Surface treatment steel material
A surface-treated steel material with a zinc-based plating layer and optimized chemical conversion coating achieves superior paint adhesion and conductivity by controlling organic functional group distribution and moisture, addressing the limitations of existing chromate-free treatments.
Patent Information
- Application Number
- JP2023084277
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Existing surface-treated steel materials, particularly those with chromate-free treatments, face challenges in achieving superior paint adhesion under severe conditions, such as high-temperature water immersion, and often compromise electrical conductivity when organic resins are included.
A surface-treated steel material with a zinc-based plating layer and a chemical conversion coating containing an organosilicon compound with siloxane bonds, phosphorus, and fluorine, optimized through FT-IR analysis to maintain uniform distribution of organic functional groups and reduce residual moisture, ensuring excellent paint adhesion and conductivity.
The solution provides a surface-treated steel material with enhanced paint adhesion and electrical conductivity, maintaining performance under severe conditions by controlling the distribution and moisture content in the chemical conversion coating.
Smart Images

Figure 2024167942000004 
Figure 2024167942000001 
Figure 2024167942000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel material. [Background technology]
[0002] Conventionally, plated steel sheets (zinc-based plated steel sheets), in which a plating layer mainly made of zinc is formed on the surface of the steel sheet, have been used for a wide range of applications, including automobiles, building materials, and home appliances. Furthermore, for the purpose of imparting corrosion resistance, paint adhesion, and the like to the surface of such zinc-based plated steel sheet, methods such as a chromate treatment using a treatment solution containing chromic acid, dichromic acid or a salt thereof as a main component, a treatment using a metal surface treatment agent that does not contain chromium, a phosphate treatment, a treatment using a silane coupling agent alone, and an organic resin coating treatment are generally known and in practical use.
[0003] As an example of a technique that mainly uses a silane coupling agent, Patent Document 1 discloses a chromate-free surface-treated metal material in which a water-based metal surface treatment agent containing an organosilicon compound (W) obtained by blending two types of silane coupling agents with specific structures in a specific mass ratio and a specific inhibitor is applied to the surface of the metal material, and then dried to form a composite coating containing each of the components. Furthermore, Patent Document 2 discloses a surface-treated metal material that has been subjected to a chromate-free surface treatment that is excellent in each of the elements of corrosion resistance, heat resistance, fingerprint resistance, electrical conductivity, paintability, and resistance to black residue during processing, and a chromium-free metal surface treatment agent that is used to impart excellent corrosion resistance and alkali resistance to metal materials. Furthermore, Patent Document 3 discloses a surface-treated steel material having a concentrated layer in which the P concentration is higher than the average P concentration in the range from the surface of a chromate-free surface treatment coating to the interface between the coating and the plating layer, which is obtained by applying a metal surface treatment agent containing a silane coupling agent and P to a plated steel sheet. Patent Document 4 also describes a chromate-free precoated metal sheet having an upper coating film (α) formed on at least one side of the metal sheet, in which (1) a silane coupling agent (A) containing an amino group in the molecule and a silane coupling agent (B) containing a glycidyl group in the molecule are blended and reacted between the metal sheet and the upper coating film (α), the silane coupling agent (A) has a cyclic siloxane bond and a chain siloxane bond in the structure, and the presence ratio of the cyclic siloxane bond and the chain siloxane bond is 1090 to 1100 cm, which indicates a cyclic siloxane bond by FT-IR reflection method. -1 The absorbance (C1) and linear siloxane bond at 1030-1040 cm -1 and (2) an inhibitor component (Y) containing at least one metal compound (E) selected from titanium compounds and zirconium compounds, a phosphate compound (J), and a fluorine compound (F), wherein the metal compound (E) is a fluorometal complex compound (E'), the fluorine compound (F) may not be contained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4776458 [Patent Document 2] Patent No. 5336002 [Patent Document 3] Patent Publication No. 2022-85512 [Patent Document 4] Patent No. 5933324 Summary of the Invention [Problem to be solved by the invention]
[0005] The techniques disclosed in Patent Documents 1 to 3 are excellent techniques that have been put to practical use as surface-treated steel sheets that have been subjected to chromate-free surface treatment and have excellent corrosion resistance, electrical conductivity, paintability, and the like. However, due to the increasing sophistication of customer needs in recent years, there are cases where the prior art is required to be put into practical use with further improvement in adhesion to the paint applied to the surface of the surface-treated material (paint adhesion). That is, in addition to the adhesion after coating film formation that has been generally evaluated up until now, the techniques described in Patent Documents 1 to 3 are required to be further improved in adhesion so that adhesion can be ensured even under harsher conditions, such as when the surface-treated steel material with a coating film is immersed in high-temperature water. In addition, in Patent Document 4, it is necessary to include an organic resin as a film-forming component. Therefore, even if the corrosion resistance and coating adhesion are excellent, there is a problem that the electrical conductivity is poor.
[0006] Therefore, an object of the present invention is to provide a surface-treated steel material having excellent paint adhesion and electrical conductivity, based on the premise of a surface-treated steel material having a chemical conversion coating on the surface of a zinc-based plated steel material having a plating layer containing zinc or a zinc alloy on the surface of the steel material. [Means for solving the problem]
[0007] The present inventors have conducted research into improving paint adhesion, and have obtained the following findings. (a) The paint adhesion of a chemical conversion coating is affected by the amount of specific organic functional groups and water content present in the chemical conversion coating. (b) The coating adhesion is improved by maintaining a uniform distribution of organic functional groups, which leads to improved coating adhesion, and by reducing the amount of moisture remaining locally in the coating film. (c) The amount of specific organic functional groups and the amount of water present in the chemical conversion coating can be evaluated from the absorbance spectrum measured by the micro FT-IR reflectance method.
[0008] The present invention has been made in view of the above findings. [1] A surface-treated steel material according to one embodiment of the present invention comprises a steel material, a plating layer containing Zn or a Zn alloy formed on the surface of the steel material, and a chemical conversion coating formed on the surface of the plating layer, the chemical conversion coating containing an organosilicon compound having a siloxane bond, P and F, and a reflection spectrum of 2750 to 3000 cm at each measurement position when a measurement pitch of 19 μm is measured by a reflection method using a microscopic FT-IR in an area of 1.2 mm × 1.2 mm of the chemical conversion coating. -1 The area of the absorbance peak of Ac is 980-1180 cm -1 The area of the absorbance peak is Asi, 1500~1700cm -1 When the area of the absorbance peak is Ah, the standard deviation of Ac / (Ac+Asi+Ah) is 0.05 to 0.30 and the average is 0.20 to 0.70, and the standard deviation of Ah / (Ac+Asi+Ah) is 0.02 to 3.00 and the average is 0.02 to 0.30. Effect of the Invention
[0009] According to the above aspect of the present invention, it is possible to provide a surface-treated steel material having excellent paint adhesion and electrical conductivity. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic diagram showing an example of a cross section of a surface-treated steel material according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A surface-treated steel material according to one embodiment of the present invention (surface-treated steel material according to this embodiment) will be described. As shown in Fig. 1, the surface-treated steel material 1 according to this embodiment has a steel material 11, a plating layer 12 containing Zn or a Zn alloy formed on the surface of the steel material 11, and a chemical conversion coating 13 formed on the surface of the plating layer 12. In Fig. 1, the plating layer 12 and the chemical conversion coating 13 are formed only on one side of the steel material 11, but they may be formed on both sides. In addition, the surface-treated steel material 1 according to this embodiment has a chemical conversion coating 13 that contains an organosilicon compound having a siloxane bond, as well as P and F. When an area of 1.2 mm × 1.2 mm of the chemical conversion coating is measured by a micro FT-IR reflection method with a measurement pitch of 19 μm, the average particle diameter at each measurement position is 2750 to 3000 cm -1 The area of the absorbance peak of Ac is 980-1180 cm -1 The area of the absorbance peak is Asi, 1500~1700cm -1 When the area of the absorbance peak is Ah, the standard deviation of Ac / (Ac+Asi+Ah) is 0.05 to 0.30 and the average is 0.20 to 0.70, and the standard deviation of Ah / (Ac+Asi+Ah) is 0.02 to 3.00 and the average is 0.02 to 0.30.
[0012] The steel material 11, the plating layer 12, and the coating 13 will be described below.
[0013] <Steel> The surface-treated steel material 1 according to this embodiment has excellent paint adhesion due to the plating layer 12 and the chemical conversion coating 13. Therefore, the steel material 11 is not particularly limited. The steel material 11 may be determined according to the product to which it is applied and the required strength and plate thickness, and for example, a steel plate such as a hot-rolled steel plate described in JIS G 3193:2019, JIS G 3131:2018, JIS G 3113:2018, or a cold-rolled steel plate described in JIS G 3141:2021, JIS G 3135:2018, or the like may be used.
[0014] <Plating layer> The plating layer 12 is not limited in chemical composition as long as it is a plating layer containing 40 mass% or more of Zn or a Zn alloy (zinc-based plating layer). For example, plating specified in JIS G 3313:2021, JIS G 3302:2019, JIS G 3323:2019, JIS G 3317:2019, or JIS G 3321:2019 can be used.
[0015] The coating weight of the plating layer 12 is not limited, but in order to improve corrosion resistance, it is set to 10 g / m per side. 2 On the other hand, the coating weight per side is preferably 200 g / m or more. 2 If the coating weight exceeds 200g / m, the corrosion resistance will saturate and it will be economically disadvantageous. 2 It is preferable that:
[0016] The type of the plating layer is not limited, and may be, for example, a hot-dip plating layer or an electroplating layer.
[0017] <Chemical conversion coating> [Containing an organosilicon compound having a siloxane bond, P and F] The chemical conversion coating 13 of the surface-treated steel material 1 according to this embodiment is obtained by applying a treatment liquid (chemical conversion coating liquid) containing a silane coupling agent, a phosphate compound, and a fluorine compound to a zinc-based plating layer (a plating layer containing zinc or a zinc alloy) under specified conditions and drying it. Therefore, the chemical conversion coating 13 of the surface-treated steel material 1 according to this embodiment contains, as a film-forming component, a silicon compound having a siloxane bond (Si-O-Si bond: including cyclic siloxane bond and linear siloxane bond) derived from a silane coupling agent, and contains P and F as inhibitor components. It is considered that P and F exist as inhibitors in the form of a phosphate compound and a fluorine compound. When a silicon compound is the film-forming component, the average Si concentration of the chemical conversion coating is, for example, 10 mass % or more. Furthermore, the chemical conversion coating 13 may contain Zr or V derived from a Zr compound or a V compound, as necessary. The chemical conversion coating 13 provided on the surface-treated steel material 1 according to this embodiment does not substantially contain organic resin.
[0018] Whether or not a chemical conversion coating contains P and F is determined by examining the surface-treated steel with an X-ray fluorescence analyzer to confirm the presence of P and F, respectively. Other elements such as Zr and V can also be analyzed in the same way if they are present. If the detection intensity of each element is three or more times higher than when measured on plated steel without a coating, it is determined that the element is contained in the coating. Whether or not the chemical conversion coating contains an organosilicon compound having a siloxane bond can be determined by FT-IR, which will be described later.
[0019] [The standard deviation of Ac / (Ac+Asi+Ah) is 0.05-0.30, and the average value is 0.20-0.70] [The standard deviation of Ah / (Ac+Asi+Ah) is 0.02-3.00, and the average value is 0.02-0.30] The paint adhesion of a chemical conversion coating is affected by the amount of organic functional groups and water present in the chemical conversion coating. If the chemical conversion coating contains a large number of organic functional groups, adhesion to the paint film improves, while if a large amount of water remains, paint adhesion decreases. In other words, if water remains in the chemical conversion coating, when a paint film (paint) is applied and dried, air bubbles will form between the paint film and the chemical conversion coating due to the evaporation of the remaining water. In an environment where surface-treated steel material with a chemical conversion coating is immersed in high-temperature water, water molecules diffuse through the paint film and penetrate into air bubbles that have formed at the interface between the paint film and the chemical conversion coating, widening the interface between the paint film and the chemical conversion coating, which is thought to result in a decrease in paint adhesion. Therefore, in the surface-treated steel material according to this embodiment, the distribution of organic functional groups, which leads to improved paint adhesion, is maintained uniformly, and the amount of moisture remaining locally in the coating film is reduced, thereby improving paint adhesion. Specifically, assuming that the chemical conversion coating contains an organosilicon compound having a siloxane bond, and P and F, the range of 2750 to 3000 cm at each measurement point was measured using a micro FT-IR reflection method with a measurement pitch of 19 μm within an area of 1.2 mm × 1.2 mm of the chemical conversion coating. -1 The area of the absorbance peak of Ac is 980-1180 cm -1 The area of the absorbance peak is Asi, 1500~1700cm -1When the area of the absorbance peak is Ah, the standard deviation of Ac / (Ac+Asi+Ah) is 0.05 to 0.30 and the average is 0.20 to 0.70, and the standard deviation of Ah / (Ac+Asi+Ah) is 0.02 to 3.00 and the average is 0.02 to 0.30. Here, in the microscopic FT-IR measurement, -1 The absorbance peak at 980-1180 cm is due to the alkylene group. -1 The absorbance peak at 1500-1700 cm is due to the siloxane bond. -1 The absorbance peak is due to water molecules. That is, the standard deviation and average value of Ac / (Ac+Asi+Ah) and Ah / (Ac+Asi+Ah) falling within a predetermined range means that in a chemical conversion coating mainly composed of a SiOx skeleton having siloxane bonds and containing a phosphate compound and a fluorine compound as inhibitor components, the distribution of alkylene bonds relative to the SiO bonds that form the skeleton of the chemical conversion coating is uniform, and the distribution of water molecules in the chemical conversion coating is uniform. In this case, the bonding sites between the coating and the chemical conversion coating can be maintained, while the water molecules that generate bubbles between the coating and the chemical conversion coating can be reduced. If the standard deviation of Ac / (Ac+Asi+Ah) exceeds 0.30 or the average value of Ac / (Ac+Asi+Ah) is less than 0.20, there will be areas with few organic functional groups, resulting in poor paint adhesion. On the other hand, if the average value of Ac / (Ac+Asi+Ah) exceeds 0.70, the chemical conversion coating will not dry sufficiently, resulting in reduced corrosion resistance. Taking into account actual manufacturing variations, the standard deviation of Ac / (Ac+Asi+Ah) will not actually be less than 0.05. Furthermore, the standard deviation of Ah / (Ac+Asi+Ah) will not substantially be less than 0.02. On the other hand, if the standard deviation of Ah / (Ac+Asi+Ah) exceeds 3.00 or the average value of Ah / (Ac+Asi+Ah) exceeds 0.30, there will be places in the coating with a large amount of moisture, resulting in poor paint adhesion. Furthermore, if the average value of Ah / (Ac+Asi+Ah) is less than 0.02, the coating will dry out excessively, which will reduce the adhesion between the coating and the plating layer and therefore poor paint adhesion.
[0020] The average value and standard deviation of Ac / (Ac+Asi+Ah) and Ah / (Ac+Asi+Ah) are obtained by the following method. Ac, Asi, and Ah are measured by a reflection method using a micro FT-IR device equipped with a sample holder described in Japanese Patent No. 7095547. In measuring absorbance by the reflection method, a 15x Cassegrain lens for infrared spectroscopy is used to irradiate infrared light from a direction inclined at 40° from the normal direction of the surface of the chemical conversion coating, and the infrared light reflected in a direction inclined at 40° from the normal direction of the surface of the chemical conversion coating is detected. At this time, the inclination of the chemical conversion coating is adjusted using the above sample holder so that the focus of the 15x Cassegrain lens for infrared spectroscopy is not lost over the entire measurement range of 1.2 mm x 1.2 mm. Then, the 4000 to 800 cm measured at each point is -1 From the infrared absorption spectrum, the absorbance of specific peaks in the wave number ranges assigned to the alkylene group, siloxane bond, and water molecule is calculated. First, in the infrared absorption spectrum measured at each point, the alkylene group is at 2750 cm -1 and 3000cm -1 , siloxane bond is 980cm -1 and 1180cm -1 , water molecule is 1500cm -1 and 1700cm -1 The straight line connecting these points is taken as the baseline. The absorbance of the infrared absorption spectrum is then subtracted from the absorbance of the baseline, and the integrated value is taken as the absorbance in each wavenumber range. The measurement conditions for the microscopic FT-IR reflection method are as follows: Measurement surface: Chemical conversion coating surface Measurement range: 1.2mm x 1.2mm Measurement pitch: 19μm Resolution: 8cm -1 Number of times: 256 Measurement atmosphere: Air
[0021] The average value of Ac / (Ac+Asi+Ah) is obtained by taking the arithmetic mean of Ac / (Ac+Asi+Ah) calculated using Ac, Asi, and Ah at each measurement point obtained in the above measurement. In addition, the standard deviation of Ac / (Ac+Asi+Ah) can be obtained by calculating the positive square root of the variance of Ac / (Ac+Asi+Ah), which is calculated using Ac, Asi, and Ah at each measurement point obtained in the above measurement. In addition, the average value of Ah / (Ac+Asi+Ah) can be obtained by taking the arithmetic mean of Ah / (Ac+Asi+Ah) calculated using Ac, Asi, and Ah at each measurement point obtained in the above measurement. In addition, the standard deviation of Ah / (Ac+Asi+Ah) can be obtained by calculating the positive square root of the variance of Ah / (Ac+Asi+Ah) calculated using Ac, Asi, and Ah at each measurement point obtained in the above measurement.
[0022] The coating weight of the chemical conversion coating 13 is 100 to 2000 mg / m 2 It is preferable that the coating amount is 100 mg / m 2 If the amount is less than 2000 mg / m, sufficient effect may not be obtained. 2 If it exceeds this value, the coating thickness becomes too thick and there is a risk of the coating peeling off.
[0023] <Manufacturing method> Next, a preferred method for producing the surface-treated steel material according to this embodiment will be described. The surface-treated steel material according to this embodiment can obtain its effects as long as it has the above-mentioned characteristics regardless of the manufacturing method, but the manufacturing method described below is preferable because it can be manufactured stably.
[0024] That is, the surface-treated steel material according to this embodiment can be manufactured by a manufacturing method including the following steps. (I) a plating process for forming a plating layer containing Zn or a Zn alloy on a surface of a steel material such as a steel sheet; (II) a coating step of coating a steel material having a plating layer with a chemical conversion treatment solution; (III) A drying-cooling process in which the steel material to which the chemical conversion treatment solution has been applied is heated and dried, and then cooled to form a chemical conversion coating. Preferable conditions for each step will be described.
[0025] [Plating process] In the plating process, a steel material such as a steel sheet is immersed in a plating bath containing Zn or a Zn alloy (hot-dip plating) or electroplated to form a plating layer on the surface. The method and conditions for forming the plating layer are not particularly limited, and a normal method may be used so long as sufficient plating adhesion is obtained. In addition, the steel sheet to be subjected to the plating process and the manufacturing method of the steel sheet are not limited. As the steel sheet to be immersed in the plating bath, for example, a hot-rolled steel sheet described in JIS G 3193:2019 or JIS G 3113:2018 or a cold-rolled steel sheet described in JIS G 3141:2021 or JIS G 3135:2018 can be used. The composition of the plating bath may be adjusted according to the chemical composition of the plating layer to be obtained. After the steel material is removed from the plating bath, the coating weight of the plating layer can be adjusted by wiping, if necessary.
[0026] [Coating process] In the coating step, a chemical conversion treatment liquid (surface treatment metal agent) containing a silane coupling agent, a phosphoric acid compound, and a fluorine compound is coated on a steel material having a plating layer containing Zn or a Zn alloy. In the coating step, the method for coating the surface-treating metal agent is not limited, and for example, coating can be performed using a roll coater, a bar coater, a spray, or the like. However, in order to ensure uniform evaporation of the water contained in the surface treatment agent applied to the steel material and to suppress volatilization of the organic matter in the coating, the temperature of the steel material during application (the sheet temperature in the case of a steel sheet) is set to 40 to 50°C. For example, when the chemical conversion treatment liquid (metal surface treatment agent) is applied by a roll coater, the temperature of the steel material when it enters the roll coater is set to 40 to 50°C. If the temperature of the steel material during application exceeds 50°C, the organic components in the surface treatment metal agent will volatilize, resulting in a large decrease in alkylene groups and making it impossible to obtain the desired paint adhesion.If the temperature of the steel material during application is below 40°C, a lot of moisture will remain in the chemical conversion coating, making it impossible to obtain the desired paint adhesion.
[0027] The chemical conversion treatment solution contains a silane coupling agent as a film-forming component. For example, a Si compound obtained by mixing a silane coupling agent (X) containing one amino group in the molecule and a silane coupling agent (Y) containing one glycidyl group in the molecule at a solid concentration ratio (X) / (Y) of 0.5 to 1.7 may be used as the silane coupling agent.
[0028] Examples of fluorine compounds contained in the chemical conversion treatment liquid include hydrofluoric acid HF, fluoroboric acid BF4H, hydrosilicic acid H2SiF6, fluorozirconic acid H2ZrF6, and hydrofluoric titanic acid H2TiF6. The compounds may be one type or a combination of two or more types. Among these, hydrofluoric acid is more preferable. When hydrofluoric acid is used, better corrosion resistance and paintability can be obtained.
[0029] The phosphate compounds contained in the chemical conversion treatment solution remain in the chemical conversion coating as an inhibitor component, P. This inhibitor component, P, improves the corrosion resistance of the chemical conversion coating. In the present embodiment, the phosphate compound contained in the chemical conversion treatment liquid is not particularly limited, but examples thereof include phosphoric acid, ammonium phosphate, potassium phosphate, and sodium phosphate. Among these, phosphoric acid is more preferable. When phosphoric acid is used, better corrosion resistance can be obtained.
[0030] When the chemical conversion treatment liquid contains a Zr compound, examples of the compound include ammonium zirconium carbonate, hexafluorozirconic acid, and ammonium hexafluorozirconium. Furthermore, when a V compound is contained, any divalent to pentavalent vanadium compound may be used, and examples thereof include vanadium pentoxide V2O5, metavanadate HVO3, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide VO2, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(COCH3CH2COCH3)2, vanadium acetylacetonate V(COCH3CH2COCH3)3, vanadium trichloride VCl3, and phosphovanadomolybdic acid.
[0031] [Drying-cooling process] In the drying and cooling process, the steel material coated with the chemical conversion treatment solution is heated, dried, and baked. After drying, it is cooled to room temperature (e.g., 20°C). This forms a chemical conversion coating on the surface of the plating layer. When obtaining the surface-treated steel material according to this embodiment, in the drying-cooling process, the PMT (Peak Metal Temperature: maximum temperature reached by the steel material) during heating (drying) is set to 150 to 180°C, the time from application of the chemical conversion treatment solution to reaching the PMT (heating time) is set to 10 to 15 seconds, and the time (cooling time) required to cool the surface-treated steel material to room temperature (20°C) after reaching the PMT (maximum temperature reached) is set to 5 seconds or less. If the PMT is too low, the amount of moisture and organic matter remaining in the chemical conversion coating will be large, and the standard deviation of Ac / (Ac+Asi+Ah) and / or Ah / (Ac+Asi+Ah) will increase, resulting in poor paint adhesion. On the other hand, if the PMT is too high, the standard deviation of Ac / (Ac+Asi+Ah) and / or Ah / (Ac+Asi+Ah) becomes too small, resulting in poor coating adhesion. If the heating time is too short, drying will occur in some areas, increasing the standard deviation of Ac / (Ac+Asi+Ah) and / or Ah / (Ac+Asi+Ah), and thus degrading paint adhesion.If the heating time is too long, the chemical conversion coating will dry out too much, causing the standard deviation of Ac / (Ac+Asi+Ah) and / or Ah / (Ac+Asi+Ah) to become too small, and thus degrading paint adhesion. Furthermore, if the cooling time is too long, the chemical conversion coating dries out too much, and the standard deviation of Ac / (Ac+Asi+Ah) and / or Ah / (Ac+Asi+Ah) becomes too small, resulting in poor paint adhesion. There are no limitations on the cooling method as long as the cooling time falls within the specified range, but cooling can be achieved, for example, by blowing cold air at 5°C or less at a volume of 100 L / sec or more onto the surface-treated steel material. EXAMPLES
[0032] Plated steel sheets (metal sheets No. 1 to 8) having plating with the plating layer composition shown in Table 1 were prepared. The coating weight of the plating layer was 70 g / m 2 Metal plate No. 1 was produced by electroplating, and Nos. 2 to 8 by hot-dip plating. In Table 1, for example, Zn-0.2%Al indicates a composition containing 0.2 mass% Al with the balance being Zn and impurities, Zn-6.0%Al-3.0%Mg indicates a composition containing 6.0 mass% Al, 3.0 mass% Mg, with the balance being Zn and impurities, and the same applies to the others. The substrate of the plated steel sheet was a cold-rolled steel sheet satisfying JIS G 3141:2021.
[0033] For each of the plated steel sheets, except for No. 132, a silicon compound obtained by mixing 3-aminopropyltrimethoxysilane (A1) or 3-aminopropyltriethoxysilane (A2) as a silane coupling agent containing one amino group (A) and 3-glycidoxypropyltrimethoxysilane as a silane coupling agent containing one glycidyl group in the molecule (B) in a solid content mass ratio of (A) / (B) of 0.5 to 2.0 (as shown in Table 2), a phosphoric acid-derived A chemical conversion treatment liquid was applied that contained phosphoric acid blended so that the ratio (P / S) of the solid mass of P (P) to the solid mass of Si derived from Si compounds (Si) was 0.2, hydrofluoric acid blended so that the ratio (F / S) of the solid mass of F derived from hydrofluoric acid (F) to the solid mass of Si derived from Si compounds was 0.075, and vanadium oxysulfate blended so that the ratio (V) of the solid mass of V derived from vanadium oxysulfate to the solid mass of Si derived from Si compounds (V / Si) was 0.075. In addition, for No. 132, 3-aminopropyltrimethoxysilane (A1) was used as the silane coupling agent (A) containing one amino group, and 3-glycidoxypropyltrimethoxysilane was used as the silane coupling agent (B) containing one glycidyl group in the molecule in a mixing ratio (A) / (B) of 0.5 in terms of solid content mass ratio. The other components were the same as those described above. A polyurethane resin was then added to the treatment liquid and applied. The sheet temperature when the chemical conversion treatment solution was applied was as shown in Table 2.
[0034] After applying the chemical conversion treatment solution, hot air was blown onto the steel sheet through a punched metal (a steel sheet having multiple through holes) to heat the steel sheet to the dry sheet temperature (PMT) in Table 2 at an average heating rate of 8 to 43°C / sec. The heating time (the time from application to reaching the PMT) was as shown in Table 2. Thereafter, the mixture was cooled to 20°C by blowing cold air through a punched metal. As a result, surface-treated steel materials No. 101 to No. 132 were obtained. In the case of No. 132, a surface-treated steel product was obtained that had a coating (chemical conversion coating) of the same composition as No. 102, and further had a coating containing polyurethane resin in an amount 0.25 times the weight of the coating of No. 102.
[0035] [Table 1]
[0036] The obtained surface-treated steel products were examined using the method described above to determine whether the chemical conversion coating contained an organosilicon compound having a siloxane bond, P, and F. The results showed that in all cases, the chemical conversion coating contained an organosilicon compound having a siloxane bond, P, and F.
[0037] In addition, the standard deviation and average value of Ac / (Ac+Asi+Ah) and Ah / (Ac+Asi+Ah) were measured for the obtained surface-treated steel material using a micro FT-IR apparatus equipped with the sample holder described in Japanese Patent No. 7095547 in the manner described above. The results are shown in Table 3.
[0038] In addition, the coating adhesion and electrical conductivity were evaluated by the following methods. The results are shown in Table 3.
[0039] <Paint Adhesion I> A melamine alkyd-based paint was applied using a bar coater so that the film thickness after baking and drying would be 25 μm, and after baking at 120°C for 20 minutes, the board was cut into 1 mm grids and adhesion was evaluated based on the percentage of remaining pieces (number of remaining pieces / number of cut pieces: 100 pieces). <Evaluation criteria> S=100% AA=95% or more A = 90% to less than 95% B=less than 90% If it was rated S, it was determined that the paint adhesion was excellent under the above conditions.
[0040] <Paint Adhesion II> A melamine alkyd paint was applied using a bar coater so that the film thickness after baking and drying would be 25 μm, and after baking at 120°C for 20 minutes, the specimen was immersed in 98°C water for 15 minutes.The specimen was then cut into 1 mm grids and adhesion was evaluated based on the percentage of remaining pieces (number of remaining pieces / number of cut pieces: 100 pieces). <Evaluation criteria> S=100% AA=95% or more A = 90% to less than 95% B=less than 90% If the rating was A or above (A, AA, or S), it was determined that the paint adhesion was excellent under the above conditions.
[0041] <Conductivity> Using JIS C 2550-4:2011 A method, the total area of 10 contact electrodes is 1000 mm 2 The interlaminar resistance coefficient was measured under the following conditions. It was determined that A had sufficient conductivity. (Evaluation criteria for electrical conductivity) A = Interlaminar resistance coefficient of 300 Ω mm 2 less than B = Interlaminar resistance coefficient of 300 Ω mm 2 End
[0042] [Table 2]
[0043] [Table 3]
[0044] As can be seen from the results in Tables 1 to 3, in the examples of the present invention, the standard deviation and average value of Ac / (Ac+Asi+Ah) and the standard deviation and average value of Ah / (Ac+Asi+Ah) were within the range of the present invention, and not only was paint adhesion I (immediately after painting) excellent, but so was paint adhesion II (after immersion in boiling water), and the electrical conductivity was also excellent. In contrast, in the comparative examples, one or more of the standard deviation and average value of Ac / (Ac+Asi+Ah) and the standard deviation and average value of Ah / (Ac+Asi+Ah) were outside the range of the present invention, and thus the coating adhesion was inferior to Class II. Also, when the chemical conversion coating contained polyurethane, the coating adhesion was excellent, but the electrical conductivity was poor. [Explanation of symbols]
[0045] 1. Surface-treated steel 11 Steel materials 12 Plating layer 13 Chemical conversion coating
Claims
1. Steel and A plating layer containing Zn or a Zn alloy formed on a surface of the steel material; A chemical conversion coating formed on a surface of the plating layer; having the chemical conversion coating contains an organosilicon compound having a siloxane bond, P and F, When the chemical conversion coating was measured in an area of 1.2 mm × 1.2 mm using a micro FT-IR reflection method with a measurement pitch of 19 μm, the average wavelength of the reflection was 2750 to 3000 cm at each measurement position. -1 The area of the absorbance peak of Ac is 980 to 1180 cm -1 The area of the absorbance peak of Asi is 1500 to 1700 cm -1 When the area of the absorbance peak is Ah, The standard deviation of Ac / (Ac+Asi+Ah) is 0.05 to 0.30, and the average value is 0.20 to 0.70, The standard deviation of Ah / (Ac+Asi+Ah) is 0.02 to 3.00, and the average value is 0.02 to 0.
30. A surface-treated steel material characterized by:
Citation Information
Patent Citations
Controls for tankless pumps
JP1978036002A
Production of ionene polymer
JP1984033324A
Surface treatment steel material
JP2022085512A
Chromate-free surface-treated metal materials with excellent corrosion resistance, heat resistance, fingerprint resistance, conductivity, paintability, and resistance to black residue during processing.
JP4776458B2