Noncombustible wooden board and manufacturing method thereof
The noncombustible wood board, using alumina cement and metal foil with boric acid or sodium polyborate impregnation, addresses nonflammability and cost issues, ensuring high fire resistance and cost-effectiveness.
Patent Information
- Application Number
- JP2023084470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-23
AI Technical Summary
Existing wood-based building materials lack sufficient nonflammability and are costly, with flame retardants causing visual issues and adhesives like phenol and isocyanate posing fire risks, while gypsum boards are expensive and lack versatility.
A noncombustible wood board using alumina cement as adhesive, impregnated with boric acid or sodium polyborate, and laminated with metal foil to enhance nonflammability and heat resistance, reducing manufacturing costs and eliminating the need for polishing.
The board achieves high noncombustibility, heat resistance, antibacterial properties, and cost-effectiveness, passing stringent fire tests without ignition and maintaining shape integrity.
Smart Images

Figure 2024168073000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-combustible wood board which has been improved to enhance its non-combustible performance and is suitable for use in building materials and indoor furnishings such as sink units (kitchen units), and to a method for producing the same. [Background technology]
[0002] Board materials made by mixing small pieces of wood with adhesive and thermo-pressing them into a plate shape are widely used as building materials, furniture, audio equipment casings, etc. However, because these products are mainly made of wood materials, they do not exhibit sufficient flame retardancy.
[0003] In order to make such board materials non-flammable, attempts have been made to mix flame retardant chemicals into the adhesive (see, for example, Patent Document 1), but this has had problems such as the chemicals precipitating on the surface of the board, making it look unsightly. Furthermore, when phenol, isocyanate, resorcinol, or the like is used as an adhesive, it is unavoidable that these components will ignite.
[0004] By the way, as an example of a building board with good fireproofing, gypsum board or plasterboard, which is made by forming gypsum into a plate and finishing its surface with special paper, is widely available. This board is not only highly fireproof, but also has excellent heat insulation, workability, and soundproofing properties, and is considered to be relatively inexpensive and low-cost among various building boards. However, despite these advantages, gypsum board is not cheap in other industries or in the general public's opinion.
[0005] Under these circumstances, the applicants have developed a non-flammable wood board that not only has enhanced flame resistance but also exhibits scratch resistance, antibacterial properties, water resistance, stain resistance, anti-termite properties, etc., and have already filed patent applications for this product (see Patent Documents 2 and 3). Since then, the applicant has been actively engaged in research and development into improving the fire resistance of board materials as well as reducing manufacturing costs. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 3919639 [Patent Document 2] Patent Publication No. 2022-21088 [Patent Document 3] Patent application 2021-184316 Summary of the Invention [Problem to be solved by the invention]
[0007] Against this background, the present invention was made in order to further reduce costs and improve non-flammability, and the technical objective was to develop a new non-flammable wood board and a manufacturing method thereof that can ensure a certain level of non-flammability while keeping manufacturing costs down. [Means for solving the problem]
[0008] That is, the non-combustible wood board described in claim 1 is a non-combustible board formed by pressing and heating a board base material together with an adhesive to form a plate-shaped body, and the board base material does not contain a wood material. It is something that can be done, The wood material contains either boric acid or sodium polyborate. Or both are impregnated, and the adhesive is alumina cement, The plate-like body has a metal foil laminated on at least one surface. Corn calories In the certification test (Building Standards Act) (Grade: Non-flammable) using the Flame Meter III, No ignition was confirmed after 20 minutes and the total heat generated did not exceed 8MJ after 20 minutes. That It is a characteristic feature.
[0009] The method for producing a non-combustible wood board according to claim 2 is a method for producing a non-combustible board in which a board base material is filled into a formwork together with an adhesive, and then pressed and heated to form a board, the board base material containing a wood material, The adhesive is alumina cement, and the wood material is impregnated with either or both of boric acid and sodium polyborate. The board substrate is characterized in that it is pressed with a metal foil placed on at least one surface thereof and then heated. The above problems are solved by the configurations of the inventions described in each of these claims. Effect of the Invention
[0010] First, claim 1 and 2 According to the described invention, the metal foil can provide the non-combustible wood board with heat resistance and non-combustibility. In addition, the polishing process is not required, so the cost of the non-combustible wood board 1 can be reduced. Furthermore, the non-combustible wood board can be made low-cost and has high non-combustible performance even though it contains wood materials. In particular, the non-combustible wood board can be imparted with non-combustible and heat-resistant effects in addition to the adhesive effect of the alumina cement. In addition, the non-combustible wood board can be provided with the flame retardant, heat resistance, termite prevention, and decay prevention effects by the use of boric acid or sodium polyborate. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a process diagram showing a method for producing a non-combustible wood board according to the present invention. [Diagram 2] 1 is a flowchart showing a method for manufacturing a non-combustible wood board. [Diagram 3] 1 is a graph showing the results of a combustion test using a cone calorimeter on a non-combustible wood board using a wood material impregnated with boric acid. [Figure 4] 1 is a graph showing the results of a combustion test using a cone calorimeter on a non-flammable wood board using a wood material impregnated with sodium polyborate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention is intended to be practiced in the following manner, and includes various modifications within the scope of the present invention.
[0013] Hereinafter, the "non-combustible wood board and its manufacturing method" of the present invention will be specifically described based on the illustrated embodiment. The non-flammable wood board 1 of the present invention is a non-flammable board formed by pressing and heating a board base material together with an adhesive to form a plate-shaped body, the board base material containing a wood material 2, and the plate-shaped body having metal foil 15 laminated on at least one side thereof. The "board base material" refers to the main component of the board raw material 10 that provides the strength of the non-combustible wood board 1, and in this embodiment, this corresponds to the wood material 2.
[0014] The non-combustible wood board 1 of the present invention will be described in detail below. The non-combustible wood board 1 may take the form of "particle board" and "OSB" as specified in JIS5908, as well as "MDF (Medium Density Fiberboard)", "insulation board", "hardboard", and the like as specified in JIS5905.
[0015] The form of the wood material 2 is either wood chips or wood fibers depending on the form of the non-combustible wood board 1 . First, the wood chips are obtained by cutting and crushing wood material, and when applied to a non-combustible wood board 1 conforming to the "particle board" specified in JIS5908, the size is 2 to 9 mm, preferably 2 to 7 mm, and more preferably 4 to 5 mm. Similarly, the wood chips applied to non-combustible wood board 1 conforming to "OSB" specified in JIS5908 are strip-shaped chips having a thickness of 0.5 to 1.0 mm called strands. Furthermore, the dryness (moisture content) of the wood chips is 8 to 30%, preferably 8 to 20%, and more preferably 8 to 13%.
[0016] On the other hand, the wood fiber is obtained by steaming and defibrating wood material, and is applied to non-combustible wood boards 1 conforming to "Medium Density Fiberboard (MDF)", "insulation board" and "hardboard" specified in JIS5905.
[0017] The wooden material 2 may be any wood material, but it is preferable to use waste materials such as thinned wood, forest residues, factory waste materials, demolition waste materials, etc. The wooden material 2 may include not only the wood of the wooden material but also bark. As for the tree species of the wood material 2, domestically grown trees include cedar, cypress, pine (larch, spruce, and todomatsu), chinaberry, cypress, fir, zelkova, oak, birch, elm, ash, ash, walnut, horse chestnut, rowan, maple, China tree, Chinese ash, paulownia, alder, and white birch. On the other hand, foreign woods include cedar, European fir, European larch, spruce, Douglas fir, hemlock, spruce, fir, bird's eye maple, curly maple, walnut, white oak, red oak, white ash, sassafras, tulip poplar, walnut burl, madrone burl, maple burl, rose (Indian), ebony, teak, bubinga, sapele, beech, sycamore, mappa burl, ash burl, mosul bjork, elm burl, radiator pine, lauan, eucalyptus, rubber, acacia, ayous, falcata, ramin, jelutong, assamela, mahogany, and jacaranda. The wood material 2 may be made of a single tree species or may be mixed with wood materials 2 of one or more other tree species.
[0018] Next, the alumina cement 3 used as the adhesive will be explained. This is a hydraulic cement whose main components are calcium aluminate Al2O3 and CaO, and is broadly classified into construction and heat-resistant cements. The construction cement is mainly composed of CaO·Al2O3 with small amounts of 12CaO·7Al2O3 etc., while refractory cement has an increased amount of Al2O3 to increase its fire resistance.
[0019] In this embodiment, "Denka High Alumina Cement Super S90" manufactured by Denka Co., Ltd. is used as the alumina cement 3. This cement has a very high aluminum oxide (Al2O3) content of about 89%, while it is prepared with a very low calcium oxide (CaO) content of about 9%. Alumina cement 3 is available at a low price of about 350 yen / kg, and by using such alumina cement 3 as the main component of the adhesive, the manufacturing cost of the non-combustible wood board 1 can be reduced.
[0020] Furthermore, in the non-flammable wood board 1 of the present invention, the adhesives used are not urea-based adhesives (thermosetting resin-based) whose main ingredients are urea (urea) and formaldehyde, melamine resin-based adhesives (thermosetting resin-based) whose main ingredients are melamine and formaldehyde, phenolic resin-based adhesives (thermosetting resin-based) whose main ingredients are phenol and formaldehyde, CMC (carboxymethyl cellulose), resorcinol, isocyanates, etc., and therefore fire caused by these components can be avoided.
[0021] In this embodiment, the wood material 2 is impregnated with either or both of boric acid 4 and sodium polyborate 40. The boric acid 4 and sodium polyborate 40 enhance the fireproofness and fireproofness due to a synergistic effect with the fireproofness and fireproofness of the aluminum compound contained in the alumina cement 3. The mechanism by which they become fireproof and flame-retardant is known to be that an aqueous solution of boric acid or sodium polyborate penetrates the interior of wood materials 2 and bonds to the cellulose, foaming when exposed to high temperatures and blocking heat, thereby preventing combustion. In this embodiment, as an example of sodium polyborate 40, "SOUFA" manufactured by Abe Home Co., Ltd. is used.
[0022] Furthermore, in this embodiment, the board raw material 10 essentially comprises a wood material 2 and an adhesive, for example alumina cement 3, and contains either or both of boric acid 4 and sodium polyborate 40, but other components such as zinc oxide may also be added.
[0023] Furthermore, in the non-combustible wood board 1 of the present invention, a metal foil 15 is laminated on at least one surface (one surface or both surfaces), and as an example, an aluminum foil having a thickness of 40 μm is applied. The JIS standard stipulates that the thickness of aluminum foil should be between 0.2mm and 0.006mm, and the thickness of typical household aluminum foil is approximately 12μm (0.012mm). The metal foil 15 may be made of a metal other than aluminum, but it is preferable to use aluminum foil because it is lightweight, inexpensive, and readily available. [Method of manufacturing non-flammable wood board]
[0024] Next, a method for producing the non-combustible wood board 1 of the present invention will be described with reference to the process diagram shown in FIG. 1 and the flow chart shown in FIG. (1) Steaming process S1 First, the wood material 2 is impregnated with either or both of boric acid 4 and sodium polyborate 40. In this embodiment, as an example, the wood material 2 and either or both of boric acid 4 and sodium polyborate 40 are placed in a pressure cooker 100 containing water 7, and then heated at normal pressure +60 kPa (approximately 161.325 kPa) and 120°C for 18 minutes.
[0025] (2) Standing / drying process S2 Next, the pressure cooker 100 is left to cool after the heating is stopped, allowing either or both of the boric acid 4 and the sodium polyborate 40 to penetrate into the wood material 2 and become fixed in the cellulose. For example, the pressure cooker 100 is left to cool for 15 hours (preferably 24 hours or more, and more preferably 2 weeks or more). Next, although not shown in the figure, the wood material 2 is drained and then dried to obtain a treated wood material 20 impregnated with either or both of boric acid 4 and sodium polyborate 40.
[0026] (3) Raw material preparation process S3 Next, the treated wood material 20 is removed from the pressure cooker 100 and placed in a suitable container containing water 7, and alumina cement 3 is also added. These are then thoroughly mixed using a suitable mixer to prepare the board raw material 10.
[0027] (4) Board raw material injection process S4 Next, the board raw material 10 is poured into the lower mold 11, and in this example, metal foil 15 is laminated on both sides. First, metal foil 15 is placed on the bottom of lower mold 11 (board raw material injection step S41). Next, a predetermined amount of board raw material 10 is poured into lower mold 11 (board raw material pouring step S42). Next, metal foil 15 is placed on board raw material 10 in lower mold 11 (board raw material injection step S43).
[0028] (5) Pressing process S5 Next, the lower die 11 is positioned below the upper die 12, and the pressure is increased to, for example, 40 tf / m 2 The board material 10 is molded by applying a pressure of 100 MPa.
[0029] (6) Heating process S6, shaping process S7 The pressed board raw material 10 is then placed into an electric kettle 200 together with the lower mold 11, heated (for example, at 220°C for 40 minutes), and then demolded and cut to the desired dimensions to obtain the non-flammable wood board 1 of the present invention. In the case of conventional wood boards, the shaping process S7 entails polishing the front and back surfaces as appropriate, but in the case of the non-flammable wood board 1 of the present invention, smoothness is ensured at least on the surface on which the metal foil 15 is provided, making polishing unnecessary.
[0030] The non-combustible wood board 1 thus obtained has wood materials 2 firmly bonded together with the alumina cement 3 functioning as an adhesive, and further has metal foil 15 firmly integrated on one or both sides thereof. Hereinafter, examples of the non-combustible wood board 1 of the present invention will be described. EXAMPLES
[0031] [Example 1] Sample A (non-flammable wood board 1) ·Steaming process S1 (normal pressure +60kPa, 120℃, heating for 18 minutes) Wood material 2: 100g Form: wood strips Dimensions: 2~20mm Boric acid 4: 200g Water 7: 1000ml -Standing and drying process S2 (Standing: until room temperature, Drying: 24 hours or more, natural drying) ·Raw material preparation process S3 Treated wood material 20: 88g Alumina cement 3: 30g Water 7: 40g Board material 10: 158g
[0032] Using this board material 10, the following sample A was prepared, in which metal foil 15 was laminated on both sides. ·Press process S5 ·Heating process S6 Pressure: 40tf / m 2 =39240kN / m 2 ) Heating temperature: 220℃ Cooking time: 40 minutes Board material 10 Before pressing and heating 158.0g Non-flammable wood board 1 After pressing and heating 88.7g Non-flammable wood board 1 (sample A) After shaping: 71.38g
[0033] [Example 2] Sample B (non-combustible wood board 1) ·Steaming process S1 (normal pressure +60kPa, 120℃, heating for 18 minutes) Wood material 2: 150g Form: wood strips Dimensions: 2~20mm Sodium polyborate 40: 250g Water 7: 1000ml -Standing and drying process S2 (standing: 15 hours, drying: 6 hours, sun drying) ·Raw material preparation process S3 Treated wood material 20: 80g Alumina cement 3: 30g Water 7: 40g Board material 10: 150g
[0034] Using this board material 10, the following sample B was prepared, in which metal foil 15 was laminated on both sides. ·Press process S5 ·Heating process S6 Pressure: 40tf / m 2 =39240kN / m 2 ) Heating temperature: 220℃ Cooking time: 40 minutes Board material 10 Before pressing and heating 150.0g Non-flammable wood board 1 After pressing and heating 98.5g Non-flammable wood board 1 (sample B) After shaping: 80.56g
[0035] [Fire resistance test results] A fire resistance test was carried out on the two samples A and B of the non-combustible wood board 1. The results are shown below. Test subject: Sample A Test method: Certification test using a cone calorimeter III (Building Standards Act) (Grade: Non-combustible) Radiation amount: 50.0kW / m 2 (Heater temperature 753.1℃) Exhaust flow rate: 0.024m 3 / sec (exhaust temperature 17.7℃, exhaust pressure 130.628Pa) . Test results: Figure 3 shows the heat release rate vs. time curve, total heat release vs. time curve, as well as the oxygen baseline and mass vs. time curve. No ignition was observed after 20 minutes. Even after 20 minutes, the total heat output did not exceed 8 MJ. After testing, Sample A weighed 61.25 g. Furthermore, there was no change in the external shape, and no cracks, chips, warping, or the like were observed.
[0036] Test subject: Sample B Test method: Certification test using a cone calorimeter III (Building Standards Act) (Grade: Non-combustible) Radiation amount: 50.0kW / m 2 (Heater temperature 753.1℃) Exhaust flow rate: 0.024m 3 / sec (exhaust temperature 17.7℃, exhaust pressure 130.628Pa) . Test results: Figure 4 shows the heat release rate vs. time curve, total heat release vs. time curve, as well as the oxygen baseline and mass vs. time curve. No ignition was observed after 20 minutes. Even after 20 minutes, the total heat output did not exceed 8 MJ. After testing, Sample A weighed 61.25 g. Furthermore, there was no change in the external shape, and no cracks, chips, warping, or the like were observed.
[0037] The test results for samples A and B confirmed that the non-flammable wood board 1 of the present invention maintains its non-flammable performance for 20 minutes and has the non-flammable performance of non-flammable materials as stipulated in Article 108-2 of the Enforcement Order of the Building Standards Act. [Explanation of symbols]
[0038] 1. Non-flammable wood board 10 Board raw materials 11 Lower mold 12 Upper mold 15 Metal foil 2. Wood materials 20 Treated wood materials 3. Alumina cement (adhesive) 4. Boric Acid 40 Sodium Polyborate 7 water 100 Pressure Cooker 200 Electric kettle S1 Steaming process S2 Standing / drying process S3 Raw material preparation process S4 Board material injection process S41 Board raw material injection process S42 Board raw material injection process S43 Board raw material injection process S5 Press Process S6 Heating process S7 Shaping process
Claims
1. A non-combustible board formed by pressing and heating a board substrate together with an adhesive to form a plate-shaped body, The board substrate includes a wood material, The non-combustible wood board is characterized in that a metal foil is laminated on at least one surface of the plate-like body.
2. 2. The non-combustible wood board according to claim 1, wherein the adhesive is an alumina cement.
3. 3. The non-combustible wood board according to claim 1, wherein the wood material is impregnated with either or both of boric acid and sodium polyborate.
4. A method for manufacturing a non-combustible board, comprising filling a board substrate together with an adhesive into a formwork, and then pressing and heating the board into a plate shape, The board substrate includes a wood material, A method for producing a non-flammable wood board is also provided, which comprises pressing the board substrate with a metal foil on at least one surface thereof and then heating the pressed substrate.
5. 5. The method for manufacturing a non-combustible wood board according to claim 4, wherein the adhesive is an alumina cement.
6. 6. The method for producing a non-combustible wood board according to claim 4, wherein the wood material is impregnated with either or both of boric acid and sodium polyborate.
Citation Information
Patent Citations
Method of making decorative laminate covered with metal foil
JP1979088977A
Preparation of lamellar material having improved wooden surface layer
JP1989226302A
Compression molding device for timber thin piece
JP1991211007A
Composite and its manufacture
JP1991258538A
Inorganic nonflammable top board of laboratory table
JP2005053181A