Piston for internal combustion engine and method for manufacturing the same

By employing a high-strength aluminum alloy with controlled silicon, copper, and nickel content, and using laser remelting and AC/DC electrolysis, the method addresses the issue of high friction in pistons by forming a smooth anodic oxide film, reducing friction and improving lubricity and thermal efficiency.

JP2024168105APending Publication Date: 2024-12-05SUZUKI MOTOR CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023084530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional anodized films on high-strength aluminum alloys used in pistons for internal combustion engines develop surface roughness exceeding 1.0 μm due to coarse primary silicon precipitation, leading to increased friction between the skirt portion and cylinder sleeve.

Method used

A method involving the use of a high-strength aluminum alloy with specific silicon, copper, and nickel content, combined with laser remelting and rapid solidification, followed by AC/DC superposition electrolysis to form a finely dispersed silicon layer and an anodic oxide film with controlled surface roughness.

Benefits of technology

The method reduces friction and improves lubricity by forming an anodic oxide film with surface roughness Ra and Rpk of 1.0 μm or less, enhancing oil retention and reducing thermal energy loss, thereby improving piston performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168105000001_ABST
    Figure 2024168105000001_ABST
Patent Text Reader

Abstract

To provide a piston for an internal combustion engine and a method for manufacturing the same, capable of reducing friction between a skirt part and a cylinder sleeve even when a high strength material is used for a piston base material.SOLUTION: A piston material 30a is formed by using an aluminum alloy containing 5.0-20.0 mass% of Si, more than 1.3 mass% to 5.0 mass% of Cu, and more than 1.5 mass% to 3.5 mass% of Ni as a base material. Laser light 51 is irradiated onto an outer peripheral surface of a skirt part 38 of the piston material, a remelting rapid solidification part or silicon dispersion layer, on which silicon is dispersed more finely than on the base material, is formed, and an anodic oxide film is formed on the silicon dispersion layer by an AC / DC superposition electrolysis method. The laser light has a processing speed of 2,000-30,000 mm / min. Granular cells of the anodic oxide film, in the state of extending in random directions to the outer peripheral surface of the skier part and branching in the random directions, have a structure surrounding the silicon in the anodic oxide film.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piston for an internal combustion engine and a manufacturing method thereof, and more particularly to a piston for an internal combustion engine having an anodized coating on a skirt portion thereof and a manufacturing method thereof. [Background technology]

[0002] In an internal combustion engine such as an engine installed in a vehicle such as an automobile, a piston reciprocates in a cylinder bore extending along a linear longitudinal axis in a direction along the longitudinal axis. At this time, the outer periphery of the piston slides against the inner periphery of the cylinder bore. Typically, the piston includes a piston body having an outer periphery that is slidable against the inner periphery of the cylinder bore, and two skirt portions that extend from the outer periphery of the piston body to the bottom side of the cylinder bore, and further, the piston is treated to reduce the frictional resistance of the outer periphery of the piston against the inner periphery of the cylinder bore.

[0003] On the other hand, it is described that by forming an anodized coating having a surface roughness Rpk of 1.00 μm or less conforming to JIS B0671-2 on the inner surface of the top ring groove of a piston for an internal combustion engine, the airtightness with the top ring can be improved and the blow-by gas flow rate and the number of exhaust particulates can be reduced. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-204287 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in aluminum alloys with improved mechanical properties (fatigue strength, tensile strength, etc.) up to high temperatures, which are called high-strength materials and have been increasingly adopted in recent years, there are cases where they contain more additive elements such as copper (Cu) and nickel (Ni) than aluminum alloys typified by conventional JIS (Japanese Industrial Standards)-AC8A (Al-Si-Cu-Ni-Mg-based) alloys. In such high-strength materials, more granular and coarse primary crystal silicon (Si) is precipitated than in conventional materials (Si grain size is about 30 to 40 μm), and such granular Si affects the formation of an anodized film, and a film with large irregularities is likely to be formed. The present inventors have found that when such high-strength materials are used, even if the anodizing treatment described in Patent Document 1 is performed, the film will have surface roughness Ra and surface roughness Rpk exceeding 1.0 μm when the anodized film has a thickness of 10 μm.

[0006] In view of the above problems, the present invention aims to provide a piston for an internal combustion engine, which is capable of reducing friction between the skirt portion and the cylinder sleeve even when a high-strength material is used for the piston base material, and a manufacturing method thereof. [Means for solving the problem]

[0007] In order to achieve the above object, one aspect of the present invention is a method for manufacturing a piston for an internal combustion engine, the method comprising the steps of: preparing a piston material comprising a piston body having an outer periphery configured to be slidable in a longitudinal direction relative to an inner periphery of a cylinder bore; and two skirt portions facing each other in the radial direction of the piston body and extending from the outer periphery of the piston body toward a bottom of the cylinder bore, the piston body and the skirt portions being formed from an aluminum alloy containing 5.0 to 20.0 mass% Si, more than 1.3 mass% and not more than 5.0 mass% Cu, and more than 1.5 mass% and not more than 3.5 mass% Ni; irradiating an outer surface of the skirt portion of the piston material with a laser beam; and forming an anodized coating on the outer surface of the skirt portion irradiated with the laser beam by an AC / DC superimposed electrolysis method, wherein in the laser beam irradiating step, a processing speed of the laser beam is in the range of 2,000 to 30,000 mm / min.

[0008] In another aspect, the present invention provides a piston for an internal combustion engine, comprising: a piston body having an outer periphery configured to be slidable in the longitudinal direction relative to an inner periphery of a cylinder bore; and two skirt portions facing each other in the radial direction of the piston body and extending from the outer periphery of the piston body toward the bottom of the cylinder bore. The piston body and the skirt portion are made of an aluminum alloy containing 5.0 to 20.0 mass% Si, more than 1.3 mass% and not more than 5.0 mass% Cu, and more than 1.5 mass% and not more than 3.5 mass% Ni as a base material. The piston for an internal combustion engine comprises a silicon dispersion layer of an aluminum alloy composition located on the outer surface of the skirt portion, in which silicon in the aluminum alloy is dispersed more finely than in the base material, and an anodized film located on the surface of the silicon dispersion layer. The anodized film has granular cells that extend in random directions relative to the outer surface of the skirt portion, and the cells are branched in random directions to surround the silicon in the anodized film. Effect of the Invention

[0009] Thus, according to the present invention, even if the base material is an aluminum alloy containing more Cu and Ni than conventionally, a silicon dispersion layer in which silicon is dispersed more finely than in the base material is formed by irradiating the laser light, and an anodized film having a predetermined structure is formed on this silicon dispersion layer. This makes it possible to obtain an anodized film with a smooth surface, with both surface roughness Ra and surface roughness Rpk being 1.0 μm or less, thereby reducing friction between the skirt portion and the cylinder sleeve. [Brief description of the drawings]

[0010] [Figure 1] 1 is an optical microscope photograph showing an example of a metal structure when a conventional aluminum alloy is used as a base material for a piston for an internal combustion engine. [Diagram 2] 1 is an optical microscope photograph showing an example of a metal structure when an aluminum alloy (high strength material) is used as a base material for a piston for an internal combustion engine according to the present invention. [Diagram 3] 1 is a schematic view and a partially enlarged view showing one embodiment of a piston for an internal combustion engine according to the present invention; [Figure 4] FIG. 2 is a flow diagram illustrating an example of a method for manufacturing a piston for an internal combustion engine according to the present invention. [Diagram 5] FIG. 2 is a perspective view illustrating an example of a laser light irradiation step in the method for manufacturing a piston for an internal combustion engine according to the present invention. [Figure 6] FIG. 2 is a schematic diagram illustrating an example of an anodizing treatment step in the manufacturing method of a piston for an internal combustion engine according to the present invention. [Figure 7] 1 is a scanning electron microscope (SEM) image showing an anodic oxide film formed on the remelted, quenched and solidified portion of Example 1 by AC / DC superimposed electrolysis. [Figure 8] 1 is a SEM image showing an anodic oxide coating formed on an untreated area of ​​Comparative Example 1 by AC / DC superimposition electrolysis. [Figure 9] 1 is a SEM image showing an anodized coating formed by a direct current electrolysis method on the remelted, quenched and solidified portion of Comparative Example 2. [Figure 10] 1 is a SEM image showing an anodized coating formed by direct current electrolysis on an untreated portion of Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of a piston for an internal combustion engine and a manufacturing method thereof according to the present invention will be described with reference to the accompanying drawings. Note that the drawings are drawn with priority given to ease of understanding and are not drawn to scale.

[0012] The internal combustion engine piston of this embodiment is formed from an aluminum alloy (hereinafter also referred to as high-strength material) containing 5.0 to 20.0 mass% silicon (Si), more than 1.3 mass% but not more than 5.0 mass% copper (Cu), and more than 1.5 mass% but not more than 3.5 mass% nickel (Ni), and a silicon dispersion layer of an aluminum alloy composition in which Si is more finely dispersed than in the base material is formed on the base material surface of the top ring groove, and an anodized coating is further formed on the surface of this silicon dispersion layer.

[0013] In high strength materials, Si is a component that crystallizes as primary silicon or eutectic silicon and improves heat resistance and wear resistance. Si also reduces the thermal expansion coefficient. If the Si content is 5.0 mass% or more, the thermal expansion coefficient is low, and wear resistance and strength at high temperatures can be improved, and if the Si content is 20.0 mass% or less, the primary silicon becomes small, and the elongation of the alloy can be improved. The Si content is more preferably 10.0 to 13.0 mass%.

[0014] Cu is a component that improves mechanical strength and wear resistance at room temperature and high temperatures. If the Cu content exceeds 1.3 mass%, the effect of improving strength and wear resistance can be exhibited, and if it is 5.0 mass% or less, there is no significant decrease in elongation of the alloy and the specific gravity of the alloy is small. On the other hand, if it exceeds 5.0 mass%, the elongation is significantly decreased and the specific gravity of the alloy becomes large. The Cu content is more preferably 2.5 to 5.0 mass%.

[0015] Ni is a component that mainly improves strength and wear resistance in high temperature ranges and reduces the thermal expansion coefficient. If the Ni content exceeds 1.5 mass%, these effects are favorably exhibited, and if it is 3.5 mass% or less, good elongation is obtained.

[0016] In this embodiment, the aluminum alloy used for the base material may be an alloy containing at least one element selected from the group consisting of chromium (Cr), titanium (Ti), zirconium (Zr), phosphorus (P), iron (Fe), manganese (Mn) and magnesium (Mg) in addition to the above-mentioned Si, Cu, and Ni, with the balance being substantially composed of Al and unavoidable impurities. Preferably, the aluminum alloy base material contains, in addition to the above-mentioned ranges of the contents of each of Si, Cu, and Ni, 0.05 to 0.15 mass% Cr, 0.05 to 0.20 mass% Ti, 0.05 to 0.30 mass% Zr, 0.10 to 0.31 mass% Fe, 0.05 mass% or less Mn, and 0.5 to 1.1 mass% Mg, with the balance being substantially composed of Al and unavoidable impurities. Since Si, Cu, and Ni have already been described, the other components and their contents will be described.

[0017] Cr is a component that strengthens the grain boundaries between crystal grains such as intermetallic compounds, primary crystal silicon, and acicular silicon crystallized in the alloy, thereby improving strength at high temperatures. A Cr content of 0.05% by mass or more favorably strengthens the grain boundaries and improves strength at high temperatures, while a Cr content of 0.15% by mass or less provides good toughness and machinability.

[0018] Ti is a component that mainly refines crystal grains to improve heat resistance, castability, and strength, and this effect is suitably exhibited if the Ti content is in the range of 0.05 to 0.20 mass %, and the Ti content is preferably 0.05 to 0.15 wt %.

[0019] Zr is a component that mainly has the effect of refining crystal grains in the alloy and contributes to improving heat resistance, castability, and strength, and if the Zr content is in the range of 0.05 to 0.30 mass%, the effect is suitably exhibited. The Zr content is preferably 0.05 to 0.15 wt%.

[0020] Fe is a component that mainly crystallizes intermetallic compounds and improves wear resistance and strength at high temperatures. If the size of these intermetallic compounds is coarse, strength decreases. If the Fe content is in the range of 0.10 to 0.31 mass%, the size of the Fe-Mn intermetallic compounds can be reduced.

[0021] Mn is a component that mainly crystallizes intermetallic compounds and improves wear resistance and strength at high temperatures. If the size of the intermetallic compounds is coarse, the strength decreases. If the Mn content is 0.05 mass% or less, the size of the Fe-Mn intermetallic compounds can be made small. The lower limit of the Mn content may be zero or may be contained in a very small amount similar to that of an impurity, for example, 0.001 mass%.

[0022] Mg is a component that mainly improves strength and toughness. If the Mg content is 0.5% by mass or more, the effect of improving strength is exerted, and if it is 1.1% by mass or less, good toughness is obtained.

[0023] When a piston material is manufactured using such an aluminum alloy called a high-strength material as a base material, a larger amount of granular coarse primary crystal silicon is precipitated during the manufacturing process than when a piston material is manufactured using a conventional aluminum alloy. FIG. 1 is an optical microscope photograph of the metal structure of a piston base material when a conventional aluminum alloy is used, and FIG. 2 is an optical microscope photograph of the metal structure of a piston base material when a high-strength aluminum alloy used in the present invention is used. As shown in FIG. 1, a conventional aluminum alloy 10 has a large number of granular or needle-like primary crystal silicon 12 precipitated in a matrix 11, but as shown in FIG. 2, it can be seen that the granular primary crystal silicon 22 precipitated in a matrix 21 of a high-strength aluminum alloy 20 is significantly smaller than the granular primary crystal silicon 22 precipitated in a matrix 21 of the high-strength aluminum alloy 20. It has been known for some time that such granular primary crystal silicon affects the formation of an anodic oxide film, and tends to form a film with large irregularities. However, the particle size of the primary crystal silicon in high-strength materials is very large, about 30 to 40 μm, and simply using AC / DC superimposed electrolysis results in the surface roughness Ra and surface roughness Rpk of the obtained anodic oxide film both exceeding 1.0 μm, making it impossible to reduce friction between the skirt portion and the cylinder sleeve.

[0024] Here, the skirt portion on which the anodized film is formed will be described. As shown in FIG. 3, the piston 30 for an internal combustion engine according to the present invention has an outer periphery configured to be slidable in the longitudinal direction relative to the inner periphery of the cylinder bore (not shown), and three ring grooves, a top ring groove 33, a second ring groove 35, and an oil ring groove 37, are formed on the outer periphery in that order from the piston crown surface 31 side. A top ring (not shown) is fitted into the top ring groove 33, a second ring (not shown) is fitted into the second ring groove 35, and an oil ring (not shown) is fitted into the oil ring groove 37. In addition, along the outer periphery of the piston 30, the space between the piston crown surface 31 and the top ring groove 33 is called a top land 32, the space between the top ring groove 33 and the second ring groove 35 is called a second land 34, and the space between the second ring groove 35 and the oil ring groove 37 is called a third land 36. The part after the oil ring groove 37 is called a skirt portion 38, and the part up to the oil ring groove 37 is called a piston main body. The skirt portion 38 is made up of two skirt portions opposed to each other in the radial direction of the piston body.

[0025] In this embodiment, a silicon dispersion layer (not shown) made of an aluminum alloy composition in which Si is dispersed more finely than in the base material is formed on the outer peripheral surface of the skirt portion 38, and an anodized film (not shown) is further formed on the surface of this silicon dispersion layer. The anodized film has granular cells that extend in random directions relative to the surface of the skirt portion, and the cells are branched in random directions and have a structure that surrounds the silicon in the anodized film.

[0026] In this way, even when a high-strength aluminum alloy is used as the base material, a silicon dispersion layer is formed in which silicon is dispersed more finely than in the base material, and an anodized film having a predetermined structure is formed on this silicon dispersion layer, thereby making it possible to obtain an anodized film with a smooth surface, with both surface roughness Ra and surface roughness Rpk being 1.0 μm or less, thereby reducing friction between the skirt portion 38 and the cylinder sleeve (not shown).

[0027] In addition, this anodic oxide film has cavities (pores) inside the cells and gaps between the cells and silicon, and the latter gaps are more numerous and have a higher ratio of gaps than an anodic oxide film formed without a silicon dispersion layer. Therefore, the Vickers hardness of the anodic oxide film is lower than that of a film formed without a silicon dispersion layer, for example, 300 to 350 HV, which is about 100 HV smaller than that of a film formed without a silicon dispersion layer. In addition, the gaps between the cells and silicon formed on the surface of all the anodic oxide films are connected to those formed inside all the anodic oxide films. This is because the cells formed by the AC / DC superimposed electrolysis method change to granular shape around the silicon and are formed to avoid the silicon. Therefore, in this embodiment, since the silicon is finely dispersed, it is easy to form an anodic oxide film in which the gaps are connected from the surface layer to the inside of the film. The presence of more gaps on the surface of the anodized film improves oil retention, and the gaps can be filled with more lubricant, improving lubrication. Furthermore, the presence of more gaps inside the anodized film improves cooling loss by suppressing the outflow of thermal energy to the cylinder wall through the skirt, thereby reducing fuel consumption.

[0028] A method for manufacturing such an internal combustion engine piston having an anodized coating having a predetermined structure on the base material surface of the skirt portion 38 via a silicon dispersion layer will be described with reference to Figs. 4 to 6.

[0029] As shown in FIG. 4(A), the method for manufacturing a piston for an internal combustion engine according to the present embodiment includes, for example, a step S1 of casting a piston material, a step S2 of machining (including finish processing) the cast piston material, a step S3 of irradiating a skirt portion of the piston material with laser light and performing a re-melting, rapid cooling and solidification treatment, a step S4 of anodizing the re-melting, rapid cooling and solidification portion of the skirt portion of the piston material, and a step S5 of impregnating the anodized coating with a lubricant.

[0030] In the casting step S1, a piston material is cast using the high-strength aluminum alloy described above. The piston material can be cast by a general method such as gravity casting, in which molten aluminum alloy (molten metal) is poured into a mold having a cavity in the shape of the piston material.

[0031] The machining process S2 is similar to processes such as cutting used in manufacturing a typical piston for an internal combustion engine, and therefore a detailed explanation will be omitted here. However, for example, the outer diameter of the piston is roughly machined, and finishing processes such as forming streaks on the outer peripheral surface of the skirt portion are performed.

[0032] In the remelting and rapid solidification process S3, as shown in Fig. 5, a laser device 50 irradiates a laser beam 51 onto the outer peripheral surface of the skirt portion 38 of the machined piston blank 30a. The laser beam is irradiated so as to remelt the high-strength material. The remelted high-strength material is rapidly solidified. As a result, a remelting and rapid solidification portion 40 is formed on the entire outer peripheral surface of the skirt portion 38 of the piston blank 30a. In the remelting and rapid solidification portion 40, silicon is finer and more uniformly dispersed than in the high-strength material of the base material.

[0033] There are various types of lasers used in the remelting quenching solidification process S3, such as TiG laser, YAG laser, and CO2 laser, and any of these lasers can be used. Before the laser light irradiation, it is preferable to perform a degreasing process using a chemical or a cleaning process using a laser so that dirt adhering to the surface of the skirt portion 38 does not get into the remelting quenching solidification portion 40. In particular, when cleaning and remelting quenching solidification are performed using a laser, it is more preferable because the processes can be performed successively with one laser device by simply changing the output conditions.

[0034] 5, the laser device 50 is fixed, and while irradiating the laser light 51 from the laser device 50, the piston material 30a may be rotated around its axis, and the laser light 51 may be irradiated in a spiral shape onto the outer peripheral surface of the skirt portion 38 to form the remelting quenching solidification portion 40. Conversely, although not shown, the piston material may be fixed, and while irradiating the laser light from the laser device, the laser device may be rotated around the piston material, and the laser light may be irradiated in a spiral shape onto the outer peripheral surface of the skirt portion to form the remelting quenching solidification portion. In terms of the structure of the device, the mechanism for rotating the piston material is simpler, so the method shown in FIG. 5 is more preferable.

[0035] In the remelting, rapid cooling and solidification treatment step S3, the treatment speed of the laser beam is set to a range of 2,000 to 30,000 mm / min. By setting the treatment speed of the laser beam to 2,000 mm / min or more, it is possible to make the surface roughness Ra and surface roughness Rpk of the subsequently formed anodized film both 1.0 μm or less.

[0036] The surface roughness Ra represents the arithmetic mean roughness of the contour curve as specified by JIS B0601. The surface roughness Rpk is an index related to the characteristics of the average height of the protruding peaks above the core of the roughness curve, and can be used to evaluate the characteristics of a plateau-structured surface. The term "plateau structure" is defined in JIS-B0671 as a structure in which the surface is formed by plateaus (flat parts) and valleys. The surface roughness Rpk can be used to evaluate the surface irregularities of the anodized film. By setting the surface roughness Rpk of the anodized film to 1.0 μm or less, the unevenness of the skirt surface is reduced, the contact area with the cylinder sleeve is increased, and the load applied per unit area can be reduced, i.e., friction can be reduced.

[0037] On the other hand, even if the treatment speed exceeds 10,000 mm / min, the surface roughness of the obtained anodized film remains almost unchanged, and the faster the treatment speed, the greater the output required, which leads to increased equipment costs and power consumption. Therefore, the treatment speed is preferably 10,000 mm / min or less.

[0038] The output of the laser light 51 is adjusted in accordance with the processing speed so that the remelted quenched solidified portion 40 is processed to a desired depth. Therefore, although it varies depending on the processing speed, it is preferable to set the output to, for example, 1 to 15 kW.

[0039] In the process shown in Fig. 4(A), since the remelting, rapid cooling and solidification treatment step S3 is performed after the machining step S2 including the finish machining, marks on the skirt portion 38 created by the finish machining may disappear depending on the shape, but since the remelting, rapid cooling and solidification treatment needs to be performed only on the outermost surface of the skirt portion 38, the treatment can be performed with less energy. Also, in the piston manufacturing method of this embodiment, as shown in Fig. 4(B), the remelting, rapid cooling and solidification treatment step S3 can be performed after the rough machining step S2a, and further the finish machining step S2b can be performed, or as shown in Fig. 4(C), the remelting, rapid cooling and solidification treatment step S3 can be performed after the casting step S1, and then the machining step S2 including the finish machining step can be performed.

[0040] In the process shown in FIG. 4(B) and FIG. 4(C), in the remelting quenching and solidification process step S3, it is necessary to process the skirt portion 38 from the surface to a deep position, including the portion cut by the finishing process, but any surface shape such as streaks can be given to the skirt portion 38 by the subsequent finishing process. In the process shown in FIG. 4(B) and FIG. 4(C), since the remelting quenching and solidification is performed to such a deep position, if the same part of the outer peripheral surface of the skirt portion 38 is irradiated with the laser light many times, cracks are likely to occur in the remelting quenching and solidification part 40, which adversely affects the surface roughness of the anodized film formed there, and also reduces the durability of the piston itself. Therefore, in order to prevent such cracks from occurring, it is preferable to irradiate the laser light in a spiral manner on the outer peripheral surface of the skirt portion 38 so that the irradiation positions of the laser light do not overlap. On the other hand, in the process of FIG. 4(A), since the remelting, rapid cooling and solidification process step S3 is performed after the machining S2, it is sufficient to remelt, rapid cool and solidify only a few tens of μm of the surface layer of the skirt portion 38. In this case, cracks are unlikely to occur, so the irradiation positions of the laser light may overlap.

[0041] In addition, since the aluminum alloy that has been subjected to the remelting and rapid solidification process has fine silicon, its hardness is improved compared to that before the process. Therefore, the cutting tool (bite) used for machining after the remelting and rapid solidification process step S3 may be a conventionally used carbide bit, or a diamond bit or CBN (cubic boron nitride) bit that is suitable for cutting harder materials.

[0042] In the anodizing process S5, an anodized coating is formed on the remelted quenched solidified portion 40 on the outer circumferential surface of the skirt portion 38. The anodized coating is a coating formed by oxidizing the aluminum in the remelted quenched solidified portion 40, and is mainly composed of amorphous aluminum oxide (Al2O3) and has excellent abrasion resistance. As a result, the outer circumferential surface of the skirt portion 38 has a structure in which the remelted quenched solidified portion 40 (also called a silicon-dispersed layer) of an aluminum alloy composition in which silicon is finer and more uniformly distributed than in the high-strength material is formed on the high-strength material as the base material, and further the anodized coating is formed on this silicon-dispersed layer 40.

[0043] Since the anodized film is formed by oxidizing aluminum in the remelted and rapidly solidified portion 40, the surface of the anodized film after anodizing is elevated by about half the thickness of the anodized film compared to the surface of the remelted and rapidly solidified portion 40 before the treatment. In other words, the surface (interface with the anodized film) of the remelted and rapidly solidified portion (silicon-dispersed layer) 40 after anodizing is lowered by about half the thickness of the anodized film.

[0044] The state of the cells of the anodized film generally has various structures that differ depending on the electrolysis conditions, but in this embodiment, the cells are granular and branched in random directions, and have a structure that surrounds the primary crystal silicon in the film. Such a structure can be formed by AC / DC superimposition electrolysis. The remelted quenched solidification portion 40 is in a state in which silicon is finely divided and uniformly dispersed. High-strength aluminum alloys have a higher silicon content than ordinary aluminum alloys. As described above, the anodized film grows (forms a film) from the surface of the remelted quenched solidification portion 40 toward the depth, but in the commonly used DC electrolysis method, the cells grow linearly, so that the growth is easily hindered by the countless silicon present, making it difficult to form a thick film, and the anodized film has an uneven surface with large surface roughness. On the other hand, in the AC / DC superimposition electrolysis method, the cells grow in a manner that bypasses the silicon, so that a thick film thickness can be easily obtained, and an anodized film with a smooth surface with small surface roughness can be obtained. In addition, in the AC / DC superimposed electrolysis method, the coating dissolves when a negative voltage is applied, so the negative voltage is preferably, for example, 10 V or less, and it is particularly preferable to perform the electrolysis by setting the positive voltage and negative voltage to different values.

[0045] From the viewpoint of wear resistance, the thickness of the anodized film is preferably 5 μm or more, and more preferably 10 μm or more, whereas the upper limit of the thickness of the anodized film is preferably 30 μm or less, and more preferably 25 μm or less, taking into consideration productivity and processing costs.

[0046] As the processing liquid used in the anodizing treatment step S5, a wide variety of conventional electrolytic processing liquids that form an anodized film can be used. For example, acidic processing liquids such as sulfuric acid (H2SO4), oxalic acid (H2C2O4), phosphoric acid (H3PO4), chromic acid (H2CrO4), etc., and basic processing liquids such as sodium hydroxide (NaOH), sodium phosphate (Na3PO4), sodium fluoride (NaF), etc. can be used, with sulfuric acid being preferred from a practical standpoint.

[0047] A more specific method of the anodizing treatment step S5 will be described with reference to Fig. 6. As shown in Fig. 6, a rubber masking jig 60 has a cylindrical shape that encases the entire piston material 30a, and has a skirt portion opening 61 at a location corresponding to the skirt portion 38 of the piston material 30a. The masking jig 60 is attached to the piston material 30a, and the piston material 30a is immersed up to the skirt portion 38 in a treatment liquid for electrolytic treatment, whereby an anodized coating can be formed on the skirt portion 38.

[0048] When an anodized coating is also formed on the inner surface of the top ring groove 33 of the piston blank 30a and on the piston crown surface 31, a crown surface opening 62 is provided in the masking jig 60 so that the top ring groove 33 is exposed from the masking jig 60, as shown in Fig. 6. By immersing the entire piston blank 30a in the treatment liquid using such a masking jig 60, an anodized coating can be simultaneously formed on the outer peripheral surface of the skirt portion 38, the inner surface of the top ring groove 33, and the surface of the piston crown surface 31. On the other hand, when it is desired to perform anodization treatment only on the outer peripheral surface of the skirt portion 38 of the piston blank 30a, the masking jig 60 may be modified to have no crown surface opening 62 and a masking jig that covers the piston crown surface 31 and the top ring groove 33 of the piston blank 30a may be attached.

[0049] After the anodization, it is preferable to wash the piston blank 30a at least once to remove the treatment liquid adhering thereto. If the washing is insufficient, the treatment liquid may remain in the anodized film, which may affect the subsequent lubricant impregnation step S6. There are no particular limitations on the water used for washing, but water with few impurities, such as ion-exchanged water or pure water, is preferable.

[0050] In step S6 of impregnating the anodized film with a lubricant, the anodized film is porous, so that the lubricant can be impregnated. In particular, the anodized film formed on the remelted and rapidly solidified portion 40 has a higher proportion of voids than an anodized film formed without the remelted and rapidly solidified treatment, as described above, so that a larger amount of lubricant can be precipitated and impregnated into the entire anodized film.

[0051] The lubricant used may be one that is commonly used as a lubricant, such as molybdenum disulfide, Teflon (registered trademark) resin, lubricating oil, etc. As for the impregnation method, a wide variety of methods suitable for the lubricant used can be adopted. EXAMPLES

[0052] EXAMPLES Hereinafter, examples and comparative examples of the present invention will be described. Note that the present invention is not limited to the following examples and comparative examples.

[0053] [Example 1] A piston material was produced using an Al-Si-Cu-Ni aluminum alloy (hereinafter also referred to as high-strength material) having the composition shown in Table 1. Then, while rotating this piston material around its axis, a laser beam was irradiated in a spiral pattern onto the outer periphery of the skirt portion, remelting and rapidly solidifying the entire surface of the skirt portion. The rotation speed of the piston was adjusted so that the treatment speed was 1,000 to 30,000 mm / min. The laser output was adjusted in the range of 1 to 15 kW according to the treatment speed so that the high-strength material was treated to the same depth.

[0054] [Table 1]

[0055] The remelted and quenched solidified portion of the skirt was anodized to produce a piston for an internal combustion engine. The anodization was performed by forming an anodized film with a thickness of about 10 μm using a sulfuric acid treatment solution with a concentration of 200 g / L by AC / DC superimposition electrolysis (frequency 12 kHz, positive voltage 35 V, negative voltage 2 V). The surface roughness Ra and surface roughness Rpk of the anodized film were measured with a surface roughness meter in accordance with JIS B0601 and JIS B0671-2, respectively. The results are shown in Table 2. The cross section of the anodized film was also photographed with a scanning electron microscope (SEM). The SEM image is shown in FIG. 7.

[0056] [Comparative Example 1] A piston for an internal combustion engine was produced in the same manner as in Example 1, except that the remelting quenching and solidification treatment by laser light irradiation was not performed. Then, the surface roughness Ra and surface roughness Rpk of the anodized film formed on the skirt portion were measured in the same manner as in Example 1. The results are shown in Table 2. Also, the cross section of the anodized film was photographed by SEM in the same manner as in Example 1. The SEM image is shown in FIG.

[0057] [Table 2]

[0058] As shown in Comparative Example 1 in Table 2, when the piston material is a high-strength material, if anodizing is performed without remelting, quenching and solidifying by laser light irradiation, the surface roughness Ra of the resulting anodized film is 1.2 μm and the surface roughness Rpk is 1.7 μm, both of which are values ​​exceeding 1.0 μm. On the other hand, in Example 1, in which anodizing is performed after remelting, quenching and solidifying, as shown in Table 2, by increasing the processing speed of laser light irradiation, the values ​​of both the surface roughness Ra and the surface roughness Rpk of the anodized film become smaller, and when the processing speed was 2,000 mm / min or more, both the surface roughness Ra and the surface roughness Rpk were 1.0 μm or less.

[0059] Also, comparing the results in Table 2 for processing speeds of 9,000mm / min, 10,000mm / min, and 30,000mm / min, the change in surface roughness of the resulting anodized film was small, despite the large difference in processing speed. Since it is necessary to remelt and rapidly solidify the high-strength material to a specified depth by a single laser beam irradiation, the faster the processing speed, the greater the output required, which leads to increased equipment costs and power consumption. Therefore, the processing speed is preferably 10,000mm / min or less, and more preferably 9,000mm / min or less.

[0060] [Comparative Example 2] For anodizing, DC electrolysis (current density 9A / dm) was used instead of AC / DC superimposed electrolysis. 2) was performed, an internal combustion engine piston was produced in the same manner as in Example 1. Then, the cross section of the anodized coating formed on the skirt portion was photographed by SEM in the same manner as in Example 1. The SEM image is shown in FIG.

[0061] [Comparative Example 3] The remelting and rapid solidification treatment by laser irradiation was not performed, and DC electrolysis (current density 2A / dm) was used instead of AC / DC superimposed electrolysis for the anodizing treatment. 2 ) was performed, an internal combustion engine piston was produced in the same manner as in Example 1. Then, the cross section of the anodized coating formed on the skirt portion was photographed by SEM in the same manner as in Example 1. The SEM image is shown in FIG.

[0062] The cross-sectional structures of the anodized films produced in Comparative Examples 1 to 3 all show a row of hollow pillars called a cell structure, as shown in Figures 8 to 10. On the other hand, the cross-sectional structure of the anodized film of Example 1 formed after the remelting and rapid solidification treatment, as shown in Figure 7, had a complex structure with many voids P not seen in Comparative Examples 1 to 3.

[0063] The voids present in the anodized film are mainly of two types: pores derived from the cell structure and gaps that occur between the anodized film and silicon. When aluminum changes to aluminum oxide during anodizing, the volume expands, but silicon does not change, resulting in gaps between the anodized film and silicon. In Example 1, since the silicon is dispersed finely and countlessly by the remelting and rapid solidification treatment, it is expected that there will be more gaps between the anodized film and silicon than in the case where the remelting and rapid solidification treatment is not performed.

[0064] Therefore, the hardness of the anodized films produced in Example 1 and Comparative Example 1 was measured using a Vickers hardness tester. The results are shown in Table 3.

[0065] [Table 3]

[0066] As shown in Table 3, the anodized film of Example 1 had a lower hardness than that of Comparative Example 1. As described above, the anodized film of Example 1 has a microstructure different from conventional ones. Since the hardness is lower than that of the anodized film of Comparative Example 1, it is presumed that the ratio of voids in the anodized film formed after the remelting and rapid solidification treatment is higher than that of an anodized film formed without the remelting and rapid solidification treatment. Since the lubricant is filled in the voids, it is presumed that the anodized film formed after the remelting and rapid solidification treatment has a structure that can contain a larger amount of lubricant. [Explanation of symbols]

[0067] 10 Conventional aluminum alloys 11, 21 Matrix 12, 22 Primary silicon 20 High strength materials 30 Piston for internal combustion engine 31 Piston crown surface 37 Oil ring groove 38 Skirt Club 40 Remelted and rapidly solidified area (silicon dispersion layer) 50 Laser device 51 Laser light 60 Masking jig 61 Skirt opening 62 Coronal opening

Claims

1. a piston material including a piston body having an outer periphery configured to be slidable in a longitudinal direction relative to an inner periphery of a cylinder bore, and two skirt portions facing each other in a radial direction of the piston body and extending from the outer periphery of the piston body toward a bottom of the cylinder bore, the piston body and the skirt portions being formed from an aluminum alloy containing 5.0 to 20.0% by mass of Si, more than 1.3% by mass and not more than 5.0% by mass of Cu, and more than 1.5% by mass and not more than 3.5% by mass of Ni; irradiating an outer surface of the skirt portion of the piston blank with a laser beam; forming an anodic oxide film on the outer surface of the skirt portion irradiated with the laser light by AC / DC superimposition electrolysis; wherein in the step of irradiating the laser beam, a processing speed of the laser beam is in the range of 2,000 to 30,000 mm / min.

2. A piston for an internal combustion engine, comprising: a piston body having an outer periphery configured to be slidable in the longitudinal direction relative to an inner periphery of a cylinder bore; and two skirt portions facing each other in the radial direction of the piston body and extending from the outer periphery of the piston body toward a bottom of the cylinder bore, the piston body and the skirt portions being constructed using an aluminum alloy as a base material containing 5.0 to 20.0% by mass of Si, more than 1.3% by mass and not more than 5.0% by mass of Cu, and more than 1.5% by mass and not more than 3.5% by mass of Ni, a silicon-dispersed layer having an aluminum alloy composition in which silicon in the aluminum alloy is dispersed more finely than in the base material and is located on an outer surface of the skirt portion; an anodized film located on the surface of the silicon dispersion layer; wherein the anodized coating has granular cells that extend in random directions relative to the outer surface of the skirt portion, and the cells are branched in random directions and surround the silicon in the anodized coating.

3. 3. The piston for an internal combustion engine according to claim 2, wherein the anodized film has a Vickers hardness in the range of 300 to 350 HV.

Citation Information

Patent Citations

  • Piston of supercharging gasoline engine

    CN102062013A

  • Member made of al alloy and its manufacture

    JP1993017899A

  • Aluminum alloy-made piston for internal combustion engine and its manufacturing method

    JP2003013799A

  • Anodized film and anodizing method

    JP2006083467A