Lithium ion secondary battery

By maintaining an aspect ratio of 5.3 or more between negative electrode active materials and voids in the mixture layer, the battery prevents conductive path breakage, thereby suppressing capacity deterioration.

JP2024166929AInactive Publication Date: 2024-11-29TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023083365
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The alignment of negative electrode active materials in the same direction during charging and discharging leads to broken conductive paths due to expansion and contraction, causing capacity deterioration in lithium ion secondary batteries.

Method used

The aspect ratio of the negative electrode active material to voids in the negative electrode mixture layer is maintained at 5.3 or more, allowing the active materials to rearrange and maintain contact during expansion, thereby preventing conductive path breakage.

Benefits of technology

This configuration suppresses capacity deterioration by ensuring continuous contact between negative electrode active materials, thus maintaining battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166929000001_ABST
    Figure 2024166929000001_ABST
Patent Text Reader

Abstract

To provide a lithium ion secondary battery in which capacity deterioration can be suppressed.SOLUTION: A lithium ion secondary battery of the present disclosure has a negative electrode mixture layer 10 including negative electrode active materials 20. A ratio of an aspect ratio of the negative electrode active materials 20 to an aspect ratio of a gap 21 existing in the negative electrode mixture layer 10 is 5.3 or more. The negative electrode mixture layer 10 can keep contact between the negative electrode active materials 20 even when the negative electrode mixture layer is expanded, and cutting of a conductive path and isolation of the negative electrode active materials 20 can be suppressed. Thereby, the lithium ion secondary battery of the present disclosure can suppress reduction in capacity-keeping rate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to lithium-ion secondary batteries. [Background technology]

[0002] In a lithium ion secondary battery, lithium ions move within the negative electrode mixture layer during charging and discharging. Patent Document 1 discloses a technology for improving the capacity retention rate of a lithium-ion secondary battery by providing voids with a Z-tensor value of 0.33 or more in a negative electrode mixture layer to promote the movement of lithium ions. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2022-074139 A Summary of the Invention [Problem to be solved by the invention]

[0004] The inventors have found the following problems with lithium ion secondary batteries. When a secondary battery is charged and discharged, the negative electrode active material expands and contracts. If the negative electrode active material in the negative electrode mixture layer is aligned, the expansion and contraction of the negative electrode active material may cause a break in the conductive path between the negative electrode active materials. Therefore, repeated charging and discharging may cause capacity degradation.

[0005] The present disclosure has been made in consideration of such problems, and has an object to provide a lithium-ion secondary battery capable of suppressing capacity degradation. [Means for solving the problem]

[0006] One aspect of achieving the above object is to A lithium ion secondary battery having a negative electrode mixture layer containing a negative electrode active material, The ratio of the aspect ratio of the negative electrode active material to the aspect ratio of voids present in the negative electrode mixture layer is 5.3 or more. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a lithium ion secondary battery capable of suppressing capacity degradation. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a partially enlarged cross-sectional view of a negative electrode mixture layer according to an embodiment. [Diagram 2] FIG. 4 is a partially enlarged cross-sectional view of the negative electrode mixture layer according to the embodiment after application of the negative electrode paste. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. However, the present disclosure is not limited to the following embodiments. In addition, the following description and drawings are appropriately simplified for clarity of explanation.

[0010] The configuration of a lithium ion secondary battery according to an embodiment will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view of a negative electrode mixture layer (negative electrode mixture layer according to an embodiment) of a lithium ion secondary battery according to an embodiment. The lithium ion secondary battery according to an embodiment has a positive electrode mixture layer, a separator, and an electrolyte, which are not shown, in addition to the negative electrode mixture layer 10 shown in Fig. 1.

[0011] The positive electrode mixture layer is a positive electrode sheet produced by applying a positive electrode paste onto a positive electrode current collector, followed by drying and rolling. The positive electrode current collector is, for example, an aluminum foil. The positive electrode paste is produced by kneading a positive electrode active material, an additive, and a solvent. The positive electrode active material is, for example, a lithium transition metal oxide or a lithium transition metal phosphate compound. The lithium transition metal oxide is, for example, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 , LiNiO2 , LiCoO 2 , LiFeO 2 , LiMn 2 O 4 , LiNi 0.5 Mn 1.5 O 4 Lithium transition metal phosphate compounds include, for example, LiFePO 4 The additives are, for example, a binder and a conductive agent. The binder is, for example, polyvinylidene fluoride (PVDF). The conductive material is, for example, carbon black such as acetylene black and other carbon materials such as graphite.

[0012] The separator separates the positive electrode mixture layer and the negative electrode mixture layer 10. The separator is a porous sheet containing a resin such as polyethylene, polypropylene, polyester, cellulose, polyamide, etc. The separator may have a single layer structure or a laminated structure of two or more layers. For example, the separator may have a three-layer structure in which polypropylene layers are laminated on both sides of a polyethylene layer. A heat-resistant layer or the like may be provided on the surface of the separator.

[0013] The electrolyte is a non-aqueous electrolyte in which a supporting electrolyte is dissolved in a non-aqueous solvent. The non-aqueous solvent is, for example, an organic solvent such as carbonates, ethers, esters, nitriles, sulfones, lactones, etc., and is preferably an organic solvent of carbonates. The organic solvent of carbonates is, for example, ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, etc. The non-aqueous solvent may be used alone or in combination of two or more. The supporting electrolyte is, for example, LiPF 6 , LiBF 4 The supporting electrolyte is a lithium salt such as lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethane)sulfonimide (LiTFSI), etc. One type of supporting electrolyte may be used alone, or two or more types may be used in combination.

[0014] The negative electrode mixture layer 10 is a negative electrode sheet produced by applying a negative electrode paste onto a negative electrode current collector, followed by drying and rolling. The negative electrode current collector is, for example, copper foil. The negative electrode paste is produced by kneading a negative electrode active material, an additive, and a solvent. The additive includes at least a void-generating additive, and may further include other additives such as a binder and a thickener. The void-generating additive 30 is a material that dissolves in the negative electrode mixture layer 10 and does not affect the cell performance even if it dissolves. The void-generating additive 30 is, for example, PVDF. The binder is, for example, styrene-butadiene rubber (SBR) and modified products thereof, acrylonitrile-butadiene rubber and modified products thereof, acrylic rubber and modified products thereof, fluororubber, etc., and is preferably SBR. Examples of the thickener include cellulose polymers such as carboxymethyl cellulose (CMC), methyl cellulose, cellulose acetate phthalate, and hydroxypropyl methyl cellulose, and polyvinyl alcohol, and preferably CMC.

[0015] FIG. 1 is a partially enlarged cross-sectional view of a negative electrode mixture layer 10 according to an embodiment. As shown in FIG. 1, the negative electrode mixture layer 10 includes a negative electrode active material 20. The negative electrode active material 20 is, for example, flake graphite. The negative electrode active material 20 preferably has an aspect ratio of 8 or more. The negative electrode mixture layer 10 has voids 21. The voids 21 are voids provided between the negative electrode active materials 20. The ratio of the aspect ratio of the voids 21 to the aspect ratio of the negative electrode active material 20 is 5.3 or more. The aspect ratio of the voids 21 is calculated, for example, by observing a cross section of the negative electrode mixture layer 10 with a scanning electron microscope (SEM). Specifically, the aspect ratio of the void 21 is calculated by binarizing the cross-sectional image of the negative electrode mixture layer 10 by image analysis, and calculating the ratio of the longest section A to the shortest section B among the distances between the points where the negative electrode active materials 20 constituting the peripheral walls of the void 21 contact each other.

[0016] As shown in FIG. 1, when the ratio of the aspect ratio of the negative electrode active material 20 to the aspect ratio of the void 21 is 5.3 or more, the negative electrode mixture layer 10 includes an elongated negative electrode active material 20 and a round void 21. Since the aspect ratio of the negative electrode active material 20 to the aspect ratio of the void 21 is 5.3 or more in the negative electrode mixture layer 10, when the negative electrode mixture layer 10 expands due to charging of the lithium ion secondary battery, the negative electrode active material 20 is rearranged and gathers in the void 21. Therefore, the negative electrode mixture layer 10 can maintain contact between the negative electrode active materials 20 even when expanding, and can suppress disconnection of the conductive path and isolation of the negative electrode active material 20. As a result, the lithium ion secondary battery according to the embodiment can suppress a decrease in the capacity retention rate.

[0017] Next, a method for producing the negative electrode mixture layer of the lithium ion secondary battery according to the embodiment will be described with reference to Fig. 2. The negative electrode mixture layer 10 is produced by applying a negative electrode paste onto a negative electrode current collector, followed by drying and rolling. Fig. 2 is a partially enlarged cross-sectional view of the negative electrode mixture layer 10 after the negative electrode paste has been applied and before drying. The negative electrode paste contains a negative electrode active material 20 and a void generating additive 30. From the viewpoint of being able to generate round voids 21, the void generating additive 30 preferably has an aspect ratio of 1.35 or less.

[0018] The present disclosure is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit and scope of the present disclosure. EXAMPLES

[0019] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited to these examples.

[0020] <Preparation of negative electrode sheet> A negative electrode material, a binder, a thickener, and a void-generating additive were mixed with ion-exchanged water in a mass ratio of graphite particles in the negative electrode material: binder: thickener: void-generating additive = 99-a: 0.5: 0.5: a to prepare a negative electrode paste. Natural graphite was used as the negative electrode material. Styrene-butadiene rubber (SBR) was used as the binder. Carboxymethyl cellulose (CMC) was used as the thickener. Granular PVDF was used as the void-generating additive. The negative electrode paste was applied to both sides of a long negative electrode current collector with a thickness of 10 μm, dried, and pressed to a predetermined thickness to produce a negative electrode sheet having a negative electrode active material layer on both sides of the negative electrode current collector. Copper foil was used as the negative electrode current collector. After the negative electrode sheet was prepared, the void-generating additive was dissolved to obtain the negative electrode sheets of Examples 1 to 4 and Comparative Examples 2 and 3. Also, a negative electrode sheet was prepared without adding the void-generating additive to obtain the negative electrode sheet of Comparative Example 3. The aspect ratios of the void-generating additives in each Example and Comparative Example are shown in Table 1.

[0021] <Preparation of lithium-ion secondary battery for evaluation> A lithium ion secondary battery for evaluation was produced using the produced negative electrode sheet. Specifically, the positive electrode active material, the conductive material, and the binder were put into a kneader in a mass ratio of positive electrode active material:conductive material:binder=92:5:3, and kneaded while adjusting the viscosity with N-methyl-2-pyrrolidone to prepare a positive electrode paste. 1 / 3 Mn 1 / 3 Co 1 / 3 O 2 The conductive material was acetylene black. The binder was PVDF. The positive electrode paste was applied to both sides of a long positive electrode collector having a thickness of 15 μm, dried, and pressed to a predetermined thickness to produce a positive electrode sheet having a positive electrode active material layer on both sides of the positive electrode collector. Aluminum foil was used as the positive electrode collector.

[0022] Next, a separator was prepared in which a 4 μm thick heat-resistant layer was provided on one side of a 24 μm thick resin porous membrane having a three-layer structure in which a polypropylene layer was laminated on both sides of a polyethylene layer. A positive electrode sheet, a negative electrode sheet, and two separators were laminated and wound, and then pressed from the side direction to produce a flat wound electrode body. Next, a positive electrode terminal and a negative electrode terminal connected to a case lid were welded to the wound electrode body, and the wound electrode body was inserted into a square battery case body having a liquid injection hole. Then, the case lid and the battery case body were welded and sealed.

[0023] Next, a non-aqueous electrolyte was injected through the injection hole of the battery case, and the injection hole was sealed airtight by tightening a sealing screw. 6 was dissolved at a concentration of 1.0 mol / L. In this manner, lithium ion secondary batteries for evaluation of each of the examples and comparative examples were obtained.

[0024] <Activation process> The lithium-ion secondary batteries for evaluation were placed in an environment of 25° C. The activation process, i.e., the initial charging, was performed using a constant current-constant voltage method, and each lithium-ion secondary battery for evaluation was charged at a constant current of 1 / 3 C up to 4.2 V, and then charged at a constant voltage until the current reached 1 / 50 C, until the battery was fully charged. After that, each lithium-ion secondary battery for evaluation was discharged at a constant current of 1 / 3 C up to 3.0 V.

[0025] <Initial characteristics> The initial capacity was measured in an environment of 25° C. Specifically, each evaluation lithium-ion secondary battery that had been subjected to activation treatment was charged at a constant current at a rate of 1 / 3 C until the voltage reached 4.1 V, and then charged at a constant voltage until the current value reached 0.02 C. Next, the battery was discharged at a constant current at a rate of 1 / 3 C until the voltage reached 3 V, and the CC discharge capacity at this time was taken as the initial capacity.

[0026] <Cycle test> In an environment of 25°C, 200 charge / discharge cycles were performed at a current value of 0.5C and a charge rate (State Of Charge, SOC) of 0-100%. The capacity was then measured. The capacity retention rate was calculated by dividing the capacity measured in the cycle test by the initial capacity. The calculated results are shown in Table 1.

[0027] [Table 1]

[0028] As shown in Table 1, the evaluation lithium ion secondary batteries of Examples 1-4 maintained their capacity compared to the evaluation lithium ion secondary batteries of Comparative Examples 1-3. [Explanation of symbols]

[0029] 10 Negative electrode mixture layer 20 Negative electrode active material 21 void 30. Additives for creating voids

Claims

[Claim 1] A lithium ion secondary battery having a negative electrode mixture layer containing a negative electrode active material, a ratio of an aspect ratio of the negative electrode active material to an aspect ratio of voids present in the negative electrode mixture layer is 5.3 or more; Lithium-ion secondary battery.

Citation Information

Patent Citations

  • Negative electrode active material, method of manufacturing negative electrode, negative electrode, and secondary battery

    JP2012119079A

  • Negative electrode for lithium-ion secondary battery and lithium-ion secondary battery

    JP2015018663A

  • Negative electrode active material, manufacturing method thereof, and battery

    JP2021022554A

  • Negative electrode active material for lithium ion secondary cell, method for manufacturing negative electrode active material for lithium ion secondary cell, and lithium ion secondary cell

    WO2015068195A1

  • Anode for lithium ion secondary battery, method for preparing the same, and lithium ion secondary battery comprising the same