Manufacturing method for nonaqueous secondary battery
The method optimizes non-aqueous secondary battery manufacturing by selectively coating the negative electrode with Li during charging, addressing uneven charge distribution and enhancing battery performance by delaying the positive electrode reaction.
Patent Information
- Application Number
- JP2023082561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for manufacturing non-aqueous secondary batteries face challenges in improving battery performance by optimizing the SEI film formation on the negative electrode while avoiding deterioration of the positive electrode active material due to uneven charge distribution, leading to reduced charge/discharge capacity.
A manufacturing method that involves charging the battery at a predetermined amount, followed by an aging process and Li precipitation step to selectively coat the negative electrode with Li, using side reactants that react before the main positive electrode active material, thereby delaying its reaction and optimizing the negative electrode potential.
This method enhances battery performance by increasing the SEI film on the negative electrode, suppressing the decrease in charge/discharge capacity, and maintaining optimal electrode potentials.
Smart Images

Figure 2024165945000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a non-aqueous secondary battery. [Background technology]
[0002] In the method for producing a nonaqueous secondary battery described in Patent Document 1, a solid electrolyte interface (SEI) film is formed on the surface of the negative electrode during the first charge. In nonaqueous secondary batteries, the capacity retention rate and Li deposition resistance change depending on the amount of the SEI film on the negative electrode surface. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2022-139577 A Summary of the Invention [Problem to be solved by the invention]
[0004] Therefore, it is conceivable that the amount of SEI coating can be increased by lowering the negative electrode potential during aging, thereby improving battery performance. On the other hand, if the charge amount of the battery cell is increased to lower the negative electrode potential during aging, the charge amount of the positive electrode also increases at the same time, causing deterioration of the positive electrode active material and reducing the charge / discharge capacity of the battery cell after aging, so it is necessary to increase only the charge amount of the negative electrode during aging. However, if only the charge amount of the negative electrode is increased during aging, the charge amount of the negative electrode remains high even after aging, so the negative electrode potential is low and the charge / discharge capacity of the battery cell is reduced. Therefore, there is a demand for improving battery performance while suppressing the decrease in charge / discharge capacity. [Means for solving the problem]
[0005] A method for manufacturing a nonaqueous secondary battery that solves the above-mentioned problems is a method for manufacturing a nonaqueous secondary battery comprising an electrode assembly in which a positive electrode sheet and a negative electrode sheet are laminated with a separator interposed therebetween, and a nonaqueous electrolyte solution containing a lithium salt, wherein the positive electrode composite constituting the positive electrode sheet contains a by-reactant that reacts before a main positive electrode active material during charging, and the method includes a charging step of charging with a predetermined charge amount, an aging step of leaving the battery at a predetermined temperature after the charging step, and a Li deposition step of depositing Li on the negative electrode sheet in an amount equivalent to the reaction amount of the by-reactant contained in the positive electrode composite by charging after the aging step.
[0006] According to the above method, since the positive electrode mixture contains a by-reactant, the by-reactant reacts first in the charging step and the aging step, and the reaction of the main positive electrode active material is delayed, so that only the negative electrode sheet can be charged first. This increases the amount of coating formed on the negative electrode sheet during aging, improving the battery performance. In addition, in the Li deposition step, Li is deposited on the negative electrode in an amount equivalent to the reaction amount of the by-reactant in the positive electrode sheet, so that the reaction of the negative electrode active material is delayed, thereby suppressing the decrease in the negative electrode potential and suppressing the decrease in the charge / discharge capacity. Therefore, the battery performance can be improved and the decrease in the charge / discharge capacity can be suppressed.
[0007] In the above-described method for producing a nonaqueous secondary battery, it is preferable that the amount of the by-reactant added is set so that the reaction amount of the by-reactant is the difference between a minimum charge amount, which is a charge amount at which the reaction resistance in the negative electrode sheet can be sufficiently reduced, and a maximum charge amount at which capacity degradation does not occur in the positive electrode sheet.
[0008] In the method for producing a nonaqueous secondary battery, the by-reactant is preferably a substance having a lower oxidation-reduction potential than the main positive electrode active material, or a substance having the same oxidation-reduction potential and an irreversible reaction.
[0009] In the method for producing a nonaqueous secondary battery, it is preferable that the predetermined charge amount is the minimum charge amount. Effect of the Invention
[0010] According to the present invention, it is possible to improve the battery performance and suppress the decrease in the charge / discharge capacity. [Brief description of the drawings]
[0011] [Figure 1] 1 is a perspective view showing a schematic configuration of a cell battery of an embodiment of a nonaqueous secondary battery. [Diagram 2] FIG. 4 is a view showing a part of the electrode body of the embodiment in an expanded form. [Diagram 3] 4 is a flowchart showing a process for determining a charge amount of the nonaqueous secondary battery according to the embodiment. [Figure 4] 4 is a graph showing the relationship between the negative electrode charging rate and reaction resistance of the nonaqueous secondary battery according to the embodiment. [Diagram 5] 4 is a graph showing the relationship between the charge amount and potential of the positive electrode and the negative electrode of the nonaqueous secondary battery of the embodiment. [Figure 6] 4 is a flowchart showing aging and Li deposition treatment of the nonaqueous secondary battery of the embodiment. [Figure 7] 4 is a graph showing the relationship between the charge amount and potential of the positive electrode and the negative electrode of the nonaqueous secondary battery of the embodiment. [Figure 8] 4 is a graph showing the relationship between the charge amount and potential of the positive electrode and the negative electrode of the nonaqueous secondary battery of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Present embodiment] An embodiment of a nonaqueous secondary battery and a method for manufacturing a nonaqueous secondary battery will be described below with reference to Figures 1 to 8. As an example of the nonaqueous secondary battery, a lithium ion secondary battery will be described.
[0013] [Lithium-ion secondary battery 10] 1, a lithium-ion secondary battery 10 is a cell battery that is combined with a plurality of lithium-ion secondary batteries 10 and sealed in a resin or metal case to form a battery pack. The battery pack is used in hybrid vehicles and electric vehicles.
[0014] The lithium ion secondary battery 10 includes a battery case 11 and a lid 12. The battery case 11 has a rectangular parallelepiped shape with an opening on the upper side. The lid 12 seals the opening of the battery case 11. The battery case 11 and the lid 12 are made of a metal such as aluminum or an aluminum alloy. The lithium ion secondary battery 10 is configured as a sealed battery container by attaching the lid 12 to the battery case 11.
[0015] The lid 12 is provided with two positive external terminals 13A and a negative external terminal 13B. The positive external terminal 13A and the negative external terminal 13B are used for charging and discharging power. The electrode body 20 is accommodated inside the battery case 11. An external film (not shown) is inserted between the battery case 11 and the electrode body 20. The positive electrode side current collector 20A, which is the end of the electrode body 20 on the positive electrode side, is electrically connected to the positive electrode external terminal 13A via the positive electrode side current collector 14A. The negative electrode side current collector 20B, which is the end of the electrode body 20 on the negative electrode side, is electrically connected to the negative electrode external terminal 13B via the negative electrode side current collector 14B. In addition, a nonaqueous electrolyte is injected into the battery case 11 through a liquid injection hole (not shown). The shapes of the positive electrode external terminal 13A and the negative electrode external terminal 13B are not limited to those shown in FIG. 1 and may be any shape.
[0016] [Electrode body 20] 2, the electrode body 20 is a flat wound body obtained by winding a laminate in which a long positive electrode sheet 21 and a negative electrode sheet 24 are stacked with a separator 27 interposed therebetween. The positive electrode sheet 21, the negative electrode sheet 24, and the separator 27 are stacked such that their respective longitudinal directions coincide with the longitudinal direction D1. In the laminate before winding, the positive electrode sheet 21, the separator 27, the negative electrode sheet 24, and the separator 27 are stacked in this order.
[0017] [Positive electrode sheet 21] The positive electrode sheet 21 includes a positive electrode current collector 22 and a positive electrode composite layer 23. The positive electrode current collector 22 is a foil-like positive electrode base material formed in an elongated shape. The positive electrode composite layer 23 is provided on each of two opposing surfaces of the positive electrode current collector 22. The positive electrode current collector 22 includes a positive electrode-side uncoated portion 22A at one end in the width direction D2 where the positive electrode composite layer 23 is not formed and the positive electrode current collector 22 is exposed.
[0018] A metal foil made of aluminum or an alloy mainly composed of aluminum is used for the positive electrode current collector 22. The positive electrode current collector 22 functions as a current collector for the positive electrode. In the wound state, the positive electrode side uncoated portion 22A of the positive electrode current collector 22 is pressed against each other at opposing surfaces to form the positive electrode side current collector 20A.
[0019] The positive electrode mixture layer 23 is a hardened body of a liquid positive electrode mixture paste. The positive electrode mixture paste includes a positive electrode active material, a positive electrode solvent, a positive electrode conductive material, and a positive electrode binder. The positive electrode mixture layer 23 is formed by drying the positive electrode mixture paste and evaporating the positive electrode solvent. Therefore, the positive electrode mixture layer 23 includes a positive electrode active material, a positive electrode conductive material, and a positive electrode binder.
[0020] The positive electrode active material is a lithium-containing composite oxide capable of absorbing and releasing lithium ions, which are charge carriers in the lithium-ion secondary battery 10. The lithium-containing composite oxide is an oxide containing lithium and a metal element other than lithium. The metal element other than lithium is at least one selected from the group consisting of nickel, cobalt, manganese, vanadium, magnesium, molybdenum, niobium, titanium, tungsten, aluminum, and iron contained in the lithium-containing composite oxide as iron phosphate.
[0021] The main positive electrode active material in this embodiment is a ternary lithium-containing composite oxide (NCM) containing nickel, cobalt, and manganese, for example, lithium nickel cobalt manganese oxide (LiNiCoMnO2). A side reactant different from the main positive electrode active material is lithium iron phosphate (LiFePO4) (LFP). The side reactant is a positive electrode active material that reacts during charging before the main positive electrode active material. That is, the side reactant is a material that has a lower redox potential than the main positive electrode active material, or a material that has the same redox potential and the reaction is irreversible. For example, NCM is 3.7V and LFP is 3.4V.
[0022] The positive electrode solvent is an NMP (N-methyl-2-pyrrolidone) solution, which is an example of an organic solvent. The positive electrode conductive material is, for example, carbon black such as acetylene black or ketjen black, carbon fiber such as carbon nanotube or carbon nanofiber, or graphite. The positive electrode binder is an example of a resin component contained in the positive electrode mixture paste. The positive electrode binder is, for example, polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), styrene butadiene rubber (SBR), or the like.
[0023] The positive electrode sheet 21 may have an insulating layer at the boundary between the positive electrode uncoated portion 22A and the positive electrode mixture layer 23. The insulating layer contains an inorganic component having insulating properties and a resin component that functions as a binder. The inorganic component is at least one selected from the group consisting of powdered boehmite, titania, and alumina. The resin component is at least one selected from the group consisting of PVDF, PVA, and acrylic.
[0024] [Negative electrode sheet 24] The negative electrode sheet 24 includes a negative electrode current collector 25 and a negative electrode composite layer 26. The negative electrode current collector 25 is a foil-like negative electrode base material formed in an elongated shape. The negative electrode composite layer 26 is provided on each of two opposing surfaces of the negative electrode current collector 25. The negative electrode current collector 25 includes a negative electrode-side uncoated portion 25A at one end in the width direction D2, which is located opposite the positive electrode-side uncoated portion 22A, where the negative electrode composite layer 26 is not formed and the negative electrode current collector 25 is exposed.
[0025] A metal foil made of copper or an alloy mainly composed of copper is used for the negative electrode current collector 25. The negative electrode current collector 25 functions as a current collector for the negative electrode. In the wound body state, the negative electrode uncoated portion 25A has opposing surfaces pressed against each other to form the negative electrode current collector 20B.
[0026] The negative electrode mixture layer 26 is a hardened body of the liquid negative electrode mixture paste. The negative electrode mixture paste includes a negative electrode active material, a negative electrode solvent, a negative electrode thickener, and a negative electrode binder. The negative electrode mixture layer 26 is formed by drying the negative electrode mixture paste and evaporating the negative electrode solvent. Therefore, the negative electrode mixture layer 26 includes the negative electrode active material, and further includes a negative electrode thickener and a negative electrode binder as additives. The negative electrode mixture layer 26 may further include an additive such as a conductive material.
[0027] The negative electrode active material is a material capable of absorbing and releasing lithium ions. For example, carbon materials such as graphite, non-graphitizable carbon, graphitizable carbon, and carbon nanotubes are used as the negative electrode active material. An example of the negative electrode solvent is water. For example, CMC (carboxymethyl cellulose) can be used as the negative electrode thickener, which is a thickener containing a sodium salt. For example, the negative electrode binder can be the same as the positive electrode binder. For example, SAR (styrene acrylic acid copolymer) can be used as the negative electrode binder, which is a binder containing a sodium salt.
[0028] [Separator 27] The separator 27 prevents contact between the positive electrode sheet 21 and the negative electrode sheet 24, and retains a nonaqueous electrolyte between the positive electrode sheet 21 and the negative electrode sheet 24. When the electrode body 20 is immersed in the nonaqueous electrolyte, the nonaqueous electrolyte permeates from the ends of the separator 27 in the width direction D2 toward the center.
[0029] The separator 27 is a nonwoven fabric made of polypropylene, etc. As the separator 27, for example, a porous polymer membrane such as a porous polyethylene membrane, a porous polyolefin membrane, a porous polyvinyl chloride membrane, an ion-conductive polymer electrolyte membrane, etc. can be used.
[0030] [Nonaqueous electrolyte] The non-aqueous electrolyte is a composition in which a supporting salt is contained in a non-aqueous solvent. As the non-aqueous solvent, one or more materials selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, etc. can be used. In addition, as the supporting salt, one or more lithium compounds (lithium salts) selected from LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, LiBOB (lithium bis(oxalate)borate), etc. can be used.
[0031] In this embodiment, ethylene carbonate is used as the non-aqueous solvent. LiBOB is added to the non-aqueous electrolyte as a lithium salt of the film forming agent. For example, LiBOB is added to the non-aqueous electrolyte so that the concentration of LiBOB in the non-aqueous electrolyte is 0.001 to 0.1 [mol / L].
[0032] [Manufacturing method] Next, a method for manufacturing the lithium ion secondary battery 10 will be described with reference to FIGS.
[0033] The manufacturing method of the lithium ion secondary battery 10 includes a charging step, an aging step, and a Li deposition step. In the charging step, the lithium ion secondary battery 10 is charged with a predetermined charge amount. In the aging step, the lithium ion secondary battery 10 is left at a predetermined temperature after the charging step. In the Li deposition step, the lithium ion secondary battery 10 is charged after the aging step, thereby depositing Li on the negative electrode sheet 24 in an amount equivalent to the reaction amount of the by-reactant.
[0034] First, before charging, the charge amount determination process shown in FIG. 3 is performed. First, the minimum charging rate of the negative electrode during aging is determined (step S1). That is, the minimum charging rate of the negative electrode during aging that can satisfy the requirements is determined based on the relationship between the charging rate of the negative electrode and the battery performance, and the required performance of the battery cell. As shown in Fig. 4, the minimum charging rate can be determined based on the required performance that can sufficiently reduce the reaction resistance in the negative electrode sheet 24.
[0035] Next, the charge amount of the negative electrode during aging is determined (step S2). That is, the minimum charge amount is determined, which is the charge amount of the negative electrode to achieve the minimum charge rate of the negative electrode determined in step S1 from the amount of negative electrode active material in the battery cell. As shown in Figure 5, the potential of the negative electrode charge curve decreases as the charge amount increases, so the minimum charge amount of the negative electrode can be determined from the required potential of this charge curve.
[0036] Next, the maximum charging rate of the positive electrode during aging is determined (step S3). That is, the maximum charging rate of the positive electrode during aging that can satisfy the requirements is determined based on the relationship between the charging rate of the positive electrode and capacity deterioration, and the required performance of the battery cell.
[0037] Next, the charge amount of the positive electrode during aging is determined (step S4). That is, the maximum charge amount is determined, which is the charge amount of the positive electrode to achieve the maximum charge rate of the positive electrode determined in step S3 from the amount of the positive electrode active material of the battery cell. As shown in Fig. 5, the charge curve of the positive electrode when no by-reactant is added to the positive electrode composite increases in potential as the charge amount increases, so the maximum charge amount of the positive electrode can be determined from the calculated potential of this charge curve.
[0038] Next, as shown in FIG. 6, aging and Li precipitation treatment are performed. First, the amount of the by-reactant to be added to the positive electrode plate is determined (step S5). That is, the amount of the by-reactant to be added is set so that the reaction amount of the by-reactant is the difference D between the minimum charge amount of the negative electrode and the maximum charge amount of the positive electrode (see FIG. 5).
[0039] Next, the lithium ion secondary battery 10 is charged with the minimum charge amount of the negative electrode determined in step S2 (step S6). That is, the active material contained in the positive electrode mixture layer 23 is reacted by charging. The predetermined charge amount in the charging step is the minimum charge amount of the negative electrode. Step S6 corresponds to the charging step.
[0040] Next, aging is performed by leaving the lithium ion secondary battery 10 at a predetermined temperature (step S7). That is, the active material contained in the positive electrode composite layer 23 reacts even during aging. If a by-reactant is contained in the positive electrode composite, as shown in FIG. 7, the by-reactant reacts before the main positive electrode active material in the charging step and the aging step, and the reaction of the main positive electrode active material is delayed, so that only the negative electrode can be charged first. By adjusting the amount of the by-reactant added, the reaction of the main positive electrode active material starts after charging the charge amount corresponding to the difference D. Step S7 corresponds to the aging step.
[0041] Then, charging is performed to deposit Li on the negative electrode (step S8). That is, charging is performed under various conditions such as temperature, charging rate, current value, and time so that the charge amount due to Li deposition on the negative electrode becomes the difference D, and Li is deposited. By charging, an amount of Li equivalent to the reaction amount of the side reactant is deposited on the negative electrode sheet 24. The number of charging cycles is determined by performing a test in a state where no side reactant is added to the positive electrode. Since the change in cell capacity corresponds to the amount of Li deposition, the number of charging cycles is determined so that the charge amount becomes the difference D. As shown in FIG. 8, in order to deposit Li in an amount equivalent to the reaction amount of the side reactant on the negative electrode, the reaction of the negative electrode active material is delayed, thereby suppressing the decrease in the negative electrode potential and suppressing the decrease in the charge / discharge capacity. Step S8 corresponds to a Li deposition process.
[0042] Next, the effects of this embodiment will be described. (1) Since the positive electrode mixture contains a by-reactant, the by-reactant reacts first in the charging step and the aging step, delaying the reaction of the main positive electrode active material, and thus only the negative electrode sheet 24 can be charged first. This increases the amount of coating formed on the negative electrode sheet 24 during aging, improving the battery performance. In addition, in the Li deposition step, Li is deposited on the negative electrode in an amount equivalent to the reaction amount of the by-reactant in the positive electrode sheet 21, and thus the reaction of the negative electrode active material is delayed, thereby suppressing the decrease in the negative electrode potential and suppressing the decrease in the charge / discharge capacity. This improves the battery performance and suppresses the decrease in the charge / discharge capacity.
[0043] (2) The reaction amount of the by-reactant is set to be the difference D between the minimum charge amount of the negative electrode sheet 24 and the maximum charge amount of the positive electrode sheet 21. This allows only the by-reactant to react during charging to an amount of charge corresponding to the difference D between the minimum charge amount of the negative electrode sheet 24 and the maximum charge amount of the positive electrode sheet 21.
[0044] (3) The by-reactant has a lower redox potential than the main positive electrode active material, or has an equivalent redox potential and is an irreversible reaction, so that the by-reactant can react before the main positive electrode active material.
[0045] (4) The predetermined charge amount in the charging step is the minimum charge amount in the negative electrode sheet 24. Therefore, only the by-products can be reacted in the charging step, and the reaction of the main positive electrode active material can be delayed.
[0046] (Other embodiments) The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined with each other to the extent that no technical contradiction occurs.
[0047] In the above embodiment, the main positive electrode active material is NCM and the by-reactant is LFP. However, the combination is not limited to these, and other combinations may be used as long as the by-reactant has a lower redox potential than the main positive electrode active material, or has the same redox potential and the reaction is irreversible.
[0048] In the above embodiment, the predetermined charge amount in the charging process is the minimum charge amount. However, the predetermined charge amount in the charging process may be any charge amount other than the minimum charge amount.
[0049] In the above embodiment, the amount of the side reactant added was set so that the reaction amount of the side reactant was equal to the difference D between the minimum charge amount and the maximum charge amount. However, the amount of the side reactant added may be set arbitrarily as long as the reaction of the main positive electrode active material can be delayed by adding the side reactant.
[0050] In the above embodiment, the electrode body 20 is a wound body obtained by winding a laminate in which the positive electrode sheet 21 and the negative electrode sheet 24 are laminated with the separator 27 interposed therebetween. However, the electrode body may be a laminate in which a plurality of positive electrode sheets 21 and a plurality of negative electrode sheets 24 are alternately stacked with the separator 27 interposed therebetween.
[0051] The lithium ion secondary battery 10 may be mounted on an automatic transport vehicle, a special vehicle for loading and unloading, an electric vehicle, a hybrid vehicle, a computer, or other electronic device, or may be part of other systems. For example, it may be mounted on a moving object such as a ship or an aircraft, or may be a power supply system that supplies power from a power plant via a substation to a building or home in which a secondary battery is installed. [Explanation of symbols]
[0052] 10...Lithium-ion secondary battery 11…Battery case 12…Lid body 13A…Positive external terminal 13B…Negative external terminal 14A…Positive electrode side current collecting member 14B: Negative electrode side current collecting member 20...Electrode body 20A…Positive electrode current collector 20B: Negative electrode current collector 21...Positive electrode sheet 22...Positive electrode current collector 22A: Uncoated area on positive electrode side 23...Positive electrode mixture layer 24...Negative electrode sheet 25...Negative electrode current collector 25A…Negative electrode uncoated area 26…Negative electrode composite material layer 27…Separator
Claims
1. A method for producing a non-aqueous secondary battery including an electrode assembly in which a positive electrode sheet and a negative electrode sheet are laminated with a separator interposed therebetween, and a non-aqueous electrolyte solution containing a lithium salt, comprising: The positive electrode mixture constituting the positive electrode sheet contains a by-reactant that reacts prior to the main positive electrode active material during charging, a charging step of charging the battery with a predetermined charge amount; an aging step of leaving the battery at a predetermined temperature after the charging step; and a Li deposition process in which charging is performed after the aging process to deposit Li on the negative electrode sheet in an amount corresponding to the reaction amount of a by-reactant contained in the positive electrode mixture. A method for manufacturing a non-aqueous secondary battery.
2. The amount of the by-reactant added is set so that the reaction amount of the by-reactant is the difference between the minimum charge amount, which is the charge amount that can sufficiently reduce the reaction resistance in the negative electrode sheet, and the maximum charge amount at which capacity degradation does not occur in the positive electrode sheet. The method for producing the nonaqueous secondary battery according to claim 1 .
3. The by-reactant is a substance having a lower redox potential than the main positive electrode active material, or a substance having the same redox potential and an irreversible reaction. The method for producing the nonaqueous secondary battery according to claim 1 or 2.
4. The predetermined charge amount is the minimum charge amount. The method for producing the nonaqueous secondary battery according to claim 2 .
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery, battery cell formed by connecting two or more of them, and method of manufacturing the same
JP2016207611A
Manufacturing method of non-aqueous electrolyte secondary battery
JP2022139577A