Resin composition for vehicular coolant transportation tube and vehicular coolant transportation tube
The resin composition for coolant transport tubes, using a propylene-α-olefin block copolymer and propylene homopolymer with inorganic filler, addresses crystallization issues in polypropylene, enhancing dispersibility and physical properties for improved tube performance.
Patent Information
- Application Number
- JP2023085038
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Polypropylene resin materials used in coolant transport tubes can crystallize due to varying external environments, leading to areas of low strength as inorganic fillers do not disperse evenly, affecting the tube's physical properties.
A resin composition comprising a propylene-α-olefin block copolymer, propylene homopolymer, and inorganic filler, with specific ratios and melt flow rates, to suppress polypropylene resin crystallization and enhance filler dispersibility.
The composition effectively suppresses polypropylene resin crystallization, ensuring both physical properties and inorganic filler dispersibility, resulting in a high-quality coolant transport tube.
Smart Images

Figure 2024168404000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for a vehicle coolant transport tube and a vehicle coolant transport tube, and more particularly to a resin composition for a vehicle coolant transport tube and a vehicle coolant transport tube that are suitable as a tube for transporting coolant in a cooling system of an automobile or the like. [Background technology]
[0002] Coolant transport tubes are used as tubes for transporting coolants in the cooling systems of gasoline-powered vehicles, electric vehicles, and the like. Polyamide resins are often used for coolant transport tubes because of their heat resistance. In recent years, cost-effective polypropylene-based resins have been considered as materials for coolant transport tubes. Polypropylene-based resins may be mixed with inorganic fillers to improve tube strength. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication 2020 / 195143 Summary of the Invention [Problem to be solved by the invention]
[0004] The external environment, such as climate and temperature, varies depending on the place and time of manufacture of the tube. If the external environment is different, the polypropylene resin material may crystallize during the extrusion molding of the tube. Since the inorganic filler cannot be inserted into the crystallized parts of the polypropylene resin, the molded tube may have weak parts.
[0005] The problem to be solved by the present invention is to provide a resin composition for a vehicle coolant transport tube, and a vehicle coolant transport tube, which can suppress crystallization of a polypropylene-based resin and thereby achieve both physical properties and dispersibility of an inorganic filler. [Means for solving the problem]
[0006] The resin composition for a vehicle coolant transport tube according to the present invention contains the following (A) to (C), in which, relative to 100 mass% of the polymer component, the following (A) is 75 mass% or more and 99 mass% or less and the following (B) is 1 mass% or more and 25 mass% or less, the following (C) is 5 mass parts or more and 35 mass parts or less per 100 mass parts of the total of the following (A) and (B), and the difference in melt flow rate between the following (A) and the following (B) measured at 230°C under a load of 2.16 kg is 5 g / 10 min or more and 50 g / 10 min or less. (A) A propylene-α-olefin block copolymer having a melt flow rate of 0.2 g / 10 min or more and 1.5 g / 10 min or less, measured at 230° C. under a load of 2.16 kg. (B) Propylene homopolymer (C) Inorganic filler
[0007] The difference between the melt flow rates of (A) and (B) measured at 230°C under a load of 2.16 kg may be 10 g / 10 min or more and 50 g / 10 min or less. The melt flow rate of (B) measured at 230°C under a load of 2.16 kg may be 10 g / 10 min or more and 50 g / 10 min or less. In 100% by mass of the polymer component, (A) may be 90% by mass or more and 97% by mass or less, and (B) may be 3% by mass or more and 10% by mass or less. (A) may be an ethylene-propylene block copolymer. The diameter of the aggregates of (C) in the polymer component may be 15 μm or more and 60 μm or less. The median diameter of (C) may be 25 μm or less.
[0008] The vehicle coolant transport tube according to the present invention is made of the above-mentioned resin composition for vehicle coolant transport tubes.
[0009] (1) The resin composition for a vehicle coolant transport tube according to the present invention contains the following (A) to (C), in which, relative to 100% by mass of the polymer component, the following (A) is 75% by mass or more and 99% by mass or less and the following (B) is 1% by mass or more and 25% by mass or less, the following (C) is 5 parts by mass or more and 35 parts by mass or less per 100 parts by mass of the total of the following (A) and (B), and the difference in melt flow rate between the following (A) and the following (B) measured at 230°C under a load of 2.16 kg is 5 g / 10 min or more and 50 g / 10 min or less. (A) A propylene-α-olefin block copolymer having a melt flow rate of 0.2 g / 10 min or more and 1.5 g / 10 min or less, measured at 230° C. under a load of 2.16 kg. (B) Propylene homopolymer (C) Inorganic filler
[0010] (2) In the above (1), the difference in melt flow rate between (A) and (B) measured at 230° C. under a load of 2.16 kg may be 10 g / 10 min or more and 50 g / 10 min or less.
[0011] (3) In the above (1) or (2), the melt flow rate of the (B) measured at 230° C. under a load of 2.16 kg is preferably 10 g / 10 min or more and 50 g / 10 min or less.
[0012] (4) In any one of the above (1) to (3), the (A) may be from 90% to 97% by mass, and the (B) may be from 3% to 10% by mass, based on 100% by mass of the polymer component.
[0013] (5) In any one of the above (1) to (4), the (A) may be an ethylene-propylene block copolymer.
[0014] (6) In any one of the above (1) to (5), the diameter of the aggregates of (C) in the polymer component may be 15 μm or more and 60 μm or less.
[0015] (7) In any one of the above (1) to (6), the median diameter of (C) is preferably 25 μm or less.
[0016] (8) A vehicle coolant transport tube according to the present invention comprises the resin composition for a vehicle coolant transport tube according to any one of (1) to (7) above. Effect of the Invention
[0017] The resin composition for vehicle coolant transport tube according to the present invention contains the above (A) to (C), and in 100% by mass of the polymer component, the above (A) is 75% by mass or more and 99% by mass or less, the above (B) is 1% by mass or more and 25% by mass or less, the above (C) is 5 parts by mass or more and 35 parts by mass or less per 100 parts by mass of the total of the above (A) and (B), and the difference in melt flow rate between the above (A) and the above (B) measured at 230°C under a load of 2.16 kg is 5 g / 10 min or more and 50 g / 10 min or less. Therefore, crystallization of the polypropylene resin is suppressed, and both physical properties and dispersibility of the inorganic filler can be achieved.
[0018] Here, when the difference in melt flow rate between (A) and (B) measured at 230°C under a load of 2.16 kg is 10 g / 10 min or more and 50 g / 10 min or less, it is possible to achieve a high degree of compatibility between physical properties and dispersibility of the inorganic filler.
[0019] Furthermore, when the melt flow rate of (B) measured at 230° C. under a load of 2.16 kg is 10 g / 10 min to 50 g / 10 min, both physical properties and dispersibility of the inorganic filler can be highly achieved.
[0020] Furthermore, when the (A) is 90% by mass or more and 97% by mass or less and the (B) is 3% by mass or more and 10% by mass or less, based on 100% by mass of the polymer component, it is possible to achieve a high degree of compatibility between the physical properties and the dispersibility of the inorganic filler.
[0021] When the (A) is an ethylene-propylene block copolymer, it is possible to obtain an excellent effect of achieving both physical properties and dispersibility of the inorganic filler.
[0022] When the diameter of the aggregates of (C) in the polymer component is 15 μm or more and 60 μm or less, it is possible to obtain an excellent effect of achieving both physical properties and dispersibility of the inorganic filler.
[0023] When the median diameter of (B) is 25 μm or less, the diameter of the aggregates of (B) can be easily controlled to 60 μm or less.
[0024] The vehicle coolant transport tube according to the present invention is made of the resin composition for a vehicle coolant transport tube, and therefore crystallization of the polypropylene resin is suppressed, and both physical properties and dispersibility of the inorganic filler can be achieved. [Brief description of the drawings]
[0025] [Figure 1] 1 is a configuration diagram showing a vehicle coolant transport tube according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The resin composition for a vehicle coolant transport tube and the vehicle coolant transport tube according to the present invention will be described in detail below.
[0027] The resin composition for a vehicle coolant transport tube according to the present invention (hereinafter sometimes referred to as the present resin composition) contains the following (A) to (C), in which, in 100% by mass of the polymer component, the following (A) is 75% by mass or more and 99% by mass or less, and the following (B) is 1% by mass or more and 25% by mass or less, the following (C) is 5 parts by mass or more and 35 parts by mass or less per 100 parts by mass of the total of the following (A) and (B), and the difference in melt flow rate between the following (A) and the following (B) measured at 230°C under a load of 2.16 kg is 5 g / 10 min or more and 50 g / 10 min or less. (A) A propylene-α-olefin block copolymer (hereinafter sometimes referred to as block polypropylene) having a melt flow rate of 0.2 g / 10 min or more and 1.5 g / 10 min or less, measured at 230 °C under a load of 2.16 kg. (B) Propylene homopolymer (hereinafter sometimes referred to as homopolypropylene) (C) Inorganic filler
[0028] The block polypropylene (A) has a specific MFR. If the MFR of the block polypropylene (A) exceeds 1.5 g / 10 min, the physical properties cannot be ensured. In addition, the torque becomes too high, and the dispersibility of (C) decreases. If the MFR of the block polypropylene (A) is less than 0.2 g / 10 min, the fluidity during extrusion cannot be ensured. If the MFR of the block polypropylene (A) is 0.2 g / 10 min or more and 1.5 g / 10 min or less, the physical properties and fluidity can be ensured. In addition, the dispersibility of (C) can be improved. The MFR of the block polypropylene (A) is more preferably 0.2 g / 10 min or more and 1.3 g / 10 min or less, even more preferably 0.2 g / 10 min or more and 1.0 g / 10 min or less, and particularly preferably 0.3 g / 10 min or more and 0.8 g / 10 min or less. The MFR is measured in accordance with JIS K 7210:1999 under conditions of 230° C. and 2.16 kg load.
[0029] The block polypropylene (A) is a propylene-α-olefin block copolymer. The propylene-α-olefin block copolymer is a block copolymer having at least a block of continuous propylene monomers and a block of continuous α-olefin monomers. The propylene-α-olefin block copolymer is not limited to the above, and may be an alloy (mixture) having a sea-island structure in which a polypropylene component such as a propylene homopolymer is in the sea phase and a polyethylene component and / or an ethylene-based rubber component is in the island phase. The propylene-α-olefin block copolymer is a concept that includes such alloys.
[0030] Examples of α-olefins include ethylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. Among them, ethylene, 1-butene, and 1-hexene are preferred, and ethylene is particularly preferred. When the block polypropylene of (A) is an ethylene-propylene block copolymer, it is excellent in the effect of achieving both the physical properties of the tube and the dispersibility of (C).
[0031] Examples of the polyethylene component include ethylene-based copolymers such as ethylene homopolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, and copolymers of ethylene and α-olefin (ethylene-propylene copolymer, ethylene-butene copolymer, ethylene-octene copolymer). Examples of the ethylene-based rubber component include ethylene-propylene-diene terpolymer (EPDM), ethylene-propylene copolymer (EPR), ethylene-butene copolymer (EBR), and ethylene-octene copolymer (EOR). The content of the polyethylene component and / or the ethylene-based rubber component in the entire alloy (mixture) is preferably 1 to 49% by mass, more preferably 2.5 to 20% by mass.
[0032] The homopolypropylene (B) can be used together with the block polypropylene (A) to suppress the crystallization of the block polypropylene (A). This is particularly effective in cases where the polypropylene resin material may crystallize during extrusion molding of the tube when the external environment, such as the climate and temperature, differs depending on the place and time of manufacture of the tube. Furthermore, by suppressing the crystallization of the block polypropylene (A), the decrease in the dispersibility of (C) is suppressed, making it possible to achieve both physical properties and dispersibility of the inorganic filler.
[0033] (B) is preferably polypropylene. When (B) is polypropylene, it has excellent compatibility with (A), which is polypropylene. Also, (B) is preferably homopolypropylene. Compared to the case of block polypropylene, this is more effective in suppressing the crystallization of (A), which is block polypropylene.
[0034] The difference in MFR between the block polypropylene (A) and the homopolypropylene (B) is 5 g / 10 min or more and 50 g / 10 min or less. The MFR is measured in accordance with JIS K 7210:1999 under conditions of 230°C and a load of 2.16 kg. When the difference in MFR is 5 g / 10 min or more, the effect of suppressing the crystallization of the block polypropylene (A) is excellent. When the difference in MFR is less than 5 g / 10 min, the effect of suppressing the crystallization of the block polypropylene (A) is not exerted. Therefore, the decrease in dispersibility of (C) cannot be suppressed. From this viewpoint, the difference in MFR is more preferably 10 g / 10 min or more, and even more preferably 12 g / 10 min or more. On the other hand, when the difference in MFR exceeds 50 g / 10 min, the physical properties are decreased due to the influence of (B). When the difference in MFR is 50 g / 10 min or less, the effect of suppressing the crystallization of the block polypropylene (A) can be exerted while ensuring the physical properties. From this viewpoint, the difference in MFR is preferably 40 g / 10 min or less, more preferably 30 g / 10 min or less. When the difference in MFR is 10 g / 10 min or more and 50 g / 10 min or less, both physical properties and dispersibility of the inorganic filler can be highly achieved.
[0035] In 100% by mass of the polymer component, the block polypropylene (A) is 75% by mass or more and 99% by mass or less, and the homopolypropylene (B) is 1% by mass or more and 25% by mass or less. If the block polypropylene (A) is less than 75% by mass, the physical properties cannot be ensured. If the block polypropylene (A) is more than 99% by mass, the amount of the homopolypropylene (B) is too small, and the effect of suppressing the crystallization of the block polypropylene (A) is not exhibited. If the ratio of the block polypropylene (A) to the homopolypropylene (B) is within the above range, the effect of suppressing the crystallization of the block polypropylene (A) can be exhibited while ensuring the physical properties. From this viewpoint, the block polypropylene (A) is more preferably 85% by mass or more and 97% by mass or less, and even more preferably 90% by mass or more and 97% by mass or less, in 100% by mass of the polymer component. Moreover, the homopolypropylene (B) is more preferably 3% by mass or more and 15% by mass or less, and even more preferably 3% by mass or more and 10% by mass or less, in 100% by mass of the polymer component. Furthermore, when the block polypropylene (A) is 90% by mass or more and 97% by mass or less and the homopolypropylene (B) is 3% by mass or more and 10% by mass or less out of 100% by mass of the polymer component, the physical properties and the dispersibility improving effect of (C) due to the crystallization suppression effect are highly compatible.
[0036] The homopolypropylene (B) preferably exhibits a specific MFR. Specifically, the homopolypropylene (B) preferably has an MFR of 6 g / 10 min or more and 50 g / 10 min or less. When the homopolypropylene (B) has an MFR of 50 g / 10 min or less, the difference in MFR between the block polypropylene (A) and the homopolypropylene (B) is not too large, so that the deterioration of physical properties is suppressed. When the homopolypropylene (B) has an MFR of 6 g / 10 min or more, the difference in MFR between the block polypropylene (A) and the homopolypropylene (B) is not too small, so that the effect of suppressing the crystallization of the block polypropylene (A) can be exerted. When the homopolypropylene (B) has an MFR of 6 g / 10 min or more and 50 g / 10 min or less, the effect of suppressing the crystallization of the block polypropylene (A) can be exerted while ensuring the physical properties. The homopolypropylene (B) more preferably has an MFR of 10 g / 10 min or more and 50 g / 10 min or less. When the MFR of the homopolypropylene (B) is 10 g / 10 min or more and 50 g / 10 min or less, the physical properties and the effect of improving the dispersibility of (C) due to the effect of suppressing crystallization are highly compatible. The MFR is measured in accordance with JIS K 7210:1999 under the conditions of 230°C and a load of 2.16 kg.
[0037] Examples of the inorganic filler (C) include talc, silica, mica, kaolin, calcium carbonate, calcium titanate, apatite, and mica. These may be used alone or in combination as the inorganic filler (C). Among these, talc is preferred from the viewpoints of excellent reinforcing properties and excellent extrusion processability.
[0038] The content of the inorganic filler (C) is 5 parts by mass or more and 35 parts by mass or less relative to 100 parts by mass of the total of the block polypropylene (A) and the homopolypropylene (B). If the content of the inorganic filler (C) is less than 5 parts by mass, the effect of improving the physical properties is reduced. On the other hand, if the content of the inorganic filler (C) is more than 35 parts by mass, the inorganic filler (C) is likely to aggregate, resulting in a decrease in physical properties and a decrease in dispersibility. From these viewpoints, the content of the inorganic filler (B) is preferably 10 parts by mass or more and 30 parts by mass or less, more preferably 15 parts by mass or more and 30 parts by mass or less, and even more preferably 20 parts by mass or more and 30 parts by mass or less relative to 100 parts by mass of the total of the block polypropylene (A) and the homopolypropylene (B).
[0039] From the viewpoint of physical properties, it is preferable that the inorganic filler (C) has small agglomerates. Specifically, the diameter of the agglomerates is preferably 60 μm or less. More preferably, it is 55 μm or less, even more preferably, it is 50 μm or less, and particularly preferably, it is 45 μm or less. In the present invention, the homopolypropylene (B) suppresses the crystallization of the block polypropylene (A), thereby improving the dispersibility of the inorganic filler (C), and suppressing the aggregation of the inorganic filler (C), thereby suppressing the agglomerates to be small. On the other hand, the lower limit of the diameter of the agglomerates is not particularly limited, but is preferably 10 μm or more from the viewpoint of the effect of the increase in viscosity on extrusion processability and the effect of the increase in elastic modulus on bending processability. More preferably, it is 15 μm or more. In addition, if the inorganic filler (C) is kneaded too much in order to improve the dispersibility, the block polypropylene (A) is likely to have a low molecular weight, and the low-temperature impact resistance is likely to deteriorate. From this viewpoint, the lower limit of the diameter of the agglomerates is preferably 10 μm or more. The diameter of the aggregates can be expressed as the median value of the maximum lengths of the largest aggregates measured at three locations in total when the cross section of the resin composition is observed under a microscope.
[0040] The median diameter of the inorganic filler (C) is preferably 25 μm or less. When the median diameter of the inorganic filler (C) is 25 μm or less, the diameter of the aggregates of the inorganic filler (C) is easily controlled to a specific size or less. From this viewpoint, the median diameter of the inorganic filler (C) is more preferably 20 μm or less, and even more preferably 15 μm or less. On the other hand, the lower limit of the median diameter of the inorganic filler (C) is not particularly limited, but is preferably 1.0 μm or more from the viewpoint of the effect on extrusion processability due to an increase in viscosity and the effect on bending processability due to an increase in elastic modulus. More preferably, it is 1.5 μm or more. The median diameter of the inorganic filler (C) can be measured using a laser diffraction type particle size distribution measuring device. Examples of the laser diffraction type particle size distribution measuring device include Microtrack MT3300EXII manufactured by Microtrack Bell.
[0041] The resin composition may contain other resin components than (A) and (B) within the range that does not impair the effects of the present invention. The other resin components may contain modified resins that make them compatible. Examples of such modified resins include acid-modified or carboxy-modified polypropylene. The content of the modified resin is not particularly limited, but is 0.5 to 10 parts by mass, preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the block polypropylene (A).
[0042] The acid or its derivative in the acid-modified product includes unsaturated carboxylic acid and its derivative. Examples of unsaturated carboxylic acid include maleic acid, fumaric acid, acrylic acid, methacrylic acid, etc. Examples of derivatives of unsaturated carboxylic acid include acid anhydrides, ester compounds, amide compounds, imide compounds, metal salts, etc. of unsaturated carboxylic acid.
[0043] The resin composition may contain other components in addition to (A), (B), and (C) to the extent that the effects of the present invention are not impaired. Examples of other components include weather stabilizers, lubricants, pigments, dyes, antistatic agents, plasticizers, and antioxidants.
[0044] Examples of the antiaging agent include phenol-based antiaging agents, amine-based antiaging agents, imidazole-based antiaging agents, and phosphoric acid-based antiaging agents. The antiaging agent may be composed of only one of these, or may be composed of two or more of these. Among these, phenol-based antiaging agents are preferred from the viewpoint of being more excellent in heat resistance. Furthermore, among the phenol-based antiaging agents, hindered phenol-based antiaging agents are particularly preferred from the viewpoint of heat resistance.
[0045] The content of the antioxidant is not particularly limited, but is usually 0.05 to 1.0 part by mass, and preferably 0.1 to 1.0 part by mass, relative to 100 parts by mass of the block polypropylene (A).
[0046] The resin composition of the above configuration uses block polypropylene (A) and homopolypropylene (B) in combination in a specific ratio as polymer components, and the difference in MFR between block polypropylene (A) and homopolypropylene (B) is 5 g / 10 min or more and 50 g / 10 min or less, so that crystallization of block polypropylene (A) can be suppressed. In particular, when the external environment such as climate and temperature differs depending on the place of manufacture or the time of manufacture of the tube, the polypropylene resin material may crystallize during extrusion molding of the tube, and this is particularly effective in such cases. Furthermore, by suppressing the crystallization of block polypropylene (A), the decrease in dispersibility of (C) is suppressed, so that both physical properties and dispersibility of inorganic filler can be achieved.
[0047] The vehicle coolant transport tube according to the present invention (hereinafter, sometimes referred to as the present resin tube) can be obtained from the present resin composition. The present resin tube is preferably embodied as a single-layered resin tube 10 as shown in Fig. 1. If necessary, other resin layers or reinforcing fiber layers may be further laminated to form a multi-layered resin tube.
[0048] From the viewpoint of its application, the present resin tube preferably has an inner diameter in the range of 2.5 to 30 mm, particularly 4 to 25 mm, and a thickness in the range of 0.5 to 5.0 mm, particularly 0.75 to 4.0 mm.
[0049] The present resin tube is used, for example, for piping coolants inside automobiles, and specifically, is suitably used as a radiator hose, heater hose, air conditioner hose, etc., or as a cooling tube for battery packs for electric automobiles and fuel cell automobiles.
[0050] The resin tube can be produced by melt extrusion molding the resin composition into a tubular shape. The resin composition can be obtained by blending and kneading (A), (B), and (C) and any other components that may be blended as required.
[0051] The kneading step of the present resin composition may be carried out using, for example, a twin-screw kneading extruder, etc. The kneading temperature is preferably 190° C. to 230° C. The kneading time is preferably 0.01 to 10 minutes.
[0052] The extrusion step of the present resin composition may be carried out using, for example, a twin-screw kneading extruder, etc. The extrusion temperature is preferably 190° C. to 255° C. from the viewpoint of low-temperature extrusion.
[0053] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the spirit of the present invention. EXAMPLES
[0054] The present invention will be described in detail below using examples and comparative examples.
[0055] (Examples 1-8, Comparative Examples 1-5) The components except for the inorganic filler were mixed in the mixing ratios (parts by mass) shown in the table and mixed for 5 minutes at 200° C. using a twin-screw kneading extruder (Toshiba Machine's "TEM-18SS"), after which the inorganic filler was added and mixed for 5 minutes at 200° C. using the twin-screw kneading extruder to obtain a kneaded mixture. The kneaded mixture was then pelletized, and the pellets were melt extruded into a tube shape at 250° C. using a melt extrusion molding machine equipped with a cylindrical die (Plastic Engineering Research Institute's "GT-40") to obtain a resin tube with an inner diameter of 18 mm and an outer diameter of 20 mm.
[0056] The materials used are as follows. The MFR was measured in accordance with JIS K 7210:1999 at 230°C and a load of 2.16 kg. (A) Propylene-α-olefin block copolymer Block PP <1> Prime Polymer "E-701G", MFR 0.5g / 10min Block PP <2> Prime Polymer "E-702MG", MFR 1.4g / 10min (B) Propylene homopolymer Homo PP <1> Prime Polymer "F704NP", MFR 7.0g / 10min Homo PP <2> : Prime Polymer "J106MG", MFR 16g / 10min Homo PP <3> : Prime Polymer "J108M", MFR45g / 10min (B') Propylene homopolymer Homo PP <4> Prime Polymer "E200GPL", MFR 1.4g / 10min Homo PP <5> : Lyondellbasell "C14EP348U", MFR70g / 10min (C) Inorganic filler Inorganic filler: Talc (Fuji Talc "FH108" median diameter 8.0 μm)
[0057] The properties of each of the obtained resin tubes were evaluated according to the following criteria, and the results are shown in Table 1 below.
[0058] <Dispersibility> The extruded tube (2000 mm) was cut at any three locations (total of nine locations) at the tip, center, and rear end to expose the cross sections, and when viewed under a viewing angle (microscope) of 1500 μm x 1500 μm, those in which the maximum length (diameter of the aggregate) of the largest inorganic filler agglomerates did not exceed 60 μm were marked with "◎", those in which one or two locations exceeded 60 μm were marked with "○", and those in which three or more locations exceeded 60 μm were marked with "×".
[0059] <Physical Properties> The resin tube was heat-treated at 160°C for 1 hour, then cut in half and punched into strips with a width of 10 mm and a length of 15 cm. The elongation at break [Eb] of the obtained strip samples was measured using a tensile tester (AGS-X, manufactured by Shimadzu Corporation) in accordance with JIS K 6251. Those with an elongation at break of 350% or more were marked with "◎", those with an elongation at break of 300% or more were marked with "◯", and those with an elongation at break of less than 300% were marked with "X".
[0060] [Table 1]
[0061] In Comparative Example 1, only block polypropylene (A) is used as the polymer component, and homopolypropylene (B) is not used. Therefore, the crystallization of block polypropylene (A) is not suppressed during extrusion molding of the tube, and the dispersibility of the inorganic filler is poor. In Comparative Example 2, block polypropylene (A) and homopolypropylene are used in combination as the polymer component, but the difference in MFR between them is less than 5 g / 10 min. Therefore, the crystallization of block polypropylene (A) is not suppressed during extrusion molding of the tube, and the dispersibility of the inorganic filler is poor. In Comparative Example 3, block polypropylene (A) and homopolypropylene are used in combination as the polymer component, but the difference in MFR between them is more than 50 g / 10 min. Therefore, the physical properties of the tube are poor. In Comparative Example 4, block polypropylene (A) and homopolypropylene (B) are used in combination as the polymer component, but the amount of homopolypropylene (B) is too large. Therefore, the physical properties of the tube are poor. In Comparative Example 5, the block polypropylene (A) and the homopolypropylene (B) are used in combination as the polymer components, but the amount of the inorganic filler (C) is too large, resulting in poor physical properties of the tube.
[0062] In contrast, in the examples, block polypropylene (A) and homopolypropylene (B) are used in combination in a specific ratio as polymer components, and the difference in MFR between block polypropylene (A) and homopolypropylene (B) is 5 g / 10 min or more and 50 g / 10 min or less. In addition, inorganic filler (C) is contained in a specific ratio. Therefore, crystallization of block polypropylene (A) is suppressed during extrusion molding, and the inorganic filler has excellent dispersibility. In addition, the physical properties of the tube are also excellent.
[0063] From the above, it has been confirmed that a resin composition containing (A) a propylene-α-olefin block copolymer having a melt flow rate of 0.2 g / 10 min to 1.5 g / 10 min measured at 230°C under a load of 2.16 kg, (B) a propylene homopolymer, and (C) an inorganic filler, in which, in 100 mass% of the polymer components, (A) is 75 mass% to 99 mass% and (B) is 1 mass% to 25 mass%, (C) is 5 mass parts to 35 mass parts per 100 mass parts of the total of (A) and (B), and the difference in melt flow rate between (A) and (B) is 5 g / 10 min to 50 g / 10 min can be achieved by suppressing the crystallization of the block polypropylene (A) and suppressing the decrease in dispersibility of (C), thereby achieving both physical properties and dispersibility of the inorganic filler.
[0064] In comparison between Examples, Examples 1, 2, and 5 show that when the difference in MFR between the block polypropylene (A) and the homopolypropylene (B) is 10 g / 10 min to 50 g / 10 min, both the physical properties and the dispersibility of the inorganic filler are achieved at a high level. Also, Examples 2, 6, and 7 show that when the block polypropylene (A) is 90 mass % to 97 mass % and the homopolypropylene (B) is 3 mass % to 10 mass % in 100 mass % of the polymer component, both the physical properties and the dispersibility of the inorganic filler are achieved at a high level.
[0065] Although the embodiments and examples of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible without departing from the spirit and scope of the present invention. [Explanation of symbols]
[0066] 10 Plastic tube
Claims
1. Contains the following (A) to (C): In 100% by mass of the polymer component, the following (A) is 75% by mass or more and 99% by mass or less, and the following (B) is 1% by mass or more and 25% by mass or less: The amount of the following (C) is 5 parts by mass or more and 35 parts by mass or less relative to 100 parts by mass of the total of the following (A) and the following (B), A resin composition for a vehicle coolant transport tube, wherein the difference in melt flow rate between the following (A) and (B) measured at 230° C. under a load of 2.16 kg is 5 g / 10 min or more and 50 g / 10 min or less: (A) A propylene-α-olefin block copolymer having a melt flow rate of 0.2 g / 10 min or more and 1.5 g / 10 min or less, measured at 230° C. under a load of 2.16 kg. (B) Propylene homopolymer (C) Inorganic filler
2. 2. The resin composition for a vehicle coolant transport tube according to claim 1, wherein a difference in melt flow rate between (A) and (B) measured at 230° C. under a load of 2.16 kg is 10 g / 10 min or more and 50 g / 10 min or less.
3. 3. The resin composition for a vehicle coolant transport tube according to claim 1, wherein the melt flow rate of the (B) measured at 230° C. under a load of 2.16 kg is 10 g / 10 min or more and 50 g / 10 min or less.
4. 3. The resin composition for a vehicle coolant transport tube according to claim 1, wherein, in 100% by mass of the polymer components, the (A) is 90% by mass or more and 97% by mass or less, and the (B) is 3% by mass or more and 10% by mass or less.
5. 3. The resin composition for a vehicle coolant transport tube according to claim 1, wherein the (A) is an ethylene-propylene block copolymer.
6. 3. The resin composition for a vehicle coolant transport tube according to claim 1, wherein the diameter of the aggregates of (C) in the polymer component is 15 μm or more and 60 μm or less.
7. 3. The resin composition for a vehicle coolant transport tube according to claim 1, wherein the median diameter of the (C) is 25 μm or less.
8. The difference in melt flow rate between the (A) and the (B) measured at 230° C. under a load of 2.16 kg is 10 g / 10 min or more and 50 g / 10 min or less, The melt flow rate of the (B) measured at 230° C. under a load of 2.16 kg is 10 g / 10 min or more and 50 g / 10 min or less, In 100% by mass of the polymer component, the (A) is 90% by mass or more and 97% by mass or less, and the (B) is 3% by mass or more and 10% by mass or less. The (A) is an ethylene-propylene block copolymer, The diameter of the aggregates of (C) in the polymer component is 15 μm or more and 60 μm or less, 2. The resin composition for a vehicle coolant transport tube according to claim 1, wherein the median diameter of the (C) is 25 μm or less.
9. A vehicle coolant transport tube comprising the resin composition for a vehicle coolant transport tube according to claim 1.
Citation Information
Patent Citations
Automobile cooling system tube and method for manufacturing same
WO2020195143A1