Etched product and method for manufacturing the same

By employing a controlled etching process with specific through-hole configurations, the method addresses the challenge of isotropic side etching in photo-etching, enabling the production of etched products with high aspect ratios and high-definition patterns.

JP2024166712AInactive Publication Date: 2024-11-29TOPPAN HOLDINGS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023083011
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional photo-etching methods face challenges in creating through-holes with high aspect ratios due to isotropic side etching, making it difficult to achieve high-definition patterns and narrow pitches in etched products.

Method used

The method involves forming a metal plate with specific through-hole configurations, including a first through-hole with a rectangular opening and surrounding second through-holes with linear openings, utilizing a controlled etching process to suppress side etching and enhance the etching factor, thereby improving the aspect ratio and definition of the patterns.

Benefits of technology

This approach allows for the easy manufacturing of etched products with high aspect ratios and high-definition patterns by effectively managing side etching, resulting in improved processing accuracy and etching efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166712000001_ABST
    Figure 2024166712000001_ABST
Patent Text Reader

Abstract

To provide a technique for simply manufacturing an etched product having a high definition pattern at a high aspect ratio.SOLUTION: An etched product is composed of a metal plate which has a first surface and a second surface as its rear face and one or more through hole groups. Each of the one or more through hole groups includes: a first through hole having a rectangular opening with a length of each side equal to or more than the thickness of the metal plate on the first surface; and a plurality of second through holes which each has a linear opening having a width less than the thickness of the metal plate on the first surface and include a plurality of second through holes arranged around the first through hole.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an etching processed product and a method for producing the same. [Background technology]

[0002] As electronic components are mounted at higher densities, the pitch of etching-processed products, which require highly precise patterns, is rapidly becoming finer, and in recent years, this pitch is approaching the limit of processing pitch for etching. Many of these components are manufactured using the photoetching method. In the photoetching method, a corrosion-resistant photoresist film is formed into the desired pattern on the surface of copper- or iron-based metal materials, and the metal parts exposed from the pattern are corroded and processed using an etching solution.

[0003] In wet etching using such an etching solution, etching proceeds isotropically from the opening of the photoresist to just below the photoresist, so side etching becomes a problem. Side etching refers to isotropic etching that penetrates below the photoresist film surface, and if the amount of side etching is large, a problem occurs in that the pitch between adjacent patterns cannot be narrowed to make the etched part of the metal material have a high aspect ratio. For this reason, when manufacturing metal etched products using conventional photoetching technology, it is difficult to form through holes with a high aspect ratio whose opening width is narrower than the thickness of the metal material, making it very difficult to respond to the above-mentioned fine pitch.

[0004] To solve this problem, a metal etched product has been developed in which a through hole formed in a metal layer by photoetching has a side wall formed by primary etching on the surface side of the metal layer, and a side wall formed by secondary etching using electrodeposited photoresist on the deeper side (see, for example, Patent Documents 1 and 2). However, since the current process cannot be used to manufacture this etched product, equipment modification and process optimization are required. In addition, this method involves two-stage etching, making the process complicated. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-204251 A [Patent Document 2] JP 2004-218033 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a technique for easily manufacturing an etched product having a high aspect ratio and a high definition pattern. [Means for solving the problem]

[0007] According to one aspect of the present invention, there is provided an etched product consisting of a metal plate having a first surface and a second surface which is the reverse surface of the first surface, and having one or more groups of through holes, each of the one or more groups of through holes including a first through hole having a rectangular opening on the first surface, the length of each side being greater than or equal to the thickness of the metal plate, and a plurality of second through holes arranged around the first through hole, each having a linear opening on the first surface, the width of which is less than the thickness of the metal plate.

[0008] According to another aspect of the present invention, there is provided an etched product relating to the above aspect, wherein the opening of each of the plurality of second through holes has a width in the range of 20 to 150 μm, and the ratio S1 / S2 of the area S1 of the opening of the first through hole to the area S2 of the opening of each of the plurality of second through holes is 10 or greater.

[0009] According to yet another aspect of the present invention, there is provided an etched product relating to any of the above aspects, wherein the ratio L1 / W2 of the length L1 of each side of the opening of the first through hole to the width W2 of the opening of each of the plurality of second through holes is within the range of 10 to 900.

[0010] According to yet another aspect of the present invention, there is provided an etched product relating to any of the above aspects, wherein in each of the one or more groups of through holes, the opening of each of the plurality of second through holes is located 3.5 mm or less away from the opening of the first through hole.

[0011] According to yet another aspect of the present invention, there is provided an etched product relating to any of the above aspects, wherein the metal plate further has a plurality of third through holes arranged to surround each of the one or more through hole groups, and the ratio L1 / L3 of the length L1 of each side of the opening of the first through hole to the dimension L3 on the first surface of each area surrounded by the array of the plurality of third through holes is 0.5 or less.

[0012] According to yet another aspect of the present invention, there is provided an etched product as described in claim 5, wherein the ratio W3 / W2 of the opening width W3 of the plurality of third through holes on the first surface to the opening width W2 of each of the plurality of second through holes is within the range of 5 to 50.

[0013] According to yet another aspect of the present invention, there is provided an etched product relating to the above aspect, wherein in each of the one or more groups of through holes, the opening of each of the plurality of second through holes has at least one of a distance to the opening of the first through hole and a shortest distance to the opening of the plurality of third through holes that is 2.0 mm or less.

[0014] According to yet another aspect of the present invention, there is provided an etched product according to any of the above aspects, wherein the one or more groups of through holes are two or more groups of through holes.

[0015] According to yet another aspect of the present invention, a method for etching a metal plate includes preparing a metal plate having a first surface and a second surface opposite to the first surface, forming an etching mask on the first surface, and spraying an etching liquid onto the first surface on which the etching mask is provided, thereby etching the metal plate, The etching mask has one or more opening patterns, each of which includes a first opening having a rectangular opening whose sides are equal to or longer than the thickness of the metal plate, and a plurality of second openings, each of which has a linear opening whose width is less than the thickness of the metal plate, and which are arranged around the first opening. A method for manufacturing an etched product is provided in which, in the etching, a difference is made in the etching rate to form a first through hole in the metal plate at the position of the first opening, and then a plurality of second through holes are formed in the metal plate at the positions of the second openings.

[0016] According to yet another aspect of the present invention, there is provided a method for producing an etched product according to the above aspect, wherein forming the etching mask includes providing a photosensitive resin layer on the first surface, exposing the photosensitive resin layer to a pattern, and developing the photosensitive resin layer after the pattern exposure.

[0017] According to yet another aspect of the present invention, there is provided a reticle for use in the pattern exposure in the method for producing an etched product according to the above aspect. Effect of the Invention

[0018] According to the present invention, it is possible to provide a technique for easily manufacturing an etched product having a high aspect ratio and a high definition pattern. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a top view showing a part of an etched product according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a partially enlarged top view of the etched product shown in FIG. [Diagram 3] FIG. 3 is a top view of an etched product obtained by dividing the etched product shown in FIG. [Figure 4] FIG. 4 is a cross-sectional view showing a step of a method for producing an etched product according to the second embodiment of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view for explaining the problems with conventional spray etching. [Figure 6] FIG. 6 is a top view of the etched product of Comparative Example 1. [Figure 7] FIG. 7 is a graph showing the relationship between the opening width of the etching mask and the etching rate in spray etching. [Figure 8] FIG. 8 is a graph showing the effect of the presence or absence of the first through hole on the etching factor (EF). [Figure 9] FIG. 9 is a graph showing the relationship between the width of the second through hole and the etching factor (EF). [Figure 10] FIG. 10 is a cross-sectional view for explaining the side etching phenomenon and the etching factor in the photoetching method. [Figure 11] FIG. 11 is a cross-sectional view for explaining the side etching phenomenon in the photoetching method. [Figure 12] FIG. 12 is a cross-sectional view for explaining the side etching phenomenon in the photoetching method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.

[0021] The embodiments described below are merely examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited by the materials, shapes, structures, etc. of the components described below. Various modifications can be made to the technical idea of ​​the present invention within the technical scope defined by the claims.

[0022] In addition, elements having the same or similar functions are given the same reference numerals in the drawings referred to below, and duplicated explanations are omitted. In addition, the drawings are schematic, and the relationship between dimensions in one direction and dimensions in another direction, the relationship between the dimensions of one member and the dimensions of another member, etc. may differ from the actual ones.

[0023] FIG. 1 is a top view showing a part of an etched product according to a first embodiment of the present invention. FIG. 2 is a top view showing a part of the etched product shown in FIG. 1 in an enlarged manner. FIG. 3 is a top view showing an etched product obtained by dividing the etched product shown in FIG. 1. Here, the term "etched product" may refer to a state before division shown in FIG. 1 used in the manufacturing process, or may refer to a state after cutting and division shown in FIG. 3, and these are used without distinction unless otherwise necessary. The etched product according to the embodiment of the present invention can be used for applications requiring high-definition patterns, such as lead frames.

[0024] The etching product 1 shown in FIG. 1 is made of a metal plate 10 having a first surface and a second surface, which is the reverse surface of the first surface, and having two or more through hole groups provided thereon, and is in a state before being singulated as described above. Each of the through hole groups is surrounded by an array of a plurality of third through holes 13 as shown in FIG. 1 and FIG. 2. The third through holes 13 are composed of third through holes 13a, 13b, and 13c having different shapes. The etching product 1 shown in FIG. 3 is obtained by cutting each area surrounded by the array of the plurality of third through holes 13 along the array of the plurality of third through holes 13 and singulating it. The symbol F in FIG. 3 indicates the outer frame of the area surrounded by the array of the plurality of third through holes 13.

[0025] Each of the through-hole groups provided in the etched product 1 includes a first through-hole 11 having a rectangular opening on a first surface of the metal plate 10, and second through-holes 12 arranged around the first through-hole 11 and each having a linear opening on the first surface. Hereinafter, the first through-holes 11 may be referred to as a "rectangular pattern" and the second through-holes 12 may be referred to as a "linear pattern."

[0026] The first through hole 11, the second through hole 12, and the third through hole 13 provided in the etching processed product 1 are through holes patterned and formed in the metal plate 10 by a photoetching method. When manufacturing a metal etching product using the photoetching method, the metal part exposed from the resist pattern formed on the surface of the metal material is corroded and processed with an etching solution. The side etching phenomenon, which is a problem of the conventional technology in this case, will be described with reference to Figures 10 to 12.

[0027] 10 to 12 are cross-sectional views for explaining the side etching phenomenon and etching factors in the photoetching method, showing three steps in chronological order. In double-sided etching using the photoetching method, a photosensitive resin layer (resist layer) 14 formed on both sides of a metal plate 10 shown in FIG. 10 is patterned into a desired pattern shape by exposure through a photomask and development, to obtain a resist pattern 14b shown in FIG. 11. Next, an etching solution is brought into contact with the metal part exposed from the resist pattern 14b to corrode it, thereby forming an etching hole 12b shown in FIG. 12.

[0028] In wet etching using such an etching solution, as described above, the etching proceeds isotropically in the depth direction and horizontal direction of the metal material, which causes the problem of side etching, in which etching penetrates below the photoresist film surface. Due to the side etching phenomenon, the opening width of the etching hole 12 becomes larger than the opening width of the resist pattern 14b, as shown in FIG.

[0029] Spray etching is known as an anisotropic wet etching method that prioritizes etching in the depth direction over the horizontal direction of the workpiece to be etched. In spray etching, the etching solution is sprayed from a nozzle, and droplets of the etching solution are sprayed onto the surface of the material. The effect of this liquid pressure in the depth direction preferentially displaces the etching solution that has accumulated at the bottom of the etching hole, thereby improving the etching rate in the depth direction. In general, when performing through-machining of metal materials using the photoetching method, spray etching, which has anisotropic etching, is said to be able to form high-definition patterns because it has a high etching factor (EF) and excellent processing accuracy.

[0030] Here, the etching factor (EF) is expressed as d / S, where d is the etching depth and S is the amount of side etching, as shown in Fig. 12. If the etching depth d is the same, the etching factor (EF) increases when the amount of side etching S is small, and decreases when the amount of side etching S is large. The larger the etching factor (EF) is, the more side etching is suppressed, indicating a pattern with excellent processing accuracy.

[0031] However, it is difficult to improve the etching factor to a desired level even by spray etching, which has anisotropy in etching, and it is difficult to manufacture etched products having high-definition patterns with high aspect ratios.

[0032] To address this problem, the etched product 1 according to this embodiment has the first through holes 11, which are a specific rectangular pattern, provided near the second through holes 12, which are a highly precise linear pattern, thereby effectively suppressing side etching during spray etching, and has a high etching factor (EF) and excellent processing accuracy. Therefore, the linear pattern of the second through holes 12 is a highly precise pattern with a high aspect ratio. The etched product 1 according to this embodiment will be described in detail below.

[0033] The material of the metal plate 10 constituting the etching processed product 1 may be any metal that can be etched, such as copper, iron, or alloys thereof. The thickness of the metal plate 10 is not particularly limited and is appropriately set depending on the application. In one example, the thickness of the metal plate 10 is preferably within a range of 50 to 300 μm, and more preferably within a range of 100 to 200 μm.

[0034] As described above, each of the through-hole groups provided in the etched product 1 includes the first through-hole 11 having a rectangular opening on the first surface of the metal plate 10. The term "rectangular" means a rectangular shape including a rectangle and a square, and may be either a rectangle or a square. The term "rectangular" may include a curved surface portion that may be unavoidably generated at the corner in the process of forming the first through-hole 11. The rectangular opening of the first through-hole 11 has side lengths Lx1 and Ly1 shown in FIG. 2 and FIG. 3 that are equal to or greater than the thickness of the metal plate 10. The side lengths Lx1 and Ly1 are different from each other when the rectangular opening is a rectangle, and are the same when the rectangular opening is a square. In the following, the length of each side of the rectangular opening of the first through-hole 11 may be expressed as L1 without distinction between Lx1 and Ly1.

[0035] As described above, each of the through hole groups includes the multiple second through holes 12 arranged around the first through hole 11. The multiple second through holes 12 each have a linear opening on the first surface of the metal plate 10. The linear opening of the second through hole 12 has a width W2 of the linear pattern shown in Figures 2 and 3 that is less than the thickness of the metal plate 10.

[0036] Thus, the length L1 of each side of the rectangular opening of the first through hole 11 is equal to or greater than the thickness of the metal plate 10, and the width W2 of the linear opening of the second through hole 12 is less than the thickness of the metal plate 10, so that there is a relationship of L1>W2. In the method for producing the etched product 1, spray etching is performed using an etching mask (resist pattern) having openings at positions corresponding to the first through hole 11 and the second through hole 12 that satisfy these requirements, so that side etching is effectively suppressed and the etching factor (EF) is improved. As a result, the etched product 1 having a high aspect ratio and a highly precise linear pattern (second through hole 12) is obtained. The mechanism by which the etching factor (EF) is improved in this way will be described in the method for producing an etched product according to the second embodiment described later.

[0037] In the etched product 1, the dimensions and arrangement of the first through holes 11 and the second through holes 12 are preferably as follows, from the viewpoint of improving the etching factor (EF).

[0038] That is, in the etched product 1, the opening of each of the multiple second through holes 12 has a width W2 that is preferably in the range of 20 to 150 μm, more preferably in the range of 20 to 100 μm, and even more preferably in the range of 20 to 40 μm.

[0039] The ratio S1 / S2 of the opening area S1 of the first through hole 11 to the opening area S2 of each of the multiple second through holes 12 is preferably 10 or more, more preferably in the range of 10 or more and 200 or less, and even more preferably in the range of 10 or more and 40 or less.

[0040] The ratio L1 / W2 of the length L1 of each side of the opening of the first through hole 11 to the width W2 of each opening of the multiple second through holes is preferably in the range of 10 to 900, more preferably in the range of 100 to 600, and even more preferably in the range of 200 to 450.

[0041] In each of the plurality of through-hole groups provided in the etched product 1, the distance between the opening of each of the plurality of second through-holes 12 and the opening of the first through-hole 11 is preferably 3.5 mm or less. This means that in the etched product 1 shown in Figures 2 and 3, the distance D12a between the opening of the second through-hole 12 located farthest from the opening of the first through-hole 11 and the opening of the first through-hole 11 is preferably 3.5 mm or less. The distance D12a is more preferably within a range of 1.5 mm or more and 3.5 mm or less, and even more preferably within a range of 1.0 mm or more and 2.5 mm or less.

[0042] As described above, in the etching product 1 shown in FIG. 1 and FIG. 2 before singulation, each of the plurality of through-hole groups is surrounded by the array of the plurality of third through-holes 13 (13a, 13b, 13c). The ratio L1 / L3 of the length L1 of each side of the opening of the first through-hole 11 to the dimension L3 of each region surrounded by the array of the plurality of third through-holes 13 is preferably 0.5 or less, more preferably 0.05 or more and 0.5 or less, and even more preferably 0.2 or more and 0.4 or less. Here, the above-mentioned region of each through-hole group surrounded by the array of the plurality of third through-holes 13 corresponds to the region surrounded by the outer frame F in the etching product 1 after singulation shown in FIG. 3. The above-mentioned dimension L3 corresponds to Lx3 and Ly3, and the above-mentioned L1 / L3 means Lx1 / Lx3 and Ly1 / Ly3. Thus, here, the dimension of the above-mentioned region may be expressed as L3 without distinguishing between Lx3 and Ly3.

[0043] In the etched product 1 before being singulated, the ratio W3 / W2 of the opening width W3 of the multiple third through holes 13 on the first surface to the opening width W2 of each of the multiple second through holes is preferably in the range of 5 to 50, more preferably in the range of 7 to 40, and even more preferably in the range of 10 to 25.

[0044] In each of the plurality of through-hole groups provided in the etched product 1 before singulation, at least one of the distance to the opening of the first through hole 11 and the shortest distance to the opening of the third through holes 13 of each of the plurality of second through holes 12 is preferably 2.0 mm or less. This means that in the etched product shown in Figures 2 and 3, at least one of the distance D12b from the opening of the first through hole 11 to the opening of the second through hole 12 located closest to the opening of the first through hole 11 and the shortest distance D12c from the opening of the second through holes 12 to the opening of the third through holes 13 is preferably 2.0 mm or less. The above distance (i.e., the shorter of the distances D12b and D12c) is more preferably within a range of 1.0 mm or more and 2.0 mm or less, and even more preferably within a range of 1.0 mm or more and 1.5 mm or less.

[0045] The etched product 1 is manufactured by a photoetching method, and the etching is performed by spray etching. A method for manufacturing an etched product according to a second embodiment of the present invention will be described below with reference to Fig. 4. Fig. 4 is a cross-sectional view showing one step of the method for manufacturing an etched product according to the second embodiment of the present invention, specifically, a cross-sectional view of a spray etching step.

[0046] The method for producing an etched product according to the second embodiment of the present invention is as follows: Preparing a metal plate 10 having a first surface and a second surface that is an opposite surface of the first surface; forming an etching mask 14a on the first surface; spraying an etching solution onto the first surface on which the etching mask 14a is provided, thereby etching the metal plate 10; Each step will be described below. Note that, although the following describes a form in which the first surface side of the metal plate 10 is etched, the manufacturing method of the etched product according to the second embodiment of the present invention also includes a form in which the second surface side of the metal plate 10 is etched in the same manner, whereby the metal plate 10 is etched on both sides.

[0047] <Preparing the metal plate> The preferred material and thickness of the metal plate 10 are as described above. A long strip-shaped metal plate 10 is usually used as the material to be etched. The above-mentioned steps are continuously carried out while the long strip-shaped metal plate 10 is conveyed on a conveying means such as a conveying roller. The metal plate 10 used has its surface cleaned to remove the oxide film layer.

[0048] <Formation of Etching Mask> An etching mask 14a is formed on the first surface of the metal plate 10. The etching mask 14a can be formed by a photolithography process. A photosensitive resin layer (resist layer) is formed on the first surface of the metal plate 10 using a photosensitive resin (photoresist). The photosensitive resin layer may be formed by using a dry film resist or by applying a liquid photoresist. When using a dry film resist, a laminator is used. When applying a liquid photoresist, a commonly used photoresist coating method such as a spin coater, roll coater, or dip coater can be used. After applying the photosensitive resin layer, it is preferable to dry it.

[0049] Next, the obtained photosensitive resin layer is exposed. The exposure may be a mask exposure method in which a reticle is used as a photomask to perform pattern exposure. As the mask exposure method, any of contact exposure in which the mask and the photosensitive resin layer are closely exposed, proximity exposure in which the mask and the photosensitive resin layer are exposed with a gap therebetween, and laser exposure can be used.

[0050] Next, the exposed photosensitive resin layer is developed, and if necessary, hardening treatment is performed. Development can be performed by immersing in an alkaline developer or spraying an alkaline developer. As the alkaline developer, an aqueous solution of sodium carbonate, sodium hydroxide, or the like is used. In addition, a defoamer or a surfactant may be added to the developer. As a development method, a shower development method, a spray development method, a dip (immersion) development method, a paddle development method, or the like can be used.

[0051] <Spray etching> Spray etching is performed using the resist pattern 14a obtained above as an etching mask. Fig. 4 is a cross-sectional view of the spray etching process. In the process shown in Fig. 4, a spray 22 of etching solution ejected from a nozzle 21 is sprayed onto the material to be etched, that is, the metal plate 10 provided with the etching mask 14a, which is transported in the direction indicated by the symbol A. As the etching solution, for example, a known etching solution such as an aqueous solution of ferric chloride can be used.

[0052] The etching mask 14a has openings at positions corresponding to the first through holes 11 and the second through holes 12 of the etched product 1 described above. That is, the etching mask 14a is provided with one or more opening patterns, and each of the one or more opening patterns includes a first opening 31 having a rectangular opening with a side length L1 equal to or greater than the thickness of the metal plate 10, and a plurality of second openings 32 each having a linear opening with a width W2 less than the thickness of the metal plate 10 and arranged around the first opening. The spray etching using this etching mask 14a can effectively suppress side etching and has excellent processing accuracy, so that the etched product 1 obtained by the manufacturing method according to this embodiment has a high aspect ratio and high-definition linear pattern 12. The mechanism behind this will be described below while pointing out the problems with conventional spray etching.

[0053] 5 is a cross-sectional view for explaining the problems in conventional spray etching. The reason why it is difficult to improve the etching factor (EF) to a desired level by conventional spray etching even if the etching is made anisotropic is as follows. That is, the etching mask 14b used in conventional spray etching has a plurality of openings 32b each having a linear opening corresponding to the second opening 32 of the etching mask 14a, but no openings having a rectangular opening corresponding to the first opening 31 of the etching mask 14a are formed around it.

[0054] As mentioned above, spray etching uses the effect of liquid pressure in the depth direction of the material to be etched to preferentially replace the etching liquid that has accumulated at the bottom of the etching hole, thereby improving the etching rate in the depth direction. In general, spray etching, which has etching anisotropy, is said to be capable of forming high-definition patterns because it has a high etching factor (EF) and excellent processing accuracy.

[0055] However, when spray etching is performed using an etching mask 14b as shown in FIG. 5, a thick liquid film 23 (for example, about 1 mm) of the etching liquid is formed on the etching mask 14b, and this liquid film prevents the etching liquid accumulated at the bottom of the etching hole 12b from being preferentially replaced. In order to reduce the thickness of this liquid film 23, for example, it is possible to suppress the formation of a thick liquid film by oscillating the spray in the left and right direction. However, depending on the surface layout, it is difficult to efficiently reduce the thickness of the liquid film when the etching processing pattern is located in the central area at a long distance from the end or due to interference between sprays sprayed from adjacent nozzles.

[0056] In contrast, the etching mask 14a used for spray etching in the manufacturing method according to this embodiment includes the first opening 31 having a rectangular opening near a plurality of second openings 32, which are a high-definition linear pattern, as described above. By performing spray etching using this etching mask 14a, a difference in etching rate is generated between the etching hole located at the first opening 31 and the etching hole located at the second opening 32. That is, the etching rate of the etching hole located at the first opening 31 is made higher than the etching rate of the etching hole located at the second opening 32. As a result, the first through hole 11 is first formed in the metal plate 10 at the position of the first opening 31, and then the second through hole 12 is formed in the metal plate 10 at the position of the second opening 32.

[0057] By forming the first through hole 11 before the second through hole 12 in this way, as shown in Fig. 4, the etching liquid is removed from the first through hole 11 at the same time as the etching of the etching hole 12a progresses, so that the liquid film 23 of the etching liquid is prevented from becoming thick. Therefore, due to the anisotropy of the spray etching, it becomes possible to preferentially replace the etching liquid that has accumulated at the bottom of the etching hole 12a, and the etching speed in the depth direction is improved, and the etching factor (EF) is improved.

[0058] The difference in etching rate occurs between the etching holes located at the first openings 31 and the etching holes located at the second openings 32 of the etching mask 14a because of the difference in opening dimensions. As described above, the length L1 of each side of the rectangular opening of the first openings 31 and the width W2 of the linear opening of each of the second openings 32 have a relationship of L1>W2, and the opening dimensions of the first openings 31 are larger than those of the second openings 32. Since the etching rate improves as the opening dimensions increase, the first through holes 11 located at the first openings 31, which have the larger opening dimensions, are formed before the second through holes 12 located at the second openings 32.

[0059] However, when the opening size exceeds a certain threshold, the rate of increase in the etching rate decreases, and beyond that, it becomes almost constant. Figure 7 is a graph showing an example of the relationship between the opening width of the photoresist and the etching rate (etching speed) in the depth direction when a metal plate is spray-etched. The etching conditions are in accordance with the conditions described in the [Examples] below.

[0060] As can be seen from Figure 7, the etching rate increases as the opening width of the etching mask increases, but when the opening width exceeds a certain threshold, the rate of increase in the etching rate drops sharply and becomes almost constant. This is presumably due to the fact that the opening width of the etching mask affects the replacement of the etching solution that has accumulated at the bottom of the etching hole. In other words, when the opening width is less than a certain threshold, the etching rate decreases as the opening width narrows, since it becomes difficult to replace the etching solution. On the other hand, when the opening width exceeds a certain threshold, the etching solution is smoothly replaced without being affected by the opening dimensions, so it is presumed that the etching rate becomes constant.

[0061] Therefore, in order to provide a suitable difference in etching rate between the etching holes located at first opening 31 and the etching holes located at second opening 32, it is preferable that at least the width W2 of the linear opening of each of the plurality of second openings 32 is smaller than the above threshold value. From this viewpoint, the width W2 of the linear opening of each of the plurality of second openings 32 is preferably less than 200 μm, and more preferably 150 μm or less. Moreover, the length L1 of each side of the rectangular opening of first opening 31 is preferably 200 μm or more, and more preferably 500 μm or more. EXAMPLES

[0062] Tests carried out in relation to the present invention will now be described. (Example 1) A copper-based metal plate having a thickness of 150 μm was prepared as the metal plate 10. The surface of this metal plate was treated with acid to remove the oxide film, and then dry film resist was laminated on both sides. The resist layer (photosensitive resin layer) 14 was exposed through a photomask and developed to perform a patterning process, thereby forming a resist pattern 14a having the above-mentioned first opening 31 and second opening 32 on both sides of the metal plate 10. Development was performed by spray development using an alkaline developer.

[0063] Next, double-sided etching was performed using the resist pattern 14a as a mask in a spray-type etching device under etching conditions of a liquid temperature of 60°C and a spray pressure of 0.6 MPa. A dichloromethane solution was used as the etching liquid. Next, the resist pattern 14a was stripped with a dedicated stripping liquid to obtain a sample similar to the etched product 1 shown in Figure 3. The dimensions and ratios of the through holes, as well as the etching factor (EF), are summarized in Table 1.

[0064] (Example 2) A sample having a through-hole group similar to that of the etched product 1 shown in Fig. 3 was manufactured in the same manner as in Example 1, except that the width W2 of the second through-hole 12 was changed from 70 µm to 80 µm by changing the opening width of the second opening 32 of the resist pattern 14a. The dimensions and ratios of the through-holes, as well as the etching factor (EF), are summarized in Table 1.

[0065] (Example 3) A sample having a through-hole group similar to that of the etched product 1 shown in Fig. 3 was manufactured in the same manner as in Example 1, except that the width W2 of the second through-hole 12 was changed from 70 µm to 50 µm by changing the opening width of the second opening 32 of the resist pattern 14a. The dimensions and ratios of the through-holes, as well as the etching factor (EF), are summarized in Table 1.

[0066] (Example 4) A sample having a through-hole group similar to that of the etched product 1 shown in Fig. 3 was manufactured in the same manner as in Example 1, except that the width W2 of the second through-hole 12 was changed from 70 µm to 60 µm by changing the opening width of the second opening 32 of the resist pattern 14a. The dimensions and ratios of the through-holes, as well as the etching factor (EF), are summarized in Table 1.

[0067] Comparative Example 1 An etched sample was manufactured in the same manner as in Example 1, except that spray etching was performed using a resist pattern 14b not including the first opening 31 as a mask instead of the resist pattern 14a. The obtained sample is shown in FIG. 6. The etched product 100 shown in FIG. 6 includes the second through-hole 12, which is a linear pattern, but does not include the first through-hole 11, which is a rectangular pattern. The dimensions and ratios of the through-holes, as well as the etching factor (EF), are summarized in Table 1.

[0068] [Table 1]

[0069] (evaluation) In Examples 1 to 4, the first through hole 11 penetrated in the spray etching before any of the multiple second through holes 12. When the first through hole 11 penetrated, the etching liquid that had become the liquid film 23 was removed from the first through hole 11, and thereafter, almost no film liquid 23 was formed. On the other hand, in Comparative Example 1, a thick film liquid 23 of the etching liquid was formed as the spray etching proceeded.

[0070] 8 is a graph comparing the etching factor (EF) of Example 1 and Comparative Example 1. Example 1 has a higher etching factor and is more accurate than Comparative Example 1. This shows that it is possible to form a high-definition pattern with a high aspect ratio.

[0071] 9 is a graph showing the relationship between the width W2 of the second through hole 12 and the etching factor (EF) for Examples 1 to 4. It can be seen that the etching factor increases as the width W2 of the second through hole 12 increases.

[0072] The present invention is not limited to the above-mentioned embodiment, and can be modified in various ways without departing from the gist of the present invention. The embodiments may be combined as appropriate, and in that case, the combined effect can be obtained. Furthermore, the above-mentioned embodiment includes various inventions, and various inventions can be extracted by combinations selected from the multiple components disclosed. For example, if the problem can be solved and the effect can be obtained even if some components are deleted from all the components shown in the embodiment, the configuration from which the components are deleted can be extracted as an invention. [Explanation of symbols]

[0073] 1...etched product, 10...metal plate, 11...first through hole, 12...second through hole, 12a, 12b...etching hole, 13, 13a, 13b, 13c...third through hole, 14...photosensitive resin layer (resist layer), 14a, 14b...resist pattern (etching mask), 21...nozzle, 22...spray, 23...liquid film, 31...first opening, 32, 32b...second opening, 100...etched product of Comparative Example 1, L1, Lx1, Ly1, L2, L3, Lx3, Ly3...length (dimension), W2, W3...width, D12a, D12b, D12c...distance, F...outer frame, d...etching depth, S...side etching amount.

Claims

1. An etched product comprising a metal plate having a first surface and a second surface which is the reverse surface of the first surface, and having one or more groups of through holes formed therein, each of the one or more groups of through holes including a first through hole having a rectangular opening on the first surface, the length of each side being equal to or greater than the thickness of the metal plate, and a plurality of second through holes each having a linear opening on the first surface, the width of which is less than the thickness of the metal plate, and arranged around the first through hole.

2. The etched product according to claim 1, wherein the opening of each of the plurality of second through holes has a width in the range of 20 to 150 μm, and a ratio S1 / S2 of an area S1 of the opening of the first through hole to an area S2 of the opening of each of the plurality of second through holes is 10 or more.

3. 2. The etched product according to claim 1, wherein a ratio L1 / W2 of a length L1 of each side of the opening of the first through hole to a width W2 of the opening of each of the plurality of second through holes is within a range of 10 to 900.

4. 2 . The etched product according to claim 1 , wherein in each of the one or more through hole groups, the opening of each of the plurality of second through holes is located 3.5 mm or less away from the opening of the first through hole.

5. The etched product of claim 1, wherein the metal plate is further provided with a plurality of third through holes arranged to surround each of the one or more through hole groups, and the ratio L1 / L3 of the length L1 of each side of the opening of the first through hole to the dimension L3 on the first surface of each region surrounded by the array of the plurality of third through holes is 0.5 or less.

6. The etched product according to claim 5, wherein the ratio W3 / W2 of the opening width W3 of the plurality of third through holes in the first surface to the opening width W2 of each of the plurality of second through holes is within a range of 5 to 50.

7. The etched product described in claim 5, wherein in each of the one or more groups of through holes, the opening of each of the plurality of second through holes has at least one of a distance to the opening of the first through hole and a shortest distance to the opening of the plurality of third through holes that is 2.0 mm or less.

8. The etched product according to claim 1 , wherein the one or more groups of through holes are two or more groups of through holes.

9. Providing a metal plate having a first surface and a second surface opposite to the first surface; forming an etch mask over the first surface; spraying an etching solution onto the first surface on which the etching mask is provided, thereby etching the metal plate; Including, The method for manufacturing an etched product includes using an etching mask having one or more opening patterns, each of which includes a first opening having a rectangular opening whose sides are equal to or longer than the thickness of the metal plate, and a plurality of second openings, each of which has a linear opening whose width is less than the thickness of the metal plate, and which are arranged around the first opening, and by using the etching mask, a difference is made in the etching rate to form a first through hole in the metal plate at the position of the first opening, and then a plurality of second through holes are formed in the metal plate at the positions of the plurality of second openings.

10. The formation of the etching mask includes: providing a photosensitive resin layer on the first surface; exposing the photosensitive resin layer to a pattern; developing the photosensitive resin layer after the pattern exposure; The method for producing an etched product according to claim 9, comprising:

11. 11. The method for producing an etched product according to claim 10, further comprising the step of: forming a reticle for use in said pattern exposure.

Citation Information

Patent Citations

  • Metal etched product and manufacturing method therefor

    JP2004204251A

  • Etching product and etching method

    JP2004218033A