Polyamide imide resin, polyamide imide resin composition, and method for producing polyamide imide resin composition

By treating terminal isocyanate groups of polyamide-imide resins with blocking agents, the resin's viscosity stability is enhanced, addressing the instability issue in DMAC-synthesized resins and ensuring consistent performance.

JP2024165865APending Publication Date: 2024-11-28RESONAC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023082421
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing polyamide-imide resins synthesized using organic solvents like DMAC exhibit poor viscosity stability during storage, leading to undesirable changes in properties, making it difficult to achieve desired performance in applications.

Method used

The synthesis of polyamide-imide resins is modified by treating terminal isocyanate groups with blocking agents, such as alcohol and monocarboxylic acids, to stabilize viscosity during storage.

Benefits of technology

The modified polyamide-imide resins demonstrate improved viscosity stability, maintaining consistent properties over time, even at lower temperatures, thus enhancing their performance in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165865000001
    Figure 2024165865000001
  • Figure 2024165865000002
    Figure 2024165865000002
  • Figure 2024165865000003
    Figure 2024165865000003
Patent Text Reader

Abstract

To provide a polyamide imide resin that employs NMP alternative solvents, achieving superior viscosity stability during storage, and a polyamide imide resin composition.SOLUTION: A polyamide imide resin has a terminal isocyanate group treated with a blocker, where the blocker includes at least one selected from the group consisting of alcohols and monocarboxylic acids.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a polyamide-imide resin, more particularly to a polyamide-imide resin having a terminal isocyanate group treated with a blocking agent. Another embodiment of the present invention relates to a resin composition containing the polyamide-imide resin of the above embodiment and an organic solvent, and a method for producing the same. [Background technology]

[0002] Polyamide-imide resins have excellent heat resistance, chemical resistance, and solvent resistance, and are therefore widely used in a variety of applications, such as paints for various devices and materials for moldings. For example, polyamide-imide resins are suitably used as materials for enameled wire varnishes, heat-resistant paints, secondary battery separators, etc. More specifically, known materials for secondary battery separators include aggregates of polyamide-imide fibers spun by electrospinning or nonwoven fabrics formed using polyamide-imide resins.

[0003] N-methyl-2-pyrrolidone (NMP) is known as a good solvent for polyamide-imide resins, and NMP is widely used in the synthesis of polyamide-imide resins. Polyamide-imide resin compositions containing NMP are also widely used in various applications. However, in recent years, from the viewpoints of environmental conservation and safety and hygiene, the use of NMP has been subject to stricter regulations. In addition, the boiling point of NMP is 200°C or higher, and high-temperature heating is required during drying. Therefore, polyamideimide resin compositions containing NMP are desired to be improved in terms of drying properties. Therefore, a polyamideimide resin composition using an organic solvent that is an alternative solvent capable of dissolving polyamideimide resins as well as NMP and that can provide good drying properties at relatively low temperatures is desired.

[0004] In response to this, various studies are being conducted on the use of N,N-dimethylacetamide (DMAC), N,N-dimethylformamide (DMF), etc., as organic solvents capable of dissolving polyamideimide resin and having a relatively low boiling point. For example, Patent Document 1 discloses polyamideimide fibers produced by producing a resin solution containing polyamideimide resin and DMAC and spinning the resin solution by electrospinning. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4797863 Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, Patent Document 1 describes that polyamideimide fibers can be spun using a solution of polyamideimide resin synthesized in the presence of DMAC. However, Patent Document 1 does not describe the specific properties of the polyamideimide fiber obtained by spinning, or the viscosity stability of the polyamideimide resin solution during storage. Generally, polyamide-imide resins synthesized in the presence of an organic solvent such as DMAC tend to have poorer properties than polyamide-imide resins synthesized in the presence of NMP using a diisocyanate and an acid component. For example, when DMAC is used in the synthesis of polyamide-imide resins, the viscosity of the resin is likely to change during storage, making it difficult to obtain the desired properties during use.

[0007] Therefore, the present invention provides a polyamideimide resin having excellent viscosity stability during storage by using an organic solvent that can be a substitute for NMP. The present invention also provides a polyamideimide resin composition constituted by using the polyamideimide resin and an organic solvent that can be a substitute for NMP, and a method for producing the same. [Means for solving the problem]

[0008] When polyamide-imide resin is synthesized by the reaction of diisocyanate with an acid component, the viscosity is likely to increase due to gelation or the like during storage due to the reaction of the terminal isocyanate groups. On the other hand, the present inventor has found through various studies that when polyamide-imide resin is synthesized using an organic solvent such as DMAC instead of NMP, the viscosity of the resin is likely to decrease during storage. This is because when polyamide-imide resin is synthesized in DMAC, the reaction between isocyanate groups tends to proceed more easily, and the number of bonds between isocyanate groups in the resin tends to increase. It is speculated that the viscosity decrease of the resin during storage is caused in part by hydrolysis of the bonds between the isocyanate groups.

[0009] In view of the above circumstances, the present inventors have conducted various studies on methods for suppressing the viscosity change, particularly the viscosity reduction, of polyamide-imide resins during storage, and have completed the present invention. That is, the embodiments of the present invention relate to the following, but are not limited to the following.

[0010] [1] A polyamide-imide resin having a terminal isocyanate group treated with a blocking agent, the blocking agent including at least one selected from the group consisting of an alcohol and a monocarboxylic acid.

[0011] [2] The polyamide-imide resin according to [1] above, wherein the blocking agent contains a monocarboxylic acid.

[0012] [3] The polyamide-imide resin according to the above [1] or [2], wherein the monocarboxylic acid includes an aliphatic monocarboxylic acid having 2 to 10 carbon atoms or benzoic acid.

[0013] [4] The polyamide-imide resin according to the above [1] or [2], having a number average molecular weight of 5,000 to 100,000.

[0014] [5] A polyamideimide resin composition obtained using a diisocyanate, an acid component containing a tribasic acid anhydride or a tribasic acid halide, an organic solvent having a structure represented by the following formula (I), and a blocking agent, wherein the blocking agent contains at least one selected from the group consisting of alcohols and monocarboxylic acids.

[0015] [ka]

[0016] In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 3 carbon atoms, or are bonded to each other to form a 5- or 6-membered heterocyclic group containing a nitrogen atom; R 3 is hydrogen or an alkyl group having 1 to 4 carbon atoms.

[0017] [6] A polyamideimide resin composition comprising: a polyamideimide resin having a terminal isocyanate group treated with a blocking agent, the blocking agent including at least one selected from the group consisting of an alcohol and a monocarboxylic acid; and an organic solvent having a structure represented by the following formula (I):

[0018] [ka]

[0019] In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 3 carbon atoms, or are bonded to each other to form a 5- or 6-membered heterocyclic group containing a nitrogen atom; R 3 is hydrogen or an alkyl group having 1 to 4 carbon atoms.

[0020] [7] A paint comprising the polyamideimide resin composition according to [5] or [6] above.

[0021] [8] An article having a coating film formed using the coating material described in [7] above.

[0022] [9] A molded product formed using the polyamideimide resin composition according to [5] or [6] above.

[0023]

[10] A method for producing a polyamideimide resin composition comprising a polyamideimide resin and an organic solvent having a structure represented by the following formula (I), reacting an isocyanate component containing a diisocyanate with an acid component containing a tribasic acid anhydride or a tribasic acid halide in the organic solvent to form a liquid containing a polyamide-imide resin having a terminal isocyanate group; and The method includes reacting a liquid containing the polyamide-imide resin having a terminal isocyanate group with a blocking agent, A method for producing a polyamideimide resin composition, wherein the blocking agent comprises at least one selected from the group consisting of alcohols and monocarboxylic acids.

[0024] [ka]

[0025] In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 3 carbon atoms, or are bonded to each other to form a 5- or 6-membered heterocyclic group containing a nitrogen atom; R 3 is hydrogen or an alkyl group having 1 to 4 carbon atoms. Effect of the Invention

[0026] According to an embodiment of the present invention, a polyamideimide resin having excellent viscosity stability during storage can be provided by using an alternative solvent to NMP. Also, according to an embodiment of the present invention, a polyamideimide resin composition and a method for producing the same can be provided, which are constituted by using the polyamideimide resin and an alternative solvent to NMP. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment. <1> Polyamide-imide resin The polyamide-imide resin is a resin obtained by reacting a diisocyanate and an acid component containing a tribasic acid anhydride or a tribasic acid halide as raw material monomers. The polyamide-imide resin of the present embodiment is a polyamide-imide resin (hereinafter referred to as a blocked polyamide-imide resin) in which the terminal isocyanate group of the polyamide-imide resin obtained by reacting the diisocyanate with the acid component is treated with a specific blocking agent such as an alcohol and / or a monocarboxylic acid.

[0028] More specifically, the blocked polyamideimide resin of the above embodiment has a terminal urethane structure formed by treatment with an alcohol and / or a terminal amide structure formed by treatment with a monocarboxylic acid. The polyamideimide resin may be a resin obtained by using any combination of two or more of the raw material monomers described below.

[0029] (Diisocyanate) The diisocyanate is not particularly limited and may be either an aromatic diisocyanate or an aliphatic diisocyanate. As a raw material monomer, a polyisocyanate other than a diisocyanate or a modified polyisocyanate such as a carbodiimide modified product may be further used as necessary. In one embodiment, the isocyanate component is preferably composed of only a diisocyanate.

[0030] Specific examples of aromatic diisocyanates include 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, 3,3'-diphenylmethane diisocyanate, 3,3'-dimethoxybiphenyl-4,4'-diisocyanate, paraphenylene diisocyanate, tolylene diisocyanate, naphthalene diisocyanate, etc. Specific examples of aliphatic diisocyanates include hexamethylene diisocyanate, isophorone diisocyanate, etc. From the viewpoint of heat resistance, aromatic diisocyanates are preferred, and among them, from the viewpoint of reactivity, it is preferred to use at least 4,4'-diphenylmethane diisocyanate.

[0031] In one embodiment, the polyamide-imide resin may use a diamine as a raw material monomer in addition to the isocyanate component. Examples of the diamine include 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, xylylenediamine, phenylenediamine, and isophoronediamine.

[0032] (acid component) The acid component includes a tribasic acid anhydride or a tribasic acid halide. The tribasic acid anhydride is not particularly limited, but an aromatic tribasic acid anhydride is preferably used, and trimellitic anhydride is particularly preferred. The tribasic acid halide is also not particularly limited, but a tribasic acid chloride is preferred, and an aromatic tribasic acid chloride is more preferred. A specific example is trimellitic anhydride chloride (trimellitic anhydride chloride), etc. From the viewpoint of reducing the burden on the environment, it is preferable to use trimellitic anhydride, etc.

[0033] In addition to the above-mentioned tribasic acid anhydride (or tribasic acid halide), the acid component may further contain a saturated or unsaturated polybasic acid such as a dicarboxylic acid, a tetracarboxylic dianhydride, etc. These saturated or unsaturated polybasic acids are preferably used within a range that does not impair the properties of the polyamide-imide resin.

[0034] The dicarboxylic acid is not particularly limited, but may be terephthalic acid, isophthalic acid, adipic acid, sebacic acid, etc. The tetracarboxylic dianhydride is not particularly limited, but may be pyromellitic dianhydride, benzophenone tetracarboxylic dianhydride, biphenyl tetracarboxylic dianhydride, etc. These may be used alone or in any combination of two or more.

[0035] From the viewpoint of maintaining the properties of the polyamideimide resin, the total amount of carboxylic acids other than the tribasic acid (dicarboxylic acid and tetracarboxylic acid) is preferably used in a range of 50 mol % or less, more preferably 30 mol % or less, based on the total amount of carboxylic acids. In one embodiment, the total amount of carboxylic acids other than the tribasic acid may be 0 mass %.

[0036] The ratio of the diisocyanate to the acid component can be adjusted in consideration of the molecular weight and crosslinking degree of the polyamideimide resin to be produced. For example, the total amount of the diisocyanate is preferably 0.8 to 1.1 mol, more preferably 0.95 to 1.08 mol, per 1.0 mol of the total amount of the acid components. In particular, from the viewpoint of easily obtaining a polyamideimide resin having a terminal isocyanate group, it is even more preferable that the total amount of the diisocyanate is 1.0 to 1.08 mol per 1.0 mol of the total amount of the acid components. The total amount of the acid components means the total amount of the tribasic acid anhydride or tribasic acid anhydride halide and the dicarboxylic acid and tetracarboxylic acid dianhydride used as necessary, and the total amount of the diisocyanate means the total amount of the diisocyanate and the diamine when the diamine is contained.

[0037] (Blocking agent) The blocking agent includes at least one selected from the group consisting of alcohols and monocarboxylic acids. A blocked polyamideimide resin in which a terminal isocyanate has been treated using such a blocking agent has a specific terminal structure, and is inhibited from not only decreasing in viscosity during storage but also increasing in viscosity, and can easily maintain excellent properties even after aging. In one embodiment, from the viewpoint of viscosity stability during storage, the polyamideimide resin preferably has a terminal isocyanate group treated with a monocarboxylic acid.

[0038] (alcohol) The alcohol that can be used as a blocking agent may be a saturated or unsaturated compound having one hydroxyl group in the molecule, and may be either an aliphatic alcohol or an aromatic alcohol. The aliphatic alcohol may have 1 to 6 carbon atoms and may have any of a linear, branched, or cyclic structure. The aromatic alcohol may be a compound in which a hydroxyl group is bonded to an aromatic ring via an alkylene group having 1 to 3 carbon atoms, such as benzyl alcohol. The aromatic alcohol may contain a substituent R other than a hydroxyl group or a carboxyl group on the aromatic ring. The substituent R is not particularly limited, and may be an alkyl group and / or an alkoxy group having 1 to 6 carbon atoms. The aromatic alcohol also includes phenolic compounds such as phenol and cresol in which a hydroxyl group is directly bonded to an aromatic ring. In one embodiment, the blocking agent is preferably an aliphatic alcohol having 1 to 6 carbon atoms. Specific examples include methanol, ethanol, propanol, isopropanol, butanol, etc. Among these, methanol is preferably used.

[0039] (Monocarboxylic acid) The monocarboxylic acid that can be used as a blocking agent may be a saturated or unsaturated aliphatic monocarboxylic acid having one carboxy group in the molecule, or an aromatic monocarboxylic acid. The carbon number of the aliphatic monocarboxylic acid may be 2 to 10. That is, the aliphatic group excluding the carbon of the carboxy group in the aliphatic monocarboxylic acid may have a carbon number of 1 to 9. The carbon number of the aliphatic monocarboxylic acid may be preferably 2 to 6, more preferably 1 to 4. The aliphatic monocarboxylic acid may have any of a linear, branched, and cyclic structure. In one embodiment, a monocarboxylic acid having a linear structure with 2 to 6 carbon atoms is preferred. Specific examples of the aliphatic monocarboxylic acid include acetic acid, propionic acid, butyric acid, methacrylic acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, and decanoic acid. Among them, propionic acid can be preferably used.

[0040] The aromatic monocarboxylic acid may have, for example, 6 to 12 carbon atoms in the aromatic ring excluding the carbon of the carboxy group. In the aromatic monocarboxylic acid, the aromatic ring may be any of a monocyclic structure, a condensed polycyclic structure, and a polycyclic structure in which aromatic groups are mutually bonded by a linking group. Specific examples of the aromatic ring include benzene, naphthalene, diphenylalkane, and diphenyl ether. The aromatic ring may further have a substituent R other than the carboxy group. The substituent R is not particularly limited, and may be an alkyl group and / or an alkoxy group having 1 to 6 carbon atoms. Specific examples of aromatic monocarboxylic acids include benzoic acid, toluic acid, cinnamic acid, etc. Toluic acid may be any of ortho, meta, and para isomers. Benzoic acid is particularly preferred.

[0041] <2> Method for producing polyamide-imide resin The polyamide-imide resin can be produced by applying a known method without any particular limitation. Typically, the method includes using diisocyanate and an acid component containing a tribasic acid anhydride and / or a tribasic acid halide as raw material monomers and reacting them in an organic solvent (polymerization step), and in addition to the polymerization step, treating the terminal isocyanate group of the polyamide-imide resin with a blocking agent (blocking step). In the polymerization step, a part of the diisocyanate may be replaced with a diamine. Each step will be described in more detail below.

[0042] (Polymerization process) The details of the raw material monomers used in the polymerization step are as described above. The polymerization step can be carried out using a well-known organic solvent (hereinafter also referred to as a synthetic solvent) such as NMP used in the synthesis (polymerization reaction) of polyamide-imide resin. In one embodiment, the organic solvent (synthetic solvent) may be an alternative solvent to NMP, and preferably contains at least an organic solvent having a structure represented by the following formula (I).

[0043] [ka]

[0044] In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 3 carbon atoms, or are bonded to each other to form a 5- or 6-membered heterocyclic group containing a nitrogen atom; R 3 is hydrogen or an alkyl group having 1 to 4 carbon atoms.

[0045] Specific examples of organic solvents having a structure represented by the above formula (I) include N,N-dimethylformamide, N,N-dimethylacetamide, 4-formylmorpholine (4-morpholinecarbaldehyde), N,N-acetylformamide, 3-methoxy-N,N-dimethylpropionamide, and N,N-dimethylpropionamide. In one embodiment, the organic solvent preferably contains at least one selected from the group consisting of N,N-dimethylformamide, N,N-dimethylacetamide, and N,N-acetylformamide. These solvents have a lower boiling point than NMP, which allows the resin solution to dry more easily. The organic solvent more preferably contains at least N,N-dimethylacetamide (DMAC).

[0046] When an organic solvent having a structure represented by the above formula (I) is used, the reaction mixture (liquid) after the polymerization reaction can be used as a polyamideimide resin composition as it is. That is, in one embodiment, an organic solvent having a structure represented by the above formula (I), such as DMAC, may be used as both the synthesis solvent and the dilution solvent described later.

[0047] The amount of the organic solvent used in the polymerization step is not particularly limited. In one embodiment, from the viewpoint of the solubility of the polyamideimide resin, the amount of the organic solvent used is preferably 50 to 500 parts by mass per 100 parts by mass of the total amount of the diisocyanate (and the diamine used as necessary) and the acid component. The reaction temperature is not particularly limited. It can be adjusted in consideration of the boiling point of the organic solvent used, and generally may be 80 to 180° C. The polymerization reaction is preferably carried out under an atmosphere of nitrogen or the like in order to reduce the influence of moisture in the air.

[0048] Specific examples of the procedure of the polymerization process for producing a polyamide-imide resin include the following. (1) A method in which an acid component and a diisocyanate are used at the same time and reacted to synthesize a polyamide-imide resin. (2) A method in which an acid component is reacted with an excess amount of diisocyanate to synthesize an amide-imide oligomer having an isocyanate group at the end, and then an acid component is added to react with the terminal isocyanate group to synthesize a polyamide-imide resin. (3) A method in which an excess amount of an acid component is reacted with a diisocyanate to synthesize an amide-imide oligomer having an acid or acid anhydride group at the terminal, and then additional diisocyanate is added to react with the terminal acid or acid anhydride group to synthesize a polyamide-imide resin.

[0049] In the manufacturing method of this embodiment, any of the above methods (1) to (3) may be applied, and diisocyanate and diamine may be used in combination as necessary. Although not particularly limited, the above method (2) is preferably applied since it is easy to obtain a polyamideimide resin having a terminal isocyanate group. The compounding ratio of diisocyanate and acid component is as described above.

[0050] (Blocking process) The blocked polyamideimide resin of the present embodiment is obtained by treating the terminal isocyanate group of the polyamideimide resin with a blocking agent (blocking step) in addition to the above polymerization step. Here, an alcohol and / or a monocarboxylic acid is used as the blocking agent. These blocking agents are as described above.

[0051] The polymerization step and the blocking step may be carried out separately, or may be carried out simultaneously, i.e., the polymerization reaction and the blocking reaction. When the steps are carried out separately, a blocking agent is reacted with the polyamide-imide resin after the polymerization step. When the two steps are carried out simultaneously, a blocking agent may be added to the synthesis solvent.

[0052] The amount of the blocking agent in blocking is preferably adjusted to within a range of 1.0 to 10.0 parts by mass, with the total amount of diisocyanate used in the polymerization step being taken as 100 parts by mass. From the viewpoint of the viscosity stability during storage of the resulting blocked polyamideimide resin composition, the amount of the blocking agent is more preferably adjusted to within a range of 2.5 to 5.0 parts by mass.

[0053] The molecular weight of the polyamide-imide resin is not particularly limited, and is preferably adjusted according to the application of the resin. The molecular weight of the polyamide-imide resin can be adjusted by adjusting the conditions during synthesis. In one embodiment, the number average molecular weight (Mn) of the polyamideimide resin is preferably at least 5,000, more preferably at least 10,000, and even more preferably at least 15,000. On the other hand, from the viewpoint of ensuring solubility in a solvent and easily obtaining a viscosity suitable for coating or various processing, the Mn of the polyamideimide resin is preferably at most 100,000, more preferably at most 80,000, and even more preferably at most 70,000.

[0054] In one embodiment, when the polyamideimide resin is used as a fiber material, from the viewpoint of ensuring mechanical strength in a spinning process, the Mn of the polyamideimide resin is preferably 5,000 to 100,000. In particular, from the viewpoint of ensuring desired heat resistance when molded into a nonwoven fabric, for example, the Mn of the polyamideimide resin is preferably 20,000 or more.

[0055] In one embodiment, the Mn of the polyamideimide resin is preferably in the range of 20,000 to 60,000. When a polyamideimide resin having an Mn within the above range is used, it becomes easy to obtain a good balance between heat resistance and solubility in a solvent, and the coating step can be carried out well. The Mn of the polyamide-imide resin can be controlled within the above-mentioned preferred range by sampling during the synthesis of the resin, measuring the Mn by gel permeation chromatography (GPC) using a calibration curve of standard polystyrene, and continuing the synthesis until the desired Mn is reached. The GPC measurement conditions are as described in the Examples.

[0056] <3> Polyamide-imide resin composition In one embodiment, the polyamideimide resin composition may be a mixture obtained by using a diisocyanate, an acid component including a tribasic acid anhydride or a tribasic acid halide, an organic solvent having a structure represented by the above formula (I), and a blocking agent. In the above embodiment, the mixture may contain an unreacted diisocyanate, an unreacted acid component, or an unreacted blocking agent. In another embodiment, the mixture may contain a polyamideimide resin having a terminal isocyanate group obtained by the reaction of a diisocyanate with an acid component, and an unreacted blocking agent.

[0057] In another embodiment, the polyamideimide resin composition may be a mixture containing a blocked polyamideimide resin having terminal isocyanate groups obtained by reacting a diisocyanate with an acid component containing a tribasic acid anhydride or a tribasic acid halide, at least a part of which has been treated with a blocking agent, and an organic solvent having the structure represented by the above formula (I). In the above embodiment, the mixture may contain a polyamideimide resin having unblocked terminal isocyanate groups and an unreacted blocking agent.

[0058] In each embodiment of the polyamideimide resin composition, the details of the organic solvent having the structure represented by the formula (I) and the blocking agent are as described above. The polyamideimide resin composition (hereinafter also referred to as a resin composition) may further contain other components depending on the application in addition to the polyamideimide resin and the organic solvent of the above embodiment.

[0059] The polyamideimide resin composition contains at least an organic solvent having the structure represented by the above formula (I) as an organic solvent. The polyamideimide resin composition may further contain other solvents not containing the structure represented by the above formula (I) within a range that does not deteriorate the effects of the present invention. As other solvents, one or more polar solvents selected from N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, dimethylsulfoxide, 1,3-dimethyl-2-imidazolidine, etc., or water can be used.

[0060] Furthermore, as a co-solvent, ether compounds such as anisole, diethyl ether, ethylene glycol, etc.; ketone compounds such as acetophenone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanenone, cyclopentanone, etc.; aromatic hydrocarbon solvents such as xylene, toluene, etc. may be optionally used. In the case where the organic solvent having the structure represented by the above formula (I) (hereinafter also referred to as organic solvent (I)) and other solvents are used to form a mixed solvent, the content of the organic solvent (I) such as DMAC in the mixed solvent is preferably 50% by mass or more, more preferably 80% by mass or more. By adjusting the content of the organic solvent (I) in the mixed solvent to the above range, the preferred effects of this embodiment can be easily obtained.

[0061] In one embodiment, the resin composition is preferably substantially free of NMP. The term "substantially free of NMP" means that the content of NMP is preferably less than 0.3% by mass based on the total mass of the resin composition. The content of NMP is preferably less than 0.2% by mass, more preferably less than 0.1% by mass. Therefore, for example, NMP that is mixed in during a process such as resin synthesis and remains in the resin composition is not completely excluded.

[0062] In the polyamideimide resin composition of the present embodiment, the content of the polyamideimide resin is not particularly limited and can be appropriately adjusted according to the application. In order to fully exert the function of the polyamideimide resin, the content of the polyamideimide resin based on the total solid content in the resin composition is preferably 10 mass% or more. Two or more polyamideimide resins may be used in combination, but by including at least the blocked polyamideimide resin of the above embodiment, it becomes easy to suppress the viscosity reduction during storage. The content of the polyamideimide resin may be more preferably 60% by mass or more, further preferably 70% by mass or more, and particularly preferably 80% by mass or more, based on the total solid content in the resin composition. In one embodiment, the content may be 100% by mass.

[0063] In one embodiment, from the viewpoint of balance with other components, the content of the polyamideimide resin based on the solid components in the resin composition is preferably 1 to 60 mass %. The content is preferably 5 mass % or more, more preferably 10 mass % or more, and even more preferably 15 mass % or more. On the other hand, the content is preferably 50 mass % or less, more preferably 40 mass % or less, and even more preferably 30 mass % or less.

[0064] By adjusting the content of the polyamideimide resin based on the total mass of the solid components in the resin composition within the above range, the resin composition can be suitably used as a paint for forming a coating film such as a protective film for various devices, or as a material for various molded products. One embodiment of the present invention may be a paint containing the resin composition. Another embodiment may be an article having a coating film formed using the paint. Another embodiment may be a molded product formed using the resin composition.

[0065] The polyamideimide resin composition of the present embodiment can be used in various applications, such as paints for forming coating films such as protective films for various articles, materials for moldings, etc. The polyamideimide resin of the present embodiment can also be suitably used in applications requiring heat resistance. Specific examples of heat-resistant applications include various applications expected to be used in high-temperature environments, such as battery separators, fuel exhaust gas filters, coatings for heat-resistant parts, etc. When such applications are expected to be used in heat-resistant applications, the resin constituting the resin composition preferably has a glass transition temperature (Tg) of 270° C. or higher in order to obtain sufficient heat resistance.

[0066] For the above heat-resistant applications, the polyamideimide resin composition of the present embodiment preferably contains (A) a polyamideimide resin having a number average molecular weight of 20,000 or more, and (B) an organic solvent having a structure represented by the above formula (I) (also referred to as organic solvent (I)). The organic solvent (I) preferably contains at least N,N-dimethylacetamide (DMAC). According to the resin composition of the above embodiment, by using a polyamideimide resin having a number average molecular weight of 20,000 or more, it is easy to obtain a glass transition temperature (Tg) of 270°C or more. Here, Tg is a value measured using a differential scanning calorimeter (DSC). In addition, since the polyamideimide resin exhibits excellent solubility in DMAC, excellent flowability can be easily obtained.

[0067] The polyamideimide resin composition of the present embodiment may further contain optional components such as pigments, fillers, defoamers, preservatives, surfactants, thickeners, etc. in addition to the polyamideimide resin and organic solvent depending on the application and form of use. The type of optional component such as the filler can be selected in consideration of its water resistance, chemical resistance, etc., and a component that is insoluble in water is preferred.

[0068] In one embodiment, the polyamideimide resin composition can be suitably used as a material for a nonwoven fabric produced by melt spinning. When melt spinning is carried out using the resin composition, a fiber having sufficient strength during spinning can be easily obtained, and a decrease in fluidity can be suppressed, thereby maintaining good workability.

[0069] In one embodiment, when a nonwoven fabric is produced using the resin composition, the resin composition preferably further contains a surfactant as necessary. The surfactant is not particularly limited, but is preferably one that does not cause layer or phase separation until the resin composition is uniformly mixed and the fibers are dried after spinning, and does not leave much residue when the fibers are assembled to form a nonwoven fabric. The content of the surfactant is not particularly limited. In order to maintain a uniform mixed state of the resin composition and to prevent adverse effects during application and processing, the content in the resin composition is preferably 0.01 to 10 mass %, more preferably 0.5 to 5 mass %.

[0070] In one embodiment, the resin composition can be used as a coating material for forming a coating film such as a protective film for various devices, and as a material for a molded article. In this case, the resin composition may further contain a filler in order to improve the water resistance, etc., of the resulting coating film and molded article. Specifically, examples of the filler include metal powder, metal oxide (aluminum oxide, zinc oxide, tin oxide, titanium oxide, etc.), glass beads, glass flakes, glass particles, ceramics, silicon carbide, silicon oxide, calcium fluoride, carbon black, graphite, mica, barium sulfate, etc. These may be used alone or in combination of two or more.

[0071] In one embodiment, the resin composition may contain a resin other than the polyamideimide resin. For example, fluororesin, polyethersulfone resin (PES), polyimide resin (PI), polyamide resin, epoxy compound, isocyanate compound, melamine compound, etc. may be used alone or in combination of two or more kinds, as necessary.

[0072] For example, the fluororesin may preferably be tetrafluoroethylene resin, tetrafluoroethylene-perfluorovinyl ether copolymer, or tetrafluoroethylene-hexafluoropropylene copolymer. Two or more of these may be used in combination. When a fluororesin is added to a resin composition, it becomes easy to impart properties such as non-adhesiveness, corrosion resistance, heat resistance, and chemical resistance.

[0073] Examples of epoxy compounds include bisphenol type epoxy resins (bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, etc.), biphenyl type epoxy resins, phenol novolac type epoxy resins, brominated phenol novolac type epoxy resins, o-cresol novolac type epoxy resins, flexible epoxy resins, polyfunctional epoxy resins, amine type epoxy resins, heterocycle-containing epoxy resins, alicyclic epoxy resins, triglycidyl isocyanurate, and bixylenol type epoxy resins.

[0074] These epoxy compounds may be used alone or in combination of two or more. The epoxy compounds may be added alone to react with the polyamide-imide resin. Alternatively, they may be added together with a curing agent or a curing accelerator so that the epoxy compound is unlikely to remain unreacted after molding.

[0075] Examples of the isocyanate compound include polyisocyanates of hexamethylene diisocyanate such as Duranate, polyisocyanates synthesized from 4,4'-diphenylmethane diisocyanate, etc. The mass average molecular weight of this polyisocyanate is preferably 500 to 9,000, more preferably 1,000 to 5,000.

[0076] The melamine compound is not particularly limited. For example, a methylol group-containing compound obtained by reacting melamine with formaldehyde, paraformaldehyde, or the like can be mentioned. The methylol group preferably has a structure etherified with an alcohol having 1 to 6 carbon atoms.

[0077] In one embodiment, the resin composition preferably further contains an epoxy compound (epoxy resin). By blending the epoxy compound, the thermal, mechanical and electrical properties of the polyamideimide resin composition can be further improved. The amount of each of the epoxy compound, isocyanate compound, and melamine compound contained in the resin composition is, for example, preferably 1 part by mass or more, and more preferably 5 parts by mass or more, relative to 100 parts by mass of the polyamideimide resin, while from the viewpoint of maintaining the heat resistance and strength of the polyamideimide resin composition, the amount is preferably 40 parts by mass or less, and more preferably 30 parts by mass or less.

[0078] <4> Method for producing polyamide-imide resin composition In one embodiment, the polyamideimide resin composition may include a blocked polyamideimide resin in which a terminal isocyanate group is treated with a blocking agent, the blocked polyamideimide resin being obtained by reacting a diisocyanate with an acid component containing a tribasic acid anhydride or a tribasic acid halide, and an organic solvent having a structure represented by the above formula (I). The blocked polyamideimide resin can be produced by reacting raw material monomers in the presence of an organic solvent (organic solvent (I)) having a structure represented by the above formula (I), and further reacting using a blocking agent. Therefore, in one embodiment, the resin composition can be produced by using the liquid (reaction mixture) obtained by the above method for producing a polyamideimide resin as it is. In this case, a diluting solvent may be added to the liquid as necessary.

[0079] That is, in one embodiment, a method for producing a polyamideimide resin composition includes reacting a diisocyanate with an acid component containing a tribasic acid anhydride or a tribasic acid halide in an organic solvent (I) containing DMAC or the like to form a liquid containing a polyamideimide resin having a terminal isocyanate group (polymerization step), and reacting the liquid containing the polyamideimide resin having a terminal isocyanate group with a blocking agent (blocking step), wherein the blocking agent contains at least one selected from the group consisting of alcohols and monocarboxylic acids.

[0080] In another embodiment, the above-mentioned production method may further include, in addition to the above-mentioned polymerization step and blocking step, adding a dilution solvent to the liquid containing the polyamideimide resin (dilution step).

[0081] In the above embodiment, the organic solvent and / or diluent solvent used in the polymerization step are as described above in the method for producing a polyamide-imide resin. In one embodiment, the organic solvent (I) preferably contains at least DMAC. As described above, the polymerization step and the blocking step may be carried out separately or simultaneously. EXAMPLES

[0082] The present invention will be described below with reference to examples. However, the preferred embodiments are not limited to these examples, and it goes without saying that the present invention includes many other embodiments based on the gist of the invention.

[0083] In the examples and comparative examples described later, the number average molecular weight of the polyamideimide resin was measured as follows. <Number average molecular weight> GPC model: Tosoh Corporation's HLC-8320GPC Detector: Tosoh RI Wavelength: 270nm Data processor: ATT 8 Column: Gelpack GL-S300MDT-5 x 2 Column size: 8mmφ×300mm Column temperature: 40℃ Solvent: DMF / THF = 1 / 1 (liters) + phosphoric acid 0.06M + lithium bromide 0.06M Sample concentration: 5mg / 1mL Injection volume: 5μL Pressure: 49kgf / cm 2 (4.8×10 6 Pa) Flow rate: 1.0mL / min

[0084] <1> Manufacture of polyamide-imide resin solution (resin composition) Example 1 96.1 g of trimellitic anhydride, 126 g of 4,4'-diphenylmethane diisocyanate, and 519 g of N,N-dimethylacetamide were placed in a flask equipped with a thermometer, a stirrer, and a cooling tube, and the temperature was gradually raised to 90°C over 1 hour while stirring in a dry nitrogen stream. After continuing heating for 3 hours, the temperature was gradually raised to 140°C while paying attention to the sudden foaming of carbon dioxide gas generated by the reaction, and heating was continued for 5 hours from the start of heating, and the reaction was stopped by cooling. Then, 3 g of methanol was added and heated at 80°C for 1 hour while stirring to obtain a polyamideimide resin solution (resin composition). The polyamideimide resin solution thus obtained was allowed to stand at room temperature, and the appearance was visually observed to be homogeneous and transparent. The non-volatile content of this polyamideimide resin solution (200°C / 2 hours) was 29 mass%, and the number average molecular weight of the polyamideimide resin was 29,000.

[0085] Example 2 96.1 g of trimellitic anhydride, 126 g of 4,4'-diphenylmethane diisocyanate, and 519 g of N,N-dimethylacetamide were placed in a flask equipped with a thermometer, a stirrer, and a cooling tube, and the temperature was gradually raised to 90°C over 1 hour while stirring in a dry nitrogen stream. After continuing heating for 3 hours, the temperature was gradually raised to 140°C while paying attention to the sudden foaming of carbon dioxide gas generated by the reaction, and heating was continued for 5 hours from the start of heating. After cooling to stop the reaction, 3 g of benzoic acid was added and heated at 80°C for 1 hour while stirring to obtain a polyamideimide resin solution (resin composition). The polyamideimide resin solution thus obtained was allowed to stand at room temperature, and the appearance was visually observed to be homogeneous and transparent. The non-volatile content of this polyamideimide resin solution (200°C / 2 hours) was 29 mass%, and the number average molecular weight of the polyamideimide resin was 28,000.

[0086] Example 3 105 g of trimellitic anhydride, 97 g of 4,4'-diphenylmethane diisocyanate, 44 g of 3,3'-dimethoxybiphenyl-4,4'-diisocyanate, and 459 g of N,N-dimethylacetamide were placed in a flask equipped with a thermometer, a stirrer, and a cooling tube, and the temperature was gradually raised to 100°C over 2 hours while stirring in a dry nitrogen stream. After continuing heating for 2 hours, the temperature was gradually raised to 140°C while paying attention to the sudden foaming of carbon dioxide gas generated by the reaction, and heating was continued for 3 hours from the start of heating. After cooling to stop the reaction, 3 g of propionic acid was added and heated at 80°C for 1 hour while stirring to obtain a polyamideimide resin solution (resin composition). The polyamideimide resin solution thus obtained was allowed to stand at room temperature, and the appearance was visually observed to be homogeneous and transparent. The non-volatile content of this polyamideimide resin solution (200°C / 2 hours) was 32 mass%, and the number average molecular weight of the polyamideimide resin was 27,000.

[0087] Comparative Example 1 105 g of trimellitic anhydride, 97 g of 4,4'-diphenylmethane diisocyanate, 44 g of 3,3'-dimethoxybiphenyl-4,4'-diisocyanate, and 459 g of N,N-dimethylacetamide were placed in a flask equipped with a thermometer, a stirrer, and a cooling tube, and the temperature was gradually raised to 100°C over 2 hours while stirring in a dry nitrogen stream. After continuing heating for 2 hours, the temperature was gradually raised to 140°C while paying attention to the sudden foaming of carbon dioxide gas generated by the reaction, and heating was continued for 3 hours from the start of heating, and the reaction was stopped by cooling to obtain a polyamideimide resin solution (resin composition). The polyamideimide resin solution thus obtained was allowed to stand at room temperature, and the appearance was visually observed to be homogeneous and transparent. The non-volatile content of this polyamideimide resin solution (200°C / 2 hours) was 32 mass%, and the number average molecular weight of the polyamideimide resin was 28,000.

[0088] Comparative Example 2 96.1 g of trimellitic anhydride, 126 g of 4,4'-diphenylmethane diisocyanate, and 519 g of N,N-dimethylacetamide were placed in a flask equipped with a thermometer, a stirrer, and a cooling tube, and the temperature was gradually raised to 90°C over 1 hour while stirring in a dry nitrogen stream. After continuing heating for 3 hours, the temperature was gradually raised to 140°C while paying attention to the sudden foaming of carbon dioxide gas generated by the reaction, and heating was continued for 6 hours from the start of heating. After cooling to stop the reaction, 3 g of water was added and heated to 80°C for 1 hour while stirring, to obtain a polyamideimide resin solution (resin composition). The polyamideimide resin solution thus obtained was allowed to stand at room temperature, and the appearance was visually observed to be homogeneous and transparent. The non-volatile content of this polyamideimide resin solution (200°C / 2 hours) was 29 mass%, and the number average molecular weight of the polyamideimide resin was 32,000.

[0089] (Reference example) 105 g of trimellitic anhydride, 97 g of 4,4'-diphenylmethane diisocyanate, 44 g of 3,3'-dimethoxybiphenyl-4,4'-diisocyanate, and 459 g of NMP were placed in a flask equipped with a thermometer, a stirrer, and a cooling tube, and the temperature was gradually raised to 100°C over 2 hours while stirring in a dry nitrogen stream. After continuing heating for 2 hours, the temperature was gradually raised to 140°C while paying attention to the sudden foaming of carbon dioxide gas generated by the reaction, and heating was continued for 2 hours from the start of heating, and the reaction was stopped by cooling to obtain a polyamideimide resin solution (resin composition). The polyamideimide resin solution thus obtained was allowed to stand at room temperature, and the appearance was visually observed to be homogeneous and transparent. The non-volatile content of this polyamideimide resin solution (200°C / 2 hours) was 32 mass%, and the number average molecular weight of the polyamideimide resin was 32,000.

[0090] <2> Evaluation of polyamide-imide resin compositions (Viscosity change rate (%)) For each of the polyamideimide resin compositions (varnishes) obtained in the above Examples, Comparative Examples, and Reference Examples, the viscosity change rate (%) before and after storage at 60° C. for 30 days was calculated according to the following procedure. First, the viscosity of the polyamideimide resin composition (varnish) was measured before storage. Next, a certain amount of the resin composition (varnish) was placed in a sealed container, and the sealed container was stored in a dryer set at 60°C for 30 days, after which the viscosity was measured. From each measured value, the viscosity change rate was calculated according to the following (Equation 1). The calculated values ​​are shown in Table 1.

[0091] (Formula 1) Viscosity change rate (%)=(V2-V1) / V1×100

[0092] In formula 1, "V1" represents the viscosity measured before storage, and "V2" represents the viscosity measured after storage at 60°C for 30 days. The viscosity measurements were performed in accordance with JIS C 2103 using a B-type rotational viscometer at 25° C. with a No. 3 rotor at a rotation speed of 6 or 12 rpm.

[0093] [Table 1]

[0094] (Evaluation Criteria) A: Viscosity increase or decrease is less than 0 to 5% B: Viscosity increase or decrease is 5% or more but less than 12% C: Viscosity increase or decrease is 12% or more

[0095] As shown in Table 1, the resin compositions of the reference examples show a clear increase in viscosity, whereas the resin composition containing a polyamideimide resin synthesized in DMAC and not treated with a blocking agent (Comparative Example 1) shows a decrease in viscosity. In particular, when water is used as a blocking agent as shown in Comparative Example 2, hydrolysis is accelerated, resulting in a large decrease in viscosity. In contrast, the resin compositions using the blocked polyamideimide resin of the present invention (Examples 1 to 3) show a suppressed decrease in viscosity during storage, and in particular, the resin compositions containing a polyamideimide resin blocked with a monocarboxylic acid (Examples 2 and 3) show a suppressed increase in viscosity. From the above, it is clear that the present invention can provide a polyamideimide resin composition having excellent viscosity stability by suppressing the viscosity decrease due to hydrolysis and also suppressing the viscosity increase.

Claims

1. A polyamide-imide resin having a terminal isocyanate group treated with a blocking agent, the blocking agent including at least one selected from the group consisting of alcohols and monocarboxylic acids.

2. The polyamideimide resin of claim 1 , wherein the blocking agent comprises a monocarboxylic acid.

3. 3. The polyamide-imide resin according to claim 1, wherein the monocarboxylic acid comprises an aliphatic monocarboxylic acid having 2 to 10 carbon atoms or benzoic acid.

4. The polyamideimide resin according to claim 1 or 2, having a number average molecular weight of 5,000 to 100,000.

5. 1. A polyamideimide resin composition obtained using a diisocyanate, an acid component containing a tribasic acid anhydride or a tribasic acid halide, an organic solvent having a structure represented by the following formula (I), and a blocking agent, wherein the blocking agent contains at least one selected from the group consisting of an alcohol and a monocarboxylic acid. 【Chemistry 1】 [In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 3 carbon atoms, or are bonded to each other to form a 5- or 6-membered heterocyclic group containing a nitrogen atom; R 3 is hydrogen or an alkyl group having 1 to 4 carbon atoms.

6. A polyamideimide resin composition comprising: a polyamideimide resin having a terminal isocyanate group treated with a blocking agent, the blocking agent including at least one selected from the group consisting of an alcohol and a monocarboxylic acid; and an organic solvent having a structure represented by the following formula (I): 【Chemistry 2】 [In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 3 carbon atoms, or are bonded to each other to form a 5- or 6-membered heterocyclic group containing a nitrogen atom; R 3 is hydrogen or an alkyl group having 1 to 4 carbon atoms.

7. A coating material comprising the polyamideimide resin composition according to claim 5 or 6.

8. An article having a coating film formed using the coating material according to claim 7.

9. A molded product formed using the polyamideimide resin composition according to claim 5 or 6.

10. A method for producing a polyamideimide resin composition comprising a polyamideimide resin and an organic solvent having a structure represented by the following formula (I): In the organic solvent, an isocyanate component containing a diisocyanate is reacted with an acid component containing a tribasic acid anhydride or a tribasic acid halide to form a liquid containing a polyamide-imide resin having a terminal isocyanate group. The method includes reacting a liquid containing the polyamide-imide resin having a terminal isocyanate group with a blocking agent, The method for producing a polyamideimide resin composition, wherein the blocking agent comprises at least one selected from the group consisting of an alcohol and a monocarboxylic acid. 【Chemistry 3】 [In the formula, R 1 and R 2 are each independently an alkyl group having 1 to 3 carbon atoms, or are bonded to each other to form a 5- or 6-membered heterocyclic group containing a nitrogen atom; R 3 is hydrogen or an alkyl group having 1 to 4 carbon atoms.

Citation Information

Patent Citations

  • Polyamide-imide fibers and nonwoven fabrics made therefrom, and methods for producing the same.

    JP4797863B2