Decorative sheet and decorative plate
The decorative sheet addresses the trade-off in conventional decorative sheets by using a polypropylene-based structure with a polycarbonate-urethane surface layer and nucleating agent vesicles, enhancing resistance properties and reducing environmental impact.
Patent Information
- Application Number
- JP2023083885
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-12-04
AI Technical Summary
Conventional decorative sheets face a trade-off between improving weather resistance, scratch resistance, and stain resistance, as increasing the amount of ultraviolet absorbers and light stabilizers in the surface protective layer deteriorates other physical properties, and adding more filler for low gloss reduces these resistances.
A decorative sheet comprising a base layer made of polypropylene resin, a surface protective layer formed with an aqueous coating liquid containing a polycarbonate-based urethane resin and a carbodiimide curing agent, and a pattern layer with nucleating agent vesicles encapsulated in a single-layer membrane, enhancing crystallinity and dispersibility.
The solution effectively suppresses deterioration in weather resistance, scratch resistance, and stain resistance while allowing for a reduced manufacturing process and lower environmental emissions, with improved design flexibility and adhesion.
Smart Images

Figure 2024167660000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative sheet and a decorative board. [Background technology]
[0002] As the environments in which decorative sheets are used become more diverse, there is an increasing demand for more advanced functionality. An important function of decorative sheets is the diversity of designs (for example, a wide range of gloss expressions), and gloss expressions are generally adjusted by the amount of filler added to the surface protective layer. Specifically, adding a large amount of filler to the surface protective layer results in low gloss, and adding a small amount of filler to the surface protective layer results in high gloss. Depending on the amount of filler added to the surface protective layer, differences occur in physical properties such as weather resistance, scratch resistance, and stain resistance, and in general, decorative sheets with low gloss designs that contain a large amount of filler tend to have reduced physical properties. In particular, weather resistance is significantly degraded by a combination of factors such as light, heat, and water. As a technique for dealing with the deterioration of weather resistance, for example, as disclosed in Patent Document 1, a technique in which an ultraviolet absorbing agent or a light stabilizer is added to a surface protective layer is disclosed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2018-203866 A Summary of the Invention [Problem to be solved by the invention]
[0004] In decorative sheets having conventional configurations, including the technology disclosed in Patent Document 1, it is common to increase the amount of ultraviolet absorber or light stabilizer added to the surface protective layer in order to improve weather resistance. However, when the amount of ultraviolet absorber or light stabilizer added to the surface protective layer is increased, there is a problem that other physical properties such as scratch resistance and stain resistance of the surface protective layer are deteriorated. That is, in decorative sheets having conventional configurations, there is a trade-off between improving weather resistance and improving scratch resistance and stain resistance. Also, by increasing the amount of filler added to the surface protective layer in order to achieve low gloss, there are problems in that scratch resistance is reduced due to the loss of filler, and weather resistance and stain resistance are generally reduced due to the effect of capillaries caused by the filler.
[0005] In view of the above-mentioned problems, an object of the present invention is to provide a decorative sheet and a decorative board that are capable of suppressing deterioration in weather resistance, scratch resistance, and stain resistance. [Means for solving the problem]
[0006] In order to solve the above-mentioned problems, one aspect of the present invention is a decorative sheet including a base layer, a surface protective layer, and a picture pattern layer. The base layer is a layer formed using a polypropylene-based resin. The surface protective layer is a layer laminated on one side of the base layer and formed using an aqueous coating liquid. The picture pattern layer is a layer laminated on the other side of the base layer and formed with a picture. The aqueous coating liquid contains a polycarbonate-based urethane resin and a carbodiimide curing agent. The surface protective layer is formed by a cured coating film formed by curing the aqueous coating liquid.
[0007] In order to solve the above-mentioned problems, one aspect of the present invention is a decorative board comprising a substrate and a decorative sheet laminated on at least one surface of the substrate. Effect of the Invention
[0008] According to one aspect of the present invention, it is possible to provide a decorative sheet and a decorative board that are capable of suppressing deterioration in weather resistance, scratch resistance, and stain resistance. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a cross-sectional view showing a configuration of a decorative board in the first embodiment. [Diagram 2]1 is a schematic diagram showing the positional relationship between the lines formed by the portion to which the gloss coat is applied and the lines forming the pattern formed in the picture pattern layer. FIG. [Diagram 3] FIG. 4 is a cross-sectional view showing a configuration of a decorative board in a modified example of the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present technology will be described with reference to the drawings. In the description of the drawings, the same or similar parts are denoted with the same or similar reference numerals, and duplicated descriptions are omitted. Each drawing is schematic and may differ from the actual one. The embodiments shown below are examples of devices and methods for embodying the technical idea of the present technology, and the technical idea of the present technology is not limited to the devices and methods exemplified in the following embodiments. The technical idea of the present technology can be modified in various ways within the technical scope described in the claims. In addition, the directions of "left and right" and "up and down" in the following description are merely definitions for the convenience of explanation and do not limit the technical idea of the present invention. Therefore, for example, if the paper is rotated 90 degrees, "left and right" and "up and down" are read interchangeably, and of course, if the paper is rotated 180 degrees, "left" becomes "right" and "right" becomes "left".
[0011] First embodiment Hereinafter, the configuration of a decorative sheet 1 in a first embodiment will be described with reference to FIG. The decorative sheet 1 is used, for example, indoors. Specifically, it is attached to the surfaces of fittings (interior doors, entrance storage) and construction materials (trimmings, moldings, baseboards, window frames, door frames), etc., and is used to match the patterns of fittings and construction materials for each house or room. As shown in FIG. 1, the decorative sheet 1 includes a base layer 2, a colored layer 3, a picture design layer 4, a surface protective layer 5, a moisture-proof layer 6, and a primer layer 7.
[0012] <Base material layer> The base layer 2 is a base layer formed using a polypropylene-based resin (thermoplastic resin), and is a layer that forms the support of the decorative sheet 1. The base layer 2 includes a first transparent layer 2a, a core layer 2b, and a second transparent layer 2c, and is manufactured by extrusion molding, for example. In FIG. 1, the base layer 2 is illustrated as if the first transparent layer 2a, the core layer 2b, and the second transparent layer 2c form separate layers, but in reality, the first transparent layer 2a, the core layer 2b, and the second transparent layer 2c are formed continuously. Therefore, there is no interface between the first transparent layer 2a and the core layer 2b, and no interface between the core layer 2b and the second transparent layer 2c. In the first embodiment, simultaneous extrusion is performed so that the ratio of the thickness of the first transparent layer 2a:the thickness of the core layer 2b:the thickness of the second transparent layer 2c is 0.5:9:0.5, and the thickness of the base layer 2 is 50 μm.
[0013] (first transparent layer) The first transparent layer 2a is formed by adding a dispersant as a nano-sized additive to a transparent polypropylene-based resin (thermoplastic resin). In addition to the dispersant as a nano-sized additive, an inorganic filler is added to the first transparent layer 2a.
[0014] Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, ethylene-α-olefin copolymer, and propylene-α-olefin copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytetramethylene terephthalate, polyethylene naphthalate, polyethylene terephthalate-isophthalate copolymer, 1,4-cyclohexanedimethanol copolymerized polyethylene terephthalate, polyarylate, and polycarbonate; and olefin copolymers such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-(meth)acrylic acid (ester) copolymer, and ethylene-unsaturated carboxylic acid copolymer metal neutralized product (ionomer). Examples of the resin that can be used include polyolefin resins such as poly(meth)acrylonitrile, polymethyl(meth)acrylate, polyethyl(meth)acrylate, polybutyl(meth)acrylate, and polyacrylamide; polyamide resins such as 6-nylon, 6,6-nylon, and 6,10-nylon; styrene resins such as polystyrene, AS resin, and ABS resin; vinyl resins such as polyvinyl chloride, polyvinyl acetate, polyvinyl alcohol, polyvinyl acetal, and polyvinyl butyral; fluorine resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, and ethylene-perfluoroalkyl vinyl ether copolymer; and mixtures, copolymers, composites, and laminates using two or more of the above-mentioned resins.
[0015] In particular, in light of the recent growing social interest in environmental issues, it is not preferable to use thermoplastic resins that contain chlorine (halogen), such as polyvinyl chloride resins, as thermoplastic resins, and it is preferable to use non-halogen thermoplastic resins. In addition, in consideration of various physical properties, processability, versatility, economic efficiency, etc., it is most preferable to use a polyester resin (amorphous or biaxially oriented) or a polyolefin resin, particularly a polyolefin resin, as the non-halogen-based thermoplastic resin. For example, it is preferable to use a polypropylene resin containing 30% by mass or more and 100% by mass or less of a highly crystalline homopolypropylene resin having an isotactic pentad fraction (mmmm fraction) of 95% or more as the polyolefin resin.
[0016] Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, ethylene-α-olefin copolymer, and propylene-α-olefin copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytetramethylene terephthalate, polyethylene naphthalate, polyethylene terephthalate-isophthalate copolymer, 1,4-cyclohexanedimethanol copolymerized polyethylene terephthalate, polyarylate, and polycarbonate; and olefin copolymers such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-(meth)acrylic acid (ester) copolymer, and ethylene-unsaturated carboxylic acid copolymer metal neutralized product (ionomer). Examples of the resin that can be used include polyolefin resins such as poly(meth)acrylonitrile, polymethyl(meth)acrylate, polyethyl(meth)acrylate, polybutyl(meth)acrylate, and polyacrylamide; polyamide resins such as 6-nylon, 6,6-nylon, and 6,10-nylon; styrene resins such as polystyrene, AS resin, and ABS resin; vinyl resins such as polyvinyl chloride, polyvinyl acetate, polyvinyl alcohol, polyvinyl acetal, and polyvinyl butyral; fluorine resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, and ethylene-perfluoroalkyl vinyl ether copolymer; and mixtures, copolymers, composites, and laminates using two or more of the above-mentioned resins.
[0017] In particular, in light of the recent growing social interest in environmental issues, it is not preferable to use thermoplastic resins that contain chlorine (halogen), such as polyvinyl chloride resins, as thermoplastic resins, and it is preferable to use non-halogen thermoplastic resins. In addition, in consideration of various physical properties, processability, versatility, economic efficiency, etc., it is most preferable to use a polyester resin (amorphous or biaxially oriented) or a polyolefin resin, particularly a polyolefin resin, as the non-halogen-based thermoplastic resin. For example, it is preferable to use a polypropylene resin containing 30% by mass or more and 100% by mass or less of a highly crystalline homopolypropylene resin having an isotactic pentad fraction (mmmm fraction) of 95% or more as the polyolefin resin.
[0018] (Nano-sized additives) A nano-sized additive is an additive that has been made into nano-sized particles by a technique for nano-sizing the additive (nanofiber processing). The nano-sized nucleating agent is used by being added to the polypropylene resin in the form of a nucleating agent vesicle, which is encapsulated in a vesicle having a single-layer outer membrane. In addition, the nucleating agent in the resin constituting the first transparent layer 2a may be encapsulated in vesicles with a portion of the nucleating agent exposed. Since the first transparent layer 2a contains a nucleating agent, it is possible to improve the crystallinity and improve the scratch resistance (scratch resistance) of the decorative sheet 1.
[0019] (Particle size of nucleating agent) It is preferable that the average particle size of the nano-sized nucleating agent is less than half the wavelength range of visible light. Specifically, since the wavelength range of visible light is 400 nm or more and 750 nm or less, it is preferable that the average particle size is less than 375 nm. Nano-sized nucleating agents have extremely small particle sizes, so the number of nucleating agents present per unit volume and their surface area increase inversely proportional to the cube of the particle diameter. As a result, the distance between each nucleating agent particle becomes closer, so that when crystal growth occurs from the surface of one nucleating agent particle added to the resin, the end from which the crystal is growing immediately comes into contact with the end of the crystal growing from the surface of another nucleating agent particle adjacent to the one nucleating agent particle, and the ends of the crystals inhibit each other's growth, stopping the growth of each crystal. Therefore, it is possible to reduce the average particle size of the spherulites in the crystalline part of the crystalline resin, for example, to reduce the spherulite size to 1 μm or less.
[0020] As a result, it is possible to produce a resin film with a high degree of crystallinity and high hardness, and since the stress concentration between spherulites that occurs during bending is efficiently dispersed, it is possible to realize a resin film that suppresses cracking and whitening during bending. When a nucleating agent is simply added, the particle size increases due to secondary aggregation of the nucleating agent in the resin. On the other hand, when nucleating agent vesicles are added, the dispersibility in the resin is improved, and the number of crystal nuclei per amount of nucleating agent added is significantly increased compared to when the nucleating agent is simply added. This reduces the average particle size of the spherulites in the crystalline portion of the resin, making it possible to suppress the occurrence of cracks and whitening during bending. Therefore, by adding a vesicle nucleating agent, the degree of crystallization can be increased, making it possible to achieve both improved elastic modulus and processability.
[0021] The first transparent layer 2a is formed, for example, from a resin material to which a nucleating agent has been added in an amount preferably in the range of 0.05 parts by mass or more and 0.5 parts by mass or less, and more preferably 0.1 parts by mass or more and 0.3 parts by mass or less, per 100 parts by mass of a polypropylene-based resin (thermoplastic resin). When nucleating agent vesicles are used, the amount of nucleating agent added to the resin material is the amount converted into the amount of nucleating agent encapsulated in the nucleating agent vesicles.
[0022] If the amount of the nucleating agent added is less than 0.05 parts by mass, the crystallinity of the polypropylene may not be improved sufficiently, and the scratch resistance of the first transparent layer 2a may not be improved sufficiently. Furthermore, if the amount of nucleating agent added exceeds 0.5 parts by mass, the spherulite growth of the polypropylene may be inhibited due to an excess of crystal nuclei, and as a result, the crystallinity of the polypropylene may not be sufficiently improved, and the scratch resistance of the first transparent layer 2a may not be sufficiently improved.
[0023] (Method to nano-size nucleating agents) In addition, the nucleating agent can be nano-sized by using, for example, a solid phase method, a liquid phase method, a gas phase method, or the like.
[0024] The solid phase method is a method in which additives are mainly mechanically pulverized to obtain nano-sized particles. For the solid phase method, a ball mill, a bead mill, a rod mill, a colloid mill, a conical mill, a disk mill, a hammer mill, a jet mill, etc. can be used. The liquid phase method is a method for synthesizing or crystallizing nano-sized particles in an additive or a solution in which the additive is dissolved, and examples of the liquid phase method that can be used include a crystallization method, a co-precipitation method, a sol-gel method, a liquid phase reduction method, and a hydrothermal synthesis method. The gas phase method is a method for synthesizing or crystallizing nano-sized particles from additives or gas or vapor formed by additives. Examples of the gas phase method that can be used include an electric furnace method, a chemical flame method, a laser method, and a thermal plasma method.
[0025] A more specific method for the nano-processing will be described below. In a specific example of the solid phase method, for example, a mixture of 100 g of isopropyl alcohol and 50 g of sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphonate is milled in a bead mill for 60 minutes using 30 μm stabilized zirconia beads to obtain nano-sized nucleating agent particles with an average particle size in the range of 100 nm to 150 nm.
[0026] In a specific example of the crystallization method, for example, a solution obtained by dissolving 50[g] of sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphonate in a mixed solvent of 96[g] of xylene, 72[g] of isopropyl alcohol, and 24[g] of water is brought into contact with a poor solvent such as ethanol in a microreactor to precipitate nano-sized nucleating agent particles with an average particle size in the range of 1[nm] to 150[nm]. The additive-encapsulating vesicle is a vesicle-like capsule having a membrane structure closed in a spherical shell shape, and particularly, one containing a liquid phase inside is called an additive-encapsulating vesicle. In the present invention, the case where an additive is contained in the liquid phase will be described.
[0027] In addition, the additive-encapsulating vesicles have extremely high dispersibility and do not cause aggregation of particles due to the mutual repulsion of the outer membranes of the vesicles, and the mutual repulsion of the outer membranes of the vesicles makes it possible to uniformly disperse the additive in the resin composition constituting each resin layer. Among the nano-processing methods, methods for obtaining nano-sized additives as additive-encapsulating vesicles (vesicle processing) that can be used include, for example, the Bangham method, extrusion method, hydration method, surfactant dialysis method, reverse phase evaporation method, freeze-thaw method, and supercritical reverse phase evaporation method.
[0028] The vesicle formation process will now be described. The Bangham method involves putting chloroform or a chloroform / methanol mixed solvent into a flask or other container, then adding and dissolving phospholipids. The solvent is then removed using an evaporator to form a thin film containing lipids, and after adding a dispersion of additives, the mixture is hydrated and dispersed in a vortex mixer to obtain vesicles.
[0029] The extrusion method is a method for obtaining vesicles by preparing a thin film of phospholipid solution and passing it through a filter instead of a mixer used as an external perturbation in the Bangham method. The hydration method is a preparation method similar to the Bangham method, but in this method, vesicles are obtained by dispersing the particles by gentle stirring without using a mixer.
[0030] The reverse phase evaporation method involves dissolving phospholipids in diethyl ether or chloroform, adding a solution containing additives to form a W / O emulsion, removing the organic solvent from the emulsion under reduced pressure, and then adding water to obtain vesicles. The freeze-thaw method uses cooling and heating as an external perturbation, and is a method for obtaining vesicles by repeating cooling and heating. In particular, a method for obtaining an additive-encapsulating vesicle having a unilamellar outer membrane includes supercritical reverse phase evaporation.
[0031] The supercritical reverse phase evaporation method is a method for producing capsules (nano-sized vesicles) encapsulating a target substance using carbon dioxide under temperature or pressure conditions in a supercritical state or above the critical point. Carbon dioxide in a supercritical state refers to carbon dioxide in a supercritical state above the critical temperature (30.98°C) and critical pressure (7.3773±0.0030MPa). Carbon dioxide under temperature or pressure conditions above the critical point means carbon dioxide under conditions where only the critical temperature or only the critical pressure exceeds the critical condition.
[0032] In the specific vesicle formation process using the supercritical reverse phase evaporation method, an emulsion of supercritical carbon dioxide and aqueous phase is generated by injecting an aqueous phase into a mixed fluid of supercritical carbon dioxide, phospholipids as an outer membrane forming substance, and additives as an encapsulating substance, and stirring the mixture.Then, by reducing the pressure, the carbon dioxide expands and evaporates, causing a phase inversion, and nanocapsules (nanovesicles) are generated in which the phospholipids cover the surface of the nucleating agent particles with a monolayer membrane. By using the supercritical reverse phase evaporation method, unlike the conventional encapsulation method in which the dispersant forms multiple layers on the surface of the additive particles, it is possible to easily produce capsules with a single layer, making it possible to prepare capsules with a smaller diameter. The nucleating agent vesicle is prepared, for example, by the Bangham method, the extrusion method, the hydration method, the surfactant dialysis method, the reverse phase evaporation method, the freeze-thaw method, the supercritical reverse phase evaporation method, etc. The nucleating agent vesicle is particularly preferably prepared by the supercritical reverse phase evaporation method.
[0033] If it is desired to make the nanocapsule into a multi-membrane capsule, it is possible to easily produce it by injecting supercritical carbon dioxide into a mixed fluid of phospholipids, additives, and an aqueous phase. Examples of phospholipids used in preparing the additive-encapsulating vesicle include glycerophospholipids such as phosphatidylcholine, phosphatidiethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiopine, yolk egg lecithin, hydrogenated yolk egg lecithin, soybean lecithin, and hydrogenated soybean lecithin, and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol. Furthermore, the additive-encapsulating vesicle can achieve excellent compatibility with resin materials by being provided with an outer membrane of phospholipids.
[0034] The additive-encapsulating vesicle may also have an outer membrane containing a dispersant, such as a polymeric surfactant, a fatty acid metal salt, a silane coupling agent, a titanate coupling agent, silicone, wax, or a modified resin. Examples of polymer surfactants include aliphatic polyvalent polycarboxylic acids, polycarboxylate alkylamines, polyacrylic acids, polymethacrylic acids, polyoxyethylene alkyl ethers, and sorbitan fatty acid esters.
[0035] Examples of fatty acid metal salts include those in which stearic acid, lauric acid, 12-hydroxystearic acid, montanic acid, behenic acid, ricinoleic acid, myristic acid, or the like is combined with lithium, sodium, potassium, magnesium, calcium, barium, zinc, aluminum, or the like. Examples of the silane coupling agent include 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0036] Titanate coupling agents include tetrakis[2,2-bis(allyloxymethyl)butoxy]titanium(IV), di-i-propoxytitanium diisostearate, (2-n-butoxycarbonylbenzoyloxy)tributoxytitanium, isopropyl titanium triisostearate, di-n-butoxy bis(triethanolaminato)titanium, tetrakis(2-ethylhexyloxy)titanium, and di-i-propoxy bis(acetylacetonato)titanium. Examples of silicones include those obtained by polymerizing olefins or pyrolyzing polyolefins, such as dimethylsilicone oil, methylphenylsilicone oil, methylhydrogensilicone oil, cyclic dimethylsilicone oil, alkyl-modified silicone oil, long-chain alkyl-modified silicone oil, and higher fatty acid-modified silicone oil, and further oxidizing or modifying them with maleic acid, sulfonic acid, carboxylic acid, rosin acid, or the like. Examples of the resin include polyolefins modified with maleic acid, sulfonic acid, carboxylic acid, rosin acid, and the like.
[0037] (The outer membrane that constitutes the nucleating agent vesicle) The outer membrane constituting the nucleating agent vesicle is, for example, composed of a monolayer membrane. Also, the outer membrane constituting the nucleating agent vesicle is, for example, composed of a substance containing a biological lipid such as a phospholipid. In the following description, a nucleating vesicle whose outer membrane is composed of a substance containing a biological lipid such as a phospholipid may be referred to as a nucleating liposome. Examples of phospholipids constituting the outer membrane include glycerophospholipids such as phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiopin, yolk egg lecithin, hydrogenated yolk egg lecithin, soybean lecithin, and hydrogenated soybean lecithin; and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol.
[0038] (Other substances that form the outer membrane) Other substances that may form the outer membrane of the vesicle include dispersants such as nonionic surfactants and mixtures of nonionic surfactants with cholesterols or triacylglycerols. As the nonionic surfactant, for example, one or more of polyglycerin ether, dialkyl glycerin, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, sorbitan fatty acid ester, polyoxyethylene polyoxypropylene copolymer, polybutadiene-polyoxyethylene copolymer, polybutadiene-poly(2-vinylpyridine), polystyrene-polyacrylic acid copolymer, polyethylene oxide-polyethylethylene copolymer, polyoxyethylene-polycaprolactam copolymer, etc. can be used.
[0039] As cholesterols, for example, cholesterol, α-cholestanol, β-cholestanol, cholestane, desmosterol (5,24-cholestadiene-3β-ol), sodium cholate, cholecalciferol, and the like can be used. The outer membrane of the liposome may also be formed from a mixture of phospholipids and a dispersing agent.
[0040] In the first embodiment, it is preferable that the nucleating agent vesicle is a radical scavenger liposome having an outer membrane formed by phospholipids. This is because by forming the outer membrane from phospholipids, it is possible to improve the compatibility between the vesicle and the resin material that is the main component of the decorative sheet 1. Note that the "main component" refers to, for example, a resin material that accounts for 50% or more by mass of the resin material that constitutes the base layer. The nucleating agent is not particularly limited as long as it is a substance that serves as a starting point for crystallization when the resin crystallizes. Examples of the nucleating agent include metal phosphate salts, metal benzoate salts, metal pimelate salts, metal rosin salts, benzylidene sorbitol, quinacridone, cyanine blue, talc, and the like. In particular, in order to maximize the effect of the nano-processing, it is preferable to use metal phosphate salts, metal benzoate salts, metal pimelate salts, and metal rosin salts that are non-melting and expected to have good transparency, but if the material itself can be made transparent by the nano-processing, colored quinacridone, cyanine blue, talc, and the like can also be used. In addition, a non-melting nucleating agent may be appropriately mixed with melting benzylidene sorbitol.
[0041] (Core layer 2b) The core layer 2b is laminated on one surface (the upper surface in FIG. 1) of the first transparent layer 2a, and is formed, for example, using a transparent polypropylene-based resin (thermoplastic resin) blended with a weathering agent. If necessary, the core layer 2b may contain one or more additives selected from various additives such as a filler, an ultraviolet absorber, a light stabilizer, a heat stabilizer, an antioxidant, an antistatic agent, a lubricant, a flame retardant, an antibacterial agent, an antifungal agent, an antifriction agent, a light scattering agent, and a gloss adjuster.
[0042] (Second transparent layer) The second transparent layer 2c is laminated on one surface (the upper surface in FIG. 1) of the core layer 2b, and is made of a transparent polypropylene-based resin (thermoplastic resin). In addition to a dispersant as a nano-sized additive, an inorganic filler is added to the second transparent layer 2c. Based on the above, in the first embodiment, a configuration of the base material layer 2 is described in which the base material layer 2 is formed of two types of three layers, that is, a first transparent layer 2a, a core layer 2b, and a second transparent layer 2c, stacked in that order.
[0043] (Characteristics of the base layer) The decorative sheet 1 is characterized in that the base layer 2 contains a resin material and a nucleating agent. Furthermore, the decorative sheet 1 is characterized in that a nucleating agent encapsulated in vesicles is added to the resin material to crystallize the resin material when forming the base layer 2. By adding the nucleating agent encapsulated in vesicles to the resin composition, the dispersibility of the nucleating agent in the resin material, i.e., in the base layer 2, is dramatically improved. On the other hand, it may be difficult to directly identify the nucleating agent encapsulated in the vesicle based on the structure and properties of the finished decorative sheet 1, depending on the circumstances, and it may be considered impractical. The reasons for this are as follows.
[0044] The nucleating agent added in the form of a vesicle is dispersed with high dispersibility, and is highly dispersed in the base layer even in the laminate state, which is the precursor of the produced decorative sheet 1. However, in the process of producing the decorative sheet 1, the laminate is usually subjected to various treatments such as compression and hardening, which may cause the outer membrane of the vesicles encapsulating the nucleating agent to break down or cause chemical reactions. Therefore, depending on the processing process of the decorative sheet 1, there is a high possibility that the outer membrane of the nucleating agent in the finished decorative sheet 1 may be broken down, or the state of the chemical reaction may vary, resulting in the nucleating agent not being encapsulated (enveloped) by the outer membrane.
[0045] Furthermore, when the nucleating agent is not encapsulated in the outer membrane, it is difficult to specify the physical properties of the nucleating agent itself within a numerical range, and it is also anticipated that it may be difficult to determine whether the material constituting the crushed outer membrane is the outer membrane of the vesicle or a material added separately from the nucleating agent. Thus, although the present disclosure differs from the prior art in that the nucleating agent is highly dispersed in the decorative sheet 1, it is anticipated that there may be cases in which it is impractical to determine the structure and characteristics of the decorative sheet 1 within a numerical range analyzed based on measurements, whether this is because the nucleating agent is added in the form of vesicles encapsulating the nucleating agent.
[0046] As described above, the base layer 2 contains a dispersion material as a nano-sized additive. The base layer 2 is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to a polypropylene-based thermoplastic resin. Furthermore, the amount of the nucleating agent vesicles added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicles, per 100 parts by mass of the polypropylene-based thermoplastic resin.
[0047] In addition, the first transparent layer 2a and the second transparent layer 2c are formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based thermoplastic resin. Additionally, nucleating vesicles are nucleating liposomes with an outer membrane formed using phospholipids. Furthermore, the nucleating agent vesicle is formed by encapsulating the nucleating agent in a vesicle having a monolayer membrane, and then forming the vesicle by supercritical reverse phase evaporation.
[0048] <Colored layer> The colored layer 3 is laminated on the other surface (the lower surface in FIG. 1) of the base layer 2 with the picture pattern layer 4 sandwiched therebetween. That is, the colored layer 3 is laminated on the surface of the picture pattern layer 4 opposite to the surface facing the base layer 2 (the lower surface in FIG. 1). The colored layer 3 is formed, for example, transparent or semi-transparent, using a known printing method (for example, gravure printing method).
[0049] <Pattern layer> The picture pattern layer 4 is laminated on the other surface of the base layer 2, and is a layer on which a picture is formed to impart design features to the decorative sheet 1. The picture pattern layer 4 is formed by printing a picture with a urethane resin by, for example, gravure printing. Note that, as a printing method for forming the picture pattern layer 4, various printing methods can be used other than gravure printing, such as offset printing, letterpress printing, flexographic printing, screen printing, inkjet printing, and electrostatic printing.
[0050] The type of pattern formed on the picture pattern layer 4 can be any type depending on the purpose of use, the preferences of the user, etc., and can be a wood grain pattern, a stone pattern, a fabric pattern, an abstract pattern, a geometric pattern, letters, symbols, a solid color, or a combination thereof. The type of pattern can also be, for example, a full-surface solid print. As the printing ink used to form the picture pattern layer 4, in addition to the urethane resin, for example, organic or inorganic dyes, pigments, and other colorants can be used.
[0051] The weight of the picture pattern layer 4 after drying is preferably 0.1 [g / m 2 ] or more than 15[g / m 2 ] or less, more preferably 3 [g / m 2 ] or more than 10[g / m 2 ] or less, more preferably 6 [g / m 2 ] or more than 9 [g / m 2 ] is within the following range. In addition, the picture pattern layer 4 may be configured to have, for example, a solid colored base material layer for concealing the color and pattern of the base to which the decorative sheet 1 is attached, and a picture layer for adding a picture to impart design features.
[0052] The thickness of the picture pattern layer 4 is set within the range of 1 μm to 10 μm, preferably 0.1 μm to 10 μm, more preferably 0.5 μm to 5 μm, and even more preferably 0.7 μm to 3 μm. This is because when the thickness of the picture pattern layer 4 is 1 μm or more, it is possible to make the printing clear. Also, when the thickness of the picture pattern layer 4 is 10 μm or less, it is possible to improve the printing workability when manufacturing the decorative sheet 1 and to suppress the manufacturing cost. In addition, functional additives such as extender pigments, plasticizers, dispersants, surfactants, tackifiers, adhesive aids, drying agents, hardeners, hardening accelerators, and hardening retarders may be added to the picture pattern layer 4 in order to impart various functions.
[0053] <Surface protective layer> The surface protective layer 5 (top coat) is laminated on one surface of the base layer 2 (the upper surface in FIG. 1). The surface protective layer 5 is formed using an aqueous coating liquid.
[0054] The aqueous coating liquid contains a polycarbonate-based urethane resin and a carbodiimide curing agent. The surface protective layer 5 is formed of a cured coating film formed by curing an aqueous coating liquid. Specifically, the surface protective layer 5 is formed by applying a coating material for the topcoat layer, which is an aqueous coating liquid, to one surface of the base layer 2 and curing the coating material.
[0055] The surface protective layer 5 includes an undercoat layer 5a and an overcoat layer 5b. The undercoat layer 5a is formed on one surface of the base layer 2, and is formed by applying a coating material containing at least the components of polycarbonate-based urethane resin and a carbodiimide curing agent to a thickness of, for example, 6 μm.
[0056] The topcoat layer 5b is laminated on one surface of the undercoat layer 5a (the upper surface in FIG. 1) and is formed by applying the same resin as the undercoat layer 5a but with a lower gloss, for example. That is, the topcoat layer 5b has a lower gloss than the undercoat layer 5a. The topcoat layer 5b is formed by printing a pattern that is in harmony with the pattern formed on the picture pattern layer 4.
[0057] Specifically, the topcoat layer 5b of the surface protection layer 5 is provided with a gloss coat and a matte coat. At least one of the lines formed by the gloss coated portions and the lines formed by the matte coated portions of the topcoat layer 5b and the lines forming the pattern formed in the pattern layer 4 at least partially overlap each other when viewed from the direction in which the pattern layer 4, the base layer 2, and the surface protection layer 5 are stacked. In addition, the lines formed by the parts that are coated with a gloss coat, the lines formed by the parts that are coated with a matte coat, and the lines forming the pattern formed in the pattern layer 4 are lines that form vessels when the pattern is, for example, a wood grain pattern.
[0058] 2, the lines GL formed by the gloss coated portion and the lines KL forming the pattern formed in the picture pattern layer 4 at least partially overlap each other when viewed from the direction in which the picture pattern layer 4, the base material layer 2, and the surface protective layer 5 are laminated. As a result, the surface protective layer 5 is formed by printing a pattern that is in harmony with the pattern formed in the picture pattern layer 4. Although not shown in the drawings, the lines formed by the matte coated portions and the lines KL forming the pattern formed in the picture pattern layer 4 may at least partially overlap each other when viewed from the direction in which the picture pattern layer 4, the base layer 2, and the surface protective layer 5 are stacked. Also, although not shown in the drawings, the lines GL formed by the gloss coated portions, the lines formed by the matte coated portions, and the lines KL forming the pattern formed in the picture pattern layer 4 may at least partially overlap each other when viewed from the direction in which the picture pattern layer 4, the base layer 2, and the surface protective layer 5 are stacked.
[0059] The materials constituting the surface protective layer 5 will be described in detail below. As a material for forming the surface protection layer 5, for example, an ionizing radiation curable resin or a thermosetting resin is suitably used.
[0060] As the ionizing radiation curable resin, for example, known resins such as various monomers and commercially available oligomers can be used. Specifically, it is preferable to use polyfunctional monomers such as pentaerythritol triacrylate (PET3A), pentaerythritol tetraacrylate (PET4A), trimethylolpropane triacrylate (TMPTA), dipentaerythritol hexaacrylate (DPHA), etc., polyfunctional oligomers such as Shikou UV-1700B (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), or mixtures of the above-mentioned materials.
[0061] As the thermosetting resin, for example, one formed by thermally curing a polymer containing a carboxy group, which will be described below, and a carbodiimide compound (carbodiimide curing agent) which is a curing agent component, is preferable. The polymer containing a carboxy group is not particularly limited, and may be, for example, a polymer capable of imparting mechanical characteristics due to elongation of the molecular structure or the like to the surface protective layer 5. The polymer containing a carboxy group is appropriately selected from, for example, various acrylic polymers, various polyesters, various polyethers, various polycarbonates, various polyurethanes, and the like.
[0062] Among the above-mentioned resins, polycarbonate-based urethane resin is most preferable as the resin material constituting the surface protective layer 5. The polycarbonate-based urethane resin is a urethane resin having polycarbonate diol as a structural unit and obtained by reacting with an isocyanate compound or a diol compound. The carbodiimide compound which is the curing agent component is not particularly limited as described above, but examples thereof include diisopropylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, N-3-dimethylaminopropyl-N'-ethylcarbodiimide, N-tert-butyl-N'-ethylcarbodiimide, N-cyclohexyl-N'-2-morpholinoethylcarbodiimide meso-p-toluenesulfonic acid, and N,N'-di-tert-butylcarbodiimide.
[0063] The amount of the carbodiimide compound added is preferably an equivalent ratio (molar equivalent of carbodiimide / molar equivalent of carboxy groups in polycarbonate-based urethane resin) of the molar equivalent of carbodiimide (mmol / g) to the molar equivalent of carboxy groups in polycarbonate-based urethane resin (mmol / g), calculated from the carbodiimide equivalent (NCN equivalent) and the acid value (mgKOH / g) of the polycarbonate-based urethane resin, of 1 or more, more preferably 1.2 or more, and even more preferably 1.3 or more. This is because when the equivalent ratio is 1 or less, the crosslink density becomes low, resulting in deterioration of scratch resistance and deterioration of stain resistance.
[0064] There is no particular upper limit to the amount of carbodiimide compound added, but the equivalent ratio of the molar equivalent (mmol / g) of carbodiimide to the molar equivalent (mmol / g) of carboxy groups in the polycarbonate-based urethane resin (molar equivalent of carbodiimide / molar equivalent of carboxy groups in polycarbonate-based urethane resin) is preferably 2 or less, more preferably 1.8 or less, and even more preferably 1.6 or less. This is because when the amount of carbodiimide compound added exceeds 2 in equivalent ratio, the content of polycarbonate-based urethane resin becomes relatively small and the amount of carbodiimide compound that does not contribute to the curing reaction becomes large, so that the hardness of the surface protection layer 5 may not be sufficiently increased.
[0065] The resin contained in the surface protective layer 5 may be a resin in which a polycarbonate-based urethane polymer (polycarbonate-based urethane resin) having an acid value of 10 mgKOH / g or more is crosslinked with a curing agent (for example, the above-mentioned carbodiimide curing agent). More preferably, the resin is a polycarbonate-based urethane polymer having a glass transition temperature of 80° C. or more and an acid value of 10 mgKOH / g or more crosslinked with a curing agent. If the glass transition temperature is 80° C. or lower, the surface hardness of the surface protective layer 5 decreases, and the scratch resistance may decrease. If the acid value is 10 mg KOH / g or lower, the crosslink density after curing is low, and the scratch resistance may decrease.
[0066] The upper limit of the glass transition temperature of the polycarbonate-based urethane polymer contained in the surface protective layer 5 is not particularly limited, but is preferably 200° C. or less, more preferably 180° C. or less, and even more preferably 160° C. or less. This is because if the glass transition temperature of the resin constituting the surface protective layer 5 exceeds 200° C., the surface hardness of the surface protective layer 5 becomes too high, which may weaken the layer against external impacts. The upper limit of the acid value of the polycarbonate-based urethane polymer contained in the surface protective layer 5 is not particularly limited, but is preferably 200 mgKOH / g or less, more preferably 100 mgKOH / g or less, and even more preferably 50 mgKOH / g or less. This is because if the acid value of the resin constituting the surface protective layer 5 exceeds 200 mgKOH / g, the crosslink density after curing becomes too high, which may make the layer vulnerable to external impacts.
[0067] Furthermore, the polycarbonate-based urethane polymer contained in the surface protective layer 5 is preferably applied in the form of an aqueous emulsion together with a curing agent. This is because, when the polycarbonate-based urethane polymer contained in the surface protective layer 5 is applied in the form of an aqueous emulsion together with a curing agent, a resin coating having a high molecular weight is obtained, and the surface hardness of the surface protective layer 5 is improved, as well as the stain resistance. Here, "aqueous emulsion" refers to an emulsion formed in water or a lower alcohol as a dispersion medium. The undercoat layer 5a and the topcoat layer 5b may each be a layer composed of a cured coating film containing at least a polycarbonate-based urethane resin and a carbodiimide curing agent, and therefore the undercoat layer 5a and the topcoat layer 5b may be cured coating films having different compositions or the same composition.
[0068] For example, the amount of the carbodiimide compound added may be greater or less than that of the topcoat layer 5b in terms of equivalent ratio (molar equivalent of carbodiimide / molar equivalent of carboxy group in polycarbonate-based urethane resin) in the undercoat layer 5a. This is because by providing a difference in the amount of the carbodiimide compound added between the undercoat layer 5a and the topcoat layer 5b, it is possible to impart flexibility to the entire surface protective layer 5. When there is a difference in the amount of carbodiimide compound added between the undercoat layer 5a and the topcoat layer 5b, the above-mentioned effect can be obtained by setting the amount of carbodiimide compound added in one layer within the range of 1.1 to 2.0 times the amount added in the other layer, more preferably within the range of 1.3 to 1.5 times.
[0069] Generally, fillers are added to the surface protective layer 5 as gloss regulators, and for example, organic materials such as acrylic beads and silicone beads, and inorganic materials such as alumina and silica can be used. In particular, silica (silica filler) formed using an inorganic material is preferable in terms of scratch resistance. Silica exhibits good scratch resistance compared to other materials, which is believed to be due to the fact that silica has an appropriate hardness. The particle size of the silica (average particle size D50) is preferably 9 [μm] or less, more preferably 7 [μm] or less, and even more preferably 5 [μm] or less. If the particle size of the silica exceeds 9 [μm], it is not preferable because the particles are likely to be chipped during the scratch test.
[0070] The lower limit of the particle size of silica is not particularly limited, but is preferably 1 [μm] or more, more preferably 2 [μm] or more, and even more preferably 3 [μm] or more. This is because if the particle size of silica added to the surface protective layer 5 is less than 1 [μm], the function as a gloss regulator may not be exerted. Moreover, it is preferable that the silica has a pore volume of 1 [mL / g] or more. When the pore volume of silica is large (specifically, 1 [mL / g] or more), the silica tends to have excellent scratch resistance, which is thought to be due to the influence of the binder resin component being impregnated into the silica pores. In addition, silica with a large pore volume has a large function of reducing gloss, and is also effective in reducing the amount of gloss regulator required to be added. The content of the gloss regulator is preferably in the range of 1 mass [%] to 30 mass [%], more preferably in the range of 2 mass [%] to 20 mass [%], based on the total mass of the surface protective layer 5. As described above, when silica (silica filler) having a pore volume of 1 mL / g or more is added as a gloss adjuster, the content of silica is preferably in the range of 1 mass [%] or more and 30 mass [%] or less, relative to the total mass of the surface protection layer 5, and more preferably in the range of 2 mass [%] or more and 20 mass [%] or less.
[0071] The silica may be in a spherical shape. Furthermore, from the viewpoint of physical property stability (imparting scratch resistance functionality), when silica (silica filler) is added only to the undercoat layer 5a, the silica content is preferably in the range of 10 mass [%] or more and 30 mass [%] or less, and more preferably in the range of 15 mass [%] or more and 25 mass [%] or less, relative to the total mass of the undercoat layer 5a. In addition, silica preferably has an oil absorption in the range of 100 [mL / 100g] to 200 [mL / 100g], more preferably 150 [mL / 100g] to 180 [mL / 100g], and even more preferably 160 [mL / 100g] to 170 [mL / 100g]. This is because silica tends to have excellent scratch resistance when it has a large oil absorption (specifically, in the range of 100 [mL / 100g] to 200 [mL / 100g]), and this is thought to be due to the increased affinity between the binder resin component and the silica surface. In addition, silica with a large oil absorption has a large function of reducing gloss, and also has a large effect of reducing the amount of gloss regulator required to be added. Therefore, when silica (silica filler) having an oil absorption in the range of 100 [mL / 100g] to 200 [mL / 100g] is added as a gloss regulator, the content of silica is preferably in the range of 1 mass [%] to 30 mass [%], more preferably in the range of 2 mass [%] to 20 mass [%], based on the total mass of the surface protective layer 5. Moreover, the content of silica is further preferably in the range of 10 mass [%] to 15 mass [%], based on the total mass of the surface protective layer 5.
[0072] In the first embodiment, a configuration may be adopted in which a filler is added only to the undercoat layer 5a and no filler is added to the topcoat layer 5b. Furthermore, in order to impart various functions to the surface protective layer 5, various additives such as a heat stabilizer, an antiblocking agent, a catalyst scavenger, a colorant, a light scattering agent, an antibacterial agent, and an antifungal agent may be blended.
[0073] If necessary, an ultraviolet absorbing agent or a light stabilizer can be added as a weathering agent to the surface protective layer 5. As the ultraviolet absorbing agent, for example, a benzotriazole-based agent, a benzoate-based agent, a benzophenone-based agent, a triazine-based agent, or the like is generally added. As the light stabilizer, for example, a hindered amine-based agent, or the like is generally added in any combination. That is, the surface protective layer 5 may contain an ultraviolet absorber having a triazine skeleton and a light stabilizer having a NOR skeleton as a weathering agent. The content of the ultraviolet absorber having a triazine skeleton in the surface protective layer 5 is preferably in the range of 1 mass [%] to 15 mass [%], more preferably in the range of 3 mass [%] to 6 mass [%], based on the total mass of the surface protective layer 5. The content of the light stabilizer having a NOR skeleton in the surface protective layer 5 is preferably in the range of 1 mass [%] to 10 mass [%], more preferably in the range of 3 mass [%] to 6 mass [%], based on the total mass of the surface protective layer 5. If the content of the ultraviolet absorber having a triazine skeleton and the content of the light stabilizer having a NOR skeleton are within the above-mentioned numerical ranges, it is possible to further improve the weather resistance while maintaining the basic functions of the surface protective layer 5, such as scratch resistance and contamination resistance.
[0074] In the surface protective layer 5, the content of the ultraviolet absorber having a triazine skeleton is preferably higher than the content of the light stabilizer having a NOR skeleton, and is preferably within a range of 1.5 to 3 times. If the content of the ultraviolet absorber having a triazine skeleton is within the above-mentioned range, it is possible to further improve the weather resistance while maintaining the basic functions of the surface protective layer 5, such as scratch resistance and contamination resistance. The undercoat layer 5a and the topcoat layer 5b constituting the surface protective layer 5 may each contain an ultraviolet absorber and a light stabilizer. For example, the undercoat layer 5a and the topcoat layer 5b may contain different types of ultraviolet absorbers and light stabilizers, or may contain the same types of ultraviolet absorbers and light stabilizers.
[0075] The amounts of the ultraviolet absorber and the light stabilizer added may be greater or less in the undercoat layer 5a than in the topcoat layer 5b. When there is a difference between the amounts of the ultraviolet absorber and the light stabilizer added in the undercoat layer 5a and the topcoat layer 5b, it is preferable to set the amount added in one layer within a range of 1.1 to 2.0 times, more preferably 1.5 to 2.0 times, of the amount added in the other layer, since this provides weather resistance that does not cause problems in use. Furthermore, particulate polyethylene wax can be added to the surface protective layer 5 as a lubricant (wax) if necessary. Here, "polyethylene wax" refers to low molecular weight polyethylene having a molecular weight of tens of thousands or less. Also, "wax" refers to "a solid or semi-solid substance at room temperature, with a melting point of 40°C or higher, which melts without decomposing when heated, and has low viscosity."
[0076] As the polyethylene wax, for example, the "Sanwax" series manufactured by Sanyo Chemical Industries, Ltd. or the "Hiwax" series manufactured by Mitsui Chemicals, Inc. can be used. The content of the polyethylene wax in the surface protective layer 5 is preferably in the range of 1 mass [%] to 10 mass [%], and more preferably in the range of 3 mass [%] to 6 mass [%], relative to the total mass of the surface protective layer 5. If the content of the polyethylene wax is within the above-mentioned numerical range, it is possible to further improve the contamination resistance while maintaining the basic functions of the surface protective layer 5, such as scratch resistance. The lubricant that can be added to the surface protective layer 5 is not limited to the particulate polyethylene wax described above, and may be, for example, a particulate polyester wax.
[0077] In order to impart functionality to the surface of the decorative sheet 1, the wax may be added only to the topcoat layer 5b without being added to the undercoat layer 5a. When wax is added only to the topcoat layer 5b, the wax content is preferably in the range of 10 mass [%] or more and 30 mass [%] or less, and more preferably in the range of 15 mass [%] or more and 25 mass [%] or less, relative to the total mass of the topcoat layer 5b. In addition, an antibacterial agent containing silver-supported phosphate can be added to the surface protective layer 5, if necessary. The phosphate is not particularly limited as long as it is known, but it is preferable that it contains one or more metals selected from the group including silver, titanium, cerium, zirconium, germanium, potassium, aluminum, and gallium. Isotopes of these metals can be used. In view of antibacterial ability, silver is particularly preferable. In addition, a known method is used as a method for producing the phosphate.
[0078] The silver-loaded phosphate was 1×10 -4 It is preferably used within the range of 1 to 15 mass% by mass, more preferably 3 to 10 mass% by mass, and most preferably 5 to 8 mass% by mass. This is because the antibacterial ability is reliably exhibited if the content of silver-supported phosphate is within the above-mentioned range. Here, in order to obtain antibacterial performance, it is preferable to add a relatively large amount of antibacterial agent, and conversely, in terms of surface strength, it is preferable to add a relatively small amount of antibacterial agent, and if the amount added is large, it is difficult to obtain sufficient surface strength. Specifically, for example, when the thickness D of the surface protective layer 5 is within the range of 3 [μm] to 20 [μm], the amount of antibacterial agent added is 1×10 with respect to the mass of the entire surface protective layer 5, as described above. -4 The antibacterial agent is preferably added in an amount of 1×10 to 20% by mass. -4 If it is less than 20% by mass, antibacterial performance cannot be exhibited, and if it is more than 20% by mass, it is difficult to ensure surface strength.
[0079] The particle size (average particle size D50) of the silver-loaded phosphate is preferably 1 [μm] or more. If the particle size is less than 1 [μm], the dispersibility decreases, and there is a possibility that the function as an antibacterial agent will not be exerted. The upper limit of the particle size of the silver-loaded phosphate is not particularly limited, but is preferably 10 μm or less, for example. If the particle size of the silver-loaded phosphate added to the surface protective layer 5 exceeds 10 μm, the antibacterial agent is likely to be chipped off in the scratch test, which is not preferable. The particle diameter of the antibacterial agent is 1 [μm] or more, and is preferably within a range of 0.1 to 1.0 times, and more preferably 0.3 to 0.4 times, the thickness D of the surface protective layer 5. This is because if the average particle diameter of the antibacterial agent is less than 0.1 times the thickness D of the surface protective layer 5, the dispersibility of the antibacterial agent decreases, making it difficult to obtain a sufficient antibacterial effect, and if it exceeds 1.0 times, the surface hardness may decrease.
[0080] In addition, when the above-mentioned antibacterial agent having a particle diameter of 1 [μm] or more and within a range of 0.1 to 1.0 times the thickness D of the surface protective layer 5 is defined as a "first antibacterial agent", and the antibacterial agent having a particle diameter of 1 [μm] or more and within a range of 1.4 to 1.6 times the thickness D of the surface protective layer 5 is defined as a "second antibacterial agent", the surface protective layer 5 may contain the first antibacterial agent and the second antibacterial agent. That is, the surface protective layer 5 may contain two or more types of antibacterial agents having different average particle diameters. By containing the second antibacterial agent, the second antibacterial agent protrudes from the surface of the surface protective layer 5, and the second antibacterial agent exerts an antibacterial effect.
[0081] Furthermore, the ratio of the amount of the first antibacterial agent added to the amount of the second antibacterial agent added (amount of the first antibacterial agent added / amount of the second antibacterial agent added) may be within a range of 1.5 to 10, more preferably within a range of 2 to 8, and even more preferably within a range of 3 to 5. When the ratio of the amount of the first antibacterial agent added / the amount of the second antibacterial agent added is within the above-mentioned numerical range, a high antibacterial effect can be obtained. Furthermore, the first antibacterial agent and the second antibacterial agent may be the same type of antibacterial agent (for example, the same type of silver-based antibacterial agent), or may be different types of antibacterial agents. As the antibacterial agent that can be added to the surface protective layer 5, in addition to the above-mentioned silver-supported phosphate, inorganic antibacterial agents such as antibacterial zeolite, antibacterial apatite, and antibacterial zirconia formed by incorporating any one of metal ions, such as silver ions, copper ions, and zinc ions, into inorganic compounds such as zeolite, apatite, and zirconia can be used. As the antibacterial agent, organic antibacterial agents such as zinc pyridione, 2-(4-thiazolyl)-benzimidazole, 10,10-oxybisphenoxanodine, organic titanium sulfur halogens, and pyridine-2-thiol-oxide can be used, but silver-based antibacterial agents (antibacterial agents containing silver-based materials) are superior in terms of antibacterial effect.
[0082] The antibacterial agent may be a silver-based material supported on an inorganic material. As the "inorganic material", for example, "glass" can be used. By supporting the silver component (silver-based material) on an inorganic substance, it is possible to prevent the silver component from falling off over time and from transferring to adjacent layers. The antibacterial agent may also contain finely ground silver. Specific examples of antibacterial agents that can be used in the first embodiment include diiodomethyl complex (product name: PBM-H7, manufactured by MIC), calcined calcium hydroxide (product name: Scallow, manufactured by Bacteriological Research Institute), and Biocide TB-B100 (product name) (manufactured by Taisho Technos Co., Ltd.).
[0083] In the above-described embodiment, an antibacterial agent is added to the surface protective layer 5. However, the antibacterial agent to be added may be an antiviral agent having antiviral properties. In other words, an antiviral agent may be added to the surface protective layer 5 instead of an antibacterial agent, or both an antibacterial agent and an antiviral agent may be added to the surface protective layer 5. When the antiviral agent is added to the surface protective layer 5, the amount added, the average particle size, and the like may be the same as those of the above-mentioned antibacterial agent. As in the case of the antibacterial agent, two or more types of antiviral agents having different average particle sizes may be added to the surface protective layer 5.
[0084] Furthermore, the resin constituting the surface protective layer 5 contains at least a polycarbonate-based urethane resin and a carbodiimide curing agent, and therefore has a crosslinked structure. It is possible to block migration of the antibacterial agent containing a silver component by forming the surface protective layer 5 into a crosslinked structure. The crosslinked structure can be crosslinked by high energy such as ultraviolet light or an electron beam, or by heat, to increase the degree of crosslinking, thereby further suppressing migration of the antibacterial agent containing a silver component.
[0085] Furthermore, like the wax described above, the antibacterial agent described above may also be added only to the topcoat layer 5b and not to the undercoat layer 5a in order to impart functionality to the surface of the decorative sheet 1. When the antibacterial agent is added only to the topcoat layer 5b, the content of the antibacterial agent is 1×10 -4 The range is preferably from 1 to 20 mass [%] by mass, more preferably from 1 to 20 mass [%] by mass, and even more preferably from 10 to 20 mass [%] by mass. There is no particular limitation on the method for forming the surface protective layer 5. The surface protective layer 5 may be formed by applying a coating liquid of the above-mentioned material by a normal method such as gravure coating, microgravure coating, comma coating, knife coating, or die coating, and then curing the coating by a method suitable for the material, such as heat curing or ultraviolet curing.
[0086] The undercoat layer 5a and the topcoat layer 5b constituting the surface protective layer 5 may have the same thickness. The undercoat layer 5a may be thicker or thinner than the topcoat layer 5b. It is more preferable that the undercoat layer 5a is thicker than the topcoat layer 5b. When there is a difference in thickness between the undercoat layer 5a and the topcoat layer 5b, it is preferable to set the thickness of one within the range of 1.1 to 2.0 times the thickness of the other, more preferably within the range of 1.5 to 2.0 times, since this provides scratch resistance to an extent that does not cause problems in use.
[0087] <Moisture-proof layer> The moisture-proof layer 6 is formed on the other surface of the base layer 2, and is formed by laminating, for example, an anchor coat layer, a deposition layer, and an overcoat layer (not shown). Note that in Fig. 1, the moisture-proof layer 6 is illustrated as a single layer. The anchor coat layer is a layer containing a first polyolefin having at least one material selected from the group consisting of a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0088] The vapor-deposited layer is disposed between the anchor coat layer and the overcoat layer, and is a layer formed by vapor-depositing a metal or an inorganic compound. The overcoat layer is a layer containing a second polyolefin having at least one material selected from the group consisting of a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0089] <Primer layer> The primer layer 7 is formed by laminating the colored layer 3, the pattern layer 4, and the moisture-proof layer 6 on the other side of the base layer 2, sandwiching them therebetween, and is formed by applying a primer (undercoat) to the other side of the moisture-proof layer 6 (the lower surface in Figure 1). The function of the primer layer 7 is mainly to improve adhesion, and further includes surface stabilization after surface treatment, corrosion prevention of metal surfaces, imparting adhesion, and preventing deterioration of adhesives.
[0090] The primer layer 7 is formed by, for example, a gravure printing method so that the solid content is 1 [g / m 2 ] is formed by coating a urethane resin. For example, urethane-based, acrylic-based, ethylene-vinyl acetate copolymer, vinyl chloride-vinyl acetate copolymer, polyester-based, etc. can be used for the primer layer 7. In particular, a two-component curing urethane-based primer agent made by blending polyester polyol and polyisocyanate is preferable. In addition, if inorganic powder such as silica, barium sulfate, calcium carbonate, etc. is added to the material for the primer layer 7 to form the primer layer 7, it is effective in improving the adhesive strength by the anchoring effect.
[0091] (Method of manufacturing decorative sheets) The manufacturing method for producing the decorative sheet 1 is an in-line method for producing the decorative sheet 1, and includes a first step, a second step, and a third step. Here, "in-line" means that there is no lamination process for laminating films together, and printing, which is usually performed in multiple steps, can be processed in one line. In other words, in the method for producing the decorative sheet 1, the production process from printing to providing the surface protective layer 5 can be performed in a single in-line process.
[0092] (1) First step The first step is a step of manufacturing a base layer 2 formed by extrusion molding a core layer 2b made of a transparent polypropylene-based thermoplastic resin, and a first transparent layer 2a and a second transparent layer 2c made of a thermoplastic resin to which a dispersant as a nano-sized additive has been added.
[0093] (2)Second process The second step is a step of forming a surface protective layer 5 on one surface of the base layer 2 produced in the first step. In the second step, that is, the step of forming the surface protective layer 5, a coating material for the top coat layer, which is an aqueous coating liquid, is applied to one surface of the base layer 2 to form the surface protective layer 5. Furthermore, the surface protective layer 5 is formed by first applying a coating material for a topcoat undercoat layer, which contains a polycarbonate-based urethane resin, a carbodiimide curing agent, an inorganic filler, an ultraviolet absorbing agent, and a light stabilizer, to one side of the base layer 2 to form an undercoat layer 5a. Then, a coating material for a topcoat overcoat layer, which contains a polycarbonate-based urethane resin, a carbodiimide curing agent, a wax, an ultraviolet absorbing agent, a light stabilizer, and an antibacterial agent, is applied to the undercoat layer 5a to form an overcoat layer 5b. This forms the surface protective layer 5. Here, the coating material for the topcoat layer (coating material for the topcoat undercoat layer, coating material for the topcoat topcoat layer) may contain at least a polycarbonate-based urethane resin and a carbodiimide curing agent. In addition, it is preferable that the polycarbonate-based urethane resin has an acid value of 10 mgKOH / g or more and is contained in the coating material for the topcoat layer (coating material for the topcoat undercoat layer, coating material for the topcoat topcoat layer) in the form of an aqueous emulsion.
[0094] (3) Third step The third step is a step of forming a colored layer 3, a picture pattern layer 4, and a primer layer 7 on the other surface (the lower surface in Figure 1) of the base layer 2 produced in the first step, either after the second step or prior to the second step. The layers formed in the third step are not limited to three layers, namely, the colored layer 3, the picture pattern layer 4, and the surface protective layer 5, but may be, for example, one layer, two layers, or four or more layers. Therefore, the method for producing the decorative sheet 1 is carried out in one of two orders: the first step, the second step, and the third step, or the first step, the third step, and the second step.
[0095] <Decorative board> The configuration of the decorative board 10 will be described with reference to FIG. As shown in FIG. 1, the decorative board 10 is formed, for example, in a plate shape, and includes a decorative sheet 1, a substrate 8, and a moisture-proof film 9.
[0096] <Substrate> The substrate 8 is disposed on the decorative sheet 1 on the other side of the primer layer 7 (the lower surface in FIG. 1). The material of the substrate 8 may be any type, such as wood, steel, or resin. For example, a non-combustible steel plate or a non-combustible material as specified by Notification No. 1400 of the Ministry of Construction may be used.
[0097] Furthermore, the substrate 8 has a folded structure or a three-dimensional structure. When the decorative sheet 1 is laminated onto the substrate 8, it may be laminated via an appropriately selected adhesive as necessary, or it may be laminated without an adhesive or the like.
[0098] The decorative sheet 1 can be laminated and bonded to the substrate 8 by a method of contacting a metal plate and pressing it with a flat pressure, or a continuous lamination method using a circular pressure system. In particular, the continuous lamination method using an endless metal belt makes it possible to continuously produce a high-quality decorative board 10 at high speed that is free of surface warping or waviness, has good interlayer adhesion, and is densely cured and integrated.
[0099] <Moisture-proof film> The moisture-proof film 9 is laminated, for example, via an adhesive or the like, on the surface of the substrate 8 opposite the surface facing the decorative sheet 1 (the lower surface in FIG. 1). The moisture-proof film 9 is formed, for example, by using a polypropylene moisture-proof film laminated with a gas barrier layer formed of a composition of a (meth)acrylic acid polymer and an ethylene-vinyl alcohol copolymer.The moisture-proof film 9 is formed, for example, by using a transparent polypropylene film stretched in the transverse direction, coated with a gas barrier layer formed of a (meth)acrylic acid polymer and an ethylene-vinyl alcohol copolymer on a laminated sheet obtained by co-extrusion of polypropylene and modified polypropylene polymer.
[0100] The above-described first embodiment is one example of the present invention, and the present invention is not limited to the above-described first embodiment. Various modifications can be made depending on the design, etc., even if the modifications are in a form other than the first embodiment, as long as they do not deviate from the technical idea of the present invention.
[0101] (Effects of the First Embodiment) The decorative sheet 1 of the first embodiment can achieve the effects described below. (1) The substrate comprises a base layer 2 formed using a polypropylene-based resin, a surface protection layer 5 laminated on one side of the base layer 2 and formed using an aqueous coating liquid, and a pattern layer 4 laminated on the other side of the base layer 2 and having a pattern formed thereon. The aqueous coating liquid contains a polycarbonate-based urethane resin and a carbodiimide curing agent. The surface protection layer 5 is formed of a cured coating film formed by curing the aqueous coating liquid. As a result, it is possible to provide a decorative sheet 1 that is capable of suppressing deterioration in weather resistance, scratch resistance, and stain resistance.
[0102] In addition, since no lamination step with other sheets is required during production, the number of production steps can be reduced, and further, the production steps can be performed in a single in-line process. In addition, because the decorative sheet 1 is a single layer, it is easy to make it thinner, unlike multi-layer decorative sheets. Furthermore, because the decorative sheet 1 is a single layer, it is possible to reduce the amount of CO2 emissions until the decorative sheet 1 is completed, compared to a configuration in which multiple decorative sheets are produced and bonded together.
[0103] Furthermore, since the surface protective layer 5 is formed by applying an aqueous coating liquid to the base layer 2, it is possible to form the surface protective layer 5 using water as a solvent. Therefore, compared to a configuration in which the surface protective layer 5 is formed using a solvent that has health and environmental problems such as the effects on the human body due to exhaust gases and exhaust gases, this is superior in terms of health and the environment, and since deinking is easy, it is possible to ensure that the decorative sheet 1 is in a state with little dirt when reused, making it possible to reduce CO2 emissions. "Deinking" refers to the process of removing ink from printed waste paper and other materials to produce DIP (Deinked Pulp). When removing ink from waste paper and other materials to produce DIP, a deinking agent is used as a chemical.
[0104] As deinking agents, fatty acids (soap), fatty acid derivatives, oil and fat derivatives, higher alcohol derivatives, polymeric alcohols, etc. are used, and polymeric alcohols are mainly used to remove the surface protective layer 5. When the surface protective layer 5 is formed using a solvent-based curable resin, it is difficult to remove the surface protective layer 5 etc. with polymeric alcohols, but the deinking agent easily penetrates into an aqueous coating liquid, i.e., an aqueous emulsion-based material, so the surface protective layer 5 can be easily removed. That is, since the surface protective layer 5 is formed by applying an aqueous coating liquid to the base layer 2, the surface protective layer 5 can be peeled off relatively easily using a polymeric alcohol remover.
[0105] (2) The surface protective layer 5 includes an undercoat layer 5a formed by lamination on one side of the base layer 2, and a topcoat layer 5b formed by lamination on the side of the undercoat layer 5a opposite the side facing the base layer 2. As a result, for example, by making the gloss of the undercoat layer 5a and the gloss of the topcoat layer 5b different, it is possible to improve the design of the decorative sheet 1.
[0106] (3) It further includes a colored layer 3 disposed between the base layer 2 and the picture pattern layer 4. As a result, it becomes possible to impart hiding properties to the decorative sheet 1.
[0107] (4) A primer layer 7 is further provided on the other surface of the base layer 2 . As a result, for example, the interlayer adhesion between the decorative sheet 1 and the substrate 8 can be improved.
[0108] (5) The base layer 2 is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to a polypropylene-based resin. As a result, even if the decorative sheet 1 has a reduced thickness, it is possible to improve the hardness, and it is possible to improve the scratch resistance and abrasion resistance. In addition, because the crystallinity of the resin material that constitutes the base layer 2 is sufficiently improved, it is possible to provide a decorative sheet 1 that has sufficient scratch resistance and abrasion resistance.
[0109] (6) The amount of the nucleating agent vesicle added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicle, per 100 parts by mass of the polypropylene-based resin. As a result, it is possible to improve the crystallinity of the resin material constituting the base layer 2 compared to a configuration in which the amount of nucleating agent vesicles added is outside the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicles, per 100 parts by mass of polypropylene-based resin.
[0110] (7) Nucleating vesicles are nucleating liposomes with an outer membrane formed using phospholipids. As a result, it is possible to improve the compatibility between the polypropylene resin, which is the main component of the base layer 2, and the vesicles.
[0111] (8) The nucleating agent vesicle is formed by encapsulating a nucleating agent in a vesicle having a monolayer membrane and then converting the vesicle into a vesicle by supercritical reverse phase evaporation. As a result, it becomes possible to easily produce unilamellar vesicles encapsulating a nucleating agent, and to prepare smaller vesicles (capsules) encapsulating a nucleating agent.
[0112] (9) The moisture-proof layer 6 is further provided between the substrate layer 2 and the primer layer 7. As a result, the moisture resistance of the decorative sheet 1 can be improved.
[0113] (10) The surface protective layer 5 is provided with at least one of a gloss coat and a matte coat. As a result, the design of the decorative sheet 1 can be improved.
[0114] (11) At least one of the lines formed by the portions to which the gloss coating is applied and the lines formed by the portions to which the matte coating is applied and the lines KL forming the pattern formed in the pattern layer 4 at least partially overlap each other when viewed from the direction in which the base layer 2, the pattern layer 4, and the surface protection layer 5 are stacked. As a result, it becomes possible to harmonize the pattern formed on the surface protective layer 5 with the pattern formed on the picture pattern layer 4, thereby improving the design of the decorative sheet 1.
[0115] Moreover, the decorative board 10 in the first embodiment can achieve the effects described below. (12) The device comprises a substrate 8 and a decorative sheet 1 laminated on at least one surface of the substrate 8. As a result, it is possible to provide a decorative board 10 that is capable of suppressing deterioration in weather resistance, scratch resistance, and stain resistance.
[0116] (13) The substrate 8 further includes a moisture-proof film 9 laminated on the surface opposite to the surface facing the decorative sheet 1. As a result, the moisture resistance of the decorative board 10 can be improved.
[0117] <Modification of the first embodiment> (1) In the first embodiment, the base layer 2 is configured to be formed of two types of three layers, including a first transparent layer 2a, a core layer 2b, and a second transparent layer 2c. However, this is not limited to this. For example, as shown in FIG. 3, the base layer 2 may be configured to be a single layer.
[0118] (2) In the first embodiment, the moisture-proof layer 6 is disposed between the base layer 2 and the primer layer 7, but this is not limited to the above. In other words, the decorative sheet 1 may be configured without the primer layer 7, and the moisture-proof layer 6 may be laminated on the other surface of the base layer 2. Even in this case, it is possible to improve the moisture-proof property of the decorative sheet 1. EXAMPLES
[0119] With reference to the first embodiment, the decorative sheets of Examples 1 to 6 and the decorative sheets of Comparative Examples 1 to 3 will be described below.
[0120] Example 1 The substrate layer was formed by adding a weathering agent to a transparent polypropylene-based thermoplastic resin and extruding the resin.
[0121] The colored layer was formed from a two-component urethane resin. The design layer was formed by printing a design with a urethane resin by gravure printing.
[0122] The surface protective layer was formed using the materials described below. Resin: Polycarbonate-based urethane polymer W-6010 (Mitsui Chemicals) Hardener: Carbodiimide hardener SV-02 (Nisshinbo Chemical), added amount 1.2 The amount of the curing agent added is the molar equivalent of carbodiimide / the molar equivalent of carboxyl groups in the resin. Filler (silica): Mizukasil P803 (Mizusawa Chemicals), particle size 5 [μm] Wax (polyethylene type): AQUAMAT263 (manufactured by BYK) UV absorber (triazine type): Tinuvin 400DW (manufactured by BASF) Light stabilizer (NOR type): Tinuvin 123DW (manufactured by BASF) The primer layer was applied by gravure printing with a solid content of 1 g / m 2 A urethane resin was applied so that the shape of the surface was as follows: In this manner, the decorative sheet of Example 1 was formed.
[0123] Example 2 A decorative sheet of Example 2 was formed in the same manner as in Example 1, except that a polycarbonate-based urethane polymer WS-5100 (manufactured by Mitsui Chemicals, Inc.) was used as the resin material for the surface protective layer.
[0124] Example 3 A decorative sheet of Example 3 was formed in the same manner as in Example 1, except that a polycarbonate-based urethane polymer D-6300 (manufactured by Dainichiseika Chemicals) was used as the resin that was the material for the surface protective layer.
[0125] Example 4 The decorative sheet of Example 4 was formed in the same manner as in Example 3, except that a rubodimide-based curing agent V-02 (manufactured by Nisshinbo Chemical) was used as the curing agent, which is the material of the surface protective layer, and the amount of curing agent added was 1.0.
[0126] Example 5 A decorative sheet of Example 5 was formed in the same manner as in Example 1, except that the particle diameter of the filler, which is the material of the surface protective layer, was set to 10 μm.
[0127] Example 6 A decorative sheet of Example 6 was formed in the same manner as in Example 1, except that Apatizer AW (manufactured by Zangi) with a particle size of 0.2 μm was added as the antibacterial agent.
[0128] Comparative Example 1 A decorative sheet of Comparative Example 1 was formed in the same manner as in Example 1, except that a polyether-based urethane polymer W-6061 (manufactured by Mitsui Chemicals) was used as the resin that was the material for the surface protective layer.
[0129] Comparative Example 2 A decorative sheet of Comparative Example 2 was formed in the same manner as in Example 1, except that an epoxy-based curing agent EX-810 (manufactured by Nagase Chemtec) was used as the curing agent, which is a material for the surface protective layer.
[0130] Comparative Example 3 The decorative sheet of Comparative Example 3 was formed in the same manner as in Example 1, except that acrylic polyol 6KW-700 (manufactured by Taisei Fine Chemical) was used as the resin material for the surface protection layer, and isocyanate Cosmonate PH (manufactured by Mitsui Chemicals Fine) was used as the curing agent material for the surface protection layer.
[0131] (Performance evaluation) The decorative sheets of Examples 1 to 6 and Comparative Examples 1 to 3 were each subjected to performance evaluations for adhesion, scratch resistance, stain resistance, weather resistance, and deinking ability.
[0132] (Adhesion) The adhesion was evaluated by carrying out a test in which a cellophane tape (registered trademark) was peeled off from the surface protective layer, the surface of which had been cross-cut with a cutter, and then visually inspecting the sample after the test. If there was no peeling, the sample was rated as "○", and if the sample peeled off easily, the sample was rated as "×".
[0133] (Scratch resistance) The scratch resistance was evaluated by visually inspecting the samples after the Hoffman scratch test using a BYK Hoffman scratch hardness tester. The test conditions were set to change the load in 100[g] intervals within the range of 100[g] to 1000[g]. The sample was evaluated as "○" when scratched with a load of 500[g] or more and no scratches were found, and as "×" when scratched with a load of less than 100[g] and no scratches were found.
[0134] (Stain resistance) The stain resistance was evaluated by dropping a 1% sodium hydroxide solution onto the surface, leaving it for 24 hours, and then visually inspecting the surface condition. If there were no traces, it was rated as "○", and if there were clear traces due to dissolution, it was rated as "×".
[0135] (weather resistance) Weather resistance was evaluated by visual inspection of the samples after testing using a super xenon tester (Atlas Weather-O-Meter Ci4000) manufactured by Toyo Seiki Co., Ltd. The test conditions were 180W light irradiation, 12min rainfall / 120min cycle, and 500hr. Samples that showed no change before and after the test were rated as "○", and samples that showed some whitening after the test but were at a level that did not pose a problem in use were rated as "△".
[0136] (Deinking property) The deinking property was evaluated by the removal rate of the surface protective layer after a decorative sheet cut into a 10 cm square was wiped 10 times with cotton soaked in polymeric alcohol. A removal rate of 80% or more was evaluated as "○", and a removal rate of less than 80% was evaluated as "×".
[0137] (Evaluation Results) The evaluation results are shown in Table 1. [Table 1]
[0138] (Evaluation Results) As shown in Table 1, the decorative sheets of Examples 1 to 6 were able to exhibit excellent performance in all of adhesion, scratch resistance, stain resistance, weather resistance, and deinking ability. On the other hand, the decorative sheets of Comparative Examples 1 to 3 were unable to exhibit excellent performance in all of adhesion, scratch resistance, stain resistance, weather resistance, and deinking ability.
[0139] The present technology can be configured as follows. (1) A base layer formed using a polypropylene-based resin; a surface protective layer formed on one surface of the base layer using an aqueous coating liquid; A pattern layer is laminated on the other surface of the base material layer and has a pattern formed thereon. The aqueous coating liquid contains a polycarbonate-based urethane resin and a carbodiimide curing agent, The surface protective layer is a decorative sheet formed of a cured coating film formed by curing the aqueous coating liquid. (2) The decorative sheet described in (1) above, wherein the surface protective layer comprises an undercoat layer formed by laminating on one side of the base layer, and a topcoat layer formed by laminating on the side of the undercoat layer opposite the side facing the base layer. (3) The decorative sheet according to (1) or (2) above, further comprising a colored layer laminated on the surface of the picture pattern layer opposite to the surface facing the base layer. (4) The decorative sheet according to any one of (1) to (3) above, further comprising a primer layer laminated on the other surface of the base layer. (5) The decorative sheet according to any one of (1) to (4), wherein the base layer is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based resin. (6) A decorative sheet as described in (5) above, in which the amount of the nucleating agent vesicle added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicle, per 100 parts by mass of the polypropylene-based resin. (7) A decorative sheet according to (5) or (6) above, wherein the nucleating agent vesicle is a nucleating agent liposome having an outer membrane formed using a phospholipid. (8) The decorative sheet according to any one of (5) to (7), wherein the nucleating agent vesicle is formed by encapsulating the nucleating agent in a vesicle having a single-layer membrane, and then forming the vesicle by supercritical reverse phase evaporation. (9) A substrate; A decorative board comprising: a decorative sheet according to any one of (1) to (8) above, laminated on at least one surface of the substrate. [Explanation of symbols]
[0140] 1...decorative sheet, 2...base material layer, 2a...first transparent layer, 2b...core layer, 2c...second transparent layer, 3...colored layer, 4...picture pattern layer, 5...surface protection layer, 5a...undercoat layer, 5b...topcoat layer, 6...moisture-proof layer, 7...primer layer, 8...substrate, 9...moisture-proof film, 10...decorative board, GL...line formed by portion to which gloss coat is applied, KL...line forming pattern formed in picture pattern layer
Claims
1. A base layer formed using a polypropylene-based resin; a surface protective layer formed on one surface of the base layer using an aqueous coating liquid; A pattern layer is laminated on the other surface of the base material layer and has a pattern formed thereon. The aqueous coating liquid contains a polycarbonate-based urethane resin and a carbodiimide curing agent, The surface protective layer is a decorative sheet formed of a cured coating film formed by curing the aqueous coating liquid.
2. The decorative sheet according to claim 1, wherein the surface protective layer comprises an undercoat layer formed by laminating on one side of the base layer, and a topcoat layer formed by laminating on the side of the undercoat layer opposite the side facing the base layer.
3. 2. The decorative sheet according to claim 1, further comprising a colored layer laminated on the surface of said picture pattern layer opposite to the surface facing said base layer.
4. 2. The decorative sheet according to claim 1, further comprising a primer layer laminated on the other surface of said base layer.
5. 2. The decorative sheet according to claim 1, wherein the base layer is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based resin.
6. A decorative sheet as described in claim 5, wherein the amount of the nucleating agent vesicle added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicle, per 100 parts by mass of the polypropylene-based resin.
7. 6. The decorative sheet according to claim 5, wherein said nucleating agent vesicle is a nucleating agent liposome having an outer membrane formed using a phospholipid.
8. 6. The decorative sheet according to claim 5, wherein said nucleating agent vesicle is formed by encapsulating said nucleating agent in a vesicle having a monolayer membrane, and further forming the vesicle by a supercritical reverse phase evaporation method.
9. A substrate; A decorative board comprising: a decorative sheet according to any one of claims 1 to 8 laminated on at least one surface of the substrate.