Metal plate and method for forming metal plate
The metal plate and forming method address the challenge of integrating press lines and laser decoration by using thermal expansion and contraction to adjust curvature, ensuring sharp character lines and cost-effective design continuity.
Patent Information
- Application Number
- JP2023084869
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-23
AI Technical Summary
Existing methods face difficulties in achieving continuity in shape between press lines and laser decoration on metal panels due to differences in the radius of curvature, making it challenging to form sharp character lines.
A metal plate and forming method that includes a bent part with a melting portion and a gradually changing width, allowing for thermal expansion and contraction to adjust the radius of curvature through laser irradiation, connecting press lines and laser decoration naturally.
Enables seamless integration of press lines and laser decoration by adjusting the radius of curvature, resulting in sharper character lines and reduced stress differences, thereby enhancing design continuity and reducing production costs.
Smart Images

Figure 2024168312000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal sheet and a method for forming a metal sheet. [Background technology]
[0002] The following Patent Document 1 discloses a technique for processing a vehicle panel member made of metal. In this prior art, the rear side of the panel member is irradiated with laser light and heated. This causes the panel member to thermally expand and contract, causing deformation of the panel member, and allows geometric patterns, lines, etc. to be processed on the design surface side of the panel member (so-called laser decoration), making it possible to apply a desired design to the panel member. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-072343 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the above-mentioned prior art, when additional laser decoration is performed on a panel member on which press lines have been formed by press processing, the radius of curvature caused by the press lines and the radius of curvature caused by the laser decoration differ, making it difficult to maintain continuity in shape between the press lines and the laser decoration.
[0005] In consideration of the above facts, the present invention aims to obtain a metal plate and a metal plate molding method that can provide continuity in shape between press lines pre-formed on a plate-shaped body and laser decoration. [Means for solving the problem]
[0006] The metal plate described in claim 1 comprises a plate-shaped main body, a bent portion bent in the thickness direction of the main body, and, on the back side of the bent portion opposite the design surface of the main body, a molten portion formed by melting the surface, and a gradual change portion formed by gradually changing the molten width of the molten portion.
[0007] The metal plate according to claim 1 comprises a main body, a bent portion, a molten portion, and a gradually changing portion. In the plate-shaped main body, the bent portion is bent in the plate thickness direction. In the bent portion, a molten portion is provided on the back side of the main body, and the molten portion is formed by melting the front surface. For example, when a metal plate is heated, thermal expansion and thermal contraction occur in the heated portion. For this reason, by heating the bent portion, it is possible to make the radius of curvature of the bent portion smaller than that of an unheated portion, and the ridge line (so-called character line) of the bent portion can be made sharper on the design surface side of the main body.
[0008] That is, for example, in press processing, it is difficult to reduce the radius of curvature of the bent part (to form a sharp character line) due to phenomena such as springback after press forming and line misalignment during press forming, but by heating the bent part formed by press processing through laser irradiation processing, it is possible to form a sharp character line on the design surface of the metal plate.
[0009] Here, in the present invention, a gradually changing portion is provided in the molten portion formed on the back side of the bent portion. In the gradually changing portion, the molten width of the molten portion formed by melting the surface on the back side of the bent portion gradually changes. For example, if the molten width is wide, the radius of curvature is large, and if the molten width is narrow, the radius of curvature is small. Therefore, in the present invention, it is possible to gradually change the radius of curvature of the bent portion by gradually changing the molten width.
[0010] Therefore, in the present invention, even if a bent portion (press line) is formed in advance on a metal plate by press processing, it is possible to naturally connect these shapes between the bent portion or other parts and the bent portion (press line + laser decoration) by laser processing.
[0011] The metal plate according to claim 2 is the metal plate according to claim 1, wherein the radius of curvature of the cross section cut along the plate thickness direction at the bent portion in the area where the fusion width is narrow is smaller than that in the area where the fusion width is wide.
[0012] In the metal plate described in claim 2, the radius of curvature of the bent portion is smaller in the area where the fusion width is narrower than in the area where the fusion width is wide, so that the character line of the bent portion is sharper on the design surface side.
[0013] The metal plate forming method according to claim 3 is the metal plate forming method according to claim 1 or claim 2, and further comprises a press forming process in which the metal plate is pressed in the thickness direction to form a predetermined shape, and a laser irradiation process in which a laser is irradiated from the back side opposite the design surface of the metal plate to the bent portion pressed by the press forming process, wherein the laser irradiation process includes a gradual change process in which a melt width of a melted portion formed by melting the surface on the back side of the metal plate is gradually changed.
[0014] The metal plate forming method according to claim 3 includes a press forming step and a laser irradiation step. In the press forming step, the metal plate is pressed in the thickness direction to form a predetermined shape. In the laser irradiation step, a laser is irradiated to the bent portion pressed in the press forming step from the back side opposite to the design surface of the metal plate.
[0015] In this way, by irradiating the bent portion of the metal plate with a laser, the surface on the back side of the metal plate is melted to form a molten portion. This causes thermal expansion and contraction in the metal plate, making it possible to make the radius of curvature at the bent portion smaller than when the laser is not irradiated, and making it possible to make the character line sharper on the design surface side of the bent portion.
[0016] Here, in the present invention, the laser irradiation process includes a gradual change process, in which the melt width formed by melting the surface gradually changes on the back side of the metal plate. This makes it possible to gradually change the curvature radius of the bent portion. Therefore, in the present invention, even if a bent portion is formed in advance on the metal plate, it is possible to naturally connect these shapes between the bent portion or other portions and the gradually changing portion.
[0017] The metal sheet shaping method according to a fourth aspect of the present invention is the metal sheet shaping method according to the third aspect, wherein in the gradual changing step, at least one of a laser focused diameter and a laser output is gradually changed.
[0018] In the metal sheet shaping method according to claim 4, in the gradual changing step, at least one of the laser focus diameter and the laser output is gradually changed, thereby making it possible to gradually change the molten width of the molten portion.
[0019] For example, in the case of a laser focusing diameter, the melt width of the melted portion is narrower and the radius of curvature of the bent portion is smaller when the laser focusing diameter is smaller than when the laser focusing diameter is larger. In addition, in the case of a laser output, the melt width of the melted portion is narrower and the radius of curvature of the bent portion is smaller when the laser output is higher than when the laser output is low. On the other hand, by lowering the laser output, it is possible to suppress the sudden heat input caused by the laser irradiation, and it is possible to reduce the stress difference generated between the part where heat is input and the other parts. Effect of the Invention
[0020] As described above, according to the metal plate and the metal plate forming method of the present invention, it is possible to provide continuity in shape between the press lines pre-formed on the plate-shaped main body and the laser decoration. [Brief description of the drawings]
[0021] [Figure 1] 1 is a front view showing a side member outer as a metal plate for explaining processing conditions in a metal plate forming method according to an embodiment of the present invention. FIG. [Diagram 2] 1 is a front view showing a side member outer as a metal plate processed by the metal plate forming method according to the present embodiment. FIG. [Diagram 3] In the metal plate according to this embodiment, the left figure is a schematic perspective view showing the state after press working, and the right figure is a schematic perspective view showing the state after press working and laser irradiation processing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Next, each embodiment of the present invention will be described with reference to the drawings. Note that the arrows FR and UP shown in each drawing indicate the forward direction (the direction in which the vehicle travels) and the upward direction of the vehicle (vehicle body), respectively. In addition, when the directions of front-rear, left-right, and up-down are simply used for the description, they indicate front-rear in the front-rear direction of the vehicle, left-right in the left-right direction of the vehicle (vehicle width direction), and up-down in the up-down direction of the vehicle, unless otherwise specified.
[0023] (Metal plate configuration) 1 shows a front view of a side member outer (metal plate) 10 as an outer panel constituting an outer side portion of a vehicle to which a metal plate according to the present embodiment is applied. The side member outer 10 is made of a metal plate made of, for example, a steel plate, an aluminum alloy, or the like.
[0024] Generally, the side member outer 10 is bent in the thickness direction of the side member outer 10 by press processing, and a bent portion (so-called press line) 12 is formed on the design surface 10A. In this manner, by forming the bent portion 12 (see FIG. 3) in the side member outer 10, it is possible to improve the tensile rigidity and design of the side member outer 10.
[0025] On the other hand, in terms of the design of the side member outer 10, it is required to have a sharp ridge line as a character line, but in the bent portion 12 formed by press processing, due to phenomena such as springback after press forming, the radius of curvature (hereinafter referred to as "R") of the side member outer 10 (of the cross section cut along the plate thickness direction) becomes large, making it difficult to obtain a sharp ridge line.
[0026] Therefore, in this embodiment, as shown in the left diagram of Figure 3, in the side member outer 10, at the bent portion 12 formed by the press molding process, laser light is irradiated to the bent portion 12 from the back surface 10B (opposite side to the design surface 10A) of the side member outer 10 by a laser irradiation process.
[0027] In this laser irradiation process, the side member outer 10 thermally expands and contracts due to the laser irradiation, so that it is possible to form the R of the side member outer 10 small, as shown in the right diagram of Fig. 3. In addition, a convex portion 13 formed smaller than the R of the bent portion 12 is formed on the design surface 10A side of the side member outer 10.
[0028] Furthermore, when a laser is applied to the back surface 10B of the side member outer 10 at the bent portion 12 formed by pressing the side member outer 10, the surface of the back surface 10B of the side member outer 10 is melted by heating with the laser light (melted portion 14). In this embodiment, when the width (melted width W) of the melted portion 14 is large, the R of the convex portion 13 of the side member outer 10 is formed large, and when the melted width W is small, the R of the convex portion 13 of the side member outer 10 is formed small.
[0029] In this case, in the laser irradiation, by changing conditions such as the focal diameter of the laser light (laser focal diameter), the output of the laser light (laser output), the scanning speed of the laser light (laser speed), and the number of scanning passes of the laser light (number of passes) in the laser device 21 (see Figure 1), it is possible to gradually change the melt width W at the bent portion 12 of the side member outer 10 and gradually change the size of R at the convex portion 13 (so-called gradual change portion 24; see Figure 2).
[0030] For example, in the case of the laser beam diameter, to reduce the R of the convex portion 13, the laser beam diameter is reduced. Also, in the case of the laser output, to reduce the R of the convex portion 13, the laser output is increased. In the case of the laser speed, to reduce the R of the convex portion 13, the laser speed is decreased. And in the case of the number of passes, to reduce the R of the convex portion 13, the number of passes is increased. By changing at least one of these conditions, it becomes possible to change the size of the R formed on the Siemens outer 10.
[0031] (Laser irradiation process) Hereinafter, the laser irradiation process will be briefly described as an example.
[0032] As shown in FIG. 1, in addition to press working, laser irradiation processing is performed on the roof side rail portion 20 provided above the openings 16 and 18 formed side by side in the vehicle front-rear direction of the Siemens outer 10. Note that the cross-section of the roof side rail portion 20 is shown linearly above the Siemens outer 10, and the laser irradiation process in the roof side rail portion 20 will be described separately for the first to fifth processes. The numbers of each process are respectively attached to the laser device 21.
[0033] In the first step of the laser irradiation process, laser irradiation by the laser device 21 is started (point A), and in the fifth step, laser irradiation by the laser device 21 ends (point E).
[0034] First, at point A, laser irradiation is started with the laser output of the laser device 21 being W1 and the laser beam diameter being D1. Also, at point B, the laser output of the laser device 21 is W2 (>W1) and the laser beam diameter is D2 (=D1). At point C, the laser output of the laser device 21 is W3 (=W2) and the laser beam diameter is D3 (<D2). Next, at point D, the laser output of the laser device 21 is W4 (<W3) and the laser beam diameter is D4 (=D3). At point E, the laser output of the laser device 21 is W5 (<W4) and the laser beam diameter is D5 (=D4), and the laser irradiation ends.
[0035] Generally, in a metal plate, when rapid heat input occurs, a stress difference is generated between the site where the rapid heat input occurs and other sites. Therefore, in the first step, at point A where the laser irradiation by the laser device 21 starts, the laser output W1 of the laser device 21 is set lower than the laser output W2 at point B (W1 < W2).
[0036] At point A, the laser output of the laser device 21 is W1 and the laser beam diameter is D1, and at point B, the laser output of the laser device 21 is W2 (>W1) and the laser beam diameter is D2 (=D1). Therefore, in the first step, the laser output of the laser device 21 is gradually increased from W1 to W2 until reaching point B from point A (so-called gradual change process). Note that due to this gradual change process, a gradually changing portion 24 (see FIG. 2) where the melting width W (see FIG. 3) gradually changes is formed in the melted portion 14 of the bent portion 12 shown in FIG. 3.
[0037] Next, at point C, the laser output of the laser device 21 is W3 (=W2) and the laser beam diameter is D3 (<D2). Therefore, in the second step, the laser beam diameter of the laser device 21 is gradually decreased from D2 to D3 until reaching point C from point B (so-called gradual change process). Note that due to this gradual change process, a gradually changing portion 26 (see FIG. 2) where the melting width W (see FIG. 3) gradually changes is formed.
[0038] On the other hand, at point D, the laser output of the laser device 21 is W4 (<W3) and the laser beam diameter is D4 (=D3), but in the third step, the laser output and the laser beam diameter of the laser device 21 are substantially constant until reaching point D from point C. That is, in the fourth step, the laser output of the laser device 21 is decreased from W3 to W4.
[0039] Also, at point E, the laser output of the laser device 21 is W5 (<W4), and the laser beam diameter is D5 (=D4). That is, in the fifth step, the laser output of the laser device 21 is decreased from W4 to W5, and the laser irradiation ends. The heating temperature by the laser device 21 increases with the passage of time from the start of laser irradiation. Therefore, at point E, the laser output W5 (<W4) of the laser device 21 is set to be even lower than the laser output W4 at point D.
[0040] As described above, in the present embodiment, in the laser irradiation process, at least one of the laser beam diameter and the laser output of the laser device 21 is gradually changed (slowly changed). In this way, by changing the conditions of laser irradiation, in the present embodiment, the melting width W (see FIG. 3) gradually changes, and it becomes possible to gradually change the R of the bent portion 12 (see FIG. 3).
[0041] (Function and effect of the metal plate) Next, the function and effect of the cement outer 10 to which the metal plate according to the present embodiment is applied will be described.
[0042] As shown in FIG. 2, in the roof side rail portion 20 of the cement outer 10, the character line 22 is formed so as to gradually become darker as it goes toward the front side of the vehicle. That is, in the present embodiment, in the roof side rail portion 20, the size of R gradually becomes smaller as it goes toward the front side of the vehicle.
[0043] In addition, in FIG. 2, the darkness (darkness of the ridge line) of the character line 22 is expressed by the lengths of the solid line and the broken line. As the character line 22 becomes darker, the length of the broken line gradually becomes longer, and the darkest state is the solid line. The cross-sectional shape of the character line 22 is shown above the character line 22 so as to be contrasted with the darkness of the character line 22.
[0044] As shown in Fig. 2, in the bent portion 12 of the side member outer 10, a molten portion 14 formed by melting the surface is provided on the back surface 10B side of the side member outer 10. When the side member outer 10 is heated, thermal expansion and thermal contraction occur in the heated portion. Therefore, as shown in Fig. 3, by heating the bent portion 12, it is possible to make the R of the bent portion 12 smaller than that of a portion that is not heated, and the character line 22 of the bent portion 12 can be made sharper on the design surface 10A side of the side member outer 10.
[0045] Here, in this embodiment, as shown in Fig. 2, gradual change portions 24, 26 are provided in the molten portion 14 formed on the back surface 10B side of the bent portion 12 shown in Fig. 3, and the molten width W in the molten portion 14 gradually changes in the gradual change portions 24, 26. For example, when the molten width W is large, R is formed large, and when the molten width W is small, R is formed small. For this reason, in this embodiment, by gradually changing the molten width W, it is possible to gradually change the R of the bent portion 12.
[0046] Therefore, in this embodiment, even if a bent portion 12 (press line) is formed in advance in the side member outer 10 by press processing, it is possible to naturally connect these shapes between the bent portion 12 or other parts and the convex portion (bent portion) 13 by laser processing shown in Figure 2.
[0047] As described above, in the first step of the laser irradiation process, the laser output by the laser device 21 is gradually increased from W1 to W2 (gradual change unit 24) from point A to point B shown in Figures 1 and 2. In other words, the laser output can be set low at point A where the laser irradiation starts. This makes it possible to suppress sudden heat input to the outer member 10, reduce the stress difference between the part where heat is input and the other parts, and suppress distortion of the outer member 10 caused by the stress difference.
[0048] In the second process, the laser focusing diameter by the laser device 21 is set to gradually decrease from D2 to D3 from point B to point C, and the R of the bent portion 12 is formed to gradually decrease (gradually changing portion 26). In other words, the character line 22 is formed to gradually become sharper from point B to point C.
[0049] In the third step, the laser output and the laser focused diameter of the laser device 21 are substantially constant from point C to point D. In other words, from point C to point D, the R of the bent portion 12 is substantially constant, and the sharpness of the character line 22 is substantially constant.
[0050] In the fourth step, at point D, the laser output by the laser device 21 is reduced from W3 to W4, and in the fifth step, at point E, the laser output by the laser device 21 is reduced from W4 to W5, and the laser irradiation is terminated. Since the heating temperature increases with the passage of time from the start of the laser irradiation, the laser output by the laser device 21 is reduced stepwise at points D and E.
[0051] Due to the above-mentioned processing conditions, in this embodiment, it is possible to form the character line 22 formed on the roof side rail portion 20 so that it gradually becomes sharper as it approaches the vehicle front side. That is, in this embodiment, it is possible to gradually reduce the radius of curvature of the bent portion 12 in the roof side rail portion 20 as it approaches the vehicle front side. In this embodiment, the radius of curvature of the bent portion 12 is approximately the same from point C to point E.
[0052] In the present embodiment, at least one of the laser focus diameter and the laser output of the laser device 21 is gradually changed in the laser irradiation process, but this is not limited thereto. For example, conditions such as the laser speed of the laser light and the number of passes of the laser light may be changed. In the present embodiment, a gradual change process is provided between point A and point C, but the location of the gradual change process can be appropriately changed depending on the density of the ridge of the character line 22.
[0053] As described above, in this embodiment, even if a bent portion 12 (press line) is formed in advance on the side member outer 10 by press processing as shown in Figure 2, it is possible to naturally connect these shapes between the bent portion 12 or other parts and the convex portion 13 (press line + laser decoration) formed by laser processing.
[0054] In this manner, in this embodiment, by performing laser irradiation processing as additional processing, it is possible to make the character line 22 formed by press processing sharper. Therefore, for example, on an existing press line, it is possible to create vehicle designs that give different impressions depending on whether or not laser irradiation processing is performed.
[0055] For example, in the case of press processing, a special mold is required, but in the case of laser irradiation processing, a special mold is not required. Therefore, if the metal plate that has been pressed can be applied to minor changes, special specification vehicles, etc. by using or not using laser irradiation processing, it will be possible to achieve a significant cost reduction.
[0056] In this embodiment, the side member outer 10 is used as a metal plate, but the present invention is not limited to this. For example, although not shown, the present invention can be applied to a belt line provided on the upper part of a door panel, a lower part of a door panel, a hood panel, a back door, etc.
[0057] Furthermore, the present invention can be practiced with various modifications without departing from the spirit and scope of the present invention, and it goes without saying that the scope of the present invention is not limited to the above-described embodiments. [Explanation of symbols]
[0058] 10. Saimenouta (metal plate) 10A Design surface 10B back side 12 Bend 13 Convex part (bent part) 14 Welding section 20 Roof side rail section (metal plate) 21 Laser device 22 Character line (bend) 24 Gradual change part 26 Gradual change part W Melting width
Claims
1. A plate-shaped body, A bent portion bent in a thickness direction of the main body; a fusion portion formed by melting a surface on a back surface side of the bent portion opposite to the design surface of the main body; A gradually changing portion formed by gradually changing the fusion width of the fusion portion; A metal plate equipped with
2. The metal plate according to claim 1 , wherein a curvature radius of a cross section cut along a plate thickness direction at the bent portion is smaller in the region where the fusion width is narrow than in the region where the fusion width is wide.
3. a press forming process in which the metal plate is pressed in the thickness direction to form a predetermined shape; a laser irradiation process of irradiating a bent portion formed by pressing in the press forming process with a laser from a back surface side opposite to a design surface of the metal plate; Equipped with 3. The metal plate forming method according to claim 1, wherein the laser irradiation step includes a gradual change step of gradually changing a melt width of a melted portion formed by melting the front surface on the rear surface side of the metal plate.
4. The method for forming a metal sheet according to claim 3 , wherein in the gradual changing step, at least one of a laser focus diameter and a laser output is gradually changed.
Citation Information
Patent Citations
Method for forming and repairing metal part
JP1993131281A
Production of mirror
JP1994148411A
Device for removing spring back
JP1995204749A
Cemented carbide thin plate tool and straightening method of cemented carbide thin plate
JP2004050316A