Protective layer transfer sheet

The protective layer transfer sheet with a critical damage load of 0.012N to 0.035N enhances adhesion and transferability, addressing durability and adhesion issues in thermal transfer images by optimizing the adhesive layer's flexibility and followability.

JP2024166857APending Publication Date: 2024-11-29DAI NIPPON PRINTING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023083243
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Thermal transfer images formed on a receiving layer suffer from poor durability and inconsistent adhesion due to variations in the followability of the protective layer transfer sheet's adhesive surface, leading to issues with transfer layer adhesion and transferability.

Method used

A protective layer transfer sheet comprising a base material with a transfer layer including a protective layer and an adhesive layer, where the adhesive layer has a critical damage load of 0.012N or more and 0.035N or less, enhancing adhesion and transferability by optimizing the flexibility and followability.

Benefits of technology

The solution improves the adhesion and transferability of the transfer layer to the transfer target, ensuring minimal untransferred areas and maintaining scratch resistance and blocking resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166857000001_ABST
    Figure 2024166857000001_ABST
Patent Text Reader

Abstract

To provide a protective layer transfer sheet that can improve the adhesion and transferability of a transfer layer to a transfer object.SOLUTION: A protective layer transfer sheet 10 includes a substrate 11, and a transfer layer 14 provided on the substrate 11. The transfer layer 14 includes a protective layer 12 provided on the substrate 11, and an adhesive layer 13 provided on the protective layer 12. The adhesive layer 13 has a critical damage load of 0.012 N or more and 0.035 N or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a protective layer transfer sheet. [Background technology]

[0002] Thermal transfer images are widely formed by the dye-sublimation thermal transfer method because it has excellent transparency, high reproducibility and gradation of intermediate colors, and can easily form high-quality images equivalent to conventional full-color photographic images (see, for example, Patent Documents 1 and 2). The dye-sublimation thermal transfer method is a method in which a thermal transfer sheet provided with a dye layer and a transferee provided with a receptor layer are used, and heat is applied to the thermal transfer sheet to transfer the color material contained in the dye layer to the receptor layer, thereby forming a thermal transfer image.

[0003] A thermally transferred image formed on a receptor layer by a dye-sublimation thermal transfer method has excellent gradation, but since the thermally transferred image formed on the receptor layer is located on the outermost surface of the transfer target, it has a problem of poor durability.

[0004] In recent years, in order to solve this problem, the durability of the thermal transfer image has been improved by superimposing a receiving layer to which the thermal transfer image has been transferred and a protective layer transfer sheet having a protective layer, and transferring a transfer layer such as a protective layer onto the receiving layer (see, for example, Patent Document 3, etc.). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-75480 A [Patent Document 2] JP 2013-82212 A [Patent Document 3] JP 2015-85554 A Summary of the Invention [Problem to be solved by the invention]

[0006] In such a protective layer transfer sheet, in addition to the durability of the transfer layer, the transfer layer is required to have high transferability so as to prevent the occurrence of untransferred areas.

[0007] In addition, the recipient on which the receiving layer is provided has a certain rigidity, and the adhesion of the transfer layer to the recipient may vary greatly depending on the conformability of the adhesive surface of the protective layer transfer sheet provided with a protective layer.

[0008] The present disclosure has been made in consideration of these points, and an object of the present disclosure is to provide a protective layer transfer sheet that can improve the adhesion and transferability of a transfer layer to a receiving body. [Means for solving the problem]

[0009] The embodiments of the present disclosure relate to the following [1] to [3].

[0010] [1] A protective layer transfer sheet comprising a substrate and a transfer layer provided on the substrate, the transfer layer having a protective layer provided on the substrate and an adhesive layer provided on the protective layer, the critical damage load of the adhesive layer being 0.012 N or more and 0.035 N or less.

[0011] [2] The protective layer transfer sheet described in [1], further comprising a release layer or peeling layer provided between the substrate and the transfer layer.

[0012] [3] The protective layer transfer sheet described in [1] or [2], wherein the transfer layer further has a primer layer provided between the protective layer and the adhesive layer. Effect of the Invention

[0013] According to the present disclosure, it is possible to improve the adhesion and transferability of a transfer layer to a receiving body. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view showing a protective layer transfer sheet according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a protective layer transfer sheet according to one embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing a protective layer transfer sheet according to one embodiment. [Figure 4] FIG. 4 is a schematic diagram illustrating the micro-scratch method. [Diagram 5] FIG. 5 is a cross-sectional view showing a transfer target according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present embodiment will be described below with reference to the drawings. FIGS. 1 to 5 are diagrams showing the present embodiment. Each of the following figures is a schematic diagram. Therefore, the size and shape of each part are appropriately exaggerated to facilitate understanding. In addition, the present invention can be modified appropriately within the scope of the technical concept. In each of the following figures, the same parts are given the same reference numerals, and some detailed explanations may be omitted. In addition, the numerical values ​​such as the dimensions of each member and the material names described in this specification are examples of the embodiment, and are not limited to these, and can be appropriately selected and used. In this specification, terms that specify shapes and geometric conditions, such as parallel, orthogonal, and vertical, are intended to include substantially the same state in addition to their strict meanings. In this specification, "upper" and "lower" refer to the upper and lower sides of the paper container in an upright state (FIG. 1), respectively. In this specification, "surface" refers to the surface facing the contents, or the surface that faces upward when the paper container is upright.

[0016] Protective layer transfer sheet As shown in FIG. 1 to FIG. 3, the protective layer transfer sheet 10 includes a substrate 11 and a transfer layer 14 provided on the substrate 11. As shown in FIG. 2, the protective layer transfer sheet 10 may further include a release layer 15 provided between the substrate 11 and the transfer layer 14. In this case, the protective layer transfer sheet 10 may further include a first primer layer 19 provided between the substrate 11 and the release layer 15. As shown in FIG. 3, the protective layer transfer sheet 10 may further include a peeling layer 16 provided between the substrate 11 and the transfer layer 14. As shown in FIG. 2 and FIG. 3, the protective layer transfer sheet 10 may further include a back layer 17 provided on the opposite side of the substrate 11 to the side on which the transfer layer 14 is provided. In the example shown in FIG. 2 and FIG. 3, the protective layer transfer sheet 10 includes only one of the release layer 15 and the peeling layer 16. However, the present invention is not limited to this, and the protective layer transfer sheet 10 may include both the release layer 15 and the peeling layer 16.

[0017] 1 to 3, the transfer layer 14 of the protective layer transfer sheet 10 has a protective layer 12 provided on a substrate 11 and an adhesive layer 13 provided on the protective layer 12. In addition, as shown in Fig. 2 and Fig. 3, the transfer layer 14 may have a second primer layer (primer layer) 18 provided between any layers. In the example shown in Fig. 2 and Fig. 3, the second primer layer 18 is provided between the protective layer 12 and the adhesive layer 13.

[0018] Such a protective layer transfer sheet 10 is a sheet for transferring a transfer layer 14 to a transferee (not shown). In the protective layer transfer sheet 10 shown in FIG. 1, when the transfer layer 14 is transferred to a transferee (not shown), the protective layer 12 and the adhesive layer 13 are transferred to the transferee as the transfer layer 14. In the protective layer transfer sheet 10 shown in FIG. 2 and FIG. 3, when the transfer layer 14 is transferred to a transferee (not shown), the protective layer 12, the second primer layer 18, and the adhesive layer 13 are transferred to the transferee as the transfer layer 14. In addition, in the protective layer transfer sheet 10 shown in FIG. 3, when the transfer layer 14 is transferred to a transferee (not shown), the peeling layer 16 is also transferred to the transferee.

[0019] Each layer constituting the protective layer transfer sheet 10 according to the present embodiment will be described below.

[0020] <Base material> The substrate 11 is a layer that supports the transfer layer 14 and the like, and also enhances the strength of the entire protective layer transfer sheet 10. There are no particular limitations on the substrate 11, as long as it is a member that has heat resistance that can withstand thermal energy applied during thermal transfer (e.g., heat from a thermal head), and has mechanical strength and solvent resistance that can support the transfer layer 14.

[0021] Examples of the substrate 11 include polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polyethylene terephthalate-isophthalate copolymer, and terephthalic acid-cyclohexanedimethanol-ethylene glycol copolymer; polyamide resins such as nylon 6 and nylon 6,6; polyolefin resins such as polyethylene (PE), polypropylene (PP), and polymethylpentene; vinyl resins such as polyvinyl chloride resin, polyvinyl alcohol resin, polyvinyl acetate resin, vinyl chloride-vinyl acetate copolymer, polyvinyl butyral resin, and polyvinylpyrrolidone resin; polyacrylate, polymethacrylate, and polymethyl methacrylate. (Meth)acrylic resins, imide resins such as polyimide and polyether polyimide, engineering resins such as polyarylate, polysulfone, polyether sulfone, polyphenylene ether, polyphenylene sulfide (PPS), polyaramid, polyether ketone, polyether nitrile, polyether ether ketone, and polyether sulfite, styrene resins such as polystyrene, high impact polystyrene, acrylonitrile-styrene copolymer (AS resin), and acrylonitrile-butadiene-styrene copolymer (ABS resin), cellulose resins such as cellophane, cellulose acetate, and nitrocellulose, and films made of polycarbonate and the like (hereinafter simply referred to as "resin film") may be used. In this specification, "(meth)acrylic" means both "acrylic" and "methacrylic", and "(meth)acrylate" means both "acrylate" and "methacrylate".

[0022] Among the above-mentioned films made of resin, films made of polyester-based resin such as PET or PEN have excellent heat resistance and mechanical strength. Therefore, the base material 11 may be a film made of polyester-based resin. In particular, the base material 11 may be a film made of PET.

[0023] Furthermore, a laminate of the above-mentioned resin films may be used as the substrate 11. In this case, the laminate can be produced by utilizing a dry lamination method, a wet lamination method, an extrusion method, or the like.

[0024] When the substrate 11 is a film made of the above-mentioned resin, the resin film may be a stretched film or an unstretched film. From the viewpoint of increasing the strength, the resin film may be a stretched film that is uniaxially or biaxially stretched.

[0025] From the viewpoint of improving adhesion to the protective layer 12 and the like and blocking resistance, the substrate 11 may have an uneven surface. Examples of means for forming unevenness on the surface of the substrate 11 include matte material kneading, sandblasting, hairline processing, matte coating, and chemical etching. The matte material kneading is a processing method for forming the substrate 11 from a resin kneaded with an inorganic or organic substance. The matte coating is a processing method for coating the surface of the substrate 11 with a coating material containing an organic or inorganic substance, thereby imparting unevenness to the surface of the substrate 11.

[0026] The thickness of the substrate 11 may be 4 μm or more and 50 μm or less, or 12 μm or more and 30 μm or less. By making the thickness of the substrate 11 within the above numerical range, the mechanical strength of the substrate 11 can be increased, and thermal energy can be effectively transferred during thermal transfer.

[0027] <Transfer layer> The transfer layer 14 is a layer that is transferred to a transfer-receiving body 30 described below. As described above, the transfer layer 14 has a protective layer 12 and an adhesive layer 13. The transfer layer 14 may also have a second primer layer 18 provided between any layers. Here, the protective layer 12 of the transfer layer 14 will be first described.

[0028] <<Protective layer>> The protective layer 12 is a layer for protecting the transfer-receiving body 30 described later. The protective layer 12 may contain a (meth)acrylic resin, a polyester resin, a cellulose resin, a polystyrene resin, a polyamide resin, an acetal resin, a polycarbonate resin, a thermosetting resin, or an actinic radiation curable resin. From the viewpoint of durability, the protective layer 12 may contain an actinic radiation curable resin. In this specification, the term "actinic radiation curable resin" refers to a resin obtained by curing an actinic radiation curable resin by irradiating the actinic radiation curable resin with actinic radiation. In this specification, the term "actinic radiation" refers to radiation that promotes polymerization by acting chemically on the actinic radiation curable resin, and specifically refers to visible light, ultraviolet light, X-rays, electron beams, α rays, β rays, γ rays, or the like. In this embodiment, the actinic radiation irradiated to the actinic radiation curable resin is preferably ultraviolet light, and the protective layer 12 preferably contains an ultraviolet light curable resin as the actinic radiation curable resin.

[0029] As the actinic radiation curable resin, any compound that can be polymerized by irradiation with actinic radiation can be used without any particular limitation. For example, as the actinic radiation curable resin, a polymerizable monomer having a radical polymerizable unsaturated group such as an acryloyl group, a vinyl group, an allyl group, and an isopropenyl group, a polymerizable oligomer, a polymerizable prepolymer, etc. may be used. In this specification, the term "oligomer" refers to a polymer having a weight average molecular weight (Mw) of more than 1,000 and less than 10,000. In this specification, the term "prepolymer" refers to a polymer having a weight average molecular weight (Mw) of more than 10,000 and less than 30,000. In this specification, the term "weight average molecular weight (Mw)" refers to a value measured by gel permeation chromatography using polystyrene as a standard substance, and can be measured by a method conforming to JIS-K-7252-1:2016.

[0030] Examples of the polymerizable monomer that may be used include urethane acrylate, epoxy acrylate, polyester acrylate, polyether acrylate, polyethylene acrylate, silicone acrylate, and polyol acrylate. Also, methacrylates, itaconates, crotonates, or maleates of these may be used. More specifically, the polymerizable monomer is (1) Monofunctional acrylates such as 2-ethylhexyl acrylate, 2-hydroxypropyl acrylate, glycerol acrylate, tetrahydrofurfuryl acrylate, phenoxyethyl acrylate, nonylphenoxyethyl acrylate, tetrahydrofurfuryloxyethyl acrylate, tetrahydrofurfuryloxyhexanolide acrylate, acrylates of ε-caprolactone adducts of 1,3-dioxane alcohol, and 1,3-dioxolane acrylate; (2) Bifunctional acrylates such as ethylene glycol diacrylate, triethylene glycol diacrylate, pentaerythritol diacrylate, hydroquinone diacrylate, resorcinol diacrylate, hexanediol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, diacrylate of neopentyl glycol hydroxypivalate, diacrylate of neopentyl glycol adipate, diacrylate of ε-caprolactone adduct of neopentyl glycol hydroxypivalate, 2-(2-hydroxy-1,1-dimethylethyl)-5-hydroxymethyl-5-ethyl-1,3-dioxane diacrylate, tricyclodecane dimethylol acrylate, ε-caprolactone adduct of tricyclodecane dimethylol acrylate, and diacrylate of diglycidyl ether of 1,6-hexanediol; (3) Polyfunctional acrylates such as trimethylolpropane triacrylate, ditrimethylolpropane tetraacrylate, trimethylolethane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, ε-caprolactone adduct of dipentaerythritol hexaacrylate, pyrogallol triacrylate, propionic acid / dipentaerythritol triacrylate, propionic acid / dipentaerythritol tetraacrylate, and hydroxypivalylaldehyde-modified dimethylolpropane triacrylate.

[0031] Examples of the polymerizable oligomer and polymerizable prepolymer include polymers of the above-mentioned polymerizable monomers, such as epoxy (meth)acrylate, urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, melamine (meth)acrylate, triazine (meth)acrylate, silicone (meth)acrylate, acrylic silicone (meth)acrylate, or polycarbonate (meth)acrylate.

[0032] Examples of the thermosetting resin include phenol-based resins, urea-based resins, diallyl phthalate-based resins, melamine-based resins, guanamine-based resins, polyurethane-based resins, and epoxy-based resins.

[0033] In one embodiment, the protective layer 12 may contain a polymerization initiator. For example, a benzoin-based, acetophenone-based, thioxanthone-based, phosphine oxide-based, peroxide-based, or azo-based compound may be used as the polymerization initiator. More specifically, for example, benzoin, benzophenone, 4,4-bis(diethylamino)benzophenone, 2,4,6-trimethylbenzophenone, methyl orthobenzoyl benzoate, 4-phenylbenzophenone, 2-methyl-[4-(methylthio)phenyl]-morpholino-1-propanone, isopropylthioxanthone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, methylbenzoyl formate, or azobisisobutyronitrile (AIBN) may be used as the polymerization initiator.

[0034] The content of the polymerization initiator in the protective layer 12 may be 0.1 parts by mass or more and 5 parts by mass or less, or may be 1 part by mass or more and 3 parts by mass or less, relative to 100 parts by mass of the actinic radiation curable resin contained in the protective layer 12.

[0035] In one embodiment, the protective layer 12 may contain a filler. Examples of the filler include an organic filler, an inorganic filler, or an organic-inorganic hybrid filler. The filler may be in the form of a powder or a sol. From the viewpoint of expanding the options of solvents when preparing the coating liquid, a powder filler may be used.

[0036] The filler contained in the protective layer 12 may have an average particle diameter of 1 nm or more and 200 nm or less, 1 nm or more and 50 nm or less, or 7 nm or more and 25 nm or less. By setting the average particle diameter of the filler within the above numerical range, transferability can be improved. In this specification, the term "average particle diameter" means the volume average particle diameter. The "average particle diameter" can be measured by a known method using a particle size distribution / particle size distribution measuring device (Nanotrack particle size distribution measuring device, manufactured by Nikkiso Co., Ltd.).

[0037] Examples of the powdered organic filler include acrylic particles such as non-crosslinked acrylic particles or crosslinked acrylic particles, polyamide particles, fluorine particles, polyethylene wax, etc. Examples of the powdered inorganic filler include calcium carbonate particles, silica particles, metal oxide particles such as titanium oxide, etc. Examples of the organic-inorganic hybrid filler include fillers in which silica particles are hybridized with acrylic resin, etc. Examples of the sol-type filler include silica sol-based or organosol-based fillers, etc. These fillers may be used alone or in combination of two or more.

[0038] The content of the filler in the protective layer 12 may be 5% by mass or more and 60% by mass or less, or may be 20% by mass or more and 50% by mass or less, thereby making it possible to improve the durability of the protective layer 12.

[0039] The thickness of the protective layer 12 may be from 1 μm to 15 μm, or from 2 μm to 8 μm. By setting the thickness of the protective layer 12 within the above numerical range, the durability and transferability of the protective layer transfer sheet 10 can be improved.

[0040] When forming the protective layer 12, first, the above-mentioned material is dispersed or dissolved in water or a suitable solvent to prepare a coating liquid. Next, the coating liquid is applied onto the substrate 11 or the like to form a coating film. The coating liquid may be applied onto the substrate 11 or the like by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. At this time, the coating film is cured by irradiating the coating film with active light rays as necessary. In this way, the protective layer 12 is formed. Here, when an electron beam is used as the active light rays, the acceleration voltage can be appropriately changed depending on the resin used and the thickness of the layer. The acceleration voltage may be, for example, 100 kV or more and 300 kV or less. The irradiation dose may be an amount sufficient to saturate the crosslink density of the active light curable resin. Specifically, the irradiation dose may be 100 kGy or more and 300 kGy or less, or 100 kGy or more and 200 kGy or less. The electron beam source is not particularly limited, and may be, for example, various electron beam accelerators such as Cockcroft-Walton type, Van de Graff type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, or high frequency type. When ultraviolet light is used as the active light, active light containing ultraviolet light having a wavelength of 190 nm or more and 380 nm or less may be irradiated to the coating film. The ultraviolet light source is not particularly limited, and may be, for example, a high pressure mercury lamp, a low pressure mercury lamp, a metal halide lamp, or a carbon arc lamp.

[0041] <<adhesive layer>> Next, the adhesive layer 13 will be described. The adhesive layer 13 is a layer for adhering the protective layer 12 to the transfer recipient 30 described below. The adhesive layer 13 is provided as the outermost layer of the protective layer transfer sheet 10. The adhesive layer 13 may contain a polyolefin resin and a (meth)acrylic resin. This can improve the adhesion and transferability of the transfer layer 14 to the transfer recipient.

[0042] The content ratio of the polyolefin resin to the (meth)acrylic resin in the adhesive layer 13 (polyolefin resin / acrylic resin) may be 9 / 1 or more and 6 / 4 or less, or 8 / 2 or more and 7 / 3 or less, on a mass basis. By setting the content ratio of the polyolefin resin to the (meth)acrylic resin within the above numerical range, the adhesion and transferability of the transfer layer 14 to the transfer recipient can be further improved. In addition, by setting the content ratio of the polyolefin resin to the (meth)acrylic resin within the above numerical range, the blocking resistance of the protective layer transfer sheet 10 can be improved.

[0043] Examples of the polyolefin resin include low density polyethylene (LDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), linear low density polyethylene (LLDPE), polypropylene (PP), polybutene, polynorbornene, ethylene-propylene copolymer, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer. Examples of the α-olefin include 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene. Acid-modified polyolefin resins obtained by graft-modifying the above-mentioned resins with (meth)acrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid may also be used. From the viewpoint of improving the adhesive strength of the transfer layer 14 to the transfer target, an acid-modified polyolefin resin may also be used as the polyolefin resin. The adhesive layer 13 may contain two or more of the above-mentioned polyolefin resins.

[0044] As described above, the polyolefin resin may be a copolymer of a polyolefin monomer and another monomer. In this case, the proportion of the polyolefin monomer relative to 100% by mass of all monomers constituting the polyolefin resin may be 50% by mass or more, 70% by mass or more, or 100% by mass, i.e., the polyolefin resin may be composed only of the polyolefin monomer. By setting the proportion of the polyolefin monomer within the above numerical range, the adhesion and transferability of the transfer layer 14 to the transferee can be improved.

[0045] The content of the polyolefin resin in the adhesive layer 13 may be 60% by mass or more and 90% by mass or less, or may be 70% by mass or more and 85% by mass or less. By setting the content of the polyolefin resin within the above numerical range, the adhesion and transferability of the transfer layer 14 to the transfer recipient can be further improved.

[0046] Examples of the (meth)acrylic resin include (1) a polymer of (meth)acrylic acid or a derivative thereof, (2) a polymer of a (meth)acrylic acid ester or a derivative thereof, (3) a copolymer of (meth)acrylic acid and another monomer or a derivative thereof, (4) a copolymer of a (meth)acrylic acid ester and another monomer or a derivative thereof, and (5) a fluorine-modified resin, a silicone-modified resin, or an epoxy-modified resin of (1) to (4).

[0047] More specifically, the (meth)acrylic resin classified into the above (1) is poly(meth)acrylic acid, the (meth)acrylic resin classified into the above (2) is polymethyl(meth)acrylate, polyethyl(meth)acrylate, polypropyl(meth)acrylate, polyisopropyl(meth)acrylate, poly-n-butyl(meth)acrylate, poly-i-butyl(meth)acrylate, poly-t-butyl(meth)acrylate, poly-n-hexyl(meth)acrylate, polylauryl(meth)acrylate, poly2-hydroxyethyl(meth)acrylate, poly2-hydroxybutyl(meth)acrylate, or a copolymer of two or more monomers constituting these, and the (meth)acrylic resin classified into the above (3) is polymethyl(meth)acrylate, polyethyl(meth)acrylate, polypropyl(meth)acrylate, polyisopropyl(meth)acrylate, poly-n-butyl(meth)acrylate, poly-n-hexyl(meth)acrylate, polylauryl(meth)acrylate, poly2-hydroxyethyl(meth)acrylate, poly2-hydroxybutyl(meth)acrylate, or a copolymer of two or more monomers constituting these. Examples of the (meth)acrylic resins classified into the above category (4) include vinyl chloride-(meth)acrylic acid copolymer, styrene-(meth)acrylic acid copolymer, and benzylstyrene-(meth)acrylic acid copolymer, while examples of the (meth)acrylic resins classified into the above category (4) include vinyl chloride-methyl(meth)acrylate copolymer, styrene-methyl(meth)acrylate copolymer, benzylstyrene-methyl(meth)acrylate copolymer, vinyl chloride-ethyl(meth)acrylate copolymer, styrene-ethyl(meth)acrylate copolymer, benzylstyrene-ethyl(meth)acrylate copolymer, vinyl chloride-propyl(meth)acrylate copolymer, styrene-propyl(meth)acrylate copolymer, and benzylstyrene-propyl(meth)acrylate copolymer. The adhesive layer 13 may contain two or more of the above-mentioned (meth)acrylic resins.

[0048] The glass transition temperature (Tg) of the (meth)acrylic resin may be 25° C. or higher and 100° C. or lower, 30° C. or higher and 80° C. or lower, or 50° C. or higher and 80° C. or lower. By setting the glass transition temperature (Tg) of the (meth)acrylic resin within the above numerical range, it is possible to improve the transferability of the transfer layer 14 and the blocking resistance of the protective layer transfer sheet 10. In this specification, the glass transition temperature (Tg) can be measured by differential scanning calorimetry in accordance with JIS-K-7121:2012.

[0049] The content of the (meth)acrylic resin in the adhesive layer 13 may be 10% by mass or more and 40% by mass or less, or may be 15% by mass or more and 30% by mass or less. By setting the content of the (meth)acrylic resin within the above numerical range, the adhesion and transferability of the transfer layer 14 to the transfer recipient can be further improved.

[0050] The adhesive layer 13 may contain a resin other than the polyolefin resin and the (meth)acrylic resin as long as the characteristics of the present embodiment are not impaired. For example, the adhesive layer 13 may contain a polyester resin, a polyamide resin, a vinyl resin, an imide resin, a styrene resin, a cellulose resin, or the like.

[0051] In one embodiment, the adhesive layer 13 may contain a wax material. By incorporating a wax material in the adhesive layer 13, the blocking resistance of the protective layer transfer sheet 10 can be improved. Examples of the wax material include polyethylene wax, carnauba wax, paraffin wax, microcrystalline wax, silicone wax, candelilla wax, whale wax, wood wax, beeswax, whale wax, ivory wax, wool wax, candelilla wax, petrolactam, and partially modified wax. From the viewpoint of improving blocking resistance, polyethylene wax may be used. The adhesive layer 13 may contain two or more of the above-mentioned wax materials.

[0052] The content of the wax material in the adhesive layer 13 may be 0.1% by mass or more and 10% by mass or less, or may be 0.5% by mass or more and 5% by mass or less. By setting the content of the wax material within the above numerical range, the blocking resistance of the protective layer transfer sheet 10 can be further improved.

[0053] In addition, the adhesive layer 13 may contain additives such as plasticizers, UV stabilizers, color prevention materials, matting materials, deodorizing materials, flame retardants, weather resistance materials, antistatic materials, yarn friction reducing materials, slip materials, release materials, antioxidants, ion exchange materials, or coloring pigments, within the range that does not impair the characteristics of this embodiment.

[0054] In this embodiment, the critical damage load of the adhesive layer 13 is 0.012N or more and 0.035N or less. When the critical damage load of the adhesive layer 13 is 0.012N or more, the scratch resistance and blocking resistance can be improved. Furthermore, when the critical damage load of the adhesive layer 13 is 0.035N or less, the adhesion and transferability of the transfer layer 14 can be improved. That is, when the critical damage load of the adhesive layer 13 is 0.035N or less, the flexibility of the adhesive layer 13 is high. Therefore, the followability of the adhesive layer 13 to the transferee 30 described later is improved. As a result, the adhesion and transferability of the transfer layer 14 to the transferee 30 described later can be improved.

[0055] The critical damage load of the adhesive layer 13 is measured by a micro-scratch method conforming to JIS-R-3255:1997. In this micro-scratch method, the surface of the sample is scratched by the measuring needle (indenter) while a load is applied to the measuring needle, and the state of the scratched surface detected by the measuring needle is converted into an electric signal. In this embodiment, the measuring needle has a curvature radius of 50 μm. During the measurement, the measuring needle is moved in the horizontal direction relative to the surface of the sample (surface of the adhesive layer 13). At this time, the moving speed of the measuring needle is set to a low speed (5 μm / s) in order to prevent measurement errors. The load applied to the measuring needle is increased in proportion to time from 0 mN to 40 mN over 60 seconds. Then, the critical damage load of the adhesive layer 13 is obtained from the shear stress (mN) perpendicular to the surface of the sample. The measurement environment is set to a temperature of about 25° C. (±10° C.) and a humidity of about 50% RH (±10%). The critical damage load of the adhesive layer 13 is measured in the state of the protective layer transfer sheet 10. In this case, the critical damage load of the adhesive layer 13 is measured in a state in which the protective layer transfer sheet 10 is placed on the glass so that the base material 11 of the protective layer transfer sheet 10 faces the glass.

[0056] When the sample surface is scratched by the measuring needle (indenter) while being pressed against the sample surface, a shear stress acts on the interface between the adhesive layer 13 and the protective layer 12. When the shear stress exceeds the adhesion strength between the adhesive layer 13 and the protective layer 12, interfacial peeling occurs at the above-mentioned interface. In this embodiment, the load at this time is referred to as the critical damage load.

[0057] Next, referring to Figure 4, we will explain the micro-scratch tester for measuring the critical damage load by the micro-scratch method. As shown in Figure 4, it is characterized by having a diamond needle (measurement needle) attached to the tip of a cantilever. Because the equivalent mass of the diamond needle is extremely small, it can capture minute changes on the sample surface with high sensitivity when the diamond needle scans over the sample surface. The vibration of the needle tip is converted into an electrical signal inside the cartridge through the cantilever. Since a cartridge with this conversion structure cannot output a DC signal, an AC signal is created by forcibly exciting the cartridge horizontally. Because the micro-scratch tester uses such a detection mechanism, it can convert the minute vibration of the diamond needle into an electrical signal with high sensitivity.

[0058] The thickness of the adhesive layer 13 may be 0.3 μm or more and 5.0 μm or less, 0.3 μm or more and 1.0 μm or less, or 0.5 μm or more and 0.8 μm or less. By setting the thickness of the adhesive layer 13 within the above numerical range, the transferability of the transfer layer 14 can be further improved. Furthermore, by setting the thickness of the adhesive layer 13 within the above numerical range, the durability of the transfer layer 14 and the adhesive strength to the transfer target can be improved.

[0059] When forming the adhesive layer 13, first, the above-mentioned material is dispersed or dissolved in water or a suitable solvent to prepare a coating liquid. Next, the coating liquid is applied onto the protective layer 12 or the like to form a coating film. The coating film may be applied onto the protective layer 12 or the like by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the adhesive layer 13 is formed.

[0060] <<Primer layer>> Next, the second primer layer 18 will be described. The second primer layer 18 serves to improve the adhesive strength between layers. The configuration of the first primer layer 19 described above may be the same as the configuration of the second primer layer 18. Therefore, a detailed description of the first primer layer described above will be omitted.

[0061] The second primer layer 18 may contain a polyester resin, a polyurethane resin, a polycarbonate resin, a (meth)acrylic resin, an epoxy resin, a polystyrene resin, a vinyl resin, a cellulose resin, or the like. The second primer layer 18 may contain an isocyanate compound in addition to the above-mentioned resins. The isocyanate compound may be a polyisocyanate compound having two or more isocyanate groups in the molecule. Examples of the isocyanate compound include xylylene diisocyanate, paraphenylene diisocyanate, 1-chloro-2,4-phenyl diisocyanate, 2-chloro-1,4-phenyl diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,5-naphthalene diisocyanate, tolidine diisocyanate, p-phenylene diisocyanate, trans-cyclohexane, 1,4-diisocyanate, hexamethylene diisocyanate, 4,4'-biphenylene diisocyanate, triphenylmethane triisocyanate, and 4,4',4''-trimethyl-3,3',2'-triisocyanate-2,4,6-triphenyl cyanurate.

[0062] The thickness of the second primer layer 18 is not particularly limited, but may be 0.1 μm or more and 5 μm or less, or 0.3 μm or more and 2 μm or less.

[0063] When forming the second primer layer 18, first, the above-mentioned materials are dispersed or dissolved in water or an appropriate solvent to prepare a coating liquid. Next, the coating liquid is applied onto the substrate 11 or the like to form a coating film. The coating film may be applied onto the substrate 11 or the like by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the second primer layer 18 is formed.

[0064] <Release layer> The release layer 15 is a layer for improving the transferability of the transfer layer 14. The release layer 15 is a layer that remains on the substrate 11 side during thermal transfer.

[0065] In one embodiment, the release layer 15 may contain a binder resin such as a (meth)acrylic resin, a urethane resin, an acetal resin, a polyamide resin, a polyester resin, a melamine resin, a polyol resin, a cellulose resin, or a silicone resin. The release layer 15 may contain a silicone resin, among the above-mentioned materials.

[0066] In one embodiment, the release layer 15 may contain a release material such as silicone oil, a phosphate ester plasticizer, a fluorine-based compound, a wax, a metal soap, or a filler.

[0067] The thickness of the release layer 15 may be 0.1 μm or more and 5 μm or less, or 0.3 μm or more and 2 μm or less.

[0068] When forming the release layer 15, first, the above-mentioned materials are dispersed or dissolved in water or an appropriate solvent to prepare a coating liquid. Next, the coating liquid is applied onto the substrate 11 to form a coating film. The coating film may be applied onto the substrate 11 by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the release layer 15 is formed.

[0069] <Release layer> The release layer 16 is a layer for improving the transferability of the transfer layer 14. The release layer 16 is a layer that is peeled off from the substrate 11 during thermal transfer and transferred to a transfer recipient together with the transfer layer 14. When the protective layer transfer sheet 10 includes the release layer 15, the release layer 16 can be provided between the release layer 15 and the protective layer 12.

[0070] In one embodiment, the release layer 16 may contain a cellulose-based resin, a vinyl-based resin, a polyurethane-based resin, a silicone-based resin, a fluorine-based resin, a fluorine-modified resin, or a wax. Examples of the wax include microcrystalline wax, carnauba wax, paraffin wax, Fischer-Tropsch wax, various low molecular weight polyethylenes, wood wax, beeswax, whale wax, ivory wax, wool wax, shellac wax, candelilla wax, petrolactam, partially modified wax, fatty acid ester, or fatty acid amide. The release layer 16 may contain a polyethylene wax, among the above-mentioned materials.

[0071] The thickness of the release layer 16 may be 0.1 μm or more and 5 μm or less, or may be 0.3 μm or more and 2 μm or less.

[0072] When forming the release layer 16, first, the above-mentioned materials are dispersed or dissolved in water or an appropriate solvent to prepare a coating liquid. Next, the coating liquid is applied onto the substrate 11 to form a coating film. The coating film may be applied onto the substrate 11 by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the release layer 16 is formed.

[0073] <Back layer> The back layer 17 serves to prevent sticking, wrinkling, and the like caused by heating during transfer.

[0074] In one embodiment, the back layer 17 may contain a binder resin. Examples of the binder resin include cellulose-based resin, styrene-based resin, vinyl-based resin, polyester-based resin, polyurethane-based resin, silicone-modified urethane-based resin, fluorine-modified urethane-based resin, and (meth)acrylic resin. From the viewpoint of preventing burn-in between the back layer 17 and a thermal head (not shown) for performing thermal transfer and from the viewpoint of preventing generation of residue during thermal transfer, the back layer 17 may contain a styrene-based resin, specifically, a styrene-acrylonitrile copolymer, among the above-mentioned materials.

[0075] In one embodiment, the back layer 17 may contain, as a binder resin, a two-component curing resin that can be cured by using an isocyanate compound, etc. Examples of such resins include polyvinyl acetal resins and polyvinyl butyral resins.

[0076] As the isocyanate compound, any conventionally known isocyanate compound may be used without any particular limitation. Among the conventionally known isocyanate compounds, an adduct of an aromatic isocyanate may be used. As the aromatic polyisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, or a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate, 1,5-naphthalene diisocyanate, tolidine diisocyanate, p-phenylene diisocyanate, trans-cyclohexane-1,4-diisocyanate, xylylene diisocyanate, triphenylmethane triisocyanate, and tris(isocyanatephenyl)thiophosphate may be mentioned, and in particular, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, or a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate may be mentioned.

[0077] In one embodiment, the back layer 17 may contain inorganic or organic fine particles. When the back layer 17 contains such fine particles, the occurrence of sticking, wrinkles, and the like due to heating during thermal transfer can be more effectively suppressed.

[0078] Examples of inorganic fine particles include clay minerals such as talc and kaolin, carbonates such as calcium carbonate and magnesium carbonate, hydroxides such as aluminum hydroxide and magnesium hydroxide, sulfates such as calcium sulfate, oxides such as silica, graphite, saltpeter, and boron nitride.

[0079] Examples of organic fine particles include organic resin fine particles made of (meth)acrylic resin, Teflon (registered trademark) resin, silicone resin, lauroyl resin, phenol resin, acetal resin, styrene resin, polyamide resin, etc., and crosslinked resin fine particles obtained by reacting these with a crosslinking agent.

[0080] The thickness of the back layer 17 may be 0.1 μm or more and 5 μm or less, or 0.3 μm or more and 2 μm or less. By setting the thickness of the back layer 17 in the above numerical range, it is possible to suppress the occurrence of sticking and wrinkles while maintaining the transferability of thermal energy during thermal transfer.

[0081] When forming the back layer 17, first, the above-mentioned materials are dispersed or dissolved in water or an appropriate solvent to prepare a coating liquid. Next, the coating liquid is applied onto the substrate 11 to form a coating film. The coating film may be applied onto the substrate 11 by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the back layer 17 is formed.

[0082] Transferred object Next, the transfer recipient 30 will be described with reference to Fig. 5. The transfer recipient 30 is a member onto which the transfer layer 14 is transferred by the protective layer transfer sheet 10.

[0083] As shown in FIG. 5, the transferred object 30 includes at least a support 31 and a receiving layer 32. In one embodiment, the transferred object 30 may further include a cushion layer 33 provided on the support 31. In one embodiment, the transferred object 30 may further include a resin layer 34 provided on the receiving layer 32. In one embodiment, the transferred object 30 may further include a barrier layer 35 provided on the support 31 or the cushion layer 33. In one embodiment, the transferred object 30 may further include a pattern layer 36 provided on the support 31 or the cushion layer 33.

[0084] Each layer constituting the transferred body 30 will now be described.

[0085] <Support> The support 31 is a layer that supports the receiving layer 32 and the like, and also enhances the strength of the entire transferred body 30. There are no particular limitations on the support 31, and any conventionally known support may be used as long as it has sufficient mechanical strength to support the receiving layer 32 and sufficient heat resistance to withstand the heat applied during thermal transfer.

[0086] As the support 31, for example, condenser paper, glassine paper, parchment paper, synthetic paper (polyolefin-based, polystyrene-based, etc.), fine paper, art paper, coated paper (RC base paper), cast coated paper, wallpaper, backing paper, synthetic resin impregnated paper, emulsion impregnated paper, synthetic rubber latex impregnated paper, synthetic resin-added paper, paperboard, cellulose fiber paper, or resin-coated paper used as a support for silver halide photographic printing paper, which is cellulose paper coated on both sides with polyethylene, may be used.

[0087] Alternatively, a film made of a polyester resin, a (meth)acrylate resin, a polycarbonate resin, a polyurethane resin, a polyimide resin, a cellulose resin, a vinyl resin, a polyolefin resin, or the like may be used as the support 31. Alternatively, a film having microvoids therein (porous film) obtained by adding a white pigment or a filler to a synthetic resin and forming the film may be used as the support 31.

[0088] Also, a laminate of any combination of the above-mentioned materials may be used as the support 31. Representative examples of the laminate include a laminate of cellulose fiber paper and synthetic paper, and a laminate of cellulose synthetic paper and plastic film. Such laminated synthetic paper may be a two-layered body, but may also be a three-layered body or a laminate of three or more layers in which synthetic paper, a plastic film, or a porous film is attached to both sides of cellulose fiber paper (used as a core material) in order to give the support 31 a feel and texture. Also, the laminate used as the support 31 may be a laminate provided with heat insulation by applying a resin layer (hollow particle layer) in which hollow particles are dispersed on the surface of coated paper, resin-coated paper, plastic film, or the like.

[0089] When the support 31 is a film made of the above-mentioned resin, the film may be a stretched film or an unstretched film. From the viewpoint of increasing strength, the resin film may be a stretched film that is uniaxially or biaxially stretched.

[0090] From the viewpoint of improving the adhesion to the receiving layer 32, the support 31 may have an uneven surface. When the uneven surface is formed on the support 31, the uneven surface can be formed by the same method as that for the base material 11 described above.

[0091] From the viewpoint of mechanical strength and heat resistance, the thickness of the support 31 may be 30 μm or more and 300 μm or less, or 50 μm or more and 200 μm or less.

[0092] <Receptive layer> The receiving layer 32 is a layer on which image information such as a face photograph, and character information such as the type of card, name, address, date of birth, and expiration date (hereinafter, these may be collectively referred to as personal information) are recorded. In addition to the image information and character information, the receiving layer 32 may be printed with a format such as a frame for the image information or fixed characters other than character information.

[0093] In one embodiment, the receiving layer 32 may contain a conventionally known resin material that easily receives a thermally transferable coloring material such as a sublimable dye or a heat-meltable ink, etc. Examples of such a resin material include polyolefin-based resins, vinyl-based resins, polyester-based resins, polystyrene-based resins, polyamide-based resins, cellulose-based resins, polycarbonate-based resins, and (meth)acrylic-based resins.

[0094] Furthermore, the dye used for recording information may be any dye known in the art. Examples of dyes include diarylmethane dyes, triarylmethane dyes, thiazole dyes, merocyanine dyes, pyrazolone dyes, methine dyes, indocyanine dyes, azomethine dyes such as acetophenone azomethine, pyrazoloazomethine, imidazole azomethine, and pyridone azomethine, xanthene dyes, oxazine dyes, cyanostyrene dyes, thiazine dyes, azine dyes, acridine dyes, benzene azo dyes, azo dyes such as pyridone azo, thiophene azo, isothiazole azo, pyrrole azo, pyrazole azo, imidazole azo, thiazole azo, triazole azo, and disazo, spiropyran dyes, indolinospiropyran dyes, fluoran dyes, rhodamine lactam dyes, naphthoquinone dyes, anthraquinone dyes, and quinophthalone dyes.

[0095] Furthermore, a post-chelate dye may be used since it can express image shading with low energy and improve image durability.

[0096] In one embodiment, the receiving layer 32 may contain a release material. By including the release material in the receiving layer 32, the releasability from the protective layer transfer sheet 10 can be improved. Examples of the release material include solid waxes such as polyethylene wax, amide wax, and Teflon (registered trademark) powder, fluorine-based or phosphate-based surfactants, silicone oil, various modified silicone oils such as reactive silicone oil and cured silicone oil, and various silicone resins. The receiving layer 32 may contain silicone oil among the above-mentioned release materials. As the silicone oil, an oily or cured silicone oil may be used. Among these, examples of the cured silicone oil include reactive cured, photocured, or catalytically cured silicone oils. In this embodiment, reactive cured or catalytically cured silicone oil may be used as the cured silicone oil.

[0097] When a post-chelating dye is used for forming an image, the receptor layer 32 may contain a metal ion-containing compound. The metal ion-containing compound is, for example, Ni 2+ , Cu 2+ , Cr 2+ , Co 2+ or Zn 2+ and salts of an aliphatic carboxylic acid such as acetic acid or stearic acid, or an aromatic carboxylic acid such as benzoic acid or salicylic acid.

[0098] In one embodiment, the receiving layer 32 may contain a pigment or filler such as titanium oxide, zinc oxide, kaolin, clay, calcium carbonate, or finely powdered silica. By containing such a pigment or filler in the receiving layer 32, the whiteness of the receiving layer 32 can be improved, thereby enhancing the clarity of the transferred image. In one embodiment, the receiving layer 32 may contain a plasticizer such as a phthalate compound, a sebacic acid ester compound, or a phosphate ester compound.

[0099] Additionally, in one embodiment, the receiving layer 32 may include additives such as plasticizers, UV stabilizers, stain inhibitors, matting agents, deodorizing agents, flame retardants, weather resistant agents, antistatic agents, yarn friction reducing agents, slip agents, release agents, antioxidants, or ion exchange agents.

[0100] The thickness of the receiving layer 32 may be 1 μm or more and 50 μm or less, or may be 2 μm or more and 10 μm or less.

[0101] When forming the receiving layer 32, first, the above-mentioned materials are dispersed or dissolved in water or an appropriate solvent to prepare a coating liquid. Next, the coating liquid is applied onto the support 31 or the like to form a coating film. The coating film may be applied onto the support 31 or the like by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the receiving layer 32 is formed.

[0102] <Cushion layer> The cushion layer 33 is a layer for improving the quality of the image formed on the receiving layer 32 .

[0103] In one embodiment, the cushion layer 33 may include a polyolefin resin, such as polyethylene, polypropylene, an ethylene-vinyl acetate copolymer, a styrene-butadiene-styrene block copolymer, a styrene-isoprene-styrene block copolymer, a styrene-ethylene-butadiene-styrene block copolymer, a styrene-hydrogenated isoprene-styrene block copolymer, or polybutadiene.

[0104] In one embodiment, the cushion layer 33 may contain an actinic radiation curable resin, which is a cured product of the actinic radiation curable resin described above. When the cushion layer 33 contains an actinic radiation curable resin, the chemical resistance of the transfer recipient 30 can be improved. In one embodiment, the cushion layer 33 may contain the polymerization initiator described above.

[0105] The thickness of the cushion layer 33 may be 3 μm or more and 50 μm or less, or may be 5 μm or more and 30 μm or less.

[0106] When forming the cushion layer 33, first, the above-mentioned materials are dispersed or dissolved in water or an appropriate solvent to prepare a coating liquid. Next, the coating liquid is applied onto the support 31 or the like to form a coating film. The coating film may be applied onto the support 31 or the like by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the cushion layer 33 is formed.

[0107] <Resin layer> The resin layer 34 plays a role in suppressing fusion between the transfer object 30 and a thermally fused coloring layer of a thermal transfer sheet, which will be described later. The resin layer 34 is also a layer for suppressing reverse transfer of the dye transferred from the thermal transfer sheet, which will be described later.

[0108] In one embodiment, the resin layer 34 may contain a polyolefin resin. In particular, the resin layer 34 may contain polyethylene or polypropylene. When the resin layer 34 contains polyethylene, the polyethylene may be ethylene acrylic modified polyethylene, urethane modified polyethylene, paraffin modified polyethylene, or low molecular weight polyethylene (weight average molecular weight 400 to 3000). The resin layer 34 may contain two or more types of polyolefin resins.

[0109] In one embodiment, the resin layer 34 may also include a polyolefin wax, such as a polyethylene wax or a polypropylene wax.

[0110] The thickness of the resin layer 34 may be 0.1 μm or more and 5 μm or less, or 0.3 μm or more and 2 μm or less.

[0111] When forming the resin layer 34, first, the above-mentioned materials are dispersed or dissolved in water or an appropriate solvent to prepare a coating liquid. Next, the coating liquid is applied onto the receiving layer 32 to form a coating film. The coating film may be applied onto the receiving layer 32 by a known means such as a roll coater, a reverse roll coater, a gravure coater, a reverse gravure coater, a bar coater, or a rod coater. Next, the coating film is dried. In this manner, the resin layer 34 is formed.

[0112] <Barrier layer> The barrier layer 35 is a layer for improving the barrier property of the transfer recipient 30. When the transfer recipient 30 includes the cushion layer 33, the barrier layer 35 may be provided on the cushion layer 33.

[0113] In one embodiment, the barrier layer 35 may contain a water-soluble resin. In this specification, the term "water-soluble resin" refers to a resin that dissolves at least 1 part by mass in 100 parts by mass of water at 25° C. under 1 atmospheric pressure. Examples of the water-soluble resin include gelatin, polyvinyl alcohol, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, polyvinyl pyrrolidone, methyl cellulose, and hydroxypropyl cellulose.

[0114] The thickness of the barrier layer 35 may be 0.5 μm or more and 10 μm or less, or may be 1 μm or more and 5 μm or less.

[0115] <Pattern layer> The design layer 36 is a layer for imparting a design. In one embodiment, the design layer 36 may contain a colorant and a binder resin.

[0116] The colorant is not particularly limited, and a conventionally known colorant may be appropriately used. Examples of the binder resin include (meth)acrylic resin, vinyl resin, polyester resin, urethane resin, cellulose resin, polyamide resin, acetal resin, polycarbonate resin, and the like. In the present embodiment, the binder resin may be a (meth)acrylic resin.

[0117] The thickness of the design layer 36 is not particularly limited, and may be 0.1 μm or more and 5 μm or less.

[0118] The design layer 36 can be formed by using a thermal transfer sheet having a thermal melt coloring layer. More specifically, the back side (the side of the substrate on which the thermal melt coloring layer is not provided) of the thermal transfer sheet having at least a substrate and a thermal melt coloring layer is heated by using a thermal head of a thermal transfer printer (not shown) to thermally transfer the thermal melt coloring layer to the transferee 30.

[0119] The transfer layer 14 can be transferred to the transfer recipient 30 as described below. First, the resin layer 34 of the transfer recipient 30 and the transfer layer 14 of the protective layer transfer sheet 10 are superposed on each other.

[0120] Next, these are laminated using a laminator (manufactured by GBC Japan, model number GL835PRO). The lamination is performed with the upper and lower roll temperatures set to 150°C, the lamination speed set to 15.07 mm / sec, and the roll nip width set to 1 mm. After lamination, the substrate 11 is peeled off from the protective layer transfer sheet 10, and the transfer layer 14 is transferred to the transferee 30 (see the dashed line in FIG. 5).

[0121] As described above, according to this embodiment, the protective layer transfer sheet 10 includes the substrate 11 and the transfer layer 14 provided on the substrate 11. The transfer layer 14 includes the protective layer 12 provided on the substrate 11 and the adhesive layer 13 provided on the protective layer 12. The critical damage load of the adhesive layer 13 is 0.012N or more and 0.035N or less. In this way, the critical damage load of the adhesive layer 13 is 0.012N or more, so that the scratch resistance and blocking resistance can be improved. The critical damage load of the adhesive layer 13 is 0.035N or less, so that the adhesion and transferability of the transfer layer 14 can be improved. That is, when the critical damage load of the adhesive layer 13 is 0.035N or less, the flexibility of the adhesive layer 13 is high. Therefore, the followability of the adhesive layer 13 to the transferee 30 is improved, and the adhesion and transferability of the transfer layer 14 to the transferee 30 can be improved. Incidentally, the fact that the above-mentioned effects can be obtained by setting the critical damage load of adhesive layer 13 to 0.012 N or more and 0.035 N or less will be explained in the examples described later. EXAMPLES

[0122] Next, a specific example of this embodiment will be described.

[0123] [Example 1] <Preparation of protective layer transfer sheet> A primer layer-forming coating solution having the following composition was applied onto a PET film having a thickness of 25 μm by gravure coating, and then dried to form a primer layer having a thickness of 0.5 μm. <Composition of Coating Solution for Forming Primer Layer> Water-based polyurethane resin (solid content 35%) 8 parts by weight (DIC Corporation, Hydran (registered trademark) AP-40N) Epoxy resin 0.3 parts by weight (DIC Corporation, Watersol (registered trademark) WSA-950) ·Water 10 parts by mass Solvent 50 parts by weight (Solmix (registered trademark) A-11, manufactured by Japan Alcohol Sales Co., Ltd.)

[0124] A release layer-forming coating solution having the following composition was applied onto the primer layer by a gravure coater and then dried to form a release layer having a thickness of 0.6 μm. <Composition of Coating Fluid for Forming Release Layer> Epoxy-containing silsesquioxane 67 parts by weight (Arakawa Chemical Industries, Ltd., Compocelan (registered trademark) SQ502-8) ·Curing catalyst 3 parts by mass (Manufactured by Daicel Corporation, Celltop (registered trademark) CAT-A) Polyester resin 3 parts by weight (Toyobo Co., Ltd., UR-3500) Toluene 100 parts by weight Methyl ethyl ketone 200 parts by weight

[0125] A coating solution for forming a protective layer having the following composition was applied onto the release layer using a gravure coater, dried, and then irradiated with ultraviolet light using a UV exposure machine (Fusion UV, F600V, LH10 lamp, H bulb, cold type reflector) under the following conditions to form a 4.5 μm thick protective layer. <Composition of Coating Solution for Forming Protective Layer> Multifunctional acrylate 20 parts by weight (NK Ester A-9300, manufactured by Shin-Nakamura Chemical Co., Ltd.) Urethane acrylate 20 parts by weight (NK Oligomer EA1020, manufactured by Shin-Nakamura Chemical Co., Ltd.) Urethane acrylate 10 parts by weight (NK Ester U-15HA, manufactured by Shin-Nakamura Chemical Co., Ltd.) Reactive binder (containing unsaturated groups) 5 parts by weight (NK Polymer C24T, manufactured by Shin-Nakamura Chemical Co., Ltd.) Filler (volume average particle size 12 nm) 40 parts by weight (Nissan Chemical Industries, Ltd., MEK-AC2140) Surfactant (acrylic surfactant) 0.1 part (Kusumoto Chemical Co., Ltd., LF-1984) Toluene 200 parts by weight Methyl ethyl ketone 200 parts by weight

[0126] A primer layer-forming coating solution having the following composition was applied onto the protective layer using a gravure coater and then dried to form a primer layer having a thickness of 0.8 μm. <Composition of Coating Solution for Forming Primer Layer> Polyester resin 3.3 parts by weight (Toyobo Co., Ltd., Vylon (registered trademark) 200) Vinyl chloride-vinyl acetate copolymer 2.7 parts by weight (Nissin Chemical Industry Co., Ltd., Solvine (registered trademark) CNL) Polyisocyanate hardener 1.5 parts by weight (Takenate (registered trademark) D110N, manufactured by Mitsui Chemicals, Inc.) Toluene 3.3 parts by weight Methyl ethyl ketone 6.7 parts by weight

[0127] On the primer layer, a coating solution for forming an adhesive layer having the following composition was applied by a gravure coater, and then dried to form an adhesive layer having a thickness of 0.6 μm, thereby obtaining a protective layer transfer sheet (polyolefin resin / (meth)acrylic resin=9 / 1). At this time, the drying temperature of the coating solution for forming an adhesive layer was set to 65° C. <Composition of Coating Fluid for Forming Adhesive Layer> Modified polyolefin resin: 20 parts by weight (Arrowbase (registered trademark) SE1030N, manufactured by Unitika Ltd.) (Meth)acrylic resin 5 parts by weight (Manufactured by Toagosei Co., Ltd., Jurimer (registered trademark) AT-510) Polyolefin resin 0.5 parts by weight (Mitsui Chemicals, Inc., Chemipearl (registered trademark) W401) ·Water 25 parts by mass 25 parts by weight of isopropyl alcohol

[0128] <Preparation of the transfer target> A cushion layer forming coating solution having the following composition was applied to one side of a white PET film having a thickness of 188 μm using a gravure coater, dried, and then exposed to a mercury lamp (300 mJ / cm 2 ) was used to irradiate the resin with active light rays, causing it to harden and form a cushion layer having a thickness of 10 μm. <Composition of the coating liquid for forming the cushion layer> Urethane acrylate oligomer 50 parts by weight (NK Oligo UA-160TM, manufactured by Shin-Nakamura Chemical Co., Ltd.) Acrylic acid ester polymer 30 parts by weight (Shin-Nakamura Chemical Co., Ltd., Vanalesin GH-5270) Urethane acrylate oligomer 18 parts by weight (NK Oligo UA-1280T, manufactured by Shin-Nakamura Chemical Co., Ltd.) Polymerization initiator: 2 parts by weight (BASF Japan, Irgacure (registered trademark) 127) Methyl ethyl ketone 100 parts by weight

[0129] Gelatin was applied to a part of the cushion layer by a gravure coater and dried to form a barrier layer having a thickness of 0.7 μm.

[0130] A coating solution for forming a receiving layer having the following composition was applied onto the barrier layer using a gravure coater and dried to form a receiving layer having a thickness of 2.45 μm. <Composition of Coating Solution for Forming Receptor Layer> Polyvinyl butyral resin 6.0 parts by weight (Sekisui Chemical Co., Ltd., S-LEC (registered trademark) BX-1) Metal ion-containing compound 4.0 parts by weight (Ni 2+ [C7H 15 COC(COOCH3)=C(CH3)O - ]2) Methyl ethyl ketone 80 parts by weight n-Butyl acetate 10 parts by weight

[0131] A resin layer-forming coating solution having the following composition was applied onto the receiving layer using a gravure coater and dried to form a resin layer having a thickness of 0.4 μm, thereby obtaining a transfer recipient. <Composition of Coating Solution for Forming Resin Layer> Polypropylene wax emulsion (30% solids) 33 parts by weight (Toho Chemical Industry Co., Ltd., Hi-Tec E433N) ·Water 67 parts by mass

[0132] <Evaluation of protective layer transfer sheet> <<Critical damage load measurement>> First, the critical damage load of the adhesive layer was measured. At this time, the critical damage load of the adhesive layer was measured by a microscratch method in accordance with JIS-R-3255:1997. During the measurement, the protective layer transfer sheet was placed on the glass so that the base material of the protective layer transfer sheet faced the glass. During the measurement, a needle with a curvature radius R of 50 μm was used as the measuring needle. Then, the measuring needle was moved in a horizontal direction relative to the surface of the protective layer. The moving speed of the measuring needle was set to 5 μm / s. The load W applied to the measuring needle was increased in proportion to time from 0 mN to 40 mN over 60 seconds. Then, the load when interfacial peeling began to occur at the interface between the adhesive layer and the protective layer was taken as the critical damage load of the adhesive layer.

[0133] <<Transferability evaluation>> Next, the transferability of the transfer layer to the receiving body was evaluated.

[0134] At this time, a transfer layer (protective layer+primer layer+adhesive layer) was transferred onto the resin layer of the transfer recipient using the protective layer transfer sheet of Example 1 under the following conditions.

[0135] When transferring the transfer layer onto the resin layer of the transferee, first, the resin layer of the transferee and the transfer layer of the protective layer transfer sheet were superimposed. Next, the transferee and the protective layer transfer sheet were laminated using a laminator (manufactured by Japan GBC Co., Ltd., model number GL835PRO). At this time, the upper and lower roll temperatures of the laminator were set to 150°C, the lamination speed was set to 15.07 mm / sec, and the roll nip width was set to 1 mm. Next, the substrate was peeled off from the protective layer transfer sheet. In this way, the transfer layer was transferred to the transferee.

[0136] The transferability of the transfer layer transferred to the transfer receiving material was evaluated based on the following evaluation criteria. (Evaluation Criteria) A: There was no area where the transfer had not occurred (hereinafter referred to as the untransferred area), or the length of the untransferred area was less than 0.5 mm from the transfer start end of the protective layer transfer sheet. B: The length of the untransferred portion was 0.5 mm or more and less than 1.0 mm from the transfer start end of the protective layer transfer sheet. C: The length of the untransferred portion was 1.0 mm or more from the transfer start end of the protective layer transfer sheet.

[0137] <<Blocking resistance evaluation>> The blocking resistance of the protective layer transfer sheet thus prepared was evaluated based on the following evaluation criteria: First, the protective layer transfer sheet was cut into pieces measuring 5 cm x 5 cm to prepare two samples each.

[0138] Next, the two samples were laminated together so that the adhesive layer of one was in contact with the substrate of the other.

[0139] Next, the overlapping samples were heated in an oven for 48 hours at a temperature of 45°C and a humidity of 85% RH while applying a load of 1.47 MPa to the overlapping samples. After heating, the two samples were peeled off by hand and the blocking resistance was evaluated. (Evaluation Criteria) A: The samples could be easily peeled off from each other. B: The samples could be peeled off from each other, but some resistance was encountered. C: The samples were firmly attached to each other and it was difficult to peel them off (including cases where they could not be peeled off at all).

[0140] [Example 2] The protective layer transfer sheet was evaluated in the same manner as in Example 1, except that the drying temperature of the adhesive layer-forming coating liquid was 70°C.

[0141] [Example 3] The protective layer transfer sheet was evaluated in the same manner as in Example 1, except that the drying temperature of the adhesive layer-forming coating liquid was 80°C.

[0142] [Example 4] The protective layer transfer sheet was evaluated in the same manner as in Example 1, except that the drying temperature of the adhesive layer-forming coating liquid was 90°C.

[0143] [Example 5] The protective layer transfer sheet was evaluated in the same manner as in Example 1, except that the drying temperature of the adhesive layer-forming coating liquid was 100°C.

[0144] [Example 6] The protective layer transfer sheet was evaluated in the same manner as in Example 1, except that the drying temperature of the adhesive layer-forming coating liquid was 105°C.

[0145] [Comparative Example 1] The protective layer transfer sheet was evaluated in the same manner as in Example 1, except that the drying temperature of the adhesive layer-forming coating liquid was 60°C.

[0146] [Comparative Example 2] The protective layer transfer sheet was evaluated in the same manner as in Example 1, except that the drying temperature of the adhesive layer-forming coating liquid was 110°C.

[0147] The above results are shown in Table 1.

[0148] [Table 1]

[0149] As a result, as shown in Table 1, the protective layer transfer sheets according to Examples 1 to 6 were able to maintain the desired performance in both transferability and blocking resistance. In particular, it was found that the protective layer transfer sheets according to Examples 1 to 3 could maintain the desired performance in blocking resistance while maintaining particularly excellent performance in transferability by setting the critical damage load of the adhesive layer to 0.0181 N or less. In addition, it was found that the protective layer transfer sheets according to Examples 4 to 6 could maintain the desired performance in transferability while maintaining particularly excellent performance in blocking resistance by setting the critical damage load of the adhesive layer to 0.0250 N or more. Furthermore, it was found that the protective layer transfer sheet according to Example 3 could maintain particularly excellent performance in transferability and blocking resistance by setting the critical damage load of the adhesive layer to 0.0181 N. Thus, it was found that the protective layer transfer sheet according to this embodiment could maintain the desired performance in both transferability and blocking resistance by setting the critical damage load of the adhesive layer to 0.012 N or more and 0.035 N or less.

[0150] The present disclosure is not limited to the above-mentioned embodiment and each modification, and the components can be modified and embodied in the implementation stage without departing from the gist of the present disclosure. In addition, various inventions can be formed by appropriate combinations of multiple components disclosed in the above-mentioned embodiment and each modification. Some components may be deleted from all the components shown in the embodiment and each modification. [Explanation of symbols]

[0151] 10: Protective layer transfer sheet 11: Base material 12:Protective layer 13: Adhesive layer 14: Transfer layer 15: Release layer 16: Release layer 17: Back layer 18: Second primer layer 20: Sample 21: Air cylinder 22: Air cylinder rod 23: Sample fixing device 24: Cellophane tape 25: Digital force gauge 30: Transferee 31:Support 32: Receptive layer 33: Cushion layer 34: Resin layer 35: Barrier layer 36: Picture layer

Claims

1. A substrate; A transfer layer provided on the substrate, The transfer layer is A protective layer provided on the substrate; an adhesive layer provided on the protective layer, A protective layer transfer sheet, wherein the critical damage load of the adhesive layer is 0.012 N or more and 0.035 N or less.

2. The protective layer transfer sheet according to claim 1 , further comprising a release layer or peeling layer provided between the substrate and the transfer layer.

3. The protective layer transfer sheet according to claim 1 , wherein the transfer layer further comprises a primer layer provided between the protective layer and the adhesive layer.

Citation Information

Patent Citations

  • Image forming method, combination of thermal transfer sheet and thermal transfer image receiving sheet

    JP2013075480A

  • Image forming method, combination of thermal transfer sheet and thermal transfer image receiving sheet

    JP2013082212A

  • Thermal transfer sheet with protective layer

    JP2015085554A