Heat insulating material

The heat insulating material with inorganic fine particles, fireproof fibers, and infrared scattering material addresses the challenge of maintaining high insulation and flexibility, offering excellent thermal performance and flexibility for curved surfaces under compressive stress.

JP2024167644AInactive Publication Date: 2024-12-04ISOLITE INSULATING PROD CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023083858
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional heat insulating materials struggle to maintain high heat insulation properties while providing flexibility, especially under compressive stress, and often suffer from plastic deformation or loss of insulation due to thermal decomposition or limited bending capability.

Method used

A heat insulating material composed of inorganic fine particles, fireproof fibers, and infrared scattering material, with the fibers oriented perpendicular to the thickness direction, achieving a bulk density of 200-500 kg/m³ and a bending strength of 15 mm or more, ensuring flexibility and high heat resistance.

Benefits of technology

The material maintains excellent heat insulating properties with a thermal conductivity of 0.05 W/(m·K) or less at 600°C, heat resistance up to 1200°C, and flexibility allowing deformation without breaking, suitable for curved surfaces and compressive stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167644000001_ABST
    Figure 2024167644000001_ABST
Patent Text Reader

Abstract

To provide a heat insulating material having appropriate flexibility in addition to a desired heat insulating property.SOLUTION: The heat insulating material is composed of a molded body in which inorganic fine particles 1 of a metal oxide, a fireproof fiber 2, an infrared scattering material 3, and a fused organic fiber 4 are mixed as main materials, wherein the molded body has the fireproof fiber 2 and the organic fiber 4 randomly oriented in a direction perpendicular to a thickness direction of the molded body, a bulk density is in a range of 200 kg / m3 or more and 500 kg / m3 or less, a deflection amount at breaking when the bending strength of a test piece formed in a thickness of 5 mm is measured in a span of 100 mm, is 15 mm or more, and a heat resistant temperature is preferably 1,000°C or more and 1,200°C or less, and a heat transfer coefficient at 600°C is 0.05 W / (m K) or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermal insulation material having both excellent thermal insulation properties and flexibility. [Background technology]

[0002] Some industrial equipment and electronic devices have a heat source, generate heat during operation, and are installed in a limited, narrow space. Insulation materials used for the insulation of industrial equipment and electronic devices used under such specific conditions are often required to not only meet the required insulation and heat resistance requirements with a thickness of, for example, several mm, but also to have flexibility that allows them to deform freely in response to compressive stress caused by thermal expansion.

[0003] For example, among secondary batteries that can be used repeatedly by charging, lithium-ion secondary batteries have been widely used in recent years as driving power sources for electric vehicles and hybrid cars, and as storage batteries for industrial and domestic use because they have a high energy density and can be made small. These batteries are often used in a stacked state of multiple battery cells, but because each battery cell generates heat as it is charged and discharged, it is necessary to provide a heat insulating material in the gap of about several millimeters between adjacent battery cells. In addition, because the exterior can of the battery cell repeatedly expands and contracts as it is heated and cooled during charging and discharging, the heat insulating material must be flexible enough to deform in response to this.

[0004] Furthermore, in lithium-ion secondary batteries, the temperature of the battery cells may rise excessively due to oxidative decomposition of the electrolyte caused by overcharging or other factors, or due to a short circuit caused by mechanical factors. If this excessive temperature rise in a battery cell is linked to other battery cells, it may lead to thermal runaway, eventually resulting in fire and a temperature rise of approximately 1000°C. Therefore, the insulating material is required to have heat insulation properties that can prevent the excessive temperature rise in a battery cell from being linked to adjacent battery cells, and heat resistance at temperatures of approximately 1000°C that may occur during the above-mentioned fire.

[0005] As described above, insulating materials used for insulating industrial equipment such as secondary batteries are required to have a desired insulating property as well as a suitable degree of flexibility, and various insulating materials that satisfy these conditions have been proposed. For example, Patent Document 1 proposes an insulating material that is preferably composed of an insulating part made of a porous body and a buffer part made of a fibrous body, an elastomer molded body, or a metal spring that is more easily compressed and deformed than the insulating part. It is described that this insulating material is suitable for use under conditions where compressive stress is applied, such as between adjacent battery cells.

[0006] Patent Document 2 proposes a technique for providing a flexible insulating material that can be bent along the outside when used as an insulating material for a tubular tube, for example. It is described that this insulating material is produced by preparing a mixture by suspending fumed silica and silicon carbide, which are low thermal conductivity materials, in a solvent such as hexane, and then filling the mixture into a textile fabric layer of an insulating fabric and then removing the solvent.

[0007] Patent Document 3 proposes a technology that uses an inorganic hydrate, such as aluminum hydroxide, as an insulating material, which exhibits a heat absorbing effect by releasing water of crystallization through thermal decomposition. It is described that by interposing this insulating material between adjacent battery cells, the inorganic hydrate is thermally decomposed by heat generated by thermal runaway of the battery cells, releasing the water of crystallization, thereby exhibiting a heat absorbing effect. Furthermore, it is described that this insulating material can exhibit a sustained insulating effect due to the porous structure formed after the release of the water of crystallization, and therefore it is possible to suppress the spread of thermal runaway from one battery cell to the other battery cell.

[0008] Patent Document 4 proposes a flexible composite insulation material consisting of a molded body of a low thermal conductivity material mainly composed of nanoparticles and a reinforcing material bonded to at least one surface of the molded body. It is described that this composite insulation material has both compressive strength that does not break under compressive pressure caused by thermal expansion and excellent insulation properties, and will not break even if bent when insulating containers with curved surfaces. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2021-140968 A [Patent Document 2] Special Publication No. 2022-508727 [Patent Document 3] JP 2020-119840 A [Patent Document 4] JP 2016-205728 A Summary of the Invention [Problem to be solved by the invention]

[0010] It is believed that the adoption of the technologies of Patent Documents 1 to 4 above makes it possible to provide a heat insulating material with desired heat insulating properties and appropriate flexibility, but in order for the heat insulating material of Patent Document 1 to be able to flexibly and elastically deform even when further compressive stress is applied under a constrained state in which a certain degree of high compressive stress is applied, it is necessary to increase the volume ratio of the buffer part in the heat insulating material. This makes it difficult to maintain high heat insulating properties because the volume ratio of the heat insulating part in the heat insulating material becomes relatively small.

[0011] In the heat insulating material of Patent Document 2, the blanket has a bulk density of 110 to 220 kg / m in the examples in order to maintain flexibility. 3 Therefore, it is thought that when compressive stress is applied to the insulation material, plastic deformation occurs. In this case, after the compressive stress is reduced, voids remain in the plastically deformed part, which reduces the insulation properties.

[0012] In the heat insulating material of Patent Document 3, the water of crystallization is thought to disappear within a few minutes to a few tens of minutes after thermal decomposition, depending on the amount of water of crystallization contained in the inorganic hydrate. Therefore, it is thought to be difficult to maintain the initial heat insulating property multiple times.

[0013] The heat insulating material of Patent Document 4 has a small bending deflection of about 14 to 15 mm at a span of 600 mm in the examples, and therefore, when applied to curved surfaces, it is limited to those with a curvature radius of about 1500 mm or more.

[0014] The present invention has been made in consideration of the problems associated with the conventional insulating materials described above, and aims to provide an insulating material that has appropriate flexibility in addition to the desired insulating properties. [Means for solving the problem]

[0015] In order to achieve the above object, the heat insulating material of the present invention is a molded body in which inorganic fine particles of a metal oxide as a main material, refractory fibers, an infrared scattering material, and fused organic fibers are mixed, and the molded body has a bulk density of 200 kg / m, in which the refractory fibers and organic fibers are randomly oriented in a direction perpendicular to the thickness direction of the molded body. 3 More than 500kg / m 3 The material is characterized by being within the range below, and when a test piece molded to a thickness of 5 mm is subjected to bending strength testing over a span of 100 mm, the deflection at break is 15 mm or more. Effect of the Invention

[0016] According to the present invention, it is possible to provide a thermal insulation material having both desired thermal insulation properties and appropriate flexibility. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic longitudinal sectional view of one specific example of a heat insulating material of the present invention. [Diagram 2] FIG. 1 is a vertical cross-sectional view showing one specific example of an apparatus for producing a heat insulating material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the heat insulating material according to the present invention will be described. As shown in FIG. 1, the heat insulating material according to the embodiment of the present invention is mainly made of inorganic fine particles 1 made of inorganic oxides such as silica and alumina, and is preferably made of a sheet-like molded body in which the inorganic fine particles 1 as the main material are mixed with refractory fibers 2, infrared scattering materials 3, and organic fibers 4 fused to the surrounding materials. Of these materials, the refractory fibers 2 and the organic fibers 4 are both randomly oriented in a direction approximately perpendicular to the thickness direction of the molded body. In other words, the rod-like refractory fibers 2 and the organic fibers 4 constituting the sheet-like heat insulating material are both extended approximately parallel to the sheet surface.

[0019] The characteristic form in which the fireproof fiber 2 and the organic fiber 4 extend almost parallel to the sheet surface is obtained by blowing an air flow from a horizontal direction onto the freely falling raw material mixture to disperse it in the stage of forming a laminate from the raw material mixture, as described later. The fused organic fiber 4 is obtained by heating and compressing it in the stage of forming a molded body, as described later. In this way, by fusing the organic fiber 4 to at least the inorganic fine particles 1 present in the periphery, the organic fiber 4 can play the role of a binder. Since the heat insulating material of the embodiment of the present invention has the above-mentioned characteristic form, the deflection amount that can be bent without breaking is larger than that of conventional ones, and the compression characteristics are also excellent. Furthermore, by containing the infrared scattering material 3 and the fireproof fiber 2, it has high heat insulating properties.

[0020] Specifically, the heat insulating material according to the embodiment of the present invention has a thermal insulation property with a thermal conductivity of 0.05 W / (m·K) or less at 600°C, which effectively reduces the amount of heat dissipated from the object to be insulated and reduces the amount of thermal energy consumed. In addition, since the heat resistance is 1000°C or more and 1200°C or less, the desired heat insulating property can be maintained for an extremely long period of time when the normal use temperature is 1000°C, and heat resistance can be ensured even in the event of fire.

[0021] Furthermore, the insulating material according to the embodiment of the present invention has excellent flexibility, with a deflection of 15 mm or more at break when a bending strength measurement was performed on a sample piece molded to a thickness of 5 mm with a span of 100 mm, so that it can be applied to a curved surface with a curvature radius of about 80 mm without breaking. Furthermore, even if the area where the insulating material is applied experiences localized thermal expansion, the insulating material can be freely deformed in response to compressive stress, and can return to its original shape when the compressive stress is eliminated by cooling, so that it can be used as a cushioning material without compromising its insulating properties even in narrow spaces such as between stacked battery cells.

[0022] Next, each material constituting the heat insulating material of the embodiment of the present invention will be specifically described. The inorganic fine particles are made of a metal oxide having a heat resistance at a high temperature of about 1000 to 1200°C. For this metal oxide, it is preferable to use silica, alumina, zirconia, or one or more of these. The heat resistance temperature of silica is about 1000°C, but by using alumina instead of or in addition to silica, the heat resistance temperature can be increased to about 1200°C, so that it can be used for a very long period of time when the normal use temperature is 1000°C. The average particle diameter of the inorganic fine particles is preferably 0.5 μm or less. This makes it possible to keep the size of the void between the inorganic fine particles and the refractory fiber or infrared scattering material small, and to suppress the convection heat transfer of gas at high temperatures. In addition, in this specification, the average particle diameter is the 50% diameter (D50) based on volume measured by a laser diffraction type particle size distribution measuring device.

[0023] The refractory fiber is a fiber made of an inorganic composition having a heat resistance temperature of about 600 to 1600°C. Representative refractory fibers include, but are not limited to, short glass fibers, long glass fibers, alumina fibers, mullite fibers, zirconia fibers, silica-alumina fibers, and AES (alkaline earth silicate) fibers. It is preferable to use one or more fibers selected from the group consisting of these fibers. The average fiber diameter of this refractory fiber is preferably 1 μm to 13 μm, more preferably 2 μm to 10 μm. In this specification, the average fiber diameter is obtained by photographing a fiber group to be measured with an electron microscope, measuring the width direction distance of 200 or more fibers selected arbitrarily from the obtained image, and calculating the arithmetic average of these.

[0024] The fire-resistant fiber may contain non-fiber particles of the same material. In this case, the content of the non-fiber particles is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, based on 100 parts by mass of the fire-resistant fiber. In particular, the content of the non-fiber particles having an average particle size of 425 μm or more is preferably 3 parts by mass or less, more preferably 1 part by mass or less.

[0025] The infrared scattering material is not particularly limited as long as it has a heat resistance of 800°C or more and is made of a composition capable of reducing heat transfer by radiation, but infrared reflectivity is preferable. Examples of such compositions include silicon carbide, titanium dioxide, zirconium silicate, etc., and it is preferable to use one or more selected from the group consisting of these compositions. In addition, the above-mentioned infrared scattering material preferably has an average particle size of 0.1 μm to 3.0 μm, and in particular, the upper limit is more preferably 2.0 μm or less, which is an average particle size equivalent to the peak wavelength at 1200°C of infrared rays that cause radiative heat transfer.

[0026] The organic fiber is preferably a material that melts at 150°C or less. Such organic fiber is not particularly limited, but it is preferable to use one or more selected from the group consisting of polyester, polyvinyl alcohol, polyethylene, and polypropylene. In particular, a polyethylene / polypropylene core-sheath structure fiber is preferable because the core part remains even after melting, and higher flexibility can be obtained. The core-sheath structure fiber is a fiber having a double structure of a core part made of polypropylene and a sheath part made of polyethylene that surrounds the core part in a substantially concentric axial shape. The fiber has a length L (unit: m) and weight W (unit: g) measured and the fiber thickness scale T (dtex) obtained by substituting these values ​​into "T = (10000 x W) / L)" is preferably in the range of 0.15 to 20 dtex, and the fiber length measured by an electron microscope is preferably in the range of 3 to 20 mm.

[0027] In the heat insulating material according to the embodiment of the present invention, the mixing ratio (content) of the above-mentioned materials is appropriately adjusted so as to obtain the desired characteristics as a heat insulating material, taking into consideration the action and effect of each of the above-mentioned materials. Specifically, the preferred contents of the above-mentioned materials constituting the heat insulating material according to the embodiment of the present invention are 40 to 82 mass% for inorganic fine particles, 5 to 40 mass% for fire-resistant fibers, 8 to 20 mass% for infrared scattering materials, and 3 to 40 mass% for organic fibers. In addition, it is preferable that these materials are contained in a total amount of 98 mass% or more, and inevitable impurities and molding aids may be contained.

[0028] In addition, the heat insulating material according to the embodiment of the present invention has a bulk density of 200 kg / m 3 More than 500kg / m 3 Within the range below, 250kg / m 3 More than 350kg / m 3 It is preferable that the bulk density is within the range below. This makes it possible to provide a thermal insulation material that has both compressive strength that is not easily damaged by compressive stress due to thermal expansion and excellent thermal insulation properties. 3 If the bulk density is less than 500 kg / m, sufficient compressive strength and deflection cannot be obtained, and handling properties may also be insufficient. 3If it exceeds this value, the compressive strength will be too high and good flexibility will not be obtained.

[0029] Next, a method for manufacturing the heat insulating material according to the embodiment of the present invention will be described. First, the inorganic fine particles, fireproof fibers, infrared scattering materials, and organic fibers are mixed in a mixer so as to have a predetermined content, and the obtained raw material mixture is dispersed with air, so that the fireproof fibers and organic fibers are both laminated so as to be horizontally oriented. During this lamination, it is preferable to adsorb the raw material mixture on the upper surface of a breathable member such as a mesh wire while exhausting air below the member. Next, the obtained laminate is heat-treated at an atmospheric temperature of about 130 to 150°C while applying pressure in the thickness direction in a single or multiple layer state. As a result, a part or the whole of the organic fibers are melted, so that they can be heat-welded at least to the inorganic fine particles, and preferably the organic fibers can be heat-welded to each other at one or more points.

[0030] The manufacturing method of the heat insulating material according to the embodiment of the present invention can be suitably carried out, for example, by a manufacturing apparatus shown in FIG. 2. That is, the manufacturing apparatus shown in FIG. 2 is composed of a cylindrical chamber 11 having a raw material supply port 11a at the top, and the raw material mixture introduced from the raw material supply port 11a falls freely in the chamber 11 toward a mesh conveyor 12 provided at the bottom of the chamber 11. During this free fall, the raw material mixture is dispersed by an air flow with an adjusted wind speed blown horizontally from an air outlet 11b provided at the middle of the height direction of the chamber 11. As a result, the refractory fiber and organic fiber contained in the raw material mixture are oriented horizontally and are deposited on the mesh conveyor 12 as is. A gas suction port 11c for exhausting the air blown into the chamber 11 is provided at the bottom of the chamber 11, and the raw material mixture deposited on the mesh conveyor 12 is sucked onto the conveyor surface of the mesh conveyor 12 to form a laminate.

[0031] The laminate made of the raw material mixture formed on the mesh conveyor 12 as described above is conveyed by the mesh conveyor 12 to the outside of the chamber 11 as it is. The laminate leaving the chamber 11 is introduced into the heat press 13 either alone or in a state of being stacked together with a laminate formed separately. Here, the laminate is sandwiched between one or more pairs of rollers, and heat treated under temperature conditions of an atmospheric temperature of about 130 to 150°C while applying pressure in the thickness direction. As a result, the organic fibers melt and are thermally fused to at least the surrounding inorganic fine particles, and a heat insulating material made of a sheet-like molded body is produced. EXAMPLES

[0032] Insulating materials according to the present invention and comparative examples were prepared, and each of them was evaluated in terms of bulk density, flexibility, compressive strength, thermal insulation, and heat resistance, as defined below. That is, bulk density was obtained by dividing mass by volume. Flexibility was evaluated by the maximum amount of deflection when a test piece having a thickness of 5 mm placed on two supports separated by a distance (span) of 100 mm was broken by pushing down the center of the test piece in a three-point bending test using a strength tester. Compressive strength was evaluated by the maximum load when the test piece was compressed using a strength tester to a strain of 10%. Thermal insulation was evaluated by the thermal conductivity at 600°C according to the flat plate comparison method (JIS A1412-2 Appendix A). Heat resistance was evaluated by the maximum temperature at which the linear heat shrinkage rate was 3% or less when the test piece was heated for 24 hours.

[0033] [Example 1] The mixture was mixed in a mixer at a blending ratio of 75% by mass of silica fine particles (average particle size 0.2 μm) as inorganic fine particles, 5% by mass of long glass fibers (E glass, average fiber diameter 13 μm, length 13 mm) as fire-resistant fibers, 15% by mass of silicon carbide (average particle size 2 μm) as infrared scattering material, and 5% by mass of polyethylene / polypropylene core-sheath structure fibers (fiber diameter 1.7 dtex, fiber length 5 mm) as organic fibers. The mixture was allowed to fall freely in a chamber, and an air flow with an adjusted wind speed was blown horizontally to laminate the fibers contained in the mixture in a horizontally oriented state, and the laminated mixture was sucked into a mesh conveyor installed at the bottom of the chamber to form a laminate. Eight of these laminates were stacked and heated and compressed at 150 ° C to produce a heat insulating material consisting of a sheet-like molded body with a thickness of 5 mm. The obtained heat insulating material had a bulk density of 320 kg / m 3 The deflection was 17.8 mm, the compressive strength was 7.8 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0034] [Example 2] The number of layers of the laminate was changed from 8 to 5, resulting in a bulk density of 200 kg / m 3 A 5 mm-thick insulating material was produced in the same manner as in Example 1, except that the material was heated and compressed so that the thickness of the insulating material was 5.2 mm. The obtained insulating material had a deflection of 15.2 mm, a compressive strength of 4.8 MPa, a thermal conductivity of 0.03 W / (m K), and a heat resistance temperature of 1000°C.

[0035] [Example 3] The number of layers of the laminate was changed from 8 to 13, resulting in a bulk density of 500 kg / m 3 A 5 mm-thick insulating material was produced in the same manner as in Example 1, except that the material was heated and compressed so that the thickness of the insulating material was 5.0 mm. The obtained insulating material had a deflection of 15.3 mm, a compressive strength of 8.8 MPa, a thermal conductivity of 0.03 W / (m K), and a heat resistance temperature of 1000°C.

[0036] [Example 4] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that the blending ratio of inorganic fine particles was changed from 75% by mass to 40% by mass, and the blending ratio of organic fibers was changed from 5% by mass to 40% by mass. The obtained thermal insulation material had a bulk density of 340 kg / m 3 The deflection was 16.5 mm, the compressive strength was 7.6 MPa, the thermal conductivity was 0.04 W / (m·K), and the heat resistance temperature was 1000°C.

[0037] [Example 5] A 5 mm thick heat insulating material was produced in the same manner as in Example 1, except that the blending ratio of inorganic fine particles was changed from 75% by mass to 82% by mass, the blending ratio of organic fibers was changed from 5% by mass to 3% by mass, and the infrared scattering material was changed from 15% by mass to 10% by mass. The obtained heat insulating material had a bulk density of 250 kg / m 3 The deflection was 15.1 mm, the compressive strength was 5.1 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0038] [Example 6] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that alumina fine particles (average particle size: 0.2 μm) were used as the inorganic fine particles instead of the silica fine particles. The obtained thermal insulation material had a bulk density of 310 kg / m 3 The deflection was 16.5 mm, the compressive strength was 7.9 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0039] [Example 7] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that short glass fibers (E glass, average fiber diameter 13 μm) were used instead of long glass fibers as the refractory fibers. The obtained thermal insulation material had a bulk density of 340 kg / m 3 The deflection was 16.5 mm, the compressive strength was 7.6 MPa, the thermal conductivity was 0.04 W / (m·K), and the heat resistance temperature was 1000°C.

[0040] [Example 8] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that alumina fibers (average fiber diameter 5 μm) were used instead of long glass fibers as the refractory fibers. The obtained thermal insulation material had a bulk density of 340 kg / m 3The deflection was 16.5 mm, the compressive strength was 6.8 MPa, the thermal conductivity was 0.05 W / (m·K), and the heat resistance temperature was 1000°C.

[0041] [Example 9] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that mullite fiber (average fiber diameter 6 μm) was used as the refractory fiber instead of the long glass fiber. The obtained thermal insulation material had a bulk density of 340 kg / m 3 The deflection was 17.0 mm, the compressive strength was 6.9 MPa, the thermal conductivity was 0.05 W / (m·K), and the heat resistance temperature was 1000°C.

[0042] [Example 10] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that zirconia fiber (average fiber diameter 5 μm) was used instead of long glass fiber as the refractory fiber. The obtained thermal insulation material had a bulk density of 340 kg / m 3 The deflection was 16.5 mm, the compressive strength was 7.1 MPa, the thermal conductivity was 0.05 W / (m·K), and the heat resistance temperature was 1000°C.

[0043] [Example 11] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that silica-alumina fibers (average fiber diameter 3 μm) were used instead of long glass fibers as the refractory fibers. The obtained thermal insulation material had a bulk density of 340 kg / m 3 The deflection was 17.5 mm, the compressive strength was 7.3 MPa, the thermal conductivity was 0.04 W / (m·K), and the heat resistance temperature was 1000°C.

[0044] [Example 12] A 5 mm thick insulating material was produced in the same manner as in Example 1, except that AES (alkaline earth silicate) fibers (average fiber diameter 3 μm, non-fiber particle content 50 parts by mass per 100 parts by mass of refractory fiber, non-fiber particles with an average particle diameter of 425 μm or more 1 part by mass) were used instead of long glass fibers as the refractory fibers. The obtained insulating material had a bulk density of 340 kg / m 3 The deflection was 16.5 mm, the compressive strength was 7.1 MPa, the thermal conductivity was 0.04 W / (m·K), and the heat resistance temperature was 1000°C.

[0045] [Example 13] A 5 mm thick insulating material was produced in the same manner as in Example 1, except that the blending ratio of the inorganic fine particles was changed from 75% by mass to 40% by mass, and the blending ratio of the fire-resistant fiber was changed from 5% by mass to 40% by mass. The obtained insulating material had a bulk density of 360 kg / m 3 The deflection was 15.5 mm, the compressive strength was 7.6 MPa, the thermal conductivity was 0.05 W / (m·K), and the heat resistance temperature was 1000°C.

[0046] [Example 14] A 5 mm thick heat insulating material was produced in the same manner as in Example 1, except that the blending ratio of the fire-resistant fiber was changed from 5% by mass to 12% by mass, and the blending ratio of the infrared scattering material was changed from 15% by mass to 8% by mass. The obtained heat insulating material had a bulk density of 340 kg / m 3 The deflection was 17.3 mm, the compressive strength was 7.2 MPa, the thermal conductivity was 0.04 W / (m·K), and the heat resistance temperature was 1000°C.

[0047] [Example 15] A 5 mm thick heat insulating material was produced in the same manner as in Example 1, except that the blending ratio of the inorganic fine particles was changed from 75% by mass to 70% by mass, and the blending ratio of the infrared scattering material was changed from 15% by mass to 20% by mass. The obtained heat insulating material had a bulk density of 340 kg / m 3 The deflection was 17.2 mm, the compressive strength was 7.1 MPa, the thermal conductivity was 0.05 W / (m·K), and the heat resistance temperature was 1000°C.

[0048] [Example 16] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that titanium dioxide (average particle size 2 μm) was used as the infrared scattering material instead of silicon carbide. The obtained thermal insulation material had a bulk density of 320 kg / m 3 The deflection was 17.2 mm, the compressive strength was 7.8 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0049] [Example 17] A heat insulating material having a thickness of 5 mm was produced in the same manner as in Example 1, except that zirconium silicate (average particle size 2 μm) was used as the infrared scattering material instead of silicon carbide. The obtained heat insulating material had a bulk density of 320 kg / m 3 The deflection was 16.2 mm, the compressive strength was 7.9 MPa, the thermal conductivity was 0.04 W / (m·K), and the heat resistance temperature was 1000°C.

[0050] [Example 18] A 5 mm thick insulating material was produced in the same manner as in Example 17, except that alumina fine particles (average particle size 0.2 μm) were used as the inorganic fine particles instead of the silica fine particles, and alumina fibers (average fiber diameter 5 μm) were used as the refractory fibers instead of the long glass fibers. The obtained insulating material had a bulk density of 340 kg / m 3 The deflection was 16.5 mm, the compressive strength was 6.8 MPa, the thermal conductivity was 0.05 W / (m·K), and the heat resistance temperature was 1200°C.

[0051] [Example 19] A 5 mm thick insulating material was produced in the same manner as in Example 1, except that polyester fiber (fiber diameter 0.15 dtex, fiber length 5 mm) was used instead of the polyethylene / polypropylene core-sheath structure fiber for the organic fiber. The obtained insulating material had a bulk density of 300 kg / m 3 The deflection was 16.9 mm, the compressive strength was 6.4 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0052] [Example 20] A 5 mm thick insulating material was produced in the same manner as in Example 1, except that polyvinyl alcohol fiber (fiber diameter 0.15 dtex, fiber length 5 mm) was used as the organic fiber instead of the polyethylene / polypropylene core-sheath structure fiber. The obtained insulating material had a bulk density of 310 kg / m 3 The deflection was 17.3 mm, the compressive strength was 6.8 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0053] [Example 21] A 5 mm thick insulating material was produced in the same manner as in Example 1, except that polyethylene fibers (fiber diameter 0.15 dtex, fiber length 5 mm) were used as the organic fibers instead of the polyethylene / polypropylene core-sheath structure fibers. The obtained insulating material had a bulk density of 310 kg / m 3 The deflection was 18.3 mm, the compressive strength was 6.2 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0054] [Example 22] A 5 mm thick heat insulating material was produced in the same manner as in Example 1, except that alumina fiber was added to the long glass fiber of the refractory fiber to produce multiple types of heat insulating material. The resulting heat insulating material had a bulk density of 300 kg / m 3 The deflection was 16.4 mm, the compressive strength was 6.3 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0055] [Example 23] A 5 mm thick insulating material was produced in the same manner as in Example 1, except that alumina fine particles were added to siliceous fine particles of the inorganic fine particles to produce a multi-type insulating material. The obtained insulating material had a bulk density of 320 kg / m 3 The deflection was 15.8 mm, the compressive strength was 6.5 MPa, the thermal conductivity was 0.04 W / (m·K), and the heat resistance temperature was 1000°C.

[0056] [Example 24] A 5 mm thick heat insulating material was produced in the same manner as in Example 1, except that titanium dioxide was added to the silicon carbide of the infrared scattering material to produce multiple types. The resulting heat insulating material had a bulk density of 310 kg / m 3 The deflection was 17.1 mm, the compressive strength was 6.2 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0057] [Example 25] A thermal insulation material having a thickness of 5 mm was produced in the same manner as in Example 1, except that zirconia-based fine particles (average particle size: 0.2 μm) were used as the inorganic fine particles instead of the silica-based fine particles. The obtained thermal insulation material had a bulk density of 300 kg / m 3The deflection was 16.5 mm, the compressive strength was 6.6 MPa, the thermal conductivity was 0.03 W / (m·K), and the heat resistance temperature was 1000°C.

[0058] The compounding ratios and physical properties / forms of the heat insulating materials of Examples 1 to 25 are summarized in Tables 1 and 2 below.

[0059] [Table 1]

[0060] [Table 2]

[0061] [Comparative Example 1] The number of layers of the laminate was changed from 8 to 5, resulting in a bulk density of 190 kg / m 3 A 5 mm-thick insulating material was produced in the same manner as in Example 1, except that the material was heated and compressed so that the thickness of the insulating material was 5 mm. The obtained insulating material had a deflection of 3.6 mm, a compressive strength of 1.9 MPa, a thermal conductivity of 0.08 W / (m K), and a heat resistance temperature of 900 °C.

[0062] [Comparative Example 2] The number of layers of the laminate was changed from 8 to 14, resulting in a bulk density of 510 kg / m 3 A 5 mm-thick insulating material was produced in the same manner as in Example 1, except that the material was heated and compressed so that the thickness of the insulating material was 5 mm. The obtained insulating material had a deflection of 10.2 mm, a compressive strength of 8.5 MPa, a thermal conductivity of 0.06 W / (m K), and a heat resistance temperature of 1000°C.

[0063] The blending ratios and physical properties / forms of Comparative Examples 1 and 2 are summarized in Table 3 below.

[0064] [Table 3] [Explanation of symbols]

[0065] 1 Inorganic fine particles 2. Fire-resistant fibers 3. Infrared scattering material 4. Organic Fibers

Claims

1. The molded body is a mixture of inorganic fine particles of metal oxide as a main material, refractory fibers, infrared scattering materials, and fused organic fibers, and the molded body has the refractory fibers and organic fibers randomly oriented in a direction perpendicular to the thickness direction of the molded body and has a bulk density of 200 kg / m 3 More than 500kg / m 3 The heat insulating material is characterized in that it is within the range below, and when a test piece molded to a thickness of 5 mm is subjected to a bending strength measurement with a span of 100 mm, the deflection at break is 15 mm or more.

2. 2. The heat insulating material according to claim 1, characterized in that the heat resistance temperature is 1000° C. or more and 1200° C. or less, and the thermal conductivity at 600° C. is 0.05 W / (m·K) or less.

3. 3. The heat insulating material according to claim 1, wherein the organic fibers are fused to at least the inorganic fine particles.

Citation Information

Patent Citations

  • Heat insulating material and method for manufacturing the same

    JP2012145217A

  • Composite heat insulating material superior in flexibility

    JP2016205728A

  • Heat transfer suppressing member and its use method

    JP2020119840A

  • Battery heat insulation material and battery

    JP2021140968A

  • Insulating fabric

    JP2022508727A