Thermoplastic carbon fiber resin substrate sheet, and production method of the same

A thin thermoplastic carbon fiber resin base sheet with oriented carbon fibers and varied resin viscosities addresses the limitations of conventional sheets, offering improved mechanical properties and handling for electronic and audio components.

JP2024167884APending Publication Date: 2024-12-04TORAY PLASTICS PRECISION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024065885
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-04-16
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Conventional carbon fiber reinforced resin sheets are thick, difficult to handle, and not suitable for applications requiring thin materials, and the production process involves expensive equipment and limited scalability.

Method used

A thin thermoplastic carbon fiber resin base sheet with carbon fibers oriented in multiple directions, containing thermoplastic resins with different viscosities, and a manufacturing method involving heating and stretching to achieve high elastic modulus, vibration damping, and reduced anisotropy.

Benefits of technology

The sheet exhibits high elastic modulus, vibration damping, and reduced anisotropy, making it suitable for electronic and audio components, with improved handling and scalability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167884000003
    Figure 2024167884000003
  • Figure 2024167884000004
    Figure 2024167884000004
  • Figure 2024167884000005
    Figure 2024167884000005
Patent Text Reader

Abstract

To obtain a thermoplastic carbon fiber resin substrate sheet including a thine and laterally stretched thermoplastic resin, and a carbon fiber.SOLUTION: A thermoplastic carbon fiber resin substrate sheet includes a thermoplastic resin and a carbon fiber, where the substrate sheet contains 5 to 60 wt% of a carbon fiber, a rate of the carbon fiber having a fiber length of 0.01 to 0.5 mm in the total carbon fibers is 60 wt% or more, and a thickness of the substrate sheet is 0.05 to 10.0 mm, and 20 wt% or more of the carbon fibers in the total carbon fibers are oriented in a multi direction of 30° or more to a sheet extrusion production direction.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic carbon fiber resin substrate sheet having improved mechanical properties, and a method for producing the same.

[0002] In particular, the present invention relates to a sheet material for diaphragms used in micro-speakers and microphones in electronic devices, and a method for producing the same. [Background technology]

[0003] Conventionally, carbon fiber composite materials have been obtained by preparing prepregs by impregnating carbon fibers with liquid thermosetting resins and then subjecting the prepregs to autoclaving at high temperature and pressure. However, this requires expensive equipment, such as low-temperature equipment for storing the prepregs at low temperatures and high-temperature equipment for the autoclave, and owning these facilities is a significant burden.

[0004] In view of this, as a method of using an easy-to-handle thermoplastic resin instead of the conventional thermosetting resin, Patent Document 1 discloses a molding material in which a thermoplastic resin is coated around a continuous carbon fiber bundle, and the molding material is cut into pieces of 50 mm or less.

[0005] However, conventional thermosetting carbon fiber reinforced plastic (CFRP) sheets and the sheet described in Patent Document 1 are thick and not suitable for applications requiring thin materials. Furthermore, the sheet described in Patent Document 2 is obtained by a method of pressing, which not only makes it difficult to increase the size, but also makes it difficult to handle and has poor continuous productivity, making it industrially inexpensive and unsuitable for general-purpose applications. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 2877052 [Patent Document 2] JP 2014-198756 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above problems in the prior art, and an object of the present invention is to provide a thin thermoplastic carbon fiber resin substrate sheet and a method for producing the same. [Means for solving the problem]

[0008] The thermoplastic carbon fiber resin substrate sheet of the present invention for achieving the above object has the following configuration. (1) A thermoplastic carbon fiber resin substrate sheet containing a thermoplastic resin and carbon fiber, the substrate sheet containing 5 to 60% by weight of carbon fiber, a ratio of carbon fiber having a fiber length of 0.01 to 0.5 mm in the total carbon fiber being 60% by weight or more, and the substrate sheet having a thickness of 0.05 to 2.5 mm; the thermoplastic resin includes at least a first thermoplastic resin and a second thermoplastic resin having different viscosities, and at a temperature 20 to 50° C. higher than the melting point, glass transition point, or softening point of the thermoplastic resin, the viscosity of the second thermoplastic resin is 3 to 70 times the viscosity of the first thermoplastic resin; A thermoplastic carbon fiber resin substrate sheet, in which 40% by weight or more of the total carbon fibers are oriented in multiple directions at an angle of 30° or more to the sheet extrusion manufacturing direction. (2) The thermoplastic carbon fiber resin substrate sheet according to (1), having a dynamic friction coefficient of 0.10 to 0.55. (3) Surface resistance is 1X10 10 ~1X10 14 (Unit: Ω) The thermoplastic carbon fiber resin substrate sheet according to (1) or (2). (4) The thermoplastic carbon fiber resin substrate sheet according to 1) or (2), having a surface roughness Ra of 0.05 to 0.2 μm. (5) The thermoplastic carbon fiber resin substrate sheet according to (1) or (2), wherein the thermoplastic resin is at least one selected from the group consisting of polypropylene, polyamide, polyester, and polyphenylsulfoxide. (6) The thermoplastic carbon fiber resin substrate sheet according to (1) or (2), wherein the surface is glass-coated. (7) The thermoplastic carbon fiber resin substrate sheet according to (1) or (2), having a plurality of through holes. (8) A method for producing a thermoplastic carbon fiber resin substrate sheet according to (1) or (2), comprising: heating a sheet made of carbon fibers oriented in one direction at a temperature 20 to 50°C lower than the melting point or softening point of the thermoplastic resin, and heat-stretching the sheet in the transverse direction. (9) An acoustic diaphragm using the thermoplastic carbon fiber resin substrate sheet according to (1). (10) An acoustic diaphragm using a thermoplastic carbon fiber resin substrate sheet obtained by the method for producing a thermoplastic carbon fiber resin substrate sheet according to (8). (11) An electronic device part having a semiconductor, which uses the acoustic diaphragm according to (9) or (10). Effect of the Invention

[0009] The thermoplastic carbon fiber resin substrate sheet of the present invention has a high elastic modulus due to the carbon fiber, and is therefore hard, has sliding properties and smoothness, and has a high vibration damping rate, low static electricity, and low anisotropy. Such a sheet can be suitably used for electronic parts, automobile parts, and audio parts. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a perspective view showing an example of an embodiment of a thermoplastic carbon fiber resin substrate sheet of the present invention. [Diagram 2] FIG. 2 is an enlarged top view of the thermoplastic carbon fiber resin substrate sheet of the present invention shown in FIG. [Diagram 3]2 is an enlarged top view of the thermoplastic carbon fiber resin substrate sheet of the present invention taken along the line AA' in FIG. 1. [Figure 4] 2 is an enlarged top view of the thermoplastic carbon fiber resin substrate sheet of the present invention taken along the line BB' in FIG. 1. [Diagram 5] FIG. 2 is a perspective view showing an example of an embodiment of the thermoplastic carbon fiber resin substrate sheet of FIG. 1 before stretching. [Figure 6] FIG. 6 is an enlarged top view of the thermoplastic carbon fiber resin substrate sheet before stretching in FIG. [Figure 7] 6 is an enlarged top view along the line CC' of the thermoplastic carbon fiber resin substrate sheet before stretching in FIG. 5. FIG. [Figure 8] 6 is an enlarged top view of the thermoplastic carbon fiber resin substrate sheet taken along the line DD' in FIG. 5 before stretching. FIG. [Figure 9] FIG. 2 is an explanatory diagram illustrating an example of an apparatus used for measuring vibration damping properties. [Figure 10] FIG. 11 is an explanatory diagram showing an example of measurement data of vibration damping properties. [Figure 11] FIG. 11 is an explanatory diagram in which the maximum values ​​of the damped oscillation waveform in FIG. 10 are plotted. [Figure 12] FIG. 4 is an explanatory diagram showing the measurement results of the seat vibration damping property of Example 1. [Figure 13] FIG. 11 is an explanatory diagram showing the measurement results of the seat vibration damping property of Comparative Example 1. [Figure 14] FIG. 2 is a schematic diagram showing the results of observing the orientation direction of carbon fibers under an electron microscope on the upper surface of a sheet made of a carbon fiber composite material according to one embodiment of the present invention. [Figure 15] FIG. 2 is a schematic diagram showing the results of observing the orientation direction of carbon fibers under an electron microscope in a cross section of a sheet made using the carbon fiber composite material according to one embodiment of the present invention. [Figure 16] FIG. 1 is a schematic perspective view of a porous structure formed using a carbon fiber composite material according to one embodiment of the present invention. [Figure 17] This is a glass-coated thermoplastic carbon fiber resin substrate sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The thermoplastic carbon fiber resin substrate sheet 1 of the present invention shown in FIG. 1 is formed from a composite material containing carbon fibers 22 and a thermoplastic resin 23, that is, a so-called carbon fiber reinforced thermoplastic resin composition 2, as shown in FIG. 2, photographed from the top surface direction 7 of 1.

[0012] The thermoplastic carbon fiber resin substrate sheet 1 of the present invention shown in FIG. 1 is obtained by heat-transversely stretching the thermoplastic carbon fiber resin substrate sheet 51 before stretching shown in FIG. 5 in a transverse stretching direction 5 relative to the sheet extrusion production direction 4.

[0013] The thermoplastic carbon fiber resin substrate sheet 51 before stretching in FIG. 5 is produced by the method described in Japanese Patent No. 5608818, for example.

[0014] (Transversely stretched thermoplastic carbon fiber resin substrate sheet 1) The thermoplastic carbon fiber resin substrate sheet 1 of the present invention is obtained by transversely stretching the thermoplastic carbon fiber resin substrate sheet 51 before stretching, and therefore has the same resin configuration.

[0015] (Configuration of transversely stretched thermoplastic carbon fiber resin substrate sheet 1) Examples of the carbon fiber in the present invention include polyacrylonitrile-based carbon fiber, pitch-based carbon fiber, and rayon-based carbon fiber, and any of these carbon fibers can be preferably used. The single fiber diameter of the carbon fiber is not particularly limited, but is preferably 5 to 10 μm, and more preferably 6 to 8 μm. The carbon fiber in the present invention may be either long fiber (roving) or short fiber (chopped strand), but is preferably short fiber.

[0016] Preferred examples of the thermoplastic resin in the present invention include polyolefins (e.g., polyethylene, polypropylene (PP), polybutylene, polystyrene), polyamides (e.g., nylon 6, nylon 66, nylon 11, nylon 12, nylon 610, aromatic nylons), polyimides, polyamideimides, polycarbonates, polyesters (e.g., polyethylene terephthalate, polybutylene terephthalate, polypropylene terephthalate), polyphenylene sulfide (PPS), polysulfoxides, polytetrafluoroethylene, acrylonitrile butadiene styrene copolymers (ABS), polyacetals, polyethers, polyether-ether-ketones, polyoxymethylene, etc. Also usable are derivatives or modified products of these thermoplastic resins, copolymers of these thermoplastic resins, and mixtures thereof.

[0017] The thermoplastic resin in the present invention is preferably polyamide, polyester, polyphenylsulfoxide, a derivative or copolymer thereof, or a mixture containing at least one of these, and more preferably nylon 6 or nylon 66.

[0018] Polyamide has toughness and water absorption properties, and therefore is preferable for post-processing that is subject to high impact such as punching and slitting, due to its toughness and durability.

[0019] As the thermoplastic resin, polyolefin is also preferable, and polyethylene and polypropylene can be used. These have a light specific gravity and are therefore preferable as a metal replacement. They are also preferable because they have chemical resistance.

[0020] As the thermoplastic resin in the present invention, polyphenylsulfoxide is preferable because it has high heat resistance and high chemical resistance.

[0021] The thermoplastic resin in the present invention preferably contains at least a first thermoplastic resin and a second thermoplastic resin having different viscosities. By containing two or more thermoplastic resins having different viscosities, springback can be caused during melt molding. In the present invention, at a predetermined temperature 20 to 50°C higher than the melting point of the thermoplastic resin, the viscosity of the second thermoplastic resin is preferably 3 to 70 times, more preferably 5 to 50 times, and even more preferably 10 to 30 times that of the first thermoplastic resin. The first thermoplastic resin and the second thermoplastic resin are preferably thermoplastic resins of the same composition with different molecular weights and copolymerization components.

[0022] In a thermoplastic carbon fiber resin substrate, if either a high-viscosity resin or a low-viscosity resin is contained in an extremely large amount, the springback is too large, and the sheet itself is broken or its strength is reduced. On the other hand, if the amount of high-viscosity resin is extremely large, the adhesion between the resin and the carbon fiber is poor, which causes cracks. In addition, melt-kneading using a high-viscosity resin causes the resin temperature to rise too much, resulting in decomposition of the resin. This is especially true when carbon fiber is mixed with a high-viscosity resin, which generates high heat and is prone to decomposition. Furthermore, in injection molding, even if a mixture of carbon fiber and resin is injection molded, it is difficult to produce a sheet because of its low fluidity.

[0023] The ratio of resins with different viscosities in the above-mentioned thermoplastic carbon fiber resin substrate is preferably 0.3 to 5.0 times, by weight, and more preferably 0.5 to 2.0 times, of the low-viscosity resin to the high-viscosity resin.

[0024] In the present invention, the carbon fibers 22 are preferably 5 to 60% by weight, more preferably 10 to 40% by weight, of the 100% by weight of the composite material containing the thermoplastic resin 23 and the carbon fibers 22. More preferably, the carbon fibers 22 are contained in an amount within the range of 20 to 40% by weight, which can stabilize the vibration damping characteristics of the thermoplastic carbon fiber resin substrate.

[0025] the thermoplastic resin includes at least a first thermoplastic resin and a second thermoplastic resin having different viscosities, and at a temperature 20 to 50° C. higher than the melting point, glass transition point, or softening point of the thermoplastic resin, the viscosity of the second thermoplastic resin is 3 to 70 times the viscosity of the first thermoplastic resin; It is preferable that the thermoplastic carbon fiber resin substrate sheet has 40% by weight or more of the total carbon fibers oriented in multiple directions at an angle of 30° or more with respect to the sheet extrusion production direction 4 .

[0026] (Method for manufacturing thermoplastic carbon fiber resin substrate sheet 51 before stretching) Next, a method for producing the thermoplastic carbon fiber resin substrate sheet 51 before being transversely stretched will be described below.

[0027] The above-mentioned thermoplastic carbon fiber resin pellets are melt-extruded into a sheet, and then molded into the thermoplastic carbon fiber resin substrate comprising a sheet in which the carbon fibers 22 are aligned in one direction.

[0028] In particular, molding by molten sheet extrusion is preferred, and a thermoplastic carbon fiber resin substrate that has strength equivalent to that of metal, is lightweight, and has a high vibration damping rate can be obtained. Furthermore, by molding a sheet made of this thermoplastic carbon fiber resin substrate, a thermoplastic carbon fiber resin substrate sheet that has high vibration damping properties, a high elastic modulus, suppresses static electricity generation, is smooth, has high carbon fiber orientation, and has a low dynamic friction coefficient, and has excellent industrial applicability can be obtained.

[0029] In the above-mentioned manufacturing method of the thermoplastic carbon fiber resin substrate sheet 51, when the thermoplastic carbon fiber resin substrate is cooled, one side of the substrate is brought into contact with a metal shaping surface, so that springback can be generated on the surface of the thermoplastic carbon fiber resin substrate that is not in contact with the metal shaping surface. This allows the surface of the thermoplastic carbon fiber resin substrate sheet to have a uniform mirror surface and uneven surface on the front and back sides. This can create a matte surface or a fitting effect when it is in close contact with other resins.

[0030] (Carbon fiber orientation of thermoplastic carbon fiber resin substrate sheet 51 before stretching) In Figures 5 and 6, when the thermoplastic carbon fiber resin substrate sheet 51 before stretching is viewed from above 58, 60% or more of the fibers are oriented within 30° to the sheet extrusion manufacturing direction 4. More preferably, 80% or more of the fibers are oriented within 30°. Even more preferably, 90% or more of the fibers are oriented within 30°. Even more preferably, 95% or more of the fibers are oriented within 30°.

[0031] As a result, when the thermoplastic carbon fiber resin substrate sheet 51 before stretching is viewed from the CC' cross section in Figures 5 and 7, the carbon fibers 22 are oriented in one direction, the extrusion manufacturing direction 4, so that the cross sections of the carbon fibers 22 can be seen.

[0032] As a result, when the thermoplastic carbon fiber resin substrate sheet 51 before stretching is viewed from the cross section DD' in Figs. 5 and 8, the carbon fibers 22 are oriented in one direction.

[0033] The orientation direction of the carbon fibers 22 can be confirmed in the ranges shown in Figs. 14 and 15 with respect to the extrusion direction of the sheet by taking enlarged photographs of Figs. 6, 7 and 8 with an electron microscope.

[0034] In order to orient 60% or more by weight of the carbon fibers 22 within 30° of the sheet extrusion manufacturing direction 4 from a predetermined direction, a method can be used in which pellets consisting of two thermoplastic resins 23 with the above-mentioned viscosity difference and carbon fibers 22 with an average fiber length of 0.01 to 0.5 mm are used, and the pellets are melted in a single-screw extruder, extruded in a certain direction from a die, and fixed in contact with a roll, as described above.

[0035] In the present invention, the thermoplastic carbon fiber resin substrate sheet 51 before stretching preferably has a high elastic modulus because the carbon fibers 22 are oriented, and in particular, the elastic modulus in the orientation direction of the carbon fibers 22 is preferably 8 GPa to 20 GPa, more preferably 10 to 17 GPa, and even more preferably 10 to 15 GPa. Note that the elastic modulus in the transverse direction of the carbon fibers 22 is 90° to the orientation direction, and is therefore 1 / 2 to 1 / 4 of the elastic modulus in the longitudinal direction.

[0036] (Method for manufacturing transversely stretched thermoplastic carbon fiber resin substrate sheet 1) The thermoplastic carbon fiber resin substrate sheet 1 of the present invention is obtained by heating and stretching a sheet made of short carbon fibers oriented in one direction in the transverse stretching direction 5 while heating a thermoplastic carbon fiber resin substrate sheet 51 before stretching, which is a sheet in which short carbon fibers are highly oriented in the sheet extrusion manufacturing direction 4 shown in Fig. 5, at a temperature 15°C to 60°C lower than the melting point and softening point of the resin, to obtain a transversely stretched thermoplastic carbon fiber resin substrate sheet 1. More preferably, the heat stretching is performed at a temperature 20°C to 50°C lower than the melting point and softening point of the resin. More preferably, the heat stretching is performed while heating at a temperature 20°C to 35°C lower than the melting point and softening point of the resin.

[0037] The stretching ratio is preferably from 1.5 to 5 times, more preferably from 1.8 to 3.5 times, and even more preferably from 1.9 to 2.5 times.

[0038] Furthermore, in the high-magnification stretching, it is preferable to stretch the film in multiple steps, such as two or three times, rather than stretching the film all at once, in order to achieve stable stretching.

[0039] In addition, the thickness of the stretched sheet is about 10 to 15% thicker than immediately after stretching due to shrinkage that occurs after cooling. As a result, the stretch ratio is not directly proportional to the thickness of the stretched sheet. (Sheet thickness) The thermoplastic carbon fiber resin substrate sheet of the present invention has a thickness of 0.05 to 2.5 mm, preferably 0.1 to 0.5 mm, and more preferably 0.1 to 0.3 mm.

[0040] When it is desired to make the film as thin as possible by transverse stretching, in order to disperse the orientation as much as possible without directing it in one direction, the target sheet can be obtained by making the film 1 / 1.5 to 1 / 5 thinner as a result of transverse stretching than the base sheet.

[0041] An example of equipment for transverse stretching is described in JP-A-9-39088, which uses clips to grip a sheet and spread it in the transverse direction.

[0042] The carbon fibers 22 are stretched laterally from one direction, and are dispersed by the transverse stretching, so that the orientation becomes multidirectional. As a result, the difference in the longitudinal and transverse elastic moduli of the sheet disappears.

[0043] The elastic modulus of the thermoplastic carbon fiber resin substrate sheet 1 of the present invention is preferably 2 GPa to 15 GPa, more preferably 3 to 10 GPa, and even more preferably 5 to 8 GPa, regardless of the direction of the sheet. The elastic modulus may be reversed between the longitudinal direction and the transverse direction of the sheet.

[0044] In other words, the elastic modulus in the machine direction of the original sheet becomes 1 / 2 to 1 / 4 by transverse stretching, while the elastic modulus in the transverse direction becomes 2 to 4 times larger. The difference between the machine direction and transverse direction is 1.2 to 0.8 times.

[0045] (Orientation direction of carbon fibers 22 in transversely stretched thermoplastic carbon fiber resin substrate sheet 1) In the thermoplastic carbon fiber resin substrate sheet 1 of the present invention, as a result of being stretched laterally, as seen in the top view enlarged in FIG. 2, 30% or more of the fibers are dispersed in multiple directions at an angle of 30° or more relative to the sheet extrusion manufacturing direction 4. It is further preferable that 40% or more of the fibers are dispersed in multiple directions at an angle of 30° or more. Even more preferably, 50% or more of the fibers are dispersed in multiple directions at an angle of 30° or more. Even more preferably, 60% or more of the fibers are dispersed in multiple directions at an angle of 30° or more.

[0046] As a result, when the thermoplastic carbon fiber resin substrate sheet 1 of the present invention is viewed from the A-A' cross section in Figure 3, the carbon fibers 22 are obliquely oriented in multiple directions, and as a result, when the thermoplastic carbon fiber resin substrate sheet 1 of the present invention is viewed from the B-B' cross section in Figure 4, the carbon fibers 22 are obliquely oriented in multiple directions.

[0047] (Characteristics of transversely stretched thermoplastic carbon fiber resin substrate sheet 1) In the thermoplastic carbon fiber resin substrate sheet of the present invention, the composite material containing the thermoplastic resin 23 and the carbon fiber 22 preferably has a logarithmic vibration damping factor of 0.07 to 0.30. If the logarithmic vibration damping factor of the composite material is less than 0.07, the vibration of the thermoplastic carbon fiber resin substrate sheet may remain for a long time when the mouse is used vigorously, which may cause an erroneous operation. If the logarithmic vibration damping factor exceeds 0.30, the vibration of the thermoplastic carbon fiber resin substrate sheet may be excessively suppressed, and the repulsion may be transmitted, which may cause an uncomfortable feeling. The logarithmic vibration damping factor is preferably in the range of 0.08 to 0.30, more preferably in the range of 0.10 to 0.30, and even more preferably in the range of 0.15 to 0.30.

[0048] The relationship between the logarithmic vibration damping rate and the loss factor is that the logarithmic vibration damping rate is equal to the loss factor multiplied by pi (logarithmic vibration damping rate = loss factor × π). If the logarithmic vibration damping rate of a composite material is five times that of a metal of the same thickness, such as stainless steel, the vibration of a thermoplastic carbon fiber resin base sheet using this composite material is reduced to 1 / 5 of the time of that of a stainless steel sheet. In other words, the residual vibration of the thermoplastic carbon fiber resin base sheet disappears five times faster, allowing it to respond very clearly to the next operation. On the other hand, since the logarithmic vibration damping rate of metal is smaller than that of a composite material of the same thickness, the vibration of the metal sheet is relatively likely to remain.

[0049] Therefore, in the thermoplastic carbon fiber resin substrate used in the present invention, the loss factor of the composite material is preferably 0.02 or more, more preferably 0.025 or more. The loss factor of the composite material is preferably 0.03 or more, more preferably 0.04 or more, even more preferably 0.05 or more, and most preferably 0.06 or more.

[0050] (acoustic use) For this reason, it can be suitably used for acoustic parts with high vibration damping and little residual sound, such as speaker housings, speaker cones (diaphragms), tweeters, woofers, and speaker covers (grilles).

[0051] (Audio diaphragms, semiconductors and parts thereof) Examples of an acoustic diaphragm using the thermoplastic carbon fiber resin substrate sheet of the present invention, or an electronic device having a semiconductor and a part thereof using the diaphragm include those described below. In particular, it can be used as a thin-film diaphragm in micro-speakers that require thinness, and is also suitable for use in MEMS (Micro Electro Mechanical Systems) speakers, which are a type of micro-speaker that require even thinner thickness.

[0052] This is because sheets containing carbon fibers have high specific elasticity and high vibration damping properties, resulting in excellent sound speed and little rattle noise, and therefore excellent acoustic properties. In particular, the thermoplastic carbon fiber resin substrate sheet of the present invention can be made thinner, making it possible to make acoustic parts smaller and thinner.

[0053] Similarly, it can be used as a thin-film diaphragm in microphones that require thinness. It can also be used favorably in MEMS microphones, a type of microspeaker that requires even thinner thickness. In particular, the thinner thickness improves sound pressure, and the improved rigidity and internal loss due to the carbon fiber reduce distortion.

[0054] MEMS elements use electronic components to make a diaphragm containing a piezoelectric element, which can be made smaller, thinner, and more energy-efficient, and can be used in mobile devices such as mobile phones, smartphones, wireless earphones, tablets, and mobile PCs.

[0055] (Precision motion application) The thermoplastic carbon fiber resin substrate sheet of the present invention can suppress vibrations early on and can therefore be used in components that require precise operation.

[0056] (Antistatic use) The thermoplastic carbon fiber resin substrate used in the thermoplastic carbon fiber resin substrate sheet 1 of the present invention contains carbon fiber 22, and therefore can suppress the generation of static electricity compared to resin products that do not contain carbon fiber. Therefore, there are fewer problems caused by static electricity in winter.

[0057] The thermoplastic carbon fiber resin substrate sheet 1 of the present invention has a surface resistance of 1×10 9 ~1X10 15 It is preferable that the concentration is 1X10 10 ~1X10 14 , more preferably 1X10 11 ~1X10 13 It is.

[0058] (Sliding applications) The thermoplastic carbon fiber resin substrate sheet 1 of the present invention preferably has a low coefficient of friction, and the smaller the friction, the better the sliding properties. Therefore, the dynamic friction coefficient is preferably 0.10 to 0.55, more preferably 0.3 to 0.5, and even more preferably 0.35 to 0.45.

[0059] The thermoplastic carbon fiber resin substrate sheet 1 of the present invention preferably has a small and constant surface roughness, and a low and constant roughness during handling allows stable parts to be produced.

[0060] The thermoplastic carbon fiber resin substrate sheet 1 of the present invention preferably has a low surface roughness R(a) of 0.02 μm to 0.25 μm, more preferably 0.05 μm to 0.20 μm, and further preferably 0.08 to 0.15 μm.

[0061] (Punching applications) The thermoplastic carbon fiber resin substrate sheet 1 of the present invention can be used as a punched thermoplastic carbon fiber resin substrate sheet. This can be produced by using the method described in Japanese Patent No. 6122375, for example.

[0062] In this case, as shown in the schematic perspective view of FIG. 16, the thermoplastic carbon fiber resin substrate sheet is a thermoplastic carbon fiber resin substrate 2 having a plurality of through holes 163, the thickness of the thermoplastic carbon fiber resin substrate 2 is preferably 0.05 mm to 10.0 mm, more preferably 0.1 mm to 2.0 mm, the diameter of the through holes 163 is preferably 0.1 mm to 10.0 mm, more preferably 0.5 mm to 5.0 mm, and even more preferably 1.0 mm to 3.0 mm, and the total opening area of ​​the plurality of through holes 163 is preferably 5% to 75% of the area of ​​the entire sheet, more preferably 20% to 70%, and even more preferably 30% to 60%.

[0063] The thermoplastic carbon fiber resin substrate used in the thermoplastic carbon fiber resin substrate sheet 1 of the present invention is less likely to break during punching and has excellent processability. Furthermore, the thermoplastic carbon fiber resin substrate can also improve water resistance and dirt resistance, and can also improve rigidity. (Strength use) The thermoplastic carbon fiber resin substrate used in the above-mentioned thermoplastic carbon fiber resin substrate sheet 1 of the present invention contains short carbon fibers at a predetermined ratio, and therefore can maintain sufficient hardness as a thermoplastic carbon fiber resin substrate sheet.

[0064] (For glass coating) In addition, the method for glass coating 172 on the thermoplastic carbon fiber resin substrate sheet 1 of the present invention can be, for example, the method described in JP-A-2022-101765.

[0065] 17, in a cross-sectional view 171 of a glass-coated thermoplastic carbon fiber resin substrate sheet, the rigidity of the sheet can be increased by 10 to 20% by coating the thermoplastic carbon fiber resin substrate sheet 1 of the present invention with a thin glass coat 172. Also, instead of the glass coat 172, the sheet can be covered with a resin laminate sheet.

[0066] (For bonding purposes) Post-processing of the thermoplastic carbon fiber resin substrate sheet 1 of the present invention will also be described.

[0067] The thermoplastic carbon fiber resin substrate sheet of the present invention can be composed of a thermoplastic carbon fiber resin substrate sheet, an adhesive, and a foam material. It can also be composed by partially including the thermoplastic carbon fiber resin substrate sheet 1 of the present invention. Since it is composed by combining the above-mentioned thermoplastic carbon fiber resin substrate sheets having high vibration damping properties, it can be used as a single sheet or a laminated product for audio and in-vehicle parts, IT parts, PC peripherals, AI, robot applications, aircraft, drones, bicycles, motorcycles, wheelchairs, beds, building equipment, etc.

[0068] The laminate is not particularly limited, but is preferably one that has high adhesion to the base sheet and is lightweight. For example, polyolefin (e.g., polyethylene, polypropylene (PP), polybutylene, polystyrene), polyamide (e.g., nylon 6, nylon 66, nylon 11, nylon 12, nylon 610, aromatic nylon), polyimide, polyamideimide, polycarbonate, polyester (e.g., polyethylene terephthalate, polybutylene terephthalate, polypropylene terephthalate), polyphenylene sulfide (PPS), polysulfoxide, polytetrafluoroethylene, acrylonitrile butadiene styrene copolymer (ABS), polyacetal, polyether, polyether-ether-ketone, polyoxymethylene, etc. may be used, and foamed materials may also be used.

[0069] In particular, the material may be a thermosetting resin such as polyurethane, a metal, a silicone resin, a woven or knitted fiber, or a nonwoven fabric. Natural materials such as wood or stone, glass, quartz, or other inorganic materials may also be used. Furthermore, multiple types of these materials may be stacked in any number of layers.

[0070] The back mat and the thermoplastic carbon fiber resin substrate can be bonded using double-sided tape or adhesive. The adhesive is not limited to these. Bonding with thermosetting resin or thermoplastic resin is also possible, making it suitable for mouse pads for personal computers.

[0071] It is also possible to heat the thermoplastic carbon fiber resin substrate sheet and bond it to the mat, or to heat the mat and bond it to the thermoplastic carbon fiber resin substrate sheet. EXAMPLES

[0072] Next, examples will be described. In each example and comparative example, the materials and measurement methods used are as follows.

[0073] (1) Materials used (A) Carbon fiber A1: Carbon fiber with a fiber diameter of 7 μm.

[0074] (B) a first thermoplastic resin B1: Nylon 6 (melting point 225°C, viscosity at 275°C: 80 poise) B2: Nylon 66 (melting point: 255°C, viscosity at 305°C: 250 poise) B3: PP (melting point: 170°C, viscosity at 220°C: 70 poise) B4: ABS (glass transition point (softening point): 190°C, viscosity at 240°C: 120 poise) B5: PPS (melting point: 285°C, viscosity at 335°C: 260 poise) B6: PC (softening point: 146°C, viscosity at 290°C: 125 poise).

[0075] (C) a second thermoplastic resin C1: Nylon 6 (melting point: 225°C, viscosity at 275°C: 1,100 poise) C2: Nylon 66 (melting point: 255°C, viscosity at 305°C: 5,500 poise) C3: PP (melting point: 170°C, viscosity at 220°C: 1,770 poise) C4: ABS (softening point: 190℃, viscosity at 240℃: 2,520 poise) C5: PPS (melting point: 285°C, viscosity at 335°C: 8,060 poise) C6: PC (softening point: 146°C, viscosity at 290°C: 1,890 poise).

[0076] (D) Composite material D1: Contains 25% by weight of A1, 50% by weight of B1, and 25% by weight of C1 D2: Contains 35% by weight of A1, 25% by weight of B1, and 40% by weight of C1 D3: Contains 30% by weight of A1, 55% by weight of B2, and 15% by weight of C2 D4: Contains 25% by weight of A1, 35% by weight of B3, and 40% by weight of C3 D5: Contains 35% by weight of A1, 25% by weight of B4, and 40% by weight of C4 D6: Contains 40% by weight of A1, 30% by weight of B5, and 30% by weight of C5 D7: Contains 30% by weight of A1, 30% by weight of B6, and 40% by weight of C6.

[0077] (E) Metal E1: Stainless steel (SUS304).

[0078] (2) Measurement of fiber length of carbon fiber The fiber length of the carbon fibers 22 was measured using a microfocus X-ray transmission fluoroscopy device (SMX-1000 PLUS manufactured by Shimadzu Corporation).

[0079] (3) Measurement of vibration damping characteristics The vibration damping characteristics were measured by a test method using a vibration damping measuring machine 91 shown in Figure 9. This method is based on JIS G0602 (1993). Specifically, it was a one-end fixed impact vibration method, and the measurement conditions were a cantilever projection length of 100 mm, the vibration position was on the free end side of the cantilever, and the vibration method was step relaxation vibration. The measurement devices used were a Keyence LK-G30 CCD laser displacement meter 94 and an Air Brown Photon I FFT analyzer 96. The measurement methods were appropriately used according to the shape based on JIS G0602 (1993).

[0080] (4) Calculation of loss factor and logarithmic vibration damping ratio The loss factor was calculated by the following formula (1). The obtained loss factor was multiplied by the circular constant π to calculate the logarithmic vibration damping factor. η=2×ln(tanθ) / √((2π) 2 +[ln(tanθ)] 2 ) (1) In the formula, η is the damping vibration rate, and θ is the slope of the line that passes through the origin and connects each point on the graph shown in Fig. 11. Note that Fig. 11 is a graph plotting the maximum values ​​of the damped vibration waveform in Fig. 10, and more specifically, it is a graph in which the maximum values ​​X0, X1... of the response displacement are read from the damped free vibration waveform shown in Fig. 10, and Xk+1 is plotted on the horizontal axis and Xk on the vertical axis, that is, the points (X2, X1), (X3, X2), and (X4, X3) are plotted.

[0081] (5) Calculation of water absorption rate 100g of composite material was dried in a vacuum dryer at 60℃ for 12 hours, then left in a 25℃ x 65% RH environment for one week, and the weight increase was divided by 100.

[0082] (6) Calculation of surface resistance Resistivity of conductive plastics measured using the four-probe method specified in JIS 7194 (1994).

[0083] (7) Calculation of dynamic friction coefficient (Suzuki method) Measured according to the sliding abrasion test method for plastics JIS 7218 (1986).

[0084] (8) Calculation method of elastic modulus Tensile test was performed according to JIS K7161 (2014).

[0085] (9) Calculation of surface roughness Calculation of surface roughness Roughness was measured according to JIS B0601 (1994).

[0086] [Example 1] A sheet having a thickness of 1.0 mm was produced using the composite material D1. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.25 mm, the ratio of the carbon fibers 22 having a fiber length of 0.01 mm to 0.5 mm to the total carbon fibers was 65% by weight, the loss factor was 0.054, the surface roughness Ra was 0.075 μm, the elastic modulus was 10.1 GPa with the orientation of the carbon fibers 22, and the elastic modulus was 3.2 GPa with the transverse orientation of the carbon fibers 22. The surface resistivity was 3.1×10 11 The elastic modulus Ω and dynamic friction coefficient were 0.38. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 98% (Table 1).

[0087] This was cut to a width of 200 mm, and stretched 3.0 times in the transverse direction at 180° C. with respect to the orientation of the carbon fibers 22 to produce a sheet with a thickness of 0.35 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.25 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 65% by weight, the loss coefficient was 0.055, the surface roughness Ra was 0.065 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 3.5 GPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 4.1 GPa. The surface resistance was 2.5×10 11 The coefficient of dynamic friction was 0.26. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. 55% of the fibers were dispersed in multiple directions at 30° or more with respect to the sheet extrusion manufacturing direction 4 (Table 1).

[0088] Furthermore, as shown in FIG. 12, in the transversely stretched thermoplastic carbon fiber resin substrate sheet of Example 1, the displacement 121 attenuates early compared to FIG. 13 of the stainless steel of Comparative Example 1 described later, and the vibration is suppressed early.

[0089] [Example 2] A sheet having a thickness of 0.3 mm was produced using the composite material D2. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.31 mm, the ratio of the carbon fibers 22 having a fiber length of 0.01 mm to 0.5 mm to the total carbon fibers was 70% by weight, and the loss factor was 0.082. The surface roughness Ra was 0.077 μm, the elastic modulus was 15.5 GPa with the carbon fibers 22 oriented, and the elastic modulus was 3.8 GPa with the carbon fibers 22 oriented laterally. The surface resistivity was 1.4×10 10 The elastic modulus Ω and dynamic friction coefficient were 0.38. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 97%.

[0090] This was cut to a width of 200 mm and stretched in the transverse direction at 190° C. to 2.7 times the width relative to the orientation of the carbon fibers 22 to produce a sheet with a thickness of 0.12 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.31 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 70% by weight, the loss coefficient was 0.089, the surface roughness Ra was 0.055 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 5.3 GPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 5.6 GPa. The surface resistance was 1.9×10 11 The coefficient of dynamic friction was 0.25. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. 63% of the fibers were dispersed in multiple directions at 30° or more with respect to the sheet extrusion manufacturing direction 4 (Table 1).

[0091] [Example 3] A sheet having a thickness of 0.5 mm was produced using the composite material D3. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.45 mm, the ratio of the carbon fibers 22 having a fiber length of 0.01 mm to 0.5 mm to the total carbon fibers was 68 weight %, and the loss factor was 0.040. The surface roughness Ra was 0.079 μm, and the elastic modulus was 9.0 GPa with the orientation of the carbon fibers 22. The elastic modulus was 3.3 GPa with the transverse orientation of the carbon fibers 22.

[0092] Surface resistance is 4.9X10 11The elastic modulus Ω and dynamic friction coefficient were 0.36. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 98%.

[0093] This was cut to a width of 200 mm and stretched 2.0 times in the transverse direction at 220°C with respect to the orientation of the carbon fibers 22 to produce a sheet with a thickness of 0.26 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.45 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 68% by weight, the loss coefficient was 0.039, the surface roughness Ra was 0.071 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 3.2 MPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 3.5 MPa. The surface resistance was 2.1×10 11 The coefficient of dynamic friction was 0.28. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. 45% of the fibers were dispersed in multiple directions at 30° or more with respect to the sheet extrusion manufacturing direction 4 (Table 1).

[0094] [Example 4] A sheet having a thickness of 1.5 mm was produced using the composite material D4. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.40 mm, the proportion of the carbon fibers 22 having a fiber length of 0.01 mm to 0.5 mm in the total carbon fibers was 71 weight %, and the loss factor was 0.045. The surface roughness Ra was 0.088 μm, and the elastic modulus was 8.8 MPa with the orientation of the carbon fibers 22. The elastic modulus was 2.5 MPa with the transverse orientation of the carbon fibers 22. The surface resistance was 4.8×10 12 The elastic modulus Ω and dynamic friction coefficient were 0.43. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 95%.

[0095] This was cut to a width of 200 mm, and stretched 5.0 times in the transverse direction at 130°C with respect to the orientation of the carbon fibers 22 to produce a sheet with a thickness of 0.33 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.40 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 71 weight %, the loss coefficient was 0.048, the surface roughness Ra was 0.079 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 2.8 MPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 3.0 MPa. The surface resistivity was 5.2×10 13 The elastic modulus Ω and dynamic friction coefficient were 0.35. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 35% (Table 1).

[0096] [Example 5] A sheet having a thickness of 0.35 mm was produced using the composite material D5. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.2 mm, the proportion of the carbon fibers 22 having a fiber length of 0.01 mm to 0.5 mm in the total carbon fibers was 66 weight %, and the loss factor was 0.115. The surface roughness Ra was 0.090 μm, and the elastic modulus was 8.6 MPa with the orientation of the carbon fibers 22. The elastic modulus was 2.6 MPa with the transverse orientation of the carbon fibers 22. The surface resistance was 8.3×10 11 The elastic modulus Ω and dynamic friction coefficient were 0.51. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 88%.

[0097] This was cut to a width of 200 mm and stretched in the transverse direction at 140° C. to 2.1 times the length of the carbon fibers 22, to produce a sheet with a thickness of 0.17 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.20 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 66% by weight, the loss coefficient was 0.108, the surface roughness Ra was 0.064 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 2.8 MPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 3.1 MPa. The surface resistivity was 9.6×10 13The coefficient of dynamic friction was 0.52. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. 40% of the fibers were dispersed in multiple directions at 30° or more with respect to the extrusion manufacturing direction 4 (Table 1).

[0098] [Example 6] A sheet having a thickness of 0.8 mm was produced using the composite material D6. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.23 mm, the proportion of the carbon fibers 22 having a fiber length of 0.01 mm to 0.5 mm in the total carbon fibers was 80 weight %, and the loss factor was 0.026. The surface roughness Ra was 0.112 μm, and the elastic modulus was 16.1 MPa with the orientation of the carbon fibers 22. The elastic modulus was 5.3 MPa with the transverse orientation of the carbon fibers 22. The surface resistance was 6.3×10 13 The elastic modulus Ω and dynamic friction coefficient were 0.56. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 97%.

[0099] This was cut to a width of 200 mm and stretched in the transverse direction at 245°C by 2.2 times relative to the orientation of the carbon fibers 22 to produce a sheet with a thickness of 0.41 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.23 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 80% by weight, the loss coefficient was 0.025, the surface roughness Ra was 0.108 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 5.1 MPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 6.3 MPa. The surface resistivity was 1.0×10 13 The coefficient of dynamic friction was 0.58. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. 41% of the fibers were dispersed in multiple directions at 30° or more with respect to the extrusion manufacturing direction 4 (Table 1).

[0100] [Example 7] A sheet having a thickness of 0.5 mm was produced using the composite material D7. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.32 mm, the ratio of the carbon fibers 22 having a length of 0.01 to 0.5 mm was 76% by weight of the total carbon fibers, and the loss factor was 0.056. The surface roughness Ra was 0.099 μm, and the elastic modulus was 9.9 MPa with the orientation of the carbon fibers 22. The elastic modulus was 3.5 MPa with the transverse orientation of the carbon fibers 22. The surface resistance was 4.7×10 12 The dynamic friction coefficient Ω was 0.51. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation rate of the carbon fibers 22 was 6%.

[0101] This was cut to a width of 200 mm and stretched in the transverse direction at 150° C. to 1.9 times the width relative to the orientation of the carbon fibers 22 to produce a sheet with a thickness of 0.33 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.32 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 76 wt %, the loss coefficient was 0.057, the surface roughness Ra was 0.089 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 3.1 MPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 4.5 MPa. The surface resistance was 2.8×10 13 The coefficient of dynamic friction was 0.50. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. 36% of the fibers were dispersed in multiple directions at 30° or more with respect to the extrusion manufacturing direction 4 (Table 1).

[0102] [Example 8] The laterally stretched sheet of Example 1 was used to prepare a porous structure (punched material) having through holes 163 arranged in a 60° staggered pattern with a hole diameter of 1.5 mm, an opening ratio of 51%, and a pitch of 2.0 mm.

[0103] [Example 9] The transversely stretched sheet obtained in Example 3 was coated with a glass coat 172 having a thickness of 7 μm. The loss factor was 0.039, the surface roughness Ra was 0.079 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 3.8 MPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 4.0 MPa. The surface resistance was 5.0×10 14 Ω, the dynamic friction coefficient was 0.21. [Example 10] A sheet having a thickness of 0.3 mm was produced using the composite material D2. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.31 mm, the ratio of the carbon fibers 22 having a fiber length of 0.01 mm to 0.5 mm to the total carbon fibers was 70% by weight, and the loss factor was 0.082. The surface roughness Ra was 0.077 μm, the elastic modulus was 15.5 GPa with the carbon fibers 22 oriented, and the elastic modulus was 3.8 GPa with the carbon fibers 22 oriented laterally. The surface resistivity was 1.4×10 10 The elastic modulus Ω and dynamic friction coefficient were 0.38. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. The orientation of the carbon fibers 22 in the same direction was 97%.

[0104] This was cut to a width of 100 mm, and stretched in the transverse direction at 195°C to 6.2 times in two stages, stretched in the transverse direction relative to the orientation of the carbon fibers 22, to produce a sheet with a thickness of 0.05 mm. In the obtained sheet, the average fiber length of the carbon fibers 22 was 0.31 mm, the proportion of carbon fibers 22 with fiber lengths of 0.01 mm to 0.5 mm in the total carbon fibers was 70 weight %, the loss coefficient was 0.090, the surface roughness Ra was 0.056 μm, and the elastic modulus in the orientation of the carbon fibers 22 was 5.3 GPa. The elastic modulus in the transverse direction of the carbon fibers 22 was 5.5 GPa. The surface resistance was 1.9×10 11 The Ω and dynamic friction coefficient were 0.25. The fiber lengths of the carbon fibers 22 were distributed in a manner close to a normal distribution. 70% of the fibers were dispersed in multiple directions at 30° or more with respect to the sheet extrusion manufacturing direction 4 (Table 1).

[0105] [Example 11] The laterally stretched sheet obtained in Example 10 was used as a diaphragm and mounted in a MEMS speaker, which is a type of micro speaker, and further mounted in a mobile phone and an earphone. [Example 12] The laterally stretched sheet obtained in Example 2 was used as a diaphragm and was mounted on a MEMS microphone, which is a type of micro earphone, and further mounted on a mobile phone and an earphone.

[0106] [Comparative Example 1] The metal E1 was used to prepare a sheet having a thickness of 0.15 mm. The loss factor of the obtained sheet was 0.016. The surface roughness Ra was 0.210 μm, the elastic modulus was 195 GPa, and the surface resistance was 5.6×10 -5 The elastic modulus was high, but the roughness was also high, and the loss factor was also high. As a result, it was not suitable for use as a sliding material or an acoustic component. In fact, as shown in FIG. 13, the material of Comparative Example 1 took a time 122 for the displacement 121 to attenuate, and the vibration suppression effect was lower than that of Example 1. (Table 1)

[0107] [Comparative Example 2] The resin B2 not containing the carbon fiber 22 was used to prepare a sheet having a thickness of 0.15 mm. The loss factor was 0.11. The surface roughness Ra was 0.028 μm, and the elastic modulus was 2.6 GPa. The surface resistivity was 7.2×10 -14 The elastic modulus was low, but the dynamic friction coefficient was high. As a result, it could not be used as a sliding material or an acoustic component.

[0108] [Comparative Example 3] Using the sheet of Comparative Example 1, a punched material was produced with through holes arranged in a 60° zigzag pattern with a hole diameter of 2 mm, an opening rate of 40%, and a pitch of 3 mm (Table 1). When used as a filter outdoors by the sea, it rusted and could not be used. This is because the oxide film of the stainless steel was destroyed by punching, accelerating the rusting.

[0109] [Comparative Example 4] An attempt was made to produce a punched material using the sheet of Comparative Example 2 with through holes arranged in a 60° staggered pattern with a hole diameter of 2 mm, an opening rate of 40%, and a pitch of 3 mm, but the sheet stretched due to the heating and stretching caused by punching, and no punched material could be obtained.

[0110] [Table 1-1]

[0111] [Table 1-2] [Explanation of symbols]

[0112] 1. Laterally stretched thermoplastic carbon fiber resin substrate sheet 2. Carbon fiber reinforced thermoplastic resin composition 4 Sheet extrusion manufacturing direction 5 Lateral stretching direction 7 1 Top view 21 Enlarged top view of 1 22 Carbon Fiber 23 Thermoplastic resin 31 A-A' seat side enlarged view 41 B-B' sheet side enlarged view 51 Thermoplastic carbon fiber resin base sheet before stretching 52 Thermoplastic carbon fiber resin substrate before stretching 58 51 top view 61 Enlarged top view of 51 71 C-C' sheet side enlarged view 81 D-D' sheet side enlarged view 91 Vibration damping measuring instrument 92 Fixture 93 Test Pieces 94 Laser Displacement Meter 95 AMP 96 FTT Analyzer 97 PC 121 Displacement 122 hours 161 is a schematic perspective view of a porous structure of a transversely stretched thermoplastic carbon fiber resin substrate sheet. 163 holes 171 Cross-sectional view of glass-coated thermoplastic carbon fiber resin substrate sheet 172 Glass Coat

Claims

1. A thermoplastic carbon fiber resin substrate sheet containing a thermoplastic resin and carbon fibers, the substrate sheet containing 5 to 60% by weight of carbon fibers, a ratio of carbon fibers having a fiber length of 0.01 to 0.5 mm being 60% by weight or more of the total carbon fibers, and the substrate sheet having a thickness of 0.05 to 2.5 mm, the thermoplastic resin includes at least a first thermoplastic resin and a second thermoplastic resin having different viscosities, and at a temperature 20 to 50° C. higher than the melting point, glass transition point, or softening point of the thermoplastic resin, the viscosity of the second thermoplastic resin is 3 to 70 times the viscosity of the first thermoplastic resin; A thermoplastic carbon fiber resin substrate sheet, in which 40% by weight or more of the total carbon fibers are oriented in multiple directions at an angle of 30° or more relative to the sheet extrusion manufacturing direction.

2. The thermoplastic carbon fiber resin substrate sheet of claim 1, having a dynamic friction coefficient of 0.10 to 0.

55.

3. Surface resistance is 1X10 10 ~1X10 14 The thermoplastic carbon fiber resin substrate sheet according to claim 1 or 2, wherein the modulus of elasticity is (unit: Ω).

4. The thermoplastic carbon fiber resin substrate sheet according to claim 1 or 2, having a surface roughness Ra of 0.05 to 0.2 μm.

5. The thermoplastic carbon fiber resin substrate sheet according to claim 1 or 2, wherein the thermoplastic resin is at least one selected from the group consisting of polypropylene, polyamide, polyester, and polyphenylsulfoxide.

6. The thermoplastic carbon fiber resin substrate sheet according to claim 1 or 2, wherein the surface is glass coated.

7. The thermoplastic carbon fiber resin substrate sheet according to claim 1 or 2, having a plurality of through holes.

8. The method for producing the thermoplastic carbon fiber resin substrate sheet according to claim 1, comprising: heating a sheet made of carbon fibers oriented in one direction at a temperature 20 to 50° C. lower than the melting point or softening point of the thermoplastic resin; and heat-stretching the sheet in the transverse direction.

9. An acoustic diaphragm using the thermoplastic carbon fiber resin substrate sheet according to claim 1.

10. An acoustic diaphragm using a thermoplastic carbon fiber resin substrate sheet obtained by the method for producing a thermoplastic carbon fiber resin substrate sheet according to claim 8.

11. An electronic device part having a semiconductor, which uses the acoustic diaphragm according to claim 9 or 10.

Citation Information

Patent Citations

  • Production method of carbon fiber resin composite material molding

    JP2014198756A

  • Fiber-reinforced thermoplastic resin sheet

    JP2877052B2