Negative electrode mixture and lithium-ion battery
Surface-modifying silicon particles with aromatic groups in lithium ion batteries addresses the aggregation issue of carbon nanotubes, enhancing the conductivity and reducing resistance in the negative electrode composite material.
Patent Information
- Application Number
- JP2023083877
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium ion batteries using carbon nanotubes as conductive additives in negative electrodes face challenges in fully utilizing their conductivity due to aggregation, leading to high resistance.
Surface-modifying silicon particles in the negative electrode composite material with aromatic groups to improve the dispersibility of carbon nanotubes, thereby reducing resistance.
The modification enhances the dispersibility of carbon nanotubes, resulting in a negative electrode composite material with lower resistance and improved conductivity.
Smart Images

Figure 2024167654000001 
Figure 2024167654000002 
Figure 2024167654000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a negative electrode mixture and a lithium ion battery. [Background technology]
[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is known as a negative electrode active material for batteries.
[0003] In this regard, it has been proposed to use carbon nanotubes as a conductive additive to reduce the resistance of the active material layer.
[0004] For example, Patent Document 1 discloses a negative electrode material for lithium ion secondary batteries containing silicon particles and carbon nanofibers, characterized in that the carbon nanofibers are SiC nanowires and / or multi-walled carbon nanotubes. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-252845 A Summary of the Invention [Problem to be solved by the invention]
[0006] In lithium ion batteries that use carbon nanotubes as a conductive additive contained in the negative electrode mixture, it is desirable to further reduce the resistance.
[0007] The present disclosure aims to provide a negative electrode mixture that contains carbon nanotubes as a conductive additive and has low resistance, and a lithium ion battery that contains such a negative electrode mixture. [Means for solving the problem]
[0008] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> The negative electrode active material includes surface-modified negative electrode active material particles and a conductive assistant, the surface-modified negative electrode active material particles have silicon particles and aromatic groups modifying the surfaces of the silicon particles; and The conductive assistant contains carbon nanotubes. Negative electrode composite material. <Aspect 2> 2. The negative electrode composition of claim 1, wherein the aromatic group is a monocyclic aryl group. <Aspect 3> 3. The negative electrode mixture of claim 1 or 2, wherein the aromatic group has 4 or more and 10 or less carbon atoms. <Aspect 4> 4. The negative electrode composite of any one of Aspects 1 to 3, wherein the surface-modified negative electrode active material particles have a silicon-oxygen-silicon-carbon bond, the silicon not bonded to the carbon is silicon of the silicon particles, and the carbon is carbon of the aromatic group. <Aspect 5> A negative electrode active material layer is provided, and The negative electrode active material layer contains the negative electrode mixture according to any one of aspects 1 to 4. Lithium-ion battery. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a negative electrode composite material that contains carbon nanotubes as a conductive assistant and has low resistance, and a lithium ion battery that contains such a negative electrode composite material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0011] 《Negative electrode mixture》 The negative electrode composite material of the present disclosure includes surface-modified negative electrode active material particles and a conductive assistant. The surface-modified negative electrode active material particles included in the negative electrode composite material of the present disclosure include silicon particles and aromatic groups on the surfaces of the silicon particles. The conductive assistant included in the negative electrode composite material of the present disclosure includes carbon nanotubes.
[0012] The present inventors have discovered that in a battery in which the negative electrode mixture contains silicon particles and carbon nanotubes as a conductive additive, the carbon nanotubes may aggregate and not fully exhibit their inherent conductivity.
[0013] In response to this, the present inventors have found that the resistance of the battery is reduced by surface-modifying silicon particles with aromatic groups. The reason for this, without intending to be bound by any theory, is believed to be that the dispersibility of carbon nanotubes in the negative electrode mixture is improved by surface-modifying silicon particles with aromatic groups. Specifically, it is believed that π-π interactions occur between the aromatic rings modifying the silicon particles and the carbon nanotubes, improving the dispersibility of the carbon nanotubes and suppressing the aggregation of the carbon nanotubes.
[0014] In the present disclosure, the term "negative electrode mixture" refers to a composition that can form a negative active material layer as it is or by further containing other components. In the present disclosure, the term "negative electrode mixture slurry" refers to a slurry that contains a dispersion medium in addition to the "negative electrode mixture" and can be applied and dried to form a negative electrode active material layer.
[0015] <Surface modified negative electrode active material particles> The negative electrode mixture of the present disclosure includes surface-modified negative electrode active material particles.
[0016] (silicon particles) The surface-modified negative electrode active material particles include silicon particles.
[0017] The composition of the silicon particles is not particularly limited. The proportion of silicon element in all elements contained in the silicon particles may be, for example, 50 mol % or more, 70 mol % or more, or 90 mol % or more.
[0018] The silicon particles may contain other elements such as Li in addition to the Si element. Examples of the other elements include Sn, Fe, Co, Ni, Ti, Cr, B, and P in addition to the Li element.
[0019] The silicon particles may contain impurities such as oxides.
[0020] The silicon particles may be amorphous or crystalline, and the crystal phase contained in the silicon particles is not particularly limited.
[0021] The shape and size of the silicon particles are not particularly limited. The average particle size of the silicon particles may be, for example, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and may be 10 μm or less, 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The average particle size can be determined by observation with an electron microscope such as an SEM, and is determined, for example, as the average value of the maximum Feret diameters of each of a plurality of particles. The number of samples is preferably large, for example, 20 or more, 50 or more, or 100 or more. The average particle size can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of the silicon particles described later or by performing a classification process.
[0022] The silicon particles contained in the surface-modified negative electrode active material particles may be porous silicon particles. The porous silicon particles contain silicon having a plurality of voids. There is no particular limitation on the shape of the voids in the porous silicon particles.
[0023] The porous silicon particles may be particles containing nanoporous silicon. Nanoporous silicon refers to silicon having a plurality of pores with pore diameters on the nanometer order (less than 1000 nm, preferably 100 nm or less).
[0024] (aromatic group) The surface-modified negative electrode active material particles have aromatic groups modifying the surfaces of the silicon particles.
[0025] In the present disclosure, the term "aromatic group" refers to a functional group having aromaticity, and may be a monocyclic aromatic group or a polycyclic aromatic group. In addition, in the present disclosure, the term "aromatic group" may be an aryl group or a heteroaryl group.
[0026] Examples of the monocyclic aryl group include an optionally substituted phenyl group, an optionally substituted biphenyl group, and an optionally substituted triphenyl group, and examples of the polycyclic aryl group include an optionally substituted naphthyl group and an optionally substituted anthracenyl group.
[0027] Examples of monocyclic heteroaryl groups include a thienyl group, a furyl group, a pyrrole group, a thiazole group, an oxazole group, a pyrazole group, a pyridyl group, etc. Examples of polycyclic heteroaryl groups include a benzothienyl group, a benzofuryl group, and an indole group, etc.
[0028] The number of carbon atoms in the aromatic group may be 4 or more and 10 or less. In addition, the number of carbon atoms may be 5 or more, or 6 or more, and may be 9 or less, 8 or less, or 7 or less.
[0029] The aromatic group is preferably a monocyclic aryl group having a carbon number of from 4 to 10. Examples of such an aromatic group include a phenyl group and a tolyl group.
[0030] The surface-modified negative electrode active material particles may have a silicon-oxygen-silicon-carbon bond, in which the silicon not bonded to carbon is silicon of a silicon particle, and the carbon is carbon of an aromatic group. That is, the carbon of an aromatic group may be bonded to silicon on the surface of a silicon particle via oxygen and silicon.
[0031] <Method for producing surface-modified negative electrode active material particles> The disclosed method of making surface-modified negative electrode active material particles includes modifying the surface of silicon particles with aromatic groups.
[0032] The surfaces of the silicon particles may be modified with aromatic groups by dehydration condensation between silanol groups on the surfaces of the silicon particles and silanol groups generated by hydrolysis of a hydrolyzable group-containing silane having an aromatic group.
[0033] As the hydrolyzable group-containing silane, a hydrolyzable group-containing silane having a structure corresponding to the above description regarding the aromatic group in this disclosure can be used.
[0034] <Conductive assistant> The negative electrode mixture of the present disclosure includes a conductive additive. The conductive additive further includes carbon nanotubes.
[0035] Examples of carbon nanotubes include single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs). The carbon nanotubes are preferably SWCNTs.
[0036] The negative electrode mixture of the present disclosure also optionally includes an electrolyte, a conductive additive other than carbon nanotubes, and a binder.
[0037] <Electrolyte> The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.
[0038] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.
[0039] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).
[0040] In addition, when the negative electrode composite material contains a solid electrolyte, the mass ratio of the surface-modified negative electrode active material particles to the solid electrolyte in the negative electrode composite material (mass of the surface-modified negative electrode active material particles:mass of the solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0041] The electrolyte preferably contains a supporting salt and a solvent.
[0042] Examples of supporting salts (lithium salts) for electrolytes having lithium ion conductivity include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3.
[0043] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.
[0044] <Conductive assistant other than carbon nanotubes> The conductive assistant other than carbon nanotubes is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanofiber (CNF), etc., but is not limited thereto. The ratio of the mass of the conductive assistant other than carbon nanotubes to the total mass of the conductive assistant may be less than 50 mass%, less than 40 mass%, less than 30 mass%, less than 20 mass%, or less than 10 mass%, or may be 0 mass%.
[0045] <binder> The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.
[0046] Lithium-ion battery The lithium ion battery of the present disclosure has a negative electrode active material layer, and the negative electrode active material layer contains the negative electrode mixture of the present disclosure. The lithium ion battery of the present disclosure may have, in this order, a negative electrode current collector layer, a negative electrode active material layer containing the negative electrode mixture of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.
[0047] The lithium ion battery of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.
[0048] The lithium ion battery may be a primary battery or a secondary battery.
[0049] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type.
[0050] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.
[0051] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0052] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure contains the negative electrode mixture of the present disclosure. For the negative electrode mixture, the above description of the negative electrode mixture of the present disclosure can be referenced.
[0053] The thickness of the negative electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0054] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. The electrolyte layer may include a binder, etc., if necessary, in addition to the electrolyte. For the electrolyte and the binder, the above description regarding the negative electrode mixture of the present disclosure can be referred to.
[0055] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.
[0056] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.
[0057] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-y Li-Mn spinel substituted with different elements, which has a composition represented by MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), and lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co, and Ni), and the like, but are not limited thereto.
[0058] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.
[0059] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0060] For the electrolyte and the binder, the above description of the negative electrode composite of the present disclosure can be referred to. The conductive assistant may be, for example, VGCF (vapor grown carbon fiber), acetylene black (AB), Ketjen black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.
[0061] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.
[0062] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0063] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.
[0064] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred. EXAMPLES
[0065] <<Preparation of surface-modified negative electrode active material particles>> Preparation of Silicon Particles (Comparative Synthesis Example 1) Silicon particles were prepared as a silicon (Si) source. The silicon particles and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed silicon particles and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere to obtain porous silicon particles.
[0066] Modification with Aromatic Groups (Synthesis Example 1) In an argon (Ar)-substituted glove box, 2 g of porous silicon particles, 20 g of ultra-dehydrated ethanol (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and 0.027 g of trimethoxy (p-tolyl) silane (manufactured by Tokyo Chemical Industry Co., Ltd.), a silane coupling agent having a p-tolyl group (-p-C6H4 (CH3)), were weighed and placed in a sealed reaction vessel and stirred at 50 ° C for 16 hours to dehydrate and condense the silanol groups on the surface of the porous Si with the silanol groups generated by hydrolysis of the silane coupling agent having a p-tolyl group (-p-C6H4 (CH3)). The solution after the reaction was suction filtered, washed with 30 mL of ethanol, and filtered five times. The obtained solid was vacuum-dried at 100 ° C for 12 hours to obtain surface-modified negative electrode active material particles in which the surfaces of silicon particles were modified with p-tolyl groups (-p-C6H4 (CH3)).
[0067] (Synthesis Example 2) Surface-modified negative electrode active material particles in which the surfaces of silicon particles were modified with phenyl groups (-CH) were prepared in the same manner as in Synthesis Example 1, except that the silane coupling agent was changed to 0.025 g of trimethoxyphenylsilane (manufactured by Tokyo Chemical Industry Co., Ltd.) having a phenyl group (-CH).
[0068] (Comparative Synthesis Example 2) Surface-modified negative electrode active material particles in which the surfaces of silicon particles were modified with hexyl groups (-(CH2)5CH3) were prepared in the same manner as in Synthesis Example 1, except that the silane coupling agent was changed to 0.06 g of hexyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) having a hexyl group (-(CH2)5CH3).
[0069] Making a Battery Preparation of Positive Electrode Mixture A polypropylene (PP) container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of polyvinylidene fluoride (PVDF) binder, and LiNi as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (average particle size: 6 μm), Li2S-P2S5-based glass ceramic as a sulfide solid electrolyte, and vapor-grown carbon fiber (VGCF) as a conductive additive were added to the container and stirred for 30 seconds with an ultrasonic disperser (UH-50 manufactured by SMT). Next, the container was shaken for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) and stirred for 30 seconds with an ultrasonic disperser. It was further shaken for 3 minutes with the shaker to obtain a slurry-like positive electrode mixture (positive electrode mixture slurry).
[0070] <Formation of Positive Electrode Active Material Layer> The obtained slurry was applied to an aluminum (Al) foil (manufactured by Showa Denko) as a positive electrode current collector layer by a blade method using an applicator. The applied slurry was dried for 30 minutes on a hot plate at 100° C. As a result, a positive electrode active material layer was formed on the positive electrode current collector layer.
[0071] <Preparation of negative electrode mixture> (Comparative Examples 1 and 2, and Examples 1 and 2) In a polypropylene (PP) container, diisobutyl ketone, a 5 wt% diisobutyl ketone solution of a PVDF-based binder (KF8300 manufactured by Kureha Corporation), single-walled carbon nanotubes (SWCNT) (manufactured by Sigma-Aldrich Corporation) as a conductive assistant, Li2S-P2S5-based glass ceramic as a solid electrolyte, and either of Comparative Synthesis Examples 1 and 2 and Silicon particles of Synthesis Examples 1 and 2 as a negative electrode active material were added to the container, and the mixture was stirred for 1 minute with an ultrasonic dispersion device (UH-50 manufactured by SMT Corporation). Furthermore, the container was shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a slurry-like negative electrode mixture (negative electrode mixture slurry) of Comparative Examples 1 and 2 and Examples 1 and 2. The numbers of the Comparative Synthesis Examples and Comparative Examples, and the numbers of the Synthesis Examples and Examples correspond to each other.
[0072] (Comparative Example 3 and Example 3) Negative electrode mixture slurries of Comparative Example 3 and Example 3 were prepared in the same manner as in Comparative Example 1 and Example 1, except that the conductive assistant was changed to multi-walled carbon nanotubes (MWCNT) (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0073] (Comparative Examples 4 and 5) Negative electrode mixture slurries of Comparative Examples 4 and 5 were prepared in the same manner as in Comparative Example 1 and Example 1, except that the conductive assistant was changed to acetylene carbon black (AB) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0074] <Formation of negative electrode active material layer> The obtained slurry was applied onto a nickel (Ni) foil as a negative electrode current collector by a blade method using an applicator. The applied slurry was dried for 30 minutes on a hot plate at 100° C. This formed a negative electrode active material layer on the negative electrode current collector layer.
[0075] <Formation of solid electrolyte layer> Heptane, a 5 wt% heptane solution of SBR-based binder, and Li2S-P2S5-based glass ceramic as a solid electrolyte were added to a polypropylene (PP) container and stirred for 30 seconds with an ultrasonic dispersing device (UH-50, manufactured by SMT). The container was then shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry. The obtained slurry was applied to an Al foil by the blade method using an applicator. The applied slurry was dried on a hot plate at 100°C for 30 minutes. This formed a solid electrolyte layer. Three solid electrolyte layers were produced.
[0076] <Battery Assembly> The positive electrode current collector layer, the positive electrode active material layer, and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. in the first pressing step to obtain a positive electrode laminate.
[0077] The negative electrode current collector layer, the negative electrode active material layer, and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. in the second pressing step to obtain a negative electrode laminate.
[0078] The negative electrode laminate and the positive electrode laminate were fabricated so that the area of the negative electrode laminate was larger than the area of the positive electrode laminate.
[0079] Further, an Al foil as a release sheet, an intermediate solid electrolyte layer formed on the Al foil, and the negative electrode laminate were laminated so that the solid electrolyte layers were in contact with each other. The laminate was set in a flat uniaxial press and temporarily pressed for 10 seconds at a pressure of 100 MPa and a temperature of 25° C. The Al foil was peeled off from the intermediate solid electrolyte layer of the laminate to obtain a negative electrode laminate further laminated with an intermediate solid electrolyte layer.
[0080] The positive electrode laminate and the negative electrode laminate further having an intermediate solid electrolyte layer laminated thereon were laminated so that the solid electrolyte layers were in contact with each other. This laminate was set in a flat uniaxial press and pressed for 1 minute at a pressure of 200 MPa and a temperature of 120°C in the third pressing step. This produced an all-solid-state battery.
[0081] "evaluation" Analysis of the surface properties of silicon particles The carbon content of the silicon particles of the Synthesis Example and Comparative Synthesis Example was measured by high-frequency combustion infrared absorption method (apparatus used: LECO, CSLS600).
[0082] In addition, the silicon particles of each example were subjected to surface analysis by time-of-flight secondary ion mass spectrometry (TOF-SIMS) (apparatus used: ION-TOF, TOF.SIMS5, primary ion source: bismuth (Bi)).
[0083] <DCIR Measurement> The prepared battery was restrained at a predetermined restraining pressure using a restraining jig, and was charged at a constant current and constant voltage at 1 / 10C to 4.55V (1 / 100C cut), and then discharged at 1C to 3.0V. Then, it was charged at a constant current and constant voltage at 1 / 3C to 4.35V (1 / 100C cut), and then discharged at a constant current and constant voltage at 1 / 3C to 3.00V (1 / 100C cut). Furthermore, it was charged at a constant current and constant voltage at 1 / 3C to 4.35V (1 / 100C cut), and then discharged at a constant current and constant voltage at 1 / 3C to 3.14V (1 / 100C cut). Then, a constant current of 5C was applied for 10s, and the direct current internal resistance (DCIR) was measured.
[0084] "result" Analysis of the surface properties of silicon particles The results of quantitative analysis of the carbon content of silicon particles in the comparative synthesis example and synthesis example are shown in Table 1.
[0085] [Table 1]
[0086] As shown in Table 1, the silicon particles of Synthesis Example had a larger amount of carbon on the particle surface than the silicon particles of Comparative Synthesis Example 1.
[0087] Furthermore, TOF-SIMS analysis of the silicon particles of the synthesis example confirmed the MS spectra originating from the p-tolyl group (-p-C6H4(CH3)) and the phenyl group (-C6H5) (C7H7: m / z = 91, C6H5: m / z = 77).
[0088] From these findings, it is believed that the surfaces of the silicon particles in the synthesis examples were successfully modified with aromatic groups.
[0089] <DCIR Measurement> The results of DCIR measurements of the batteries of each example are shown in Tables 2 to 4. The DCIR values are expressed as relative values assuming that the measurement results of Comparative Example 1 for Examples 1 and 2 and Comparative Example 2, the measurement results of Comparative Example 3 for Example 3, and the measurement results of Comparative Example 4 for Comparative Example 5 are 1.00.
[0090] [Table 2]
[0091] [Table 3]
[0092] [Table 4]
[0093] As shown in Table 2, the DCIR value of the battery of the Example in which the surface of the silicon particles was modified with an aromatic group and SWCNT was used as the conductive assistant was smaller than the DCIR value of the battery of the Comparative Example in which the silicon particles were unmodified or modified with a cyclic hydrocarbon group. In particular, the DCIR value of the battery of Example 1 was the smallest.
[0094] As shown in Table 3, the DCIR value of the battery of Example 3, in which the surface of the silicon particles was modified with aromatic groups and MWCNT was used as the conductive assistant, was smaller than the DCIR value of the battery of Comparative Example 3, in which the silicon particles were not modified.
[0095] As shown in Table 4, the DCIR value of the battery of Comparative Example 5, in which the surface of the silicon particles was modified with aromatic groups while AB was used as the conductive assistant, was equivalent to the DCIR value of the battery of Comparative Example 4, in which the silicon particles were not modified.
Claims
1. The negative electrode active material includes surface-modified negative electrode active material particles and a conductive assistant, the surface-modified negative electrode active material particles have silicon particles and aromatic groups modifying the surfaces of the silicon particles; and The conductive assistant contains carbon nanotubes. Negative electrode composite material.
2. 2. The negative electrode composition of claim 1, wherein the aromatic group is a monocyclic aryl group.
3. The negative electrode mixture according to claim 1 , wherein the aromatic group has 4 or more and 10 or less carbon atoms.
4. 2. The negative electrode mixture according to claim 1, wherein the surface-modified negative electrode active material particles have a silicon-oxygen-silicon-carbon bond, the silicon not bonded to the carbon is silicon of the silicon particles, and the carbon is carbon of the aromatic group.
5. A negative electrode active material layer is provided, and The negative electrode active material layer contains the negative electrode mixture according to any one of claims 1 to 4. Lithium-ion battery.
Citation Information
Patent Citations
Surface-modified silicon particle
JP2011011928A
Organic polymer-silicon composite particles, methods for producing the same, and negative electrode and lithium secondary battery containing the same
JP2013522820A
Negative electrode composition, method for manufacturing a negative electrode, and lithium ion battery
JP2018538675A
Negative electrode composition, method of manufacturing negative electrode, and lithium ion battery
JP2019523976A
Electrical conduction material slurry
JP2022181696A