Polyamide resin composition and molded product therefrom

A polyamide resin composition with semi-aromatic polyamide, glass fiber, and a low-dielectric thermoplastic resin maintains mechanical and dielectric properties under moisture absorption, addressing the issue of increased dielectric constants in electronic devices.

JP2024168243AInactive Publication Date: 2024-12-05UNITIKA LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023084741
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyamide resin compositions used in electronic devices suffer from increased dielectric constants under moisture-absorbed conditions, compromising their mechanical and dielectric properties.

Method used

A polyamide resin composition comprising semi-aromatic polyamide, glass fiber with a low dielectric constant, and a thermoplastic resin with a dielectric constant of 3.0 or less, blended in specific proportions to maintain excellent mechanical and dielectric properties even under moisture absorption.

Benefits of technology

The composition achieves improved heat resistance, mechanical properties, and dielectric properties that remain stable under moisture absorption, ensuring effective performance in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168243000001
    Figure 2024168243000001
  • Figure 2024168243000002
    Figure 2024168243000002
Patent Text Reader

Abstract

To provide a polyamide resin composition that offers superior heat resistance, mechanical properties, and dielectric properties, while maintaining the superior mechanical and dielectric properties even under conditions of moisture absorption.SOLUTION: A polyamide resin composition contains (A) 100 pts.mass of a semi-aromatic polyamide with a melting point of 280-350°C, (B) 10-250 pts.mass of a glass fiber composed of glass with a relative dielectric constant of 5.5 or less, and (C) 1-45 pts.mass of a thermoplastic resin, different from (A), with a relative dielectric constant of 3.0 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide resin composition which is excellent in heat resistance, mechanical properties and dielectric properties and which can maintain the excellent mechanical properties and dielectric properties even under moisture absorption. [Background technology]

[0002] Polyamide is widely used as a molding material due to its excellent heat resistance and mechanical properties. In recent years, polyamide has been considered for use in the housings of electrical and electronic communication devices such as personal computers, tablets, and mobile phones that use megahertz and gigahertz radio waves for communication.

[0003] For example, Patent Document 1 discloses a polyamide resin composition having a low dielectric constant, which is composed of a semi-aromatic polyamide and glass fibers. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-66839 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the polyamide resin composition of Patent Document 1 has a problem in that the relative dielectric constant in a hygroscopic state in an actual usage environment becomes higher than that immediately after molding.

[0006] The present invention solves the above problems, and aims to provide a polyamide resin composition that has excellent heat resistance, mechanical properties and dielectric properties and can maintain its excellent mechanical properties and dielectric properties even under moisture absorption. [Means for solving the problem]

[0007] As a result of intensive research into solving the above problems, the inventors have found that the above problems can be solved by blending a semi-aromatic polyamide having a melting point of 280 to 350°C with a specific amount of glass fiber made of glass having a relative dielectric constant of 5.5 or less and a thermoplastic resin having a relative dielectric constant of 3.0 or less different from the semi-aromatic polyamide having a melting point of 280 to 350°C, and have arrived at the present invention.

[0008] That is, the gist of the present invention is as follows. (1) A polyamide resin composition containing 100 parts by mass of a semi-aromatic polyamide (A) having a melting point of 280 to 350°C, 10 to 250 parts by mass of glass fiber (B) made of glass with a relative dielectric constant of 5.5 or less, and 1 to 45 parts by mass of a thermoplastic resin (C) different from (A) and having a relative dielectric constant of 3.0 or less. (2) The polyamide resin composition according to (1), wherein the thermoplastic resin (C) is one or more resins selected from the group consisting of polyolefin resins, polyphenylene ether resins and fluororesins. (3) The polyamide resin composition according to (1) or (2), wherein a molded article obtained from the polyamide resin composition has a relative dielectric constant of 4.0 or less after being subjected to a moisture absorption treatment at a temperature of 70°C and a relative humidity of 62% until the molded article reaches an equilibrium state. (4) The polyamide resin composition according to (1) or (2), wherein a molded article obtained from the polyamide resin composition has a flexural modulus of 3.0 GPa or more after moisture absorption treatment at a temperature of 70°C and a relative humidity of 62% until the molded article reaches an equilibrium state. (5) A molded article obtained by molding the polyamide resin composition according to (1) or (2). Effect of the Invention

[0009] According to the present invention, it is possible to provide a polyamide resin composition which is excellent in heat resistance, mechanical properties and dielectric properties, and which can maintain the excellent mechanical properties and dielectric properties even under hygroscopic conditions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The polyamide resin composition of the present invention contains a semi-aromatic polyamide (A), glass fibers (B) and a thermoplastic resin (C).

[0011] The semi-aromatic polyamide (A) is composed of an aromatic dicarboxylic acid component and an aliphatic diamine component. The semi-aromatic polyamide (A) may contain a copolymer component, but is preferably composed of a single aromatic dicarboxylic acid component and a single aliphatic diamine component that are not copolymerized, since this improves heat resistance and reduces the relative dielectric constant.

[0012] In the present invention, examples of the aromatic dicarboxylic acid component constituting the semi-aromatic polyamide (A) include terephthalic acid, phthalic acid, isophthalic acid, and naphthalenedicarboxylic acid. Among them, terephthalic acid is preferred because it improves heat resistance.

[0013] The semi-aromatic polyamide (A) of the present invention may be copolymerized with an acid component other than the aromatic dicarboxylic acid component. Examples of the acid component other than the aromatic dicarboxylic acid component include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid, and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. The copolymerization amount of aromatic dicarboxylic acids, aliphatic dicarboxylic acids, and alicyclic dicarboxylic acids other than terephthalic acid is preferably 5 mol% or less relative to the total mole number of raw material monomers, and more preferably is not substantially contained, in order not to reduce heat resistance.

[0014] In the present invention, examples of the aliphatic diamine components constituting the semi-aromatic polyamide (A) include 1,2-ethanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 2-methyl-1,5-pentanediamine, and 2-methyl-1,8-octanediamine. The aliphatic diamine components can suppress the increase in dielectric constant due to water absorption, so it is preferable to use one aliphatic diamine with a large number of carbon atoms alone, and it is more preferable to use 1,10-decanediamine or 1,12-dodecanediamine alone.

[0015] The semi-aromatic polyamide (A) of the present invention may contain a diamine component other than the aliphatic diamine component. Examples of the diamine component other than the aliphatic diamine component include alicyclic diamines such as cyclohexanediamine, and aromatic diamines such as xylylenediamine and benzenediamine. In order not to reduce the heat resistance, the copolymerization amount of the diamine component other than the aliphatic diamine component is preferably 5 mol % or less relative to the total mole number of the raw material monomers, and more preferably is not substantially contained.

[0016] In the present invention, other copolymerization components constituting the semi-aromatic polyamide (A) than those mentioned above include lactams such as caprolactam and laurolactam, and ω-aminocarboxylic acids such as aminocaproic acid and 11-aminoundecanoic acid. In order not to reduce the heat resistance, the copolymerization amount of these is preferably 5 mol % or less based on the total mole number of the raw material monomers, and more preferably is not substantially contained.

[0017] The polyamide resin composition of the present invention may be used alone or may contain two or more semi-aromatic polyamides (A) having different constituent monomer components. However, it is preferable to use the polyamide resin composition alone, since the heat resistance is improved and the relative dielectric constant is reduced.

[0018] In the present invention, the semi-aromatic polyamide (A) preferably contains a monocarboxylic acid component as a constituent component, since this improves the flowability during melt processing and the releasability during molding. The content of the monocarboxylic acid component is preferably 0.3 to 4.0 mol %, more preferably 0.3 to 3.0 mol %, and even more preferably 0.3 to 2.5 mol %, based on the total monomer components constituting the semi-aromatic polyamide (A).

[0019] The molecular weight of the monocarboxylic acid is preferably 140 or more, more preferably 170 or more. When the molecular weight of the monocarboxylic acid is 140 or more, the semi-aromatic polyamide (A) has improved fluidity during melt processing and improved mold releasability during molding. Furthermore, the improved fluidity during melt processing makes it possible to lower the processing temperature, and thermal degradation during melt processing can be suppressed.

[0020] Examples of the monocarboxylic acid component include aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, and aromatic monocarboxylic acids, with aliphatic monocarboxylic acids being preferred since they improve the flowability during melt processing and the mold releasability during molding.

[0021] Examples of aliphatic monocarboxylic acids having a molecular weight of 140 or more include caprylic acid, nonanoic acid, decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid. Among them, stearic acid is preferred because of its high versatility. Examples of alicyclic monocarboxylic acids having a molecular weight of 140 or more include 4-ethylcyclohexanecarboxylic acid, 4-hexylcyclohexanecarboxylic acid, and 4-laurylcyclohexanecarboxylic acid. Examples of aromatic monocarboxylic acids having a molecular weight of 140 or more include 4-ethylbenzoic acid, 4-hexylbenzoic acid, 4-laurylbenzoic acid, alkylbenzoic acids, 1-naphthoic acid, 2-naphthoic acid, and derivatives thereof.

[0022] The monocarboxylic acid components may be used alone or in combination. A monocarboxylic acid having a molecular weight of 140 or more may be used in combination with a monocarboxylic acid having a molecular weight of less than 140. In the present invention, the molecular weight of the monocarboxylic acid refers to the molecular weight of the monocarboxylic acid as a raw material.

[0023] In the present invention, the semi-aromatic polyamide (A) must have a melting point of 280 to 350°C, preferably 300 to 350°C, more preferably 305 to 340°C, and even more preferably 310 to 335°C. If the melting point of the semi-aromatic polyamide (A) is less than 280°C, the resulting polyamide resin composition will have insufficient crystallinity and a high relative dielectric constant, which is not preferred. On the other hand, if the melting point of the semi-aromatic polyamide (A) exceeds 350°C, the decomposition temperature of the polyamide bond is about 350°C, and carbonization and decomposition will proceed during melt processing, which is not preferred. In the present invention, the melting point is the top of the endothermic peak when the temperature is increased at a rate of 20°C / min using a differential scanning calorimeter (DSC).

[0024] In the present invention, the relative viscosity of the semi-aromatic polyamide (A) measured in 96% sulfuric acid at 25° C. and a concentration of 1 g / dL is preferably 1.8 or more, more preferably 1.8 to 3.5, and even more preferably 2.2 to 3.1, in order to improve mechanical properties. If the semi-aromatic polyamide (A) has a relative viscosity of more than 3.5, it may become difficult to melt process it.

[0025] The method for producing the semi-aromatic polyamide (A) is not particularly limited, but a conventionally known heating polymerization method or solution polymerization method can be used. Among them, the heating polymerization method is preferably used because it is industrially advantageous. The heating polymerization method includes a method comprising a step (i) of obtaining a reaction product from an aromatic dicarboxylic acid component and an aliphatic diamine component, and a step (ii) of polymerizing the obtained reaction product.

[0026] As the step (i), for example, the aromatic dicarboxylic acid powder is heated in advance to a temperature above the melting point of the aliphatic diamine and below the melting point of the aromatic dicarboxylic acid, and the aliphatic diamine is added to the aromatic dicarboxylic acid powder at this temperature without containing substantially water so as to maintain the state of the aromatic dicarboxylic acid powder; or the suspension of the molten aliphatic diamine and the solid aromatic dicarboxylic acid is stirred and mixed to obtain a mixed liquid, and then, at a temperature below the melting point of the semi-aromatic polyamide finally produced, a reaction to produce a salt by the reaction of the aromatic dicarboxylic acid and the aliphatic diamine and a reaction to produce a low polymer by polymerization of the salt produced are carried out to obtain a mixture of the salt and the low polymer. In this case, the crushing may be carried out while the reaction is being carried out, or the crushing may be carried out after the reaction and once removed. The former is preferable for the step (i), because it is easy to control the shape of the reaction product.

[0027] As an example of step (ii), the reaction product obtained in step (i) is solid-phase polymerized at a temperature lower than the melting point of the semi-aromatic polyamide to be finally produced, and the molecular weight is increased to a predetermined molecular weight to obtain a semi-aromatic polyamide. The solid-phase polymerization is preferably carried out in an inert gas stream such as nitrogen at a polymerization temperature of 180 to 270°C and a reaction time of 0.5 to 10 hours.

[0028] The reaction apparatus for step (i) and step (ii) is not particularly limited, and any known apparatus may be used. Step (i) and step (ii) may be carried out in the same apparatus or in different apparatuses.

[0029] The heating method in the thermal polymerization method is not particularly limited, but examples thereof include a method of heating a reaction vessel with a medium such as water, steam, or thermal oil, a method of heating a reaction vessel with an electric heater, and a method of utilizing frictional heat accompanying the movement of the contents, such as heat generated by stirring. These methods may also be combined.

[0030] In the production of the semi-aromatic polyamide (A), a polymerization catalyst may be used to increase the efficiency of polymerization. Examples of the polymerization catalyst include phosphoric acid, phosphorous acid, hypophosphorous acid, and salts thereof. The amount of the polymerization catalyst added is usually preferably 2 mol % or less based on the total monomer components constituting the semi-aromatic polyamide (A).

[0031] The polyamide resin composition of the present invention must contain glass fiber (B). The relative dielectric constant of the glass fiber (B) must be 5.5 or less, and is preferably 3.7 to 5.0. When glass fiber having a relative dielectric constant exceeding 5.5 is used, the dielectric properties are not improved, which is not preferable. The lower limit is preferably as low as possible, but is essentially 3.7, which is the relative dielectric constant of the SiO2 simple substance constituting the glass.

[0032] The composition of the glass is not particularly limited, but it contains SiO2, Al2O3, B2O3, CaO, MgO, LiO2, Na2O, K2O, and TiO2, and the composition of each component is preferably 50-70% by weight of SiO2, 1-20% by weight of Al2O3, 15-30% by weight of B2O3, 0.1-5% by weight of CaO, 0.1-5% by weight of MgO, 0-1% by weight of LiO2, 0-1.5% by weight of NaO2, 0-1.5% by weight of K2O, and 0-5% by weight of TiO2. Glass with a relative dielectric constant of 5.5 or less contains more B2O3 and less CaO than the composition of E glass, which is widely used. The relative dielectric constant of glass can be determined by placing glass in a platinum crucible and melting it in an electric furnace at about 1580°C for 4 to 15 hours, pouring the molten glass onto a carbon plate and forming it into a plate shape, followed by annealing to remove distortion, and evaluating the electrostatic capacitance of the plate-shaped glass product using an LCR meter or the like.

[0033] The glass fiber (B) of the present invention is preferably treated with a surface treatment agent such as a sizing agent, since this improves the mechanical properties of the resulting molded article. The main component of the sizing agent is preferably a coupling agent or a film-forming agent.

[0034] Examples of the coupling agent include vinylsilane-based, acrylic silane-based, epoxy silane-based, amino silane-based, amino titanium-based, etc. Among them, aminosilane-based coupling agents are preferred because they have a high adhesion effect between the semi-aromatic polyamide (A) and the glass fiber and are excellent in heat resistance.

[0035] Examples of the film-forming agent include urethane-based, epoxy-based, and acrylic-based resins. Among them, urethane-based resins are preferred because they have a high adhesion effect with glass fibers and excellent heat resistance. The film-forming agent preferably contains an acid component because the hydrolysis resistance of the resin composition is improved. The acid component is preferably copolymerized with the resin that is the main component of the film-forming agent. Examples of the acid component include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and cinnamic acid, unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid, and maleic anhydride.

[0036] The fiber length of the glass fiber (B) of the present invention is not particularly limited, but is preferably 0.1 to 7 mm, and more preferably 0.5 to 6 mm. The fiber length of the glass fiber (B) of the present invention is 0.1 to 7 mm, so that the resin composition can be reinforced without adversely affecting moldability. The fiber diameter of the glass fiber (B) is not particularly limited, but is preferably 3 to 20 μm, and more preferably 5 to 14 μm. The fiber diameter of the glass fiber (B) is 3 to 20 μm, so that the resin composition can be reinforced without being broken during melt kneading. The cross-sectional shape of the glass fiber (B) may be, for example, a circle, a rectangle, an ellipse, or other irregular cross-section, and among these, a circle is preferable.

[0037] The content of the glass fiber (B) of the present invention is required to be 10 to 250 parts by mass, preferably 20 to 230 parts by mass, and more preferably 30 to 150 parts by mass, relative to 100 parts by mass of the semi-aromatic polyamide (A). If the content of the glass fiber (B) is less than 10 parts by mass, the effect of improving the mechanical properties is small, which is not preferable. On the other hand, if the content exceeds 250 parts by mass, not only is the effect of improving the mechanical properties saturated and no further improvement can be expected, but also the workability during melt kneading is reduced, making it difficult to obtain pellets of the polyamide resin composition, which is not preferable. In addition, the fluidity during melt processing is significantly impaired, so that the resin temperature increases due to shear heat, or the resin temperature must be increased to improve the fluidity, which may result in a decrease in molecular weight or a decrease in mechanical properties.

[0038] The polyamide resin composition of the present invention is required to contain a thermoplastic resin (C) different from the semi-aromatic polyamide (A) having a melting point of 280 to 350° C. The thermoplastic resin (C) is required to have a relative dielectric constant of 3.0 or less, and the lower limit of the relative dielectric constant is preferably as low as possible.

[0039] The thermoplastic resin (C) is not particularly limited as long as it has a relative dielectric constant of 3.0 or less, and examples thereof include polyolefin resins, polystyrene resins, polyphenylene ether resins, and fluororesins. Examples of polyolefin resins include (ultra-high molecular weight) polyethylene, polypropylene, (ethylene and / or propylene)·α-olefin copolymers, (ethylene and / or propylene)·(α,β-unsaturated carboxylic acid and / or unsaturated carboxylic acid ester) copolymers; olefin polymers such as ionomer polymers; elastomers such as styrene elastomers, urethane elastomers, fluorine elastomers, vinyl chloride elastomers, polyester elastomers, and polyamide elastomers; and synthetic rubbers such as thiokol rubber, polysulfide rubber, acrylic rubber, silicone rubber, polyether rubber, and epichlorohydrin rubber. Examples of fluororesins include polytetrafluoroethylene, polytetrafluoroethylene-perfluoroalkoxyethylene copolymers, and polytetrafluoroethylene-polyhexafluoropropylene copolymers. Among them, ultra-high molecular weight polyethylene olefin polymers, (ethylene and / or propylene)·α-olefin copolymers, polyphenylene ether resins, and fluororesins are preferred because of their excellent heat resistance and compatibility with semi-aromatic polyamides. As the thermoplastic resin (C), one of the above may be used alone, or two or more of them may be used in combination.

[0040] (Ethylene and / or propylene)-α-olefin copolymers are polymers obtained by copolymerizing ethylene and / or propylene with α-olefins having 3 or more carbon atoms. Examples of α-olefins having 3 or more carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-butene, 5-methyl-1-butene, 6-methyl-1-butene, 7-methyl-1-butene, 8-methyl-1-butene, 9-methyl-1-butene, 10-methyl-1-butene, 11-methyl-1-butene, 12-methyl-1-butene, 13-methyl-1-butene, 14-methyl-1-butene, 15-methyl-1-butene, 16-methyl-1-butene, 17-methyl-1-butene, 18-methyl-1-butene, 19-methyl-1-butene, 20-methyl-1-butene, 21-methyl-1-butene, 22-methyl-1-butene, 23-methyl-1-butene, 24-methyl-1-butene, 25-methyl-1-butene, 26-methyl-1-butene, 27-methyl-1-butene, 28-methyl-1-butene, 29-methyl-1-butene, 29-methyl-1-butene, 30-methyl-1-butene, 31-methyl-1-butene, 32-methyl 1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene and combinations thereof.

[0041] The polyolefin resin may be modified with a carboxylic acid and / or a derivative thereof. By modifying with the above-mentioned component, a functional group having affinity for the semi-aromatic polyamide can be introduced into the molecule. Examples of the functional group having affinity for the semi-aromatic polyamide include a carboxylic acid group, a carboxylic anhydride group, a carboxylic ester group, a carboxylic acid metal salt group, a carboxylic acid imide group, a carboxylic acid amide group, and an epoxy group.

[0042] Examples of the compound having a functional group having high affinity with the semi-aromatic polyamide include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, methyl maleic acid, methyl fumaric acid, mesaconic acid, citraconic acid, glutaconic acid, cis-4-cyclohexene-1,2-dicarboxylic acid, endo-bicyclo[2.2.1]-5-heptene-2,3-dicarboxylic acid, and metal salts of these carboxylic acids; monomethyl maleate, monomethyl itaconate, methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, hydroxyethyl acrylate, and the like. Examples of the methacrylamide include methyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, aminoethyl methacrylate, dimethyl maleate, dimethyl itaconate, maleic anhydride, itaconic anhydride, citraconic anhydride, endo-bicyclo-[2.2.1]-5-heptene-2,3-dicarboxylic anhydride, maleimide, N-ethylmaleimide, N-butylmaleimide, N-phenylmaleimide, acrylamide, methacrylamide, glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, glycidyl itaconate, and glycidyl citraconate.

[0043] The content of the thermoplastic resin (C) is required to be 1 to 45 parts by mass, and is preferably 5 to 40 parts by mass, based on 100 parts by mass of the semi-aromatic polyamide (A). If the content of the thermoplastic resin (C) is less than 5 parts by mass, the dielectric properties are not improved, which is not preferable. On the other hand, if the content exceeds 45 parts by mass, the workability during melt kneading decreases, and it becomes difficult to obtain pellets of the polyamide resin composition, which is not preferable.

[0044] The polyamide resin composition of the present invention may contain other polyamides other than the semi-aromatic polyamide (A) having a melting point of 280 to 350° C. The other polyamides other than the semi-aromatic polyamide (A) (hereinafter, may be abbreviated as "other polyamides") are not particularly limited, and examples thereof include semi-aromatic polyamides and aliphatic polyamides having a melting point of less than 280° C.

[0045] An example of a semi-aromatic polyamide having a melting point of less than 280° C. is a copolymer of terephthalic acid, isophthalic acid, and an aliphatic diamine.

[0046] Examples of aliphatic polyamides include polyamide 6, polyamide 11, polyamide 12, polyamide 46, polyamide 410, polyamide 412, polyamide 510, polyamide 512, polyamide 66, polyamide 610, polyamide 612, polyamide 1010, polyamide 1012, polyamide 6 / 66, polyamide 66 / 1010, polyamide 66 / 612, polyamide 2Me5C, polyamide 6C, polyamide 8C, polyamide 9C, polyamide 10C, and polyamide 12C. Note that C stands for 1,4-cyclohexanedicarboxylic acid, and 2Me5 stands for 2-methylpentamethylenediamine.

[0047] When the other polyamide is contained, the content is preferably 1 to 100 parts by mass, more preferably 3 to 80 parts by mass, and even more preferably 3 to 50 parts by mass, relative to 100 parts by mass of the semi-aromatic polyamide (A) having a melting point of 280 to 350°C. By containing 1 to 100 parts by mass of the other polyamide, the flowability during melt processing is improved, so that the moldability is improved and the surface appearance of the obtained molded product is also improved. Furthermore, since the melt processing temperature can be lowered due to the high flowability, the melt processing temperature can be lowered and thermal deterioration during melt processing can be suppressed. If the content is less than 1 part by mass, the above effect may not be obtained. On the other hand, if the content exceeds 100 parts by mass, the heat resistance and mechanical properties may be reduced.

[0048] The polyamide resin composition of the present invention may further contain additives such as antioxidants, light stabilizers, heat stabilizers, fillers other than glass fiber, colorants, and antistatic agents, as necessary. Examples of antioxidants include hindered phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. Examples of light stabilizers include hindered amine-based light stabilizers. Examples of heat stabilizers include copper-based heat stabilizers and polyhydric alcohol-based heat stabilizers. Examples of fillers other than glass fiber include swelling clay minerals, silica, alumina, glass beads, and graphite. Examples of colorants include pigments such as titanium oxide and carbon black, and dyes such as nigrosine. Examples of antistatic agents include alkyl sulfonates, sorbitan fatty acid esters, and polyglycerin fatty acid esters. When an antioxidant, a light stabilizer, a heat stabilizer, a colorant, or an antistatic agent is used, the content thereof is preferably 0.01 to 5.0 parts by mass, and more preferably 0.05 to 3.0 parts by mass, per 100 parts by mass of the semi-aromatic polyamide (A).

[0049] In the present invention, the method for producing the polyamide resin composition of the present invention by blending the semi-aromatic polyamide (A) having a melting point of 280 to 350°C, the glass fiber (B), the thermoplastic resin (C) having a relative dielectric constant of 3.0 or less different from (A), and additives added as necessary, etc., is not particularly limited, but the melt kneading method is preferred. Examples of the melt kneading method include a method using a batch kneader such as Brabender, a Banbury mixer, a Henschel mixer, a helical rotor, a roll, a single screw extruder, a twin screw extruder, etc. The melt kneading temperature is not particularly limited as long as the semi-aromatic polyamide (A) melts and does not decompose, but if it is too high, the semi-aromatic polyamide (A) decomposes, so it is preferably (melting point of semi-aromatic polyamide -20°C) or more and (melting point of semi-aromatic polyamide +40°C) or less.

[0050] The molten resin composition can be processed into various shapes by a method such as extruding the composition into a strand shape and shaping it into a pellet shape, hot cutting or underwater cutting into a pellet shape, extruding the composition into a sheet shape and cutting it, or extruding the composition into a block shape and pulverizing it into a powder shape.

[0051] The molded article of the present invention is obtained by molding the polyamide resin composition. Examples of the molding method include injection molding, extrusion molding, blow molding, and sintering molding, and the injection molding method is preferred because it has a large effect of improving mechanical properties and moldability.

[0052] The injection molding machine is not particularly limited, but examples thereof include a screw in-line injection molding machine and a plunger injection molding machine. The polyamide resin composition heated and melted in the cylinder of the injection molding machine is measured for each shot, injected in a molten state into a mold, cooled and solidified in a predetermined shape, and then removed from the mold as a molded body. It is more preferable that the resin temperature during injection molding is equal to or higher than (melting point of semi-aromatic polyamide - 20 ° C) and lower than (melting point of semi-aromatic polyamide + 40 ° C).

[0053] When melt processing the polyamide resin composition, it is preferable to use polyamide resin composition pellets that have been sufficiently dried. If a polyamide resin composition containing a large amount of water is used, the resin may foam in the cylinder of the injection molding machine, making it difficult to obtain an optimal molded product. The water content of the polyamide resin composition pellets used for injection molding is preferably less than 0.3 parts by mass, more preferably less than 0.1 parts by mass, based on 100 parts by mass of the polyamide resin composition.

[0054] The polyamide resin composition of the present invention can be used in a wide range of applications, such as automobile parts, electric and electronic parts, communication devices, miscellaneous goods, industrial equipment parts, civil engineering and construction products, etc. In particular, the polyamide resin composition of the present invention can be suitably used for communication devices, such as components, housings or housing parts of devices that communicate using electromagnetic waves with frequencies of 0.1 to 500 GHz.

[0055] Examples of communication devices include transceiver devices, mobile phones, tablets, laptops, navigation devices, surveillance cameras, photographic cameras, sensors, diving computers, audio units, remote controls, headphones, radios, televisions, household appliances, kitchen appliances, door or gate openers, operating devices for central vehicle locking, keyless car keys, temperature measuring or indicating devices, measuring devices, components of control devices, housings and housing parts. Examples of automotive parts, electrical and electronic parts, miscellaneous goods, industrial equipment parts, and civil engineering and construction products include electrical insulating materials for water heater motors, air conditioner motors, drive motors, etc., film capacitors, speaker diaphragms, magnetic tapes for recording, printed circuit board materials, peripheral parts for printed circuit boards, connectors, sockets, relay cases, plugs, semiconductor packages, semiconductor carrier trays, process and release films, protective films, film sensors for automobiles, insulating tapes for wire cables, insulating washers in lithium ion batteries, tubes for hot water, cooling water, and chemicals, fuel tubes for automobiles, hot water piping, chemical piping for chemical plants, etc., piping for ultrapure water and ultrahigh purity solvents, automobile piping, piping pipes for fluorocarbons and supercritical carbon dioxide refrigerants, workpiece retaining rings for polishing devices, etc. Other examples include coated molded bodies for windings for motor coils in hybrid automobiles, electric automobiles, railways, and power generation equipment, heat-resistant electric wires and cables for home appliances, wire harnesses and control wires such as flat cables used for wiring inside automobiles, and coated molded bodies for windings of signal transformers or on-board transformers for communication, transmission, high frequency, audio, measurement, etc. EXAMPLES

[0056] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0057] 1.Measurement method The physical properties of the semi-aromatic polyamide and the polyamide resin composition were measured by the following methods. (1) Melting point Using a differential scanning calorimeter DSC-7 (PerkinElmer), the temperature was raised to 360°C at a rate of 20°C / min under a nitrogen atmosphere, then held at 360°C for 5 minutes, cooled to 25°C at a rate of 20°C / min, held at 25°C for a further 5 minutes, and then heated again at a rate of 20°C / min. The top of the endothermic peak was taken as the melting point.

[0058] (2) Water absorption rate The obtained pellets of the resin composition were thoroughly dried and then molded into test pieces of 20 mm x 20 mm x 2.0 mm using an injection molding machine (J35-AD manufactured by Japan Steel Works, Ltd.) under conditions of a cylinder temperature (melting point + 15°C), a mold temperature of 140°C, and a molding cycle of 25 seconds. The test piece was subjected to moisture absorption treatment in accordance with ISO1110 at a temperature of 70°C and a relative humidity of 62% until it reached equilibrium, and the water absorption rate was calculated from the mass before and after the moisture absorption treatment using the following formula. Water absorption rate [%] = (mass after moisture absorption treatment - mass before moisture absorption) / (mass before moisture absorption treatment) x 100

[0059] (3) Flexural modulus The obtained pellets of the resin composition were thoroughly dried and then injection molded using an injection molding machine (FANUC S2000i-100B type) under conditions of a cylinder temperature (melting point + 15°C), a mold temperature of 130°C, and a molding cycle of 35 seconds to prepare dumbbell test pieces. The flexural modulus of the obtained dumbbell test piece was measured in an atmosphere of 23° C. in accordance with ISO178. In addition, after subjecting the dumbbell test pieces to the same moisture absorption treatment as described in (2), the flexural modulus was measured in an atmosphere of 23° C. in accordance with ISO 178. A flexural modulus of 3.0 MPa or more before moisture absorption treatment was considered to be acceptable.

[0060] (4) Dielectric constant The obtained pellets of the resin composition were thoroughly dried and then injection molded using an injection molding machine (FANUC S2000i-100B type) under conditions of a cylinder temperature (melting point + 15°C), a mold temperature of 130°C, and a molding cycle of 35 seconds to prepare dumbbell test pieces. The relative dielectric constant of the obtained dumbbell test piece at 1 GHz was measured using an impedance material analyzer (Agilent Technologies). In addition, after subjecting the dumbbell test pieces to the same moisture absorption treatment as described in (2), the relative dielectric constant at 1 GHz was measured using an impedance material analyzer (Agilent Technologies). A dielectric constant of 4.0 or less before moisture absorption treatment was considered acceptable.

[0061] The raw materials used in the examples and comparative examples are shown below. (1) Polyamide Semi-aromatic polyamide (A-1) 4.81 kg of powdered terephthalic acid (TPA) as a dicarboxylic acid component, 0.15 kg of stearic acid (STA) as a monocarboxylic acid component, and 9.3 g of sodium hypophosphite monohydrate as a polymerization catalyst were placed in a ribbon blender-type reactor, and heated to 170°C while stirring at a rotation speed of 30 rpm under nitrogen sealing. Then, while maintaining the temperature at 170°C and the rotation speed at 30 rpm, 5.04 kg of 1,10-decanediamine (DDA) heated to 100°C as a diamine component was continuously added (continuous liquid injection method) using a liquid injection device over 2.5 hours to obtain a reaction product. The molar ratio of the raw material monomers was TPA:DDA:STA = 49.3:49.8:0.9 (the equivalent ratio of the functional groups of the raw material monomers was TPA:DDA:STA = 49.5:50.0:0.5). The resulting reaction product was then polymerized in the same reactor at 250°C for 8 hours at 30 rpm under a nitrogen stream to produce a semi-aromatic polyamide powder. Thereafter, the obtained powder of semi-aromatic polyamide was formed into a strand shape using a twin-screw kneader, the strand was passed through a water tank to cool and solidify, and the strand was cut with a pelletizer to obtain pellets of semi-aromatic polyamide (A-1).

[0062] Semi-aromatic polyamides (A-2) to (A-5) Except for changing the resin composition as shown in Table 1, semi-aromatic polyamide pellets were obtained in the same manner as for the semi-aromatic polyamide (A-1).

[0063] Table 1 shows the resin compositions and characteristic values ​​of the semi-aromatic polyamides (A-1) to (A-5).

[0064] [Table 1]

[0065] Aliphatic polyamide (A-6): Polyamide 6 (Unitika, A1030SR), melting point 220℃

[0066] (2) Glass fiber B-1: Glass fiber made of low dielectric glass (CN 3J-256 manufactured by Nitto Boseki Co., Ltd.) B-2: Glass fiber made of E glass (Nitto Boseki CSX 3J-451)

[0067] (3) Resins other than polyamides with a relative dielectric constant of 3.0 or less C-1: Maleic anhydride modified ethylene-1-butene copolymer (Tafmer MH7510, manufactured by Mitsui Chemicals) C-2: Polyphenylene ether resin (Global Polyacetal Corporation, Iupiace PX100F) C-3: Acid-modified ultra-high molecular weight polyethylene (Mitsui Chemicals, LUBMER LY1040) C-4: Polytetrafluoroethylene (Daikin Industries, Ltd. Lubron L-5)

[0068] Example 1 After mixing 100 parts by mass of semi-aromatic polyamide (A-1) and 1 part by mass of (C-1), the mixture was weighed using a loss-in-weight type continuous quantitative feeder CE-W-1 type (manufactured by Kubota Corporation), and fed to the main feed port of a synchronous twin-screw extruder TEM26SS type (manufactured by Toshiba Machine Co., Ltd.) with a screw diameter of 26 mm and L / D of 50, and melt-kneaded. During the process, 10 parts by mass of glass fiber (B-1) were fed from a side feeder, and further kneaded. After being taken out of the die in the form of a strand, it was passed through a water tank to be cooled and solidified, and cut with a pelletizer to obtain polyamide resin composition pellets. The barrel temperature setting of the extruder was (melting point of semi-aromatic polyamide + 5°C) to (melting point of semi-aromatic polyamide + 15°C), the screw rotation speed was 250 rpm, and the discharge rate was 25 kg / h.

[0069] Examples 2 to 18, Comparative Examples 1 to 3, 6, and 7 Resin composition pellets were obtained in the same manner as in Example 1, except that the components of the resin composition were changed as shown in Table 2.

[0070] Comparative Example 4 Except for changing the composition of the resin composition as shown in Table 2, the same operation as in Example 1 was carried out to obtain resin composition pellets. However, since the content of thermoplastic resin (C) was high, melt kneading was not possible.

[0071] Comparative Example 5 An attempt was made to obtain resin composition pellets by the same procedure as in Example 1, except that the composition of the resin composition was changed as shown in Table 2. However, because the glass fiber content was high, melt kneading was not possible.

[0072] The obtained resin composition pellets were used to carry out various evaluation tests, the results of which are shown in Table 2.

[0073] [Table 2]

[0074] Since the polyamide resin compositions of Examples 1 to 18 satisfied the requirements of the present invention, the flexural modulus and relative dielectric constant of the molded articles obtained therefrom were 3.0 GPa or more and 4.0 or less, respectively, and the rate of change of each before and after the moisture absorption treatment maintained the value before the moisture absorption treatment.

[0075] The polyamide resin compositions of Comparative Examples 1 and 3 did not contain glass fibers, and therefore the flexural modulus of the molded articles obtained therefrom was low. The polyamide resin composition of Comparative Example 2 did not contain the thermoplastic resin (C), and therefore the rate of change in flexural modulus of the molded article obtained therefrom was large. The polyamide resin composition of Comparative Example 6 used E glass, and therefore the molded article obtained therefrom had a high relative dielectric constant of more than 4.0. The polyamide resin composition of Comparative Example 7, which used an aliphatic polyamide, had a high water absorption rate, and the molded article obtained therefrom had a large rate of change in flexural modulus and a large rate of change in relative dielectric constant.

Claims

1. The polyamide resin composition contains 100 parts by mass of a semi-aromatic polyamide (A) having a melting point of 280 to 350°C, 10 to 250 parts by mass of a glass fiber (B) made of glass and having a relative dielectric constant of 5.5 or less, and 1 to 45 parts by mass of a thermoplastic resin (C) different from (A) and having a relative dielectric constant of 3.0 or less.

2. 2. The polyamide resin composition according to claim 1, wherein the thermoplastic resin (C) is at least one resin selected from the group consisting of polyolefin resins, polyphenylene ether resins and fluororesins.

3. 3. The polyamide resin composition according to claim 1, wherein a molded article obtained from the polyamide resin composition has a relative dielectric constant of 4.0 or less after being subjected to a moisture absorption treatment at a temperature of 70°C and a relative humidity of 62% until it reaches an equilibrium state.

4. 3. The polyamide resin composition according to claim 1 or 2, wherein a molded article obtained from the polyamide resin composition has a flexural modulus of 3.0 GPa or more after moisture absorption treatment at a temperature of 70°C and a relative humidity of 62% until the molded article reaches an equilibrium state.

5. A molded article obtained by molding the polyamide resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polyamide resin composition, and molded article molded from the same

    JP2022066839A