that the damage coefficient α is determined based on the charge / discharge current I and the battery temperature T. When charging / discharging is not performed in the charge depth region P, the damage coefficient α may be set to 0.

[0039] The map may be configured as a matrix with the charge / discharge current I set on the vertical axis and the battery temperature T set on the horizontal axis. A damage coefficient α for a specific charge / discharge current I and battery temperature T may be set in the map. According to the map, the damage coefficient α is specified based on the charge / discharge current I acquired by the current sensor 71b and the battery temperature T acquired by the temperature sensor 71c.

[0040] The map may be previously set by tests, simulations, theoretical calculations, etc. according to the composition of the positive electrode active material, and the like, and stored. The setting of the map will be described later. The configuration of the map is not limited to such a form. The map may be configured so that the damage coefficient α is specified based on other parameters detected or estimated by the control device 70, such as the battery voltage, SOC, and charge / discharge capacity Q. In addition, a plurality of maps may be stored in the control device 70. For example, a plurality of maps may be stored in the control device 70 for each damage amount D. In this case, the damage coefficient α at a specific charge / discharge current I and battery temperature T can be updated by using a map based on the accumulated damage amount D.

[0041] According to trials by the present inventors, the damage to the positive electrode active material is smaller as the charge / discharge current I during charging / discharging is larger. The larger the charge / discharge current I, the smaller the damage coefficient α, and the smaller the charge / discharge current I, the larger the damage coefficient α. Furthermore, the lower the battery temperature T during charging / discharging is, the smaller the damage coefficient α. The smaller the battery temperature T, the smaller the damage coefficient α, and the higher the battery temperature T, the larger the damage coefficient α.

[0042] The memory unit 77 stores the damage amount D. The stored damage amount D is obtained by accumulating the damage coefficient α previously calculated. The calculation unit 76 adds the currently calculated damage coefficient α to the damage amount D. After the currently calculated damage coefficient α is added to the damage amount D, it is then determined whether the damage amount D is equal to or greater than the threshold value Th. The next time charging or discharging is performed in the charge depth region P, a new damage coefficient α is added to the currently stored damage amount D.

[0043] The calculation of the damage amount D is not limited to the above-mentioned manner. The calculation of the damage amount D may be calculated, for example, based on the number of times the charge depth region P is crossed during charging and discharging (for example, in this embodiment, the number of times the charge depth reaches 85% or more and 95% or less during charging and discharging) without using a map. In this way, a specific condition for controlling charging and discharging may be set based on the number of times the charge depth region P is crossed during charging and discharging.

[0044] <Process S50 for comparing the amount of damage D with the threshold value Th> In process S50 (see FIG. 4), the comparison unit 78 compares the amount of damage D with the threshold value Th. If the amount of damage D stored in process S40 is equal to or greater than the threshold value Th (Yes), the process proceeds to process S60. If the amount of damage D stored in process S40 is not equal to or greater than the threshold value Th (No), the process ends and the upper limit of the SOC during charging and discharging is not changed.

[0045] The threshold value Th may be determined in advance by a test, a simulation, a theoretical calculation, or the like. For example, the relationship between the amount of damage D and the capacity maintenance rate may be obtained by a test, and the threshold value Th may be determined based on the amount of damage that increases the rate of change in the capacity maintenance rate. Alternatively, the threshold value Th may be determined based on the relationship between the amount of damage D and the resistance increase rate. The determined threshold value Th may be stored in the control device 70 and referred to by the comparison unit 78.

[0046] <Process S60 for changing upper limit SOC> In process S60 (see FIG. 4), the control unit 79 changes the upper limit SOC during charging and discharging. When the damage amount D exceeds the threshold value Th, the control unit 79 restricts the use of the charge depth region (phase change region) P where a phase change occurs. The value of the upper limit SOC to be changed may be determined according to the composition of the positive electrode active material, etc. In this embodiment, the upper limit SOC is changed to 80% (charge / discharge capacity Q is 160 Ah). As shown in FIG. 5, in Examples 1 and 2, when the charge / discharge capacity Q is about 170 Ah, dV / dQ becomes maximum, and the phase change of the positive electrode active material may progress. By limiting the charge / discharge capacity Q to 160 Ah, the progress of the phase change of the positive electrode active material can be suppressed.

[0047] In this way, in the battery system 100, after a specific condition is reached (in this embodiment, after the damage amount D becomes equal to or greater than the threshold value Th), charging and discharging are controlled so as not to charge and discharge in the charge depth region (phase change region) P where a phase change occurs. This suppresses the phase change of the positive electrode active material, making it easier to maintain the capacity of the nonaqueous electrolyte secondary battery. In addition, the resistance of the nonaqueous electrolyte secondary battery is less likely to increase. In addition, before the upper limit SOC is changed, the upper limit SOC is set high (100% in this embodiment). As a result, a high-capacity battery system 100 is realized.

[0048] Furthermore, the control of charging and discharging the nonaqueous electrolyte secondary battery 1 is not limited to not charging and discharging in the phase change region P, and may be realized by limiting charging and discharging. For example, after limiting charging and discharging, the SOC is limited so that it does not exceed the changed upper limit SOC during normal use. When a preset condition such as an emergency is met, charging and discharging may be controlled so that charging and discharging exceed the upper limit SOC.

[0049] The upper limit SOC may be gradually changed according to the accumulation of the damage amount D. In other words, the limit amount (charge / discharge capacity Q whose use is restricted, the upper limit SOC, etc.) may be gradually changed with respect to the accumulated value of the damage amount D. For example, the upper limit SOC may be set to 100% until the damage amount D exceeds 80. As described above, when the damage amount D exceeds 100, the upper limit SOC may be changed to 80%. In this case, the control unit 79 may control the upper limit SOC so that the upper limit SOC changes linearly from 100% to 80% until the damage amount becomes from 80 to 100, for example. The upper limit SOC is not limited to being linearly limited, and may be controlled in stages (for example, the upper limit SOC is lowered by 5% every time the damage amount D is accumulated by 5). In this way, the limit amount is gradually changed, so that the progress of the phase change of the positive electrode active material can be easily suppressed while reducing the influence on the usability of the battery system 100. In addition, the user of the battery system 100 can easily deal with the charge / discharge restriction.

[0050] In addition, the use of the charge depth region P may be limited when a predetermined condition is satisfied. For example, when the damage amount D exceeds the threshold value Th, the use of only the low current region may be limited. The use of the charge depth region P may be limited when the charge / discharge current I is low, and the use of the charge depth region P may not be limited when the charge / discharge current I is high. According to the inventor's trial, the lower the charge / discharge current I, the more likely the phase change of the positive electrode active material progresses, and the higher the charge / discharge current I, the less likely the phase change of the positive electrode active material progresses. In other words, the lower the charge / discharge current I, the greater the damage to the positive electrode active material, and the higher the charge / discharge current I, the less the damage to the positive electrode active material. Therefore, by limiting the use of the charge depth region P when the charge / discharge current I is low, the effect of suppressing the progress of the phase change of the positive electrode active material is large. When the charge / discharge current I is high, the phase change of the positive electrode active material is less likely to progress even if the use of the charge / discharge current P is not limited. Although not particularly limited, it is preferable to restrict the use of the charge depth region P when the charge / discharge current I is less than 0.5 C, and not to restrict the use of the charge depth region P when the charge / discharge current I is 0.5 C or more. For example, when the battery system 100 is used as an in-vehicle battery, the current may be restricted to decelerate by regenerative braking when the current is 0.5 C or more, and to decelerate by hydraulic braking when the current is less than 0.5 C. This can minimize damage to the positive electrode active material, recover regenerative energy, and improve energy efficiency.

[0051] Examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.

[0052] <Preparation of lithium-ion secondary batteries> A lithium nickel manganese cobalt composite oxide as a positive electrode active material layer, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in a mass ratio of binder:AB:PVdF=97.5:1.5:1.0. The molar ratio of nickel, cobalt, and manganese in the lithium nickel manganese cobalt composite oxide was nickel:cobalt:manganese=80:10:10. An appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to the resulting mixture to prepare a positive electrode composite slurry. The positive electrode composite slurry was applied to both sides of a long aluminum foil and dried. Here, the weight of the positive electrode active material layer after drying was 10 cm. 2 The amount of the positive electrode composite slurry applied was adjusted to 390 mg per electrode, and the coating was then roll-pressed with a pressure roller to produce a positive electrode plate.

[0053] Graphite as the negative electrode active material layer, carboxymethyl cellulose (CMC) as a thickener, and styrene butadiene rubber (SBR) as a binder were mixed in ion-exchanged water in a mass ratio of graphite:CMC:SBR=98.3:0.7:1.0 to prepare a negative electrode composite slurry. The negative electrode composite slurry was applied to both sides of a long copper foil and dried. Here, the weight of the negative electrode active material layer after drying was 10 cm 2 The amount of the negative electrode mixture slurry applied was adjusted to 255 mg per one piece, and the coating was then roll-pressed with a pressure roller to produce a negative electrode plate.

[0054] A separator was prepared, which was made of polyethylene (PE) with aluminum oxide provided on its surface via polyvinylidene fluoride (PVdF).

[0055] A mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1 was prepared. 6 was dissolved to a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte.

[0056] The positive and negative electrode plates were wound with a separator interposed therebetween to prepare a wound-type electrode body. The electrode body was housed in a square battery case together with the prepared non-aqueous electrolyte and sealed airtight to obtain a lithium ion secondary battery of Example 1. The upper limit voltage of the lithium ion secondary battery of Example 1 was set to 4.2V.

[0057] As the positive electrode active material, a lithium nickel manganese cobalt composite oxide was used in which the molar ratio of nickel, cobalt, and manganese was nickel:cobalt:manganese=70:10:20. When the weight of the positive electrode active material layer after drying was 10 cm 2 The amount of the positive electrode composite slurry applied was adjusted to 425 mg per unit area, and the positive electrode composite slurry was applied. A lithium ion secondary battery of Example 2 was obtained in the same manner as in Example 1, except for the above. The upper limit voltage of the lithium ion secondary battery of Example 2 was set to 4.25 V.

[0058] As the positive electrode active material, a lithium nickel manganese cobalt composite oxide was used in which the molar ratio of nickel, cobalt, and manganese was nickel:cobalt:manganese=60:20:20. When the weight of the positive electrode active material layer after drying was 10 cm 2 The amount of the positive electrode composite slurry applied was adjusted to 440 mg per unit area, and the positive electrode composite slurry was applied. A lithium ion secondary battery of Example 3 was obtained in the same manner as in Example 1, except for the above. The upper limit voltage of the lithium ion secondary battery of Example 3 was set to 4.25 V. The weight of the positive electrode active material was set so that the lithium ion secondary batteries of Examples 1 to 3 had the same capacity.

[0059] <Measurement of initial resistance> The lithium ion secondary batteries of Examples 1 to 3 were adjusted to a state of SOC 50%. Then, various current values ​​were applied in an environment of -10°C, and the battery voltage was measured after 2 seconds. Then, the applied current and the voltage change were linearly interpolated, and the resistance value (initial resistance) was calculated from the slope.

[0060] <Evaluation of Capacity Retention Rate> 7 and 8 are graphs showing the relationship between the number of cycles and the capacity retention rate. Fig. 7 shows the relationship between the number of cycles and the capacity retention rate for the lithium ion secondary batteries of Example 1, Example 3, and Example 4 described later. Fig. 8 shows the relationship between the number of cycles and the capacity retention rate for the lithium ion secondary batteries of Example 2, Example 3, and Example 5 described later.

[0061] The capacity retention rate was evaluated for the lithium ion secondary battery of Example 1. First, the battery was discharged at a current of 50A until the battery voltage reached 3.0V. Next, the battery was charged at a current of 50A until the battery voltage reached 4.2V. Next, the battery was discharged at a current of 50A until the battery voltage reached 3.0V. The capacity of the test lithium ion secondary battery at this time was defined as the initial capacity. The lithium ion secondary battery after the initial capacity measurement was subjected to 1000 cycles of charge and discharge at a current of 50A with SOC of 0 to 100%. Here, SOC 0% was defined as an open circuit voltage (OCV) of 3.0V, and SOC 100% was defined as an OCV of 4.2V. The battery capacities after 250 cycles, 500 cycles, and 1000 cycles were obtained and defined as post-endurance capacity. Using the initial capacity and post-endurance capacity, the following formula (1): Capacity retention rate (%) = Capacity after durability / Initial capacity x 100 (1) The capacity retention rate (%) in the cycle test was calculated based on the above. For the lithium ion secondary batteries of Examples 2 and 3, the capacity retention rate was evaluated in the same manner as for the lithium ion secondary battery of Example 1, except that the upper limit battery voltage (battery voltage at SOC 100%) was set to 4.25 V.

[0062] Furthermore, for a lithium ion secondary battery (Example 4) similar to Example 1, the initial resistance was measured, and a cycle test was performed under the same conditions as above, while comparing the damage amount D with the threshold value Th according to the flow chart shown in FIG. 4. Since the damage amount D became equal to or greater than the threshold value Th after 250 cycles, the upper limit SOC was set to 80%, and charging and discharging were performed with SOC 0 to 80% until 1000 cycles. Furthermore, for a lithium ion secondary battery (Example 5) similar to Example 2, the initial resistance was measured, and a cycle test was performed under the same conditions as above, while comparing the damage amount D with the threshold value Th according to the flow chart shown in FIG. 4. Since the damage amount D became equal to or greater than the threshold value Th after 500 cycles, the upper limit SOC was set to 80%, and charging and discharging were performed with SOC 0 to 80% until 1000 cycles. The results of the evaluation of the capacity retention rate are shown in FIG. 7 and FIG. 8.

[0063] <Evaluation of Resistance Increase Rate> 9 and 10 are graphs showing the relationship between the number of cycles and the resistance increase rate. Fig. 9 shows the relationship between the number of cycles and the capacity retention rate for the lithium ion secondary batteries of Examples 1, 3, and 4. Fig. 10 shows the relationship between the number of cycles and the capacity retention rate for the lithium ion secondary batteries of Examples 2, 3, and 5.

[0064] For the lithium ion secondary batteries of Examples 1 to 5, the post-durability resistances after 250 cycles, 500 cycles, and 1000 cycles were measured in the same manner as in the measurement of the initial resistance. Using the initial resistance and the post-durability resistance, the following formula (2): Resistance increase rate (%) = Resistance after durability / Initial resistance x 100 (2) The resistance increase rate (%) in the cycle test was calculated based on the above. The evaluation results of the resistance increase rate are shown in Figs. 9 and 10.

[0065] A comparison between Example 1 and Example 4 (see FIG. 7) and a comparison between Example 2 and Example 5 (see FIG. 8) shows that when the charge / discharge conditions are controlled so that charging / discharging does not occur in a depth of charge region where a phase change occurs after the amount of damage D becomes equal to or greater than the threshold Th, the capacity is more likely to be maintained than when the charge / discharge conditions are not controlled. A comparison between Example 1 and Example 4 (see FIG. 9) and a comparison between Example 2 and Example 5 (see FIG. 10) shows that when the charge / discharge conditions are controlled so that charging / discharging does not occur in a depth of charge region where a phase change occurs after the amount of damage D becomes equal to or greater than the threshold Th, the resistance is less likely to increase than when the charge / discharge conditions are not controlled.

[0066] Comparison between Example 3 and Example 4 (see Figures 7 and 9) and comparison between Example 3 and Example 5 (see Figures 8 and 10) reveals that even when a high Ni-containing lithium composite oxide is used as the positive electrode active material, by controlling the charge and discharge conditions as described above, the capacity retention rate and the resistance increase rate can be achieved at the same levels as those of a lithium ion secondary battery that does not use a high Ni-containing lithium composite oxide.

[0067] The damage coefficient α used in calculating the amount of damage D will be described below. Here, an example of a method for setting the damage coefficient α by testing will be described for the lithium ion secondary batteries of Example 1 and Example 2. Note that the following description is not intended to limit the present invention to such an embodiment.

[0068] <Damage coefficient α setting> The damage coefficient α can be set based on the capacity retention rate during the cycle test. Here, the setting of the damage coefficient α will be described based on the results obtained during the evaluation of the capacity retention rate described above. Note that the method for setting the damage coefficient α is not limited to the following method, and the coefficient α may be appropriately set by a prior test or the like.

[0069] In Fig. 7 and Fig. 8, the horizontal axis of the graph is the square root of the number of cycles, and the vertical axis is the capacity retention rate. The capacity retention rate is plotted for each number of cycles. According to the inventor's trial, when the positive electrode active material does not deteriorate abnormally, the capacity retention rate for each number of cycles is plotted on an approximately straight line. When the positive electrode active material deteriorates abnormally due to a phase change, the capacity retention rate drops significantly at that point, and the slope of the graph changes. In other words, an inflection point appears in the graph showing the relationship between the square root of the number of cycles and the capacity retention rate. Here, the damage amount D at the inflection point on the graph is set to 100.

[0070] As shown in Fig. 7, in the lithium ion secondary battery of Example 1, an inflection point appears after 250 cycles. The damage coefficient α may be calculated based on the inflection point and the number of cycles at which the inflection point appears. The damage coefficient α for the positive electrode active material of the lithium ion secondary battery of Example 1 is, for example, 100 / (250 cycles) 1 / 2 =6.33 As shown in FIG. 8, in the lithium ion secondary battery of Example 2, an inflection point appears after 500 cycles. The damage coefficient α for the positive electrode active material of the lithium ion secondary battery of Example 2 can be calculated as follows: 100 / (500 cycles) 1 / 2 =4.48 In this case, the damage amount D can be calculated using the following formula (3): Damage amount D = Damage coefficient α × (number of cycles) 1 / 2 (3) The damage coefficient α may be calculated based on the above formula. The threshold value Th may be set to 100. The method of calculating the damage coefficient α is not limited to the above method.

[0071] A map of the damage coefficient α may be prepared by carrying out cycle tests while changing the conditions of parameters related to damage to the positive electrode active material, such as changes in charge / discharge current I, battery temperature T, dV / dQ, etc. Hereinafter, as an example, the preparation of a map of the damage coefficient α determined based on changes in charge / discharge current I, battery temperature T, and dV / dQ will be described.

[0072] A cycle test was performed at different charge / discharge currents I, and the damage coefficient α was calculated for each charge / discharge current I. Here, using the lithium ion secondary battery of Example 1, a cycle test was performed in the same manner as above for each of the cases where the charge / discharge current I was set to 50A, 100A, and 200A. Here, the battery temperature T was fixed at 60°C. FIG. 11 is a graph showing the relationship between the number of cycles and the capacity retention rate. As shown in FIG. 11, the smaller the charge / discharge current I, the greater the decrease in the capacity retention rate, and the larger the charge / discharge current I, the smaller the decrease in the capacity retention rate. According to the knowledge of the present inventor, the larger the charge / discharge current I, the earlier the phase change region P is passed, so that the phase change can be suppressed.

[0073] The damage coefficient α was calculated based on the graph obtained when a cycle test was performed with different charge / discharge currents I. Here, similar to the method for calculating the damage coefficient α described above, the damage coefficient α was calculated based on the inflection points of the graph. Detailed calculations are omitted, but the damage coefficient α was 10.0 when the charge / discharge current I was set to 50A. The damage coefficient α was 6.3 when the charge / discharge current I was set to 100A. The damage coefficient α was 5.6 when the charge / discharge current I was set to 50A.

[0074] In addition, cycle tests were performed at different battery temperatures T, and the damage coefficient α was calculated for each battery temperature T. Here, using the lithium ion secondary battery of Example 1, cycle tests were performed in the same manner as above for each of the cases where the battery temperature T was set to 60°C, 25°C, and -10°C. Here, the charge / discharge current I was fixed to 50A. FIG. 12 is a graph showing the relationship between the number of cycles and the capacity retention rate. As shown in FIG. 12, the higher the battery temperature T, the greater the decrease in the capacity retention rate, and the lower the battery temperature T, the smaller the decrease in the capacity retention rate. According to the knowledge of the present inventor, the higher the battery temperature T, the more cracks and the like are generated in the positive electrode active material, and the more the phase change may progress.

[0075] The damage coefficient α was calculated based on the graph obtained when a cycle test was performed at different battery temperatures T. Detailed calculations are omitted, but the damage coefficient α was 10.0 when the battery temperature T was set to 60°C. The damage coefficient α was 4.2 when the battery temperature T was set to 25°C. The damage coefficient α was 0 when the battery temperature T was set to -10°C.

[0076] In addition, cycle tests were performed in different charge / discharge ranges, and the damage coefficient α was calculated for each charge / discharge range. The charge / discharge range was set based on the SOC. The lower limit SOC of the charge / discharge range was fixed to 0%. It was set by changing the upper limit SOC of the charge / discharge range. Here, using the lithium ion secondary battery of Example 1, cycle tests were performed in the same manner as above for the cases where the upper limit SOC of the charge / discharge range was set to 100%, 93%, and 87%. FIG. 13 is a graph showing the relationship between the number of cycles and the capacity retention rate. As shown in FIG. 13, when the upper limit SOC was set to 87%, the decrease in the capacity retention rate was smaller than when the upper limit SOC was set to 93% or 100%. When the upper limit SOC was set to 93% and when it was set to 100%, the decrease in the capacity retention rate was about the same. According to the knowledge of the present inventor, the greater the change in dV / dQ in the phase change region P, the more cracks and the like are generated in the positive electrode active material, and the phase change may progress. In addition to the capacity retention rate, the resistance increase rate when the upper limit SOC was changed was evaluated in the same manner as above. Although a detailed explanation is omitted, as with the capacity retention rate, when the upper limit SOC was set to 87%, the resistance increase rate was lower than when the upper limit SOC was set to 93% or 100%.

[0077] The damage coefficient α was calculated based on the graph obtained when cycle tests were performed with different upper SOC limits. Detailed calculations are omitted, but the damage coefficient α was 6.3 when the upper SOC limit was set to 100% and 93%. The damage coefficient α was 5.3 when the upper SOC limit was set to 87%.

[0078] In this way, a map for calculating the damage coefficient α may be prepared by performing tests while changing parameters such as the charge / discharge current I, the battery temperature T, and the changes in dV / dQ, and determining the relationship between each parameter and the damage coefficient α.

[0079] The technology disclosed herein has been described above in various ways. Unless otherwise specified, the embodiments and the like described herein do not limit the present invention. Furthermore, the technology disclosed herein can be modified in various ways, and each component and each process described herein can be omitted or combined as appropriate unless a particular problem occurs. Furthermore, this specification includes the disclosures described in the following sections.

[0080] Section 1: A method for controlling a battery system including a nonaqueous electrolyte secondary battery, comprising: The nonaqueous electrolyte secondary battery includes a positive electrode active material and a negative electrode active material, the positive electrode active material undergoes a phase change upon charging and discharging of the nonaqueous electrolyte secondary battery, After a specific condition is reached, charging / discharging is not performed in a charge depth region where the phase change occurs, or charging / discharging is limited. A method for controlling a battery system.

[0081] Section 2: The battery system includes: A detection unit that detects a charge depth region where the phase change occurs based on a voltage change amount relative to a charge / discharge capacity; a calculation unit for calculating an amount of damage caused by charging and discharging in a charge depth region in which the phase change occurs; a control unit that limits use of a charge depth region in which the phase change occurs when the amount of damage exceeds a threshold; Item 2. A method for controlling a battery system according to item 1, comprising:

[0082] Section 3: 3. The method for controlling a battery system according to item 2, wherein the amount of voltage change is detected below a certain current value, and is substituted with SOC-dV / dSOC for current values ​​above that value.

[0083] Section 4: 4. The method for controlling a battery system according to item 2 or 3, wherein a limit amount is gradually changed with respect to the integrated value of the amount of damage.

[0084] Section 5: 5. The method for controlling a battery system according to any one of items 2 to 4, further comprising restricting use only in a low current region when the amount of damage exceeds the threshold value. [Explanation of symbols]

[0085] 1 Nonaqueous electrolyte secondary battery 10 Cases 12 Positive terminal 14 Negative terminal 20 Electrode body 30 Positive plate 32 Positive electrode core 34 Cathode active material layer 40 Negative plate 42 Negative electrode core 44 Negative electrode active material layer 50 Separator 70 Control device 71 Sensors 71a Voltage Sensor 71b Current Sensor 71c Temperature Sensor 72 Charge / discharge capacity detection section 73 SOC detector 74 Detection section 75 Judgment section 76 Calculation section 77 Memory section 78 Comparison Section 79 Control Unit 100 Battery System

Claims

1. A method for controlling a battery system including a nonaqueous electrolyte secondary battery, comprising: The nonaqueous electrolyte secondary battery includes a positive electrode active material and a negative electrode active material, the positive electrode active material undergoes a phase change upon charging and discharging of the nonaqueous electrolyte secondary battery, After a specific condition is reached, charging / discharging is not performed in a charge depth region where the phase change occurs, or charging / discharging is limited. A method for controlling a battery system.

2. The battery system includes: A detection unit that detects a charge depth region where the phase change occurs based on a voltage change amount relative to a charge / discharge capacity; a calculation unit for calculating an amount of damage caused by charging and discharging in a charge depth region in which the phase change occurs; a control unit that limits use of a charge depth region in which the phase change occurs when the amount of damage exceeds a threshold; The method for controlling a battery system according to claim 1 , comprising:

3. 3. The method for controlling a battery system according to claim 2, wherein the amount of voltage change is detected at a current value equal to or less than a certain value, and is substituted with SOC-dV / dSOC at current values ​​higher than that.

4. The method for controlling a battery system according to claim 2 or 3, wherein a limit amount is gradually changed with respect to the integrated value of the amount of damage.

5. The method for controlling a battery system according to claim 2 or 3, further comprising restricting use only in a low current range when the amount of damage exceeds the threshold value.

Citation Information

Patent Citations

  • Charge / Discharge controlling device for hybrid vehicle

    JP2000324616A

  • Lithium ion secondary battery system and method for controlling lithium ion secondary battery system

    JP2013196805A

  • Storage battery management apparatus, storage battery managing method, and program

    JP2014077785A

  • Battery system

    JP2019212392A