Manufacturing method of non-aqueous electrolyte secondary battery

The described manufacturing method for non-aqueous electrolyte secondary batteries optimizes the distribution of difluorophosphate and fluoroethylene carbonate through staged impregnation, addressing the deterioration of battery characteristics in Si-containing batteries, resulting in improved initial resistance and cycle life.

JP2024167672AActive Publication Date: 2024-12-04PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023083901
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
2043-05-22

AI Technical Summary

Technical Problem

Non-aqueous electrolyte secondary batteries containing Si-containing materials and fluoroethylene carbonate as an additive face deteriorated battery characteristics, such as increased initial resistance and reduced cycle life, when using the manufacturing method of Patent Document 1, which involves adding FEC and difluorophosphate in separate stages.

Method used

A manufacturing method for non-aqueous electrolyte secondary batteries that includes a first impregnation step with a non-fluorinated electrolyte containing difluorophosphate, followed by a second impregnation step with fluoroethylene carbonate, to form protective films on the positive and negative electrodes, respectively, optimizing the distribution and adsorption of these components.

Benefits of technology

This method results in batteries with improved initial resistance and cycle characteristics by ensuring adequate adsorption of difluorophosphate on the positive electrode and fluoroethylene carbonate near the negative electrode, enhancing the durability and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167672000001_ABST
    Figure 2024167672000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a non-aqueous electrolyte secondary battery.SOLUTION: A manufacturing method disclosed here, contains: a construction step (step S1) of constructing an assembly by housing an electrode body in a battery case; a first impregnation step (step S2) of injecting a first non-aqueous electrolyte, which contains difluorophosphate and a non-fluorination carbonate and does not actually contain fluoroethylene carbonate, into the battery case, and impregnating it into the electrode body; a second impregnation step (step S4) of injecting a second non-aqueous electrolyte containing the fluoroethylene carbonate into the battery case, and impregnating it into the electrode body; and a charging step (step S5) of charging the assembly.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a non-aqueous electrolyte secondary battery. [Background technology]

[0002] Conventionally, non-aqueous electrolyte secondary batteries having a positive electrode, a negative electrode, and a non-aqueous electrolyte are known. In non-aqueous electrolyte secondary batteries, a part of the non-aqueous electrolyte (typically an additive or a non-aqueous solvent) contained in the non-aqueous electrolyte is decomposed during initial charging, and a coating (Solid Electrolyte Interface film: SEI film) containing the decomposition product is deposited on the surface of the electrode (positive electrode and / or negative electrode). This coating stabilizes the interface between the electrode and the non-aqueous electrolyte, which can improve the battery performance.

[0003] As a related prior art, for example, Patent Document 1 describes a manufacturing method in which a first nonaqueous electrolyte solution containing a specific additive and no difluorophosphate is injected into a battery case, an initial charge / discharge is performed, and then a second nonaqueous electrolyte solution containing a difluorophosphate and no specific additive is injected into the battery case, and a second charge / discharge is performed. Patent Document 1 describes that by injecting the electrolyte solution stepwise as described above, it is possible to prevent a coating derived from difluorophosphate from reacting with the additive to form a high-resistance coating. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-28875 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, non-aqueous electrolyte secondary batteries have been known that contain a Si (silicon)-containing material in the negative electrode and fluoroethylene carbonate (FEC) as an additive in the non-aqueous electrolyte for the purpose of increasing capacity, etc. However, according to the study by the present inventors, it has been newly discovered that when manufacturing such a battery, for example, by applying the technology of Patent Document 1 to add FEC as an additive to the first non-aqueous electrolyte and adding difluorophosphate to the second non-aqueous electrolyte, the battery characteristics (for example, initial resistance and cycle characteristics) are rather deteriorated compared to, for example, the case where FEC and difluorophosphate are added at once.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a nonaqueous electrolyte secondary battery which contains a Si-containing material in the negative electrode and has excellent battery characteristics. [Means for solving the problem]

[0007] The present invention provides a method for producing a nonaqueous electrolyte secondary battery comprising an electrode assembly having a positive electrode and a negative electrode, a nonaqueous electrolyte, and a battery case, the negative electrode containing a Si-containing material. The method includes a construction step of housing the electrode assembly in the battery case to construct an assembly, a first impregnation step of injecting a first nonaqueous electrolyte, which contains a difluorophosphate and a non-fluorinated carbonate and is substantially free of fluoroethylene carbonate, into the battery case to impregnate the electrode assembly, a second impregnation step of injecting a second nonaqueous electrolyte, which contains fluoroethylene carbonate, into the battery case to impregnate the electrode assembly after the first impregnation step, and a charging step of charging the assembly after the second impregnation step.

[0008] As a result of extensive research by the present inventors, it has been found that fluoroethylene carbonate (FEC) is easily adsorbed to the positive electrode (specifically, the surface of the positive electrode active material) due to, for example, a carbonate skeleton, and therefore, it has been suggested that when FEC is added to the first nonaqueous electrolyte as described in Patent Document 1, the absolute amount of FEC acting on the Si-containing material of the negative electrode is reduced, thereby reducing the effect of adding FEC to the Si-containing material.

[0009] Therefore, in the present invention, when difluorophosphate and FEC are used in combination, the electrode body is impregnated with a first nonaqueous electrolyte solution containing difluorophosphate in the first impregnation step, and then the electrode body is impregnated with a second nonaqueous electrolyte solution containing FEC in the second impregnation step. As a result, the difluorophosphate can be suitably adsorbed to the positive electrode in the first impregnation step, so that a good protective coating containing a component derived from difluorophosphate can be formed on the surface of the positive electrode. In addition, in the second impregnation step, the FEC can be suitably arranged in the vicinity of the negative electrode while suppressing the adsorption of FEC to the positive electrode, so that a protective coating containing a component derived from FEC can be stably formed on the surface of the negative electrode, particularly on the surface of the Si-containing material. Therefore, according to the technology disclosed herein, a nonaqueous electrolyte secondary battery having excellent battery characteristics (for example, initial resistance and cycle characteristics) can be suitably manufactured. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view that illustrates a nonaqueous electrolyte secondary battery according to one embodiment. [Diagram 2] FIG. 2 is a schematic vertical cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a schematic diagram showing the configuration of the electrode body. [Figure 4] FIG. 4 is a flow chart of a manufacturing method according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, some preferred embodiments of the technology disclosed herein will be described with reference to the drawings. Note that matters other than those specifically mentioned in this specification and necessary for carrying out the present invention (for example, the general configuration and manufacturing process of a non-aqueous electrolyte secondary battery that does not characterize the present invention) can be understood as design matters of a person skilled in the art based on the prior art in the field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the field.

[0012] In this specification, the term "non-aqueous electrolyte secondary battery" refers to any battery that can be repeatedly charged and discharged by the movement of charge carriers between the positive electrode and the negative electrode via the non-aqueous electrolyte. The concept of non-aqueous electrolyte secondary battery includes so-called storage batteries such as lithium ion secondary batteries, and capacitors such as lithium ion capacitors and electric double layer capacitors. In this specification, the expression "A to B" indicating a range includes the meaning of "greater than A" and "smaller than B" as well as the meaning of "A or more and B or less."

[0013] <Battery 100> First, a nonaqueous electrolyte secondary battery (hereinafter, simply referred to as a battery) 100 manufactured by the manufacturing method disclosed herein will be described. FIG. 1 is a perspective view of the battery 100. FIG. 2 is a schematic longitudinal sectional view taken along line II-II in FIG. 1. In the following description, the symbols L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom, and the symbols X, Y, and Z in the drawings represent the short side direction, the long side direction perpendicular to the short side direction, and the up-down direction perpendicular to the short side direction and the long side direction, respectively, of the battery 100. However, these directions are merely for the convenience of description, and do not limit the installation form of the battery 100 in any way.

[0014] 2, the battery 100 includes a battery case 10, an electrode assembly 20, a positive electrode terminal 30, a negative electrode terminal 40, a positive electrode current collector 50, a negative electrode current collector 60, and a non-aqueous electrolyte (not shown). The battery 100 here is a lithium ion secondary battery. The battery 100 is preferably a lithium ion secondary battery.

[0015] The battery case 10 is a housing that contains the electrode assembly 20 and the nonaqueous electrolyte. As shown in FIG. 1, the battery case 10 has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. The material of the battery case 10 may be the same as that used conventionally, and is not particularly limited. The battery case 10 is preferably made of a metal, and more preferably made of, for example, aluminum, an aluminum alloy, iron, an iron alloy, or the like. However, in other embodiments, the battery case 10 may be in the shape of a bag made of, for example, a laminate film. As shown in FIG. 2, the battery case 10 includes an exterior body 12 having an opening 12h, and a sealing plate (lid body) 14 that closes the opening 12h. The sealing plate 14 is attached to the exterior body 12 so as to close the opening 12h of the exterior body 12. The battery case 10 is integrated by joining (for example, welding) the sealing plate 14 to the periphery of the opening 12h of the exterior body 12. The battery case 10 is hermetically sealed (sealed).

[0016] As shown in Fig. 2, the sealing plate 14 is provided with a liquid injection hole 15 and two terminal extraction holes 18, 19. The liquid injection hole 15 is for injecting a non-aqueous electrolyte into the battery case 10 after the sealing plate 14 is assembled to the exterior body 12. The sealing plate 14 is preferably provided with the liquid injection hole 15. The liquid injection hole 15 is sealed with a sealing member 16. The terminal extraction holes 18, 19 are formed at both ends of the sealing plate 14 in the long side direction Y (the left end and the right end in Fig. 2). The terminal extraction holes 18, 19 penetrate the sealing plate 14 in the thickness direction (the up-down direction Z).

[0017] As shown in Fig. 2, the positive electrode terminal 30 and the negative electrode terminal 40 extend from the inside to the outside of the sealing plate 14 through the terminal pull-out holes 18, 19. Here, the positive electrode terminal 30 and the negative electrode terminal 40 are crimped to the peripheral portion surrounding the terminal pull-out holes 18, 19 of the sealing plate 14 by crimping. Crimped portions 30c, 40c are formed on the ends of the positive electrode terminal 30 and the negative electrode terminal 40 on the side of the exterior body 12 (the lower ends in Fig. 2).

[0018] The positive electrode terminal 30 is electrically connected to the positive electrode tab group 23 of the electrode body 20 through the positive electrode current collector 50 inside the battery case 10. The positive electrode terminal 30 is insulated from the sealing plate 14 by a positive electrode insulating member 70 and a gasket 90. The positive electrode terminal 30 is preferably made of metal, more preferably made of aluminum or an aluminum alloy, for example. The negative electrode terminal 40 is electrically connected to the negative electrode tab group 25 of the electrode body 20 through the negative electrode current collector 60 inside the battery case 10. The negative electrode terminal 40 is insulated from the sealing plate 14 by a negative electrode insulating member 80 and a gasket 90. The negative electrode terminal 40 is preferably made of metal, more preferably made of copper or a copper alloy, for example.

[0019] 2, the electrode body 20 is housed inside the battery case 10 (more specifically, inside the exterior body 12). The number of electrode bodies 20 arranged inside one battery case 10 is not particularly limited, and may be one or two or more (plural).

[0020] FIG. 3 is a schematic diagram showing the configuration of the electrode body 20. As shown in FIG. 3, the electrode body 20 includes a positive electrode 22, a negative electrode 24, and a separator 26. Here, the electrode body 20 is a flat-shaped wound electrode body. The electrode body 20 is configured by stacking a strip-shaped positive electrode 22 and a strip-shaped negative electrode 24 with a strip-shaped separator 26 interposed therebetween, and winding the electrodes around a winding axis WL. However, the electrode body 20 may be a laminated electrode body in which a square-shaped (typically rectangular) positive electrode and a square-shaped (typically rectangular) negative electrode are stacked in an insulated state.

[0021] The positive electrode 22 may be the same as a conventional one, and is not particularly limited. The positive electrode 22 has a positive electrode collector 22c, and a positive electrode active material layer 22a and a positive electrode protective layer 22p fixed on at least one surface of the positive electrode collector 22c. However, the positive electrode protective layer 22p is not essential and can be omitted in other embodiments. The positive electrode collector 22c is strip-shaped. The positive electrode collector 22c is made of a conductive metal such as aluminum, an aluminum alloy, nickel, or stainless steel. Here, the positive electrode collector 22c is a metal foil, specifically an aluminum foil.

[0022] A plurality of positive electrode tabs 22t are provided at one end (left end in FIG. 3) in the long side direction Y of the positive electrode collector 22c. The positive electrode tab 22t is a part of the positive electrode collector 22c and is made of metal foil (aluminum foil). The plurality of positive electrode tabs 22t are stacked at one end (left end in FIG. 3) in the long side direction Y to form a positive electrode tab group 23 as shown in FIG. 2. A positive electrode current collector 50 is attached (more specifically, joined) to the positive electrode tab group 23. The positive electrode tab group 23 is electrically connected to the positive electrode terminal 30 via the positive electrode current collector 50.

[0023] The positive electrode active material layer 22a is provided in a strip shape along the longitudinal direction of the strip-shaped positive electrode current collector 22c. The positive electrode active material layer 22a contains a positive electrode active material capable of reversibly absorbing and releasing charge carriers. The positive electrode active material is not particularly limited and may be the same as a conventional material. The positive electrode active material preferably contains a lithium transition metal composite oxide. The crystal structure of the lithium transition metal composite oxide is not particularly limited and may be a layered structure, a spinel structure, an olivine structure, or the like. In some embodiments, the lithium transition metal composite oxide preferably has a layered rock-salt crystal structure of space group C2 / m (so-called lithium-excess crystal structure) from the viewpoint of realizing a high energy density. An example of such a compound is a lithium-excess transition metal composite oxide represented by the following formula (I). A specific example is Li(Li 1 / 3 Mn 2 / 3 As described in the test examples below, when the positive electrode contains a lithium-excess transition metal composite oxide, the effects of the technology disclosed herein are exhibited at a particularly high level.

[0024] Li (Li a Ni x Mn y M z )O2 formula (I) In formula (I), a, x, y, and z satisfy 0.1 ≦ a ≦ 0.4, 0 ≦ x ≦ 0.5, 0.5 ≦ y ≦ 0.7, 0 ≦ z ≦ 0.2, and a + x + y + z = 1. When 0 < z, M is one or more elements among Co, Al, Mg, Ca, Ti, V, Cr, Si, Y, Zr, Nb, Mo, Hf, Ta, and W.

[0025] In formula (I), a preferably satisfies 0.2 ≦ a ≦ 0.4. In one example, a = 1 / 3. x preferably satisfies 0 ≦ x ≦ 0.2. In one example, x = 0. y preferably satisfies 0.6 ≦ y ≦ 0.7. In one example, y = 2 / 3. z preferably satisfies 0 ≦ z ≦ 0.1. In one example, z = 0.

[0026] In some other embodiments, the lithium transition metal composite oxide preferably has a layered rock salt crystal structure of space group R-3m. Examples of such compounds include lithium transition metal composite oxides represented by the following formula (II): LiMeO2 (Me is one or more transition metal elements other than Li). Preferably, Me contains at least one of Ni, Co, and Mn, and more preferably contains all of Ni, Co, and Mn. That is, a lithium nickel cobalt manganese-containing composite oxide is more preferred.

[0027] The positive electrode active material layer 22a may contain optional components other than the positive electrode active material, such as a binder, a conductive material, various additive components, etc. As the binder, for example, polyvinylidene fluoride (PVdF) etc. can be preferably used. As the conductive material, for example, carbon materials such as acetylene black (AB) etc. can be preferably used.

[0028] The positive electrode protective layer 22p is provided between the positive electrode current collector 22c and the positive electrode active material layer 22a in the long side direction Y. The positive electrode protective layer 22p is provided in a strip shape along the positive electrode active material layer 22a. The positive electrode protective layer 22p contains an inorganic filler (e.g., alumina). The positive electrode protective layer 22p may contain any component other than the inorganic filler, such as a conductive material, a binder, various additive components, and the like. The conductive material and the binder may be the same as those exemplified as those that may be contained in the positive electrode active material layer 22a.

[0029] The negative electrode 24 has a negative electrode current collector 24c and a negative electrode active material layer 24a fixed on at least one surface of the negative electrode current collector 24c. The negative electrode current collector 24c is strip-shaped. The negative electrode current collector 24c is made of a conductive metal such as copper, a copper alloy, nickel, or stainless steel. Here, the negative electrode current collector 24c is a metal foil, specifically a copper foil.

[0030] A plurality of negative electrode tabs 24t are provided at one end (right end in FIG. 3) in the long side direction Y of the negative electrode current collector 24c. The negative electrode tab 24t is a part of the negative electrode current collector 24c here, and is made of metal foil (copper foil). The plurality of negative electrode tabs 24t are stacked at one end (right end in FIG. 3) in the long side direction Y to form a negative electrode tab group 25 as shown in FIG. 2. A negative electrode current collector 60 is attached (more specifically, joined) to the negative electrode tab group 25. The negative electrode tab group 25 is electrically connected to the negative electrode terminal 40 via the negative electrode current collector 60.

[0031] The negative electrode active material layer 24a is provided in a strip shape along the longitudinal direction of the strip-shaped negative electrode current collector 24c. The negative electrode active material layer 24a contains a negative electrode active material capable of reversibly absorbing and releasing charge carriers. In this embodiment, the negative electrode active material essentially contains a Si-containing material from the viewpoint of increasing capacity and the like. Suitable examples of the Si-containing material include Si, SiO (silicon oxide), SiC-containing material (including silicon carbide and SiC composites in which carbon is dispersed inside silicon particles), SiN-containing material (silicon nitride), nano-Si particles dispersed in porous particles, and the like. Among them, it is preferable to contain at least one of Si, SiO, and SiC-containing material. Although not particularly limited, when the total amount of the negative electrode active material is taken as 100 mass%, the content ratio of the Si-containing material is typically 50 mass% or less, for example, 1 to 30 mass% is preferable, and 5 to 20 mass% is more preferable.

[0032] From the viewpoint of having a high level of battery characteristics (for example, high capacity and cycle characteristics), the negative electrode active material preferably contains graphite such as artificial graphite or natural graphite in addition to the Si-containing material. In this case, it is preferable that the content of graphite is higher than that of the Si-containing material on a mass basis. Although not particularly limited, when the total of the Si-containing material and the graphite is 100 mass%, the content of the Si-containing material is typically 50 mass% or less, for example, 1 to 30 mass% is preferable, and 5 to 20 mass% is more preferable. The negative electrode active material may contain a negative electrode active material other than the Si-containing material and graphite. Specific examples of the negative electrode active material other than the Si-containing material and graphite include carbon materials such as hard carbon, soft carbon, and amorphous carbon.

[0033] The negative electrode active material layer 24a may contain any component other than the negative electrode active material, such as a binder, a dispersant, a conductive material, various additive components, etc. As the binder, for example, rubbers such as styrene butadiene rubber (SBR) or acrylic resins such as polyacrylic acid (PAA) can be suitably used. As the dispersant, for example, celluloses such as carboxymethyl cellulose (CMC) can be suitably used. As the conductive material, for example, carbon materials such as carbon fibers and carbon nanotubes can be suitably used.

[0034] The separator 26 is a member that insulates the positive electrode active material layer 22a of the positive electrode 22 from the negative electrode active material layer 24a of the negative electrode 24. The separator 26 may be the same as a conventional one and is not particularly limited. The separator 26 is preferably a resin porous sheet made of a polyolefin resin such as polyethylene (PE) or polypropylene (PP). The separator 26 may have a heat resistance layer (HRL) or an adhesive layer on the surface of the base material portion made of a resin porous sheet. The configuration of the heat resistance layer and adhesive layer may be the same as a conventional one.

[0035] The non-aqueous electrolyte may be the same as in the past, and is not particularly limited. The non-aqueous electrolyte typically contains a non-aqueous solvent and a supporting salt (electrolyte salt). As the non-aqueous solvent, one or more of those that are known to be usable in non-aqueous electrolyte secondary batteries can be used. Examples of the non-aqueous solvent include organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones. The non-aqueous solvent preferably contains carbonates.

[0036] Carbonates are divided into non-fluorinated carbonates and fluorinated carbonates, depending on whether or not they contain fluorine (F) as a constituent element. Carbonates are also divided into chain carbonates and cyclic carbonates, depending on their chemical structure. Chain carbonates are acyclic (chain) carbonate compounds with a carbonate skeleton (O-CO-O). Cyclic carbonates are carbonate compounds with a carbonate skeleton closed in a ring shape by a C-C bond.

[0037] In this embodiment, the non-aqueous solvent preferably contains at least a non-fluorinated carbonate. Examples of the non-fluorinated carbonate include non-fluorinated chain carbonates such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), and non-fluorinated cyclic carbonates such as ethylene carbonate (EC), vinylene carbonate (VC), and propylene carbonate (PC). The non-fluorinated carbonate preferably contains at least one of DMC, DEC, EMC, EC, and VC. The non-fluorinated carbonate more preferably contains a non-fluorinated chain carbonate and a non-fluorinated cyclic carbonate.

[0038] In a preferred embodiment, the non-aqueous solvent contains fluoroethylene carbonate (FEC) in addition to the non-fluorinated carbonate. However, as will be described in detail in the section on the manufacturing method, FEC may be electrically decomposed in a charging process or the like during battery manufacturing, and consumed to form a coating on the negative electrode active material layer 24a or the like. Therefore, in the state of the battery 100, FEC may or may not be contained (remains) in the non-aqueous electrolyte. The non-aqueous solvent may further contain a fluorinated carbonate other than FEC, such as a fluorinated chain carbonate or a fluorinated cyclic carbonate other than FEC.

[0039] The supporting salt is not particularly limited as long as it contains a charge carrier, and one or more of the salts that are known to be usable in non-aqueous electrolyte secondary batteries can be used. In the case of a lithium ion secondary battery, examples of the supporting salt include fluorine-containing lithium salts such as LiPF6 and LiBF4. The supporting salt preferably contains LiPF6.

[0040] The non-aqueous electrolyte may further contain additional components (additives). As the additive, for example, a film forming agent or the like, which is conventionally known to be added to a non-aqueous electrolyte, one or more kinds can be used. In a preferred embodiment, the non-aqueous electrolyte contains a difluorophosphate. The difluorophosphate is PO2F2 - The difluorophosphate salt is a salt of an anion represented by the formula: and a cation. Examples of the cation include alkali metal ions such as Li, Na, and K, and ammonium ions, among which Li is preferred. A specific example of the difluorophosphate salt is lithium difluorophosphate (lithium difluorophosphate (LiDFP), LiPO2F2).

[0041] <Manufacturing method of battery 100> Fig. 4 is a flowchart of a manufacturing method according to one embodiment. As shown in Fig. 4, the battery 100 can be manufactured by a manufacturing method including, for example, a construction step (step S1), a first impregnation step (step S2), an initial charging step (step S3), a second impregnation step (step S4), and a charging step (step S5) in this order. However, the initial charging step (step S3) is optional and can be omitted. Furthermore, other steps may be included at any stage.

[0042] The construction step (step S1) is a step of housing the electrode body 20 in the battery case 10 to construct an assembly (a combination of the battery case 10 and the electrode body 20). In a preferred embodiment, this step includes an electrode fabrication step (step S1-1), an electrode body fabrication step (step S1-2), an arrangement step (step S1-3), and a welding and joining step (step S1-4). In addition, other steps may be included at any stage.

[0043] First, in the electrode preparation step (step S1-1), the positive electrode 22 and the negative electrode 24 are prepared. The positive electrode 22 can be prepared, for example, by mixing a positive electrode active material, a conductive material, a binder, and a dispersion solvent to prepare a positive electrode composite slurry, applying the prepared positive electrode composite slurry onto the positive electrode current collector 22c by a conventionally known method, drying, and appropriately pressing. As the positive electrode active material, one type of material as described above can be used alone or two or more types can be mixed and appropriately used. Among them, the lithium-excess transition metal composite oxide represented by the above formula (I) and the lithium transition metal composite oxide represented by the above formula (II) can be preferably used.

[0044] The negative electrode 24 can be produced, for example, by mixing a negative electrode active material, a binder, a dispersant, and a dispersion solvent to prepare a negative electrode composite slurry, applying the prepared negative electrode composite slurry onto the negative electrode current collector 24c by a conventionally known method, drying, and appropriately pressing. As the negative electrode active material, a Si-containing material (preferably at least one of Si, SiO, and SiC-containing materials) is used as an essential material, and one or more of the above-mentioned materials can be further used. Among them, graphite can be preferably used in addition to the Si-containing material. In this embodiment, electrodes (positive electrode 22 and / or negative electrode 24) are produced, but in other embodiments, the electrodes may be purchased as commercially available products.

[0045] Next, in the electrode body preparation step (step S1-2), the positive electrode 22 and the negative electrode 24 prepared above are opposed to each other with the separator 26 interposed therebetween to prepare the electrode body 20. Next, in the arrangement step (step S1-3), the electrode body 20 is arranged inside the exterior body 12. For example, the electrode body 20 is accommodated inside the exterior body 12 through the opening 12h of the exterior body 12. Next, in the welding and joining step (step S1-4), the sealing plate 14 is fitted into the opening 12h of the exterior body 12 and welded to the periphery of the opening 12h to integrate the exterior body 12 and the sealing plate 14.

[0046] The first impregnation step (step S2) is a step of injecting a first nonaqueous electrolyte into the inside of the battery case 10 to impregnate the electrode body 20 with the nonaqueous electrolyte. In this step, the first nonaqueous electrolyte is first prepared. The first nonaqueous electrolyte essentially contains a difluorophosphate and a non-fluorinated carbonate. LiPO2F2 can be suitably used as the difluorophosphate. Although not particularly limited, it is preferable to add the difluorophosphate to the first nonaqueous electrolyte so that the proportion of the difluorophosphate in the entire nonaqueous electrolyte (the sum of the first nonaqueous electrolyte and the second nonaqueous electrolyte described later) before the charging step is approximately 0.1 mass% or more, for example, 0.5 mass% or more, from the viewpoint of exerting the effects of the technology disclosed herein at a high level. On the other hand, from the viewpoint of suppressing an increase in resistance, it is preferable to add the difluorophosphate to the first nonaqueous electrolyte solution so that the proportion of the difluorophosphate in the entire nonaqueous electrolyte solution before the charging step is approximately 5% by mass or less, for example, 2% by mass or less, or 1% by mass or less.

[0047] The non-fluorinated carbonate is typically a non-aqueous solvent for dissolving the difluorophosphate. As the non-fluorinated carbonate, one of the above-mentioned materials can be used alone or two or more of them can be mixed appropriately, and it is preferable that the non-fluorinated carbonate contains at least one of DMC, DEC, EMC, EC, and VC. It is more preferable that the non-fluorinated carbonate contains a non-fluorinated chain carbonate (e.g., one or more of DMC, DEC, and EMC) and a non-fluorinated cyclic carbonate (e.g., EC and / or VC). Although not particularly limited, the ratio of the non-fluorinated chain carbonate in the first non-aqueous electrolyte is preferably higher than the non-fluorinated cyclic carbonate on a volume basis.

[0048] In a preferred embodiment, the first nonaqueous electrolyte contains a supporting salt (lithium salt in the case of a lithium ion secondary battery) in addition to a difluorophosphate and a non-fluorinated carbonate. As the supporting salt, one of the above-mentioned materials can be used alone or two or more of them can be mixed appropriately, and LiPF6 can be used preferably.

[0049] In this embodiment, the first nonaqueous electrolyte does not substantially contain FEC. According to the study by the present inventors, FEC is easily adsorbed to the surface of the positive electrode 22 (specifically, the surface of the positive electrode active material) by having, for example, a carbonate skeleton. Therefore, when FEC is added to the first nonaqueous electrolyte, the absolute amount of FEC acting on the Si-containing material of the negative electrode 24 decreases, and the effect of adding FEC to the Si-containing material may be reduced. In addition, the action of the difluorophosphate salt added in the second impregnation step (step S4) described later on the surface of the positive electrode 22 (specifically, the surface of the positive electrode active material) may be reduced, and as a result, the resistance of the positive electrode (particularly, the interface resistance with the nonaqueous electrolyte) may be increased. It is more preferable that the first nonaqueous electrolyte does not substantially contain fluorinated carbonates in general (i.e., fluorinated carbonates other than FEC).

[0050] In this specification, the term "substantially free" is a term that allows for the inclusion of a very small amount of the target component as long as it does not significantly impair the effects of the technology disclosed herein, and refers to the proportion of the target component in the total (for example, the proportion of FEC in the entire first nonaqueous electrolyte) being less than 0.1 mass%. The proportion of the target component in the total (for example, the proportion of FEC in the entire first nonaqueous electrolyte) is preferably less than 0.05 mass%, more preferably less than 0.01 mass%.

[0051] In this step, the prepared first nonaqueous electrolyte is then injected into the battery case 10 through the injection hole 15 of the sealing plate 14. The injection may be performed at atmospheric pressure, or may be performed under reduced pressure in the battery case 10, for example, for the purpose of improving the impregnation of the nonaqueous electrolyte into the electrode body 20. The first nonaqueous electrolyte injected through the injection hole 15 is impregnated into the electrode body 20. In other words, the first nonaqueous electrolyte is uniformly distributed throughout the electrode body 20. In this embodiment, the first nonaqueous electrolyte contains difluorophosphate and is substantially free of FEC. Difluorophosphate is a material that easily interacts with the surface of an active material and is easily adsorbed to the surface of the active material. Therefore, in this step, the difluorophosphate contained in the first nonaqueous electrolyte can be specifically adsorbed onto, for example, the surface of the positive electrode 22 (specifically, the surface of the positive electrode active material).

[0052] In a preferred embodiment, the assembly is left (held) for a predetermined time after the injection. As a result, even if the length of the long side direction Y is relatively long, the nonaqueous electrolyte is evenly distributed in the long side direction Y, and the electrode body 20 can be thoroughly impregnated with the first nonaqueous electrolyte. The temperature for leaving the electrode body 20 may be room temperature (for example, about 25°C ± 10°C, about 25°C ± 5°C), or may be a high temperature environment of about 35 to 45°C for the purpose of improving the impregnation of the nonaqueous electrolyte into the electrode body 20. The leaving time is not particularly limited because it depends on, for example, the size of the electrode body 20 (particularly the length of the long side direction Y), the viscosity of the first nonaqueous electrolyte, the presence or absence of pressure reduction, the leaving temperature, etc., but is preferably 5 minutes or more, more preferably 10 minutes or more, and particularly preferably 1 hour or more. In addition, from the viewpoint of production efficiency, etc., it is preferably within 240 hours (10 days), more preferably within 48 hours (2 days), and particularly preferably within 24 hours (1 day).

[0053] The initial charging step (step S3) is a step of charging the assembly into which the first nonaqueous electrolyte solution has been injected at least once. The charging of the assembly can be performed in the same manner as in the past. Typically, an external power source is connected between the positive electrode terminal and the negative electrode terminal of the assembly, and charging is performed until the assembly reaches a predetermined voltage. Although not particularly limited, it is preferable to charge until the voltage reaches about 4V or more, preferably 4.1V or more, 4.2V or more, for example, 4.2V. When a lithium-excess transition metal composite oxide is used as the positive electrode active material, it is more preferable to charge until the voltage reaches about 4.6V or more, preferably 4.7V or more, for example, 4.7V, from the viewpoint of expressing a high capacity as an electrochemically active state. The charge / discharge rate can be, for example, about 0.1 to 2C. As a result, the difluorophosphate contained in the first nonaqueous electrolyte is typically electrolyzed (mainly oxidatively decomposed) prior to other components (non-fluorinated carbonate and supporting salt) in the first nonaqueous electrolyte, and a high-quality protective coating containing a component derived from the difluorophosphate is formed, particularly on the surface of the positive electrode 22 (more specifically, the surface of the positive electrode active material). Therefore, the protective effect of the difluorophosphate can reduce the resistance of the positive electrode 22.

[0054] Charging may be performed once, or may be repeated two or more times, for example, with a discharge in between. Discharging may also be performed after charging. In a preferred embodiment, the assembly may be discharged until the state of charge (SOC) is about 20% or less, preferably 10% or less, for example 0%. Alternatively, the assembly may be discharged until the voltage is about 3.5V or less, 3.0V or less, for example 3.0V. This step may be performed in a room temperature environment (for example, about 25°C ± 10°C, about 25°C ± 5°C) or in a high temperature environment of about 35 to 45°C, for example, for the purpose of promoting the formation of a coating.

[0055] The second impregnation step (step S4) is a step of injecting a second nonaqueous electrolyte into the battery case 10 to impregnate the electrode body 20 with the nonaqueous electrolyte. In this step, the second nonaqueous electrolyte is first prepared. The second nonaqueous electrolyte essentially contains fluoroethylene carbonate (FEC). Although not particularly limited, from the viewpoint of exerting the effects of the technology disclosed herein at a high level, it is preferable to add FEC to the second nonaqueous electrolyte so that the proportion of FEC in the total of carbonates (for example, the total of non-fluorinated carbonate and FEC) in the entire nonaqueous electrolyte (the total of the first nonaqueous electrolyte and the second nonaqueous electrolyte) before the charging step is approximately 1% by volume or more, for example 5% by volume or more. On the other hand, from the viewpoint of suppressing an increase in resistance, it is preferable to add FEC to the second nonaqueous electrolyte solution so that the proportion of FEC in the total of the carbonates is approximately 30% by volume or less, for example 20% by volume or less, or 10% by volume or less.

[0056] In a preferred embodiment, the second non-aqueous electrolyte contains a non-fluorinated carbonate in addition to FEC. The non-fluorinated carbonate may be the same type as that added to the first non-aqueous electrolyte, or may be a different type. More preferably, the non-fluorinated carbonate contains a non-fluorinated chain carbonate (e.g., one or more of DMC, DEC, and EMC). It is preferred that the second non-aqueous electrolyte does not substantially contain a non-fluorinated cyclic carbonate (e.g., EC and / or VC).

[0057] The second nonaqueous electrolyte may contain a supporting salt (lithium salt in the case of a lithium ion secondary battery). The supporting salt may be the same as or different from that added to the first nonaqueous electrolyte.

[0058] The second electrolyte may contain a difluorophosphate as long as it does not significantly impair the effects of the technology disclosed herein. In a preferred embodiment, the second nonaqueous electrolyte does not substantially contain a difluorophosphate (e.g., LiPO2F2). This prevents an excessive coating from being formed on the positive electrode 22 in the charging step (step S5) described later, and allows the effects of the technology disclosed herein to be exhibited at a high level.

[0059] In this step, the prepared second nonaqueous electrolyte is then injected into the battery case 10 through the injection hole 15 of the sealing plate 14. The injection may be performed at atmospheric pressure, or may be performed under reduced pressure in the battery case 10, for example, for the purpose of improving the impregnation of the nonaqueous electrolyte into the electrode body 20. The second nonaqueous electrolyte injected through the injection hole 15 is impregnated into the electrode body 20. In other words, the second nonaqueous electrolyte is evenly distributed throughout the electrode body 20. This allows the FEC contained in the second nonaqueous electrolyte to be suitably disposed, for example, near the negative electrode 24 (more specifically, near the negative electrode active material).

[0060] In a preferred embodiment, the assembly is left (held) for a predetermined time after the injection. As a result, even if the length of the long side direction Y is relatively long, the nonaqueous electrolyte is evenly distributed in the long side direction Y, and the electrode body 20 can be thoroughly impregnated with the second nonaqueous electrolyte. The temperature for leaving the electrode body 20 may be room temperature (for example, about 25°C ± 10°C, about 25°C ± 5°C), or may be a high temperature environment of about 35 to 45°C for the purpose of improving the impregnation of the nonaqueous electrolyte into the electrode body 20. The leaving time is not particularly limited because it depends on, for example, the size of the electrode body 20 (particularly the length of the long side direction Y), the viscosity of the second nonaqueous electrolyte, the presence or absence of pressure reduction, the leaving temperature, etc., but is preferably 5 minutes or more, more preferably 10 minutes or more, and particularly preferably 1 hour or more. In addition, from the viewpoint of production efficiency, etc., it is preferably within 240 hours (10 days), more preferably within 48 hours (2 days), and particularly preferably within 24 hours (1 day).

[0061] The charging step (step S5) is a step of charging the assembly into which the second nonaqueous electrolyte is injected at least once. The charging of the assembly can be performed in accordance with the initial charging step (step S3). Although not particularly limited, in a preferred embodiment, the assembly is charged until the state of charge (SOC) is about 80% or more, preferably 90% or more, for example 100%. Alternatively, it is preferable to charge the assembly until the voltage is about 4V or more, preferably 4.1V or more, 4.2V or more, for example 4.2V. In addition, when the initial charging step (step S3) is performed, the above SOC or voltage may be used even if a lithium-excess transition metal composite oxide is used as the positive electrode active material. However, when a lithium-excess transition metal composite oxide is used as the positive electrode active material and the initial charging step (step S3) is omitted, it is preferable to charge the assembly until the voltage is about 4.6V or more, preferably 4.7V or more, for example 4.7V, from the viewpoint of expressing a high capacity as an electrochemically active state. The charge / discharge rate may be, for example, about 0.1 to 2 C. As a result, the FEC contained in the second nonaqueous electrolyte is typically electrolyzed (mainly reductively decomposed) prior to other components (e.g., non-fluorinated carbonate and supporting salt) in the nonaqueous electrolyte. Then, a protective film containing a component derived from the FEC is stably formed particularly on the surface of the negative electrode 24 (more specifically, the surface of the negative electrode active material, particularly the surface of the Si-containing material). Therefore, the protective effect of the FEC can make the negative electrode 24 highly durable. In this manner, the battery 100 can be suitably manufactured.

[0062] <Uses of Battery 100> Battery 100 can be used for various purposes, but for example, because it has reduced resistance and excellent durability, it can be suitably used as a power source (driving power source) for motors mounted on vehicles such as passenger cars and trucks. The type of vehicle is not particularly limited, but examples include plug-in hybrid electric vehicles (PHEVs), hybrid electric vehicles (HEVs), battery electric vehicles (BEVs), and the like.

[0063] Several examples of the present invention will be described below, but it is not intended that the present invention be limited to these examples.

[0064] <Test Example I (Examples 1 and 2, Comparative Examples 1 and 2)> <Construction of non-aqueous electrolyte secondary battery> First, a positive electrode and a negative electrode were prepared. The positive electrode was prepared as follows. First, Li (Li 1 / 3 Mn 2 / 3 )O2, AB as a conductive material, and PVdF as a binder were mixed in a mass ratio of active material:AB:PVdF=100:1:1, and the fluidity was adjusted with a dispersion solvent (NMP) to prepare a positive electrode composite slurry. Next, the prepared positive electrode composite slurry was applied onto an Al foil as a positive electrode current collector, dried, and pressed to a predetermined thickness. Then, the mixture was cut to a predetermined size to prepare a positive electrode.

[0065] The negative electrode was prepared as follows. First, graphite and SiO (Si-containing material) as the negative electrode active material were mixed in a mass ratio of graphite:SiO = 95:5 to obtain a mixture. Next, SBR as a binder and CMC as a dispersant were added in a ratio of 1 part by mass each to the obtained mixture (100 parts by mass), and the fluidity was adjusted with a dispersion solvent (water) to prepare a negative electrode composite slurry. Next, the prepared negative electrode composite slurry was applied onto Cu foil as a negative electrode current collector, dried, and pressed to a predetermined thickness. Then, the negative electrode was prepared by cutting into a predetermined size.

[0066] Next, an assembly was constructed. First, the positive and negative electrodes prepared above were opposed to each other with a separator (a porous sheet consisting of three layers of PP / PE / PP) interposed therebetween to prepare an electrode body. Next, the electrode body was housed in a bag-shaped battery case made of an aluminum laminate film to construct an assembly. This process was repeated to prepare multiple assemblies (construction process).

[0067] (Example 1) First, non-aqueous electrolytes A and B were prepared. The following two types of non-aqueous electrolytes were prepared so that the composition of the entire non-aqueous electrolyte (total amount of electrolyte injected) before the charging process was LiPF6 (1 mol / L) as a supporting salt, LiPO2F2 (0.5 mass%) as a difluorophosphate, and FEC+EC+EMC (volume ratio 1:4:15) as a non-aqueous solvent. ·Non-aqueous electrolyte A: LiPF6 (1mol / L), LiPO2F2 (0.625% by mass), EC+EMC (1:3 by volume) ·Non-aqueous electrolyte B: LiPF6 (1mol / L), FEC+EMC (1:3 by volume)

[0068] Next, 80% of the total amount of non-aqueous electrolyte A (non-aqueous electrolyte containing LiPO2F2 and not containing FEC) was injected into the battery case, and the battery case was left standing for 12 hours, thereby impregnating the electrode body with the non-aqueous electrolyte A (first impregnation step). Next, 20% of the total amount of non-aqueous electrolyte B (non-aqueous electrolyte containing FEC and not containing LiPO2F2) was injected into the battery case, and the battery case was sealed and left standing for 12 hours, thereby impregnating the electrode body with the non-aqueous electrolyte B (second impregnation step). After the second impregnation step, the assembly was charged at a constant current to 4.7 V at a charge rate of 0.1 C, and then discharged at a constant current to 3.0 V at a discharge rate of 0.1 C (charging step). In this manner, a non-aqueous electrolyte secondary battery (Example 1) was constructed.

[0069] Comparative Example 1 First, the following two types of non-aqueous electrolyte solutions C and D were prepared. ·Non-aqueous electrolyte C: LiPF6 (1mol / L), FEC+EC+EMC (volume ratio 1:3:12) ·Non-aqueous electrolyte D: LiPF6 (1mol / L), LiPO2F2 (2.5% by mass), EC+EMC (1:3 by volume) A nonaqueous electrolyte secondary battery (Comparative Example 1) was constructed in the same manner as in Example 1 above, except that in the first impregnation step, 80% of the total amount of nonaqueous electrolyte C (a nonaqueous electrolyte containing FEC and not containing LiPO2F2) was injected, and in the second impregnation step, 20% of the total amount of nonaqueous electrolyte D (a nonaqueous electrolyte containing LiPO2F2 and not containing FEC) was injected.

[0070] Comparative Example 2 First, one type of non-aqueous electrolyte solution E was prepared. Nonaqueous electrolyte E: LiPF6 (1 mol / L), LiPO2F2 (0.5 mass%), FEC+EC+EMC (volume ratio 1:4:15) as nonaqueous solvent Then, a nonaqueous electrolyte secondary battery (Comparative Example 2) was constructed in the same manner as in Example 1 above, except that in the first impregnation step, nonaqueous electrolyte E (nonaqueous electrolyte containing FEC and LiPO2F2) was injected and the second impregnation step was not performed.

[0071] (Example 2) An initial charging step was carried out between the first impregnation step and the second impregnation step in the above Example 1. The charge / discharge conditions in the initial charging step were the same as those in the charging step in Example 1 (constant current charging of the assembly to 4.7 V at a charge rate of 0.1 C, followed by constant current discharging to 3.0 V at a discharge rate of 0.1 C). In addition, in the charging step in Example 2, the charging voltage was 4.2 V. A nonaqueous electrolyte secondary battery (Example 2) was constructed in the same manner as in the above Example 1 except for these.

[0072] <Evaluation of initial characteristics (initial capacitance and initial resistance)> The initial capacity was determined by the discharge capacity when the battery was charged at a constant current of 0.1C to 4.2V in an environment of 25°C, and then discharged at a constant current of 0.1C to 3.0V. The state of charge of the battery was then adjusted to SOC50% in an environment of 25°C, and after resting for 1 hour, a constant current discharge was performed at a constant current of 5C for 10 seconds. The initial resistance (mΩ) was calculated from the open circuit voltage (V0) immediately before discharge and the closed circuit voltage (V1) after 10 seconds of discharge using the following formula: initial resistance = (V0-V1) / current value of 5C. The results are shown in Table 1.

[0073] <Evaluation of cycle characteristics> In an environment of 25°C, a constant current charge was performed at a charge rate of 0.4C up to 4.2V, followed by a constant current discharge at a discharge rate of 0.4C up to 3.0V. 100 charge / discharge cycles were repeated. Then, the "capacity after cycling" was measured in the same manner as the initial capacity, and the capacity retention rate (%) was calculated by the following formula: Capacity retention rate = (capacity after cycling / initial capacity) x 100. The results are shown in Table 1.

[0074] [Table 1]

[0075] As shown in Table 1, in Comparative Example 1, in which nonaqueous electrolyte C (nonaqueous electrolyte containing FEC) was injected in the first impregnation step and nonaqueous electrolyte D (nonaqueous electrolyte containing LiPO2F2) was injected in the second impregnation step, the battery characteristics were rather deteriorated compared to Comparative Example 2, in which nonaqueous electrolyte E (nonaqueous electrolyte containing FEC and LiPO2F2) was added in the first impregnation step. The reasons for this are considered to be: (1) FEC has a high adsorption property to the positive electrode, so by adding FEC in the first impregnation step, FEC was also adsorbed to the positive electrode, and the absolute amount of FEC acting on the Si-containing material in the negative electrode was reduced, and the effect of adding FEC was reduced; (2) FEC was adsorbed to the positive electrode in the first impregnation step, so the effect of the difluorophosphate added in the second impregnation step on the positive electrode was reduced; etc.

[0076] In contrast to Comparative Example 2, in Example 1, in which nonaqueous electrolyte A containing LiPO2F2 was added in the first impregnation step and nonaqueous electrolyte B containing FEC was added in the second impregnation step, the battery resistance was relatively reduced and the cycle characteristics were also improved. Although it is not intended to be particularly limited, the reasons for this are considered to be that (1) the difluorophosphate added in the first impregnation step was specifically adsorbed on the positive electrode surface, forming a good protective film; (2) the absolute amount of FEC acting on the Si-containing material in the negative electrode was increased while suppressing the adsorption of FEC to the positive electrode by adding FEC in the second impregnation step; and as a result, the positive electrode surface was made low-resistance by the protective effect of the difluorophosphate, and the negative electrode surface (particularly the surface of the Si-containing material) was made highly durable by the protective effect of FEC. Such results indicate the significance of the technology disclosed herein.

[0077] Moreover, Example 2, in which the initial charge was performed between the first impregnation step and the second impregnation step, had improved cycle characteristics compared to Example 1. Although it is not intended to be interpreted in a particularly restrictive manner, it is believed that the reason for this is that in Example 2, the oxidative decomposition of FEC was suppressed by performing high voltage treatment in a state in which FEC was not contained.

[0078] <Test Example II (Examples 3 and 4, Comparative Examples 3 and 4)> In this test example, LiNi was used as the positive electrode active material. 0.8 Co 0.1 Mn 0.1 Examples 1 and 2 of Test Example I, Comparative Examples 1 and 2, and nonaqueous electrolyte secondary batteries (Examples 3 and 4, Comparative Examples 3 and 4) were constructed and evaluated, except that O2 (NCM811) was used and the charging voltage in the charging process (or the initial charging process) was set to 4.2 V. The results are shown in Table 2.

[0079] [Table 2]

[0080] As shown in Table 2, similar effects were obtained even when the type of positive electrode active material was different. Therefore, it was found that the effects of the technology disclosed herein can be exerted regardless of the type of positive electrode active material.

[0081] Although several embodiments of the present invention have been described above, the above embodiments are merely examples. The present invention can be implemented in various other forms. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes of the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modification, and it is also possible to add another modification to the above-mentioned embodiment. Furthermore, if a technical feature is not described as essential, it can be appropriately deleted.

[0082] 1, the outer shape of the battery 100 is a rectangular parallelepiped (rectangular). However, this is not limiting. In other embodiments, the battery 100 may be, for example, a sheet shape, a cylindrical shape, a button shape, a coin shape, or the like.

[0083] 4 includes the initial charging step (step S3), but as described above, the initial charging step (step S3) is optional and can be omitted. In that case, in the charging step (step S5), a coating containing a component derived from difluorophosphate is formed on the positive electrode 22 side, and a coating containing a component derived from FEC is formed on the negative electrode 24 side.

[0084] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A method for producing a nonaqueous electrolyte secondary battery comprising an electrode assembly having a positive electrode and a negative electrode, a nonaqueous electrolyte, and a battery case, wherein the negative electrode contains a Si-containing material, the method comprising: an assembly step of housing the electrode assembly in the battery case to construct an assembly; a first impregnation step of injecting a first nonaqueous electrolyte solution that contains a difluorophosphate and a non-fluorinated carbonate and is substantially free of fluoroethylene carbonate into the battery case to impregnate the electrode assembly; a second impregnation step of injecting a second nonaqueous electrolyte solution that contains fluoroethylene carbonate into the battery case to impregnate the electrode assembly after the first impregnation step; and a charging step of charging the assembly after the second impregnation step. Item 2: The manufacturing method according to item 1, further comprising an initial charging step of charging the assembly after the first liquid injection step and before the second liquid injection step. Item 3: The method according to item 1 or 2, wherein the second nonaqueous electrolyte solution is substantially free of difluorophosphate. Item 4: The method according to any one of Items 1 to 3, wherein the first nonaqueous electrolyte contains a supporting salt. Item 5: The method according to any one of Items 1 to 4, wherein the Si-containing material is at least one of Si, SiO, and SiC. Item 6: The method according to any one of Items 1 to 5, wherein the non-fluorinated carbonate is at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, and vinylene carbonate. [Explanation of symbols]

[0085] 10 Battery case 20 Electrode body 22 Positive electrode 22a Cathode active material layer 24 Negative electrode 24a Negative electrode active material layer 100 batteries S1 construction process S2 1st impregnation process S3 Initial charging process S4 2nd impregnation process S5 charging process

Claims

1. A method for producing a non-aqueous electrolyte secondary battery comprising: an electrode assembly having a positive electrode and a negative electrode; a non-aqueous electrolyte; and a battery case, the negative electrode including a Si-containing material, the method comprising the steps of: a construction step of housing the electrode body in the battery case to construct an assembly; a first impregnation step of injecting a first nonaqueous electrolyte solution containing a difluorophosphate and a non-fluorinated carbonate and substantially not containing fluoroethylene carbonate into the battery case to impregnate the electrode body; a second impregnation step of injecting a second nonaqueous electrolyte solution containing fluoroethylene carbonate into the battery case after the first impregnation step to impregnate the electrode body; a charging step of charging the assembly after the second impregnation step; The method for producing a non-aqueous electrolyte secondary battery includes the steps of:

2. a first charging step of charging the assembly after the first impregnation step and before the second impregnation step; The method of claim 1 .

3. The second non-aqueous electrolyte solution is substantially free of difluorophosphate. The method according to claim 1 or 2.

4. The first nonaqueous electrolyte contains a supporting salt. The method according to claim 1 or 2.

5. The Si-containing material is at least one of Si, SiO, and SiC-containing materials; The method according to claim 1 or 2.

6. The non-fluorinated carbonate is at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, and vinylene carbonate; The method according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for manufacturing lithium ion secondary battery

    JP2018190582A

  • Method for manufacturing nonaqueous electrolyte secondary battery

    WO2013076847A1

  • Method for manufacturing nonaqueous electrolyte secondary battery

    JP2015028875A