High-mobility substrate with δ-doped layer and method for manufacturing high-mobility substrate
A silicon-based substrate with δ-doped layers improves mobility and uniformity by sandwiching a thin silicon film between δ-doped layers with larger band gaps, addressing the challenges of forming high-mobility substrates over large areas and achieving comparable performance to two-dimensional materials like MoS2.
Patent Information
- Application Number
- JP2023085935
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods struggle to uniformly form high-mobility substrates over large-area substrates, particularly due to challenges in achieving uniformity and maintaining mobility across the entire surface, especially with materials like MoS2, which are difficult to attach and form into large-diameter films.
A high-mobility substrate structure is created by sandwiching a thin film of silicon between δ-doped layers, where the δ-doped layers have a larger band gap than the silicon, promoting band curvature and reducing interface roughness, thereby improving mobility and enabling uniform formation across large areas.
The proposed structure achieves high mobility comparable to two-dimensional materials like MoS2, while being cost-effective by using common semiconductor materials like silicon, and ensures uniformity and practicality on large-diameter substrates.
Smart Images

Figure 2024168899000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a high mobility substrate having a δ-doped layer and a method for manufacturing the high mobility substrate. [Background technology]
[0002] Two-dimensional materials such as MoS2 are being actively researched as channel materials for the next generation after the currently mainstream FinFET (Fin Field Effect Transistor) and the partially commercialized GAAFET (Gate All Around Field Effect Transistor). This is because there is a limit to how much performance can be achieved through the advancement of miniaturization, and this technology aims to improve performance by using a material with high mobility as the channel material.
[0003] However, the proposed two-dimensional materials include the aforementioned MoS2, graphene, BN, and other materials, and although the significance of their properties has been demonstrated, it is still difficult to obtain a film with a large diameter. Non-Patent Document 1 shows an example of BN, but it seems to be a film formation situation from the center to about halfway of a silicon substrate with a diameter of 100 mm.
[0004] In addition to the difficulty of forming the film, it is easy to imagine that the characteristics of the material (which exists stably as a two-dimensional thin film) make it difficult to attach or fix it to a substrate. In devices where operation has been proven, the two-dimensional material appears to be fixed using source and drain electrode materials.
[0005] On the other hand, when it comes to silicon materials, it has been known since the dawn of SOI (Silicon on Insulator) that mobility can be improved by sandwiching thin silicon of about 2 to 3 nm between silicon oxide films, and it is possible to achieve mobility equivalent to that of two-dimensional materials such as MoS2 (Non-Patent Documents 2 and 3).
[0006] As mentioned above, if silicon is covered (sandwiched) with an insulating film, the mobility can be improved and the mobility can be equivalent to that of two-dimensional materials. However, it is difficult to make the structure uniform over the entire surface of a wafer, for example, the entire surface of a 300 mm diameter substrate. In the conventional method, first, a wafer with an oxide film is sandwiched between H + By bonding and peeling the ion-implanted substrates together, the silicon layer is transferred onto the oxide film, and then an oxide film is formed, but it is difficult to control the thickness to 2-3 nm uniformly over the entire surface of a diameter of 300 mm due to the problem of the in-plane uniformity of the oxide film. (The in-plane uniformity of the oxidation furnace must be kept to 0.1 nm or less over a diameter of 300 mm.) [Prior art documents] [Non-patent literature]
[0007] [Non-Patent Document 1] ISSCC2021.1.1, Mark Liu,“Unleashing the Future of Innovation” [Non-Patent Document 2] ISSCC2023.27.3, D. Verrreck et. al.,“The promise of 2-D materials for scaled digital and analog applications” [Non-Patent Document 3] Sumida et al., “Optimal design of channel material and plane orientation for ultra-thin nMOSFETs utilizing anisotropy of electron valley to suppress surface roughness scattering,” Abstracts of the 70th Spring Meeting of the Japan Society of Applied Physics, 2023, 16p-A403-2. Summary of the Invention [Problem to be solved by the invention]
[0008] As mentioned above, it was previously known that high mobility could be achieved by thinning silicon and covering (sandwiching) it with an oxide film, but it was difficult to create the film uniformly over the entire substrate, making it impractical.
[0009] The present invention has been made in consideration of the above-mentioned problems in the conventional technology, and has an object to provide a practical high mobility substrate and a method for manufacturing a high mobility substrate, which can be uniformly formed over the entire surface of a large-area substrate while achieving high mobility. [Means for solving the problem]
[0010] In order to solve the above problems, the high mobility substrate of the present invention has a semiconductor substrate, a first δ-doped layer on the semiconductor substrate and having a band gap larger than that of the semiconductor substrate, a thin film made of the same material as the semiconductor substrate on the first δ-doped layer, and a second δ-doped layer on the thin film and having a band gap larger than that of the semiconductor substrate, with the thin film sandwiched between the first δ-doped layer and the second δ-doped layer.
[0011] In such a high-mobility substrate, the first δ-doped layer and the second δ-doped layer have a larger band gap than the thin film, and therefore at the junction interface between the thin film and each δ-doped layer, a band curvature (also called band bending) occurs, as seen at the junction between a semiconductor and an insulator with a larger band gap than the semiconductor, forming a groove with low potential, thereby improving the mobility. Furthermore, the use of a δ-doped layer prevents interface roughness from increasing, preventing a decrease in mobility due to interface scattering and maintaining high mobility. Furthermore, the δ-doped layer can be easily doped onto semiconductor substrates and thin films, and can be uniformly formed over the entire surface of large-area substrates, especially substrates with large diameters. The definition of δ-doping is that the doped layer is thin (for example, 3 nm or less).
[0012] It is also preferable that the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers, the semiconductor substrate and the thin film are silicon, and the thickness of the thin film is 2 nm or more and 3 nm or less.
[0013] With this type of oxygen delta-doped layer, a silicon oxide film SiO2 is formed as an insulating film on a silicon substrate or a silicon thin film, and a thin silicon layer of 2 nm to 3 nm is sandwiched between the silicon oxide films, which reliably improves mobility and enables the realization of mobility equivalent to that of two-dimensional materials such as MoS2.
[0014] In addition, a method for manufacturing a high mobility substrate of the present invention is a method in which a first δ-doped layer having a band gap larger than that of the semiconductor substrate is formed on a semiconductor substrate, a thin film made of the same material as the semiconductor substrate is formed on the first δ-doped layer, a second δ-doped layer having a band gap larger than that of the semiconductor substrate is formed on the second δ-doped layer, and the thin film is sandwiched between the first δ-doped layer and the second δ-doped layer.
[0015] In such a method for manufacturing a high mobility substrate, the first δ-doped layer and the second δ-doped layer have a larger band gap than the thin film, and therefore at the junction interface between the thin film and each δ-doped layer, a band curvature (also called band bending) occurs, as seen at the junction between a semiconductor and an insulator having a larger band gap than the semiconductor, forming a groove with low potential, thereby improving the mobility. Furthermore, by using the δ-doped layer, the interface roughness is not increased, so that the mobility is prevented from decreasing due to interface scattering, and high mobility can be maintained. Furthermore, δ-doped layers can be easily doped onto semiconductor substrates and thin films, and can be made uniform over the entire surface of large area substrates, especially substrates with large diameters.
[0016] It is also preferable that the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers, the semiconductor substrate and the thin film are silicon, and the thin film has a thickness of 2 nm to 3 nm.
[0017] By using such an oxygen delta-doped layer, a silicon oxide film SiO2 is formed as an insulating film on a silicon substrate or a silicon thin film, and a thin silicon layer of 2 nm to 3 nm is sandwiched between the silicon oxide films, which reliably improves mobility and makes it possible to achieve mobility equivalent to that of two-dimensional materials such as MoS2.
[0018] In addition, it is preferable that the thin film is formed to a thickness that takes into account the fact that it will become thinner due to oxidation, and then the thin film is oxidized to form the second δ-doped layer.
[0019] This method can prevent the thin film from becoming too thin and ensure that it is formed to the desired thickness.
[0020] It is also preferable to repeat the process of forming silicon to a thickness of 1 nm or more and 3 nm or less on the first δ-doped layer and then forming an oxygen δ-doped layer multiple times, and then form the thin silicon film on top to a thickness of 2 nm or more and 3 nm or less.
[0021] By using this method, a high mobility substrate can be reliably manufactured even if it has a laminated structure. Effect of the Invention
[0022] The high mobility substrate and the method for manufacturing a high mobility substrate of the present invention are practical because they can realize high mobility while being uniformly formed over the entire surface of a large-area substrate, particularly a substrate with a large diameter. Furthermore, by using thin film layers that mimic such two-dimensional materials, it becomes possible to form high mobility channel materials over the entire surface of large area substrates, especially substrates with large diameters. Furthermore, it is inexpensive because it can be realized using common semiconductor materials such as silicon, without using expensive two-dimensional materials such as MoS2. [Brief description of the drawings]
[0023] [Figure 1] 1 is a schematic diagram of a high mobility substrate in a first embodiment of the present invention. [Diagram 2]4 is a schematic diagram of a high mobility substrate in a second embodiment of the present invention. [Diagram 3] FIG. 11 is a schematic diagram of a high mobility substrate in a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will be described in detail below, but the present invention is not limited thereto.
[0025] As a result of intensive research into the above-mentioned problems, the inventors have found a structure having a semiconductor substrate, a first δ-doped layer on the semiconductor substrate having a band gap larger than that of the semiconductor substrate, a thin film made of the same material as the semiconductor substrate on the first δ-doped layer, and a second δ-doped layer on the thin film having a band gap larger than that of the semiconductor substrate, and the thin film is sandwiched between the first δ-doped layer and the second δ-doped layer, thereby completing the present invention. That is, specifically, by combining lamination of δ-doping and thin-film silicon and oxidation treatment, a structure in which a thin-film silicon having a thickness of 2 nm to 3 nm is sandwiched between an oxide film (more specifically, SiO2, a material with a band gap larger than that of silicon) which is an insulator as the δ-doped layer is formed, and it has been found that a substrate of higher quality can be obtained without using expensive two-dimensional materials, and the present invention has been completed.
[0026] This can be achieved, for example, by delta-doping a silicon substrate with oxygen atoms, stacking silicon on top of that to a thickness of 2 nm to 3 nm to form a thin film of silicon, and then delta-doping the silicon with oxygen atoms.
[0027] Furthermore, it can also be provided by delta-doping a silicon substrate with oxygen atoms, laminating silicon on top of that to a thickness that takes into account the fact that it will become thinner due to oxidation, to form a thin film of silicon, and then oxidizing it.
[0028] Furthermore, it can also be provided by delta-doping oxygen atoms onto a silicon substrate, laminating silicon to a thickness of 1 nm or more and 3 nm or less, preferably 1 nm, and further delta-doping oxygen atoms multiple times, and then laminating silicon on top to a thickness of 2 to 3 nm to form a thin film silicon, which is then further delta-doped with oxygen atoms.
[0029] A first embodiment of the present invention will now be described with reference to the drawings. First, the configuration of a high mobility substrate 1 will be described with reference to FIG. As shown in FIG. 1, the high mobility substrate 1 of this embodiment has a semiconductor substrate (support substrate) 2, a first δ-doped layer (first oxide film layer) 3-1 on the semiconductor substrate 2 and having a larger band gap than the semiconductor substrate 2, a thin film (silicon) 4 made of the same material as the semiconductor substrate 2 on the first δ-doped layer 3-1, and a second δ-doped layer (second oxide film layer) 3-2 on the thin film 4 and having a larger band gap than the semiconductor substrate 2, with the thin film 4 sandwiched between the first δ-doped layer 3-1 and the second δ-doped layer 3-2.
[0030] Here, in a more preferred embodiment, the first δ-doped layer 3-1 and the second δ-doped layer 3-2 are oxygen δ-doped layers, each of which forms an oxide film. The semiconductor substrate 2 and the thin film 4 are silicon, and have a thickness of 2 nm to 3 nm in order to achieve high mobility. If the thickness is 2 nm or more, the thin film (silicon) 4 layer is likely to become a perfect crystal, and mobility can be improved. On the other hand, if the thickness is 3 nm or less, the characteristics will be different from those of normal bulk silicon, and mobility can be improved more effectively. Below, as a preferred embodiment, the case where the semiconductor substrate 2 is a silicon substrate and the δ-doped layer is an oxide film layer will be mainly described. In addition, in the case of oxygen doping, δ-doping can be formed by thermal oxidation or natural oxidation.
[0031] In the high-mobility substrate 1 of this embodiment, the first δ-doped layer 3-1 and the second δ-doped layer 3-2 have a larger band gap than the thin film 4, so that at the junction interface between the thin film 4 and each δ-doped layer, a band curvature (also called band bending) occurs, as seen at the junction between a semiconductor and an insulator having a larger band gap than the semiconductor, forming a groove with low potential, thereby improving the mobility. Furthermore, the use of a δ-doped layer prevents interface roughness from increasing, preventing a decrease in mobility due to interface scattering and maintaining high mobility. Furthermore, the δ-doped layer can be easily doped onto semiconductor substrates and thin films, and can be formed uniformly over the entire surface of large-area substrates, especially substrates with large diameters.
[0032] In the case of the oxygen δ-doped layers (first δ-doped layer 3-1 and second δ-doped layer 3-2) of this embodiment, a silicon oxide film SiO2 is formed as an insulating film on a silicon substrate (semiconductor substrate 2) or a silicon thin film (thin film 4), and a thin silicon (thin film 4) having a thickness of 2 nm to 3 nm is sandwiched between silicon oxide films, which reliably improves mobility and makes it possible to achieve mobility equivalent to that of two-dimensional materials such as MoS2.
[0033] Next, a specific manufacturing flow of the high mobility substrate 1 of this embodiment will be described with reference to Fig. 1. A semiconductor substrate (support substrate) 2 is prepared, which can be a general silicon substrate. In the case of a silicon substrate, a (100) orientation is preferable from the viewpoint of electron mobility, but a (110) substrate may also be used in consideration of the balance of hole mobility, and the substrate surface orientation can be selected depending on the application.
[0034] Next, a first δ-doped layer (first oxide film layer) 3-1 of oxygen having a band gap larger than that of the semiconductor substrate 2 is formed on the semiconductor substrate (support substrate) 2. The method of forming a δ-doped layer on the semiconductor substrate 2 allows the δ-doped layer to be formed uniformly even on a large diameter substrate such as a substrate with a diameter of 300 mm.
[0035] There is no particular restriction on the method of forming the δ-doped layer, but the oxygen concentration can be set to a concentration at which silicon single crystal can grow, in anticipation of forming a thin film (silicon) 4 of the same material as the semiconductor substrate on the δ-doped layer. In this case, the oxygen concentration is set to 1×10 15 atoms / cm 2 It is preferable to set it to around 100 mm.
[0036] Next, a thin film (silicon) 4 layer made of the same material as the semiconductor substrate 2 is grown on the first δ-doped layer 3-1. When growing a thin film having a thickness of 2 nm to 3 nm, there are no particular restrictions on the growth method, but it can be easily grown by using an apparatus that can set low temperature and reduced pressure conditions.
[0037] Next, a second δ-doped layer (second oxide film layer) 3-2 of oxygen having a band gap larger than that of the semiconductor substrate 2 is formed on the thin film 4. This method may be the same as the method for forming the first δ-doped layer (first oxide film layer) 3-1.
[0038] In this manner, the thin film 4 can be sandwiched between the first δ-doped layer 3-1 and the second δ-doped layer 3-2, and the high mobility substrate 1 as shown in FIG. 1 can be manufactured.
[0039] In the manufacturing method of the high mobility substrate 1 of this embodiment, the first δ-doped layer 3-1 and the second δ-doped layer 3-2 have a larger band gap than the thin film 4, so that at the junction interface between the thin film 4 and each δ-doped layer, a band curvature (also called band bending) occurs, as seen at the junction between a semiconductor and an insulator having a larger band gap than the semiconductor, and a groove with low potential is formed, thereby improving the mobility. Furthermore, by using the δ-doped layer, the interface roughness is not increased, so that the mobility is prevented from decreasing due to interface scattering, and high mobility can be maintained. Furthermore, δ-doped layers can be easily doped onto semiconductor substrates and thin films, and can be made uniform over the entire surface of large area substrates, especially substrates with large diameters.
[0040] In the case of the oxygen δ-doped layers (first δ-doped layer 3-1 and second δ-doped layer 3-2) of this embodiment, a silicon oxide film SiO2 is formed as an insulating film on a silicon substrate (semiconductor substrate 2) or a silicon thin film (thin film 4), and a thin silicon (thin film 4) having a thickness of 2 nm to 3 nm is sandwiched between the silicon oxide films, thereby reliably improving the mobility and achieving a mobility equivalent to that of two-dimensional materials such as MoS2.
[0041] The second embodiment will be described with reference to FIG. The method for manufacturing the high mobility substrate of this embodiment is a method in which, when forming a thin film, the thin film is formed to a thickness that takes into account the fact that it will become thinner due to oxidation, and then the thin film is oxidized to form the second δ-doped layer.
[0042] 2 shows the state before the thin film (silicon) 5 is oxidized, and the thin film (silicon) 5 has a portion 5-1 that is oxidized to form the second δ-doped layer and a portion 5-2 that is not oxidized and remains as the thin film (silicon). In order to make the portion 5-2 that is not oxidized and remains as the thin film (silicon) 2 nm to 3 nm thick, the thin film (silicon) 5 is grown in advance to a thickness greater than 2 nm to 3 nm. The oxidation method may be a method of thermally oxidizing the thin film 5.
[0043] Here, the extent to which the thickness should be increased in anticipation of the thinning can be determined based on the fact that when silicon is oxidized to form an oxide film, approximately half of the oxide film is silicon (for example, in an oxide film of 100 Å, 44 Å of silicon is used), but it is advisable to confirm this more accurately through preliminary experiments, etc.
[0044] By using such a method, the portion 5-2 of the thin film 5 that is not oxidized and remains as a thin film (silicon) can be prevented from becoming too thin, less than 2 nm or more and 3 nm or less, and can be reliably formed to a desired thickness.
[0045] A third embodiment will be described with reference to FIG. The method for manufacturing the high mobility substrate of this embodiment involves forming silicon to a thickness of 1 nm or more and 3 nm or less on a first δ-doped layer, and then forming an oxygen δ-doped layer multiple times, and then forming a thin silicon film to a thickness of 2 nm or more and 3 nm or less on top of that.
[0046] Referring to FIG. 3, silicon 7-1 is formed on a first oxygen δ-doped layer 6-1 to a thickness of 1 nm or more and 3 nm or less, then an oxygen δ-doped layer 6-2 is formed, then silicon 7-2 is formed to a thickness of 1 nm or more and 3 nm or less, then an oxygen δ-doped layer 6-3 is formed, and then a thin film (silicon) 4 is formed thereon to a thickness of 2 nm or more and 3 nm or less.
[0047] By using this method, a high mobility substrate can be reliably manufactured even if it has a laminated structure.
[0048] Here, it is shown that the silicon and δ-doped layers can be repeated multiple times to form a stacked structure. On the other hand, in the CFET (Complementary Field Effect Transistor) structure, which is expected to be realized in the 2030s as the next-generation transistor structure, a structure in which the channel is stacked in three or four layers is assumed to obtain a sufficient current value, and this embodiment can be applied to such a stacked structure. EXAMPLES
[0049] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto.
[0050] [Example 1] Example 1 is an example in which the above-mentioned first embodiment is implemented, and a high mobility substrate as shown in FIG. 1 is manufactured.
[0051] First, a silicon (110) single crystal substrate with a diameter of 300 mm, boron doped p-type, and resistivity of 10 Ω·cm was prepared as the semiconductor substrate (support substrate) 2. This was immersed in a 1% concentration hydrofluoric acid solution for 3 minutes, and after removing the native oxide film, it was left in the atmosphere (temperature 23°C ± 1°C, humidity 39% ± 3%) for 3 hours to form a first δ-doped layer 3-1 of oxygen. It was then placed in a reduced pressure epitaxial device, and a thin film (silicon) layer 4 was grown for 60 seconds under the conditions of a temperature of 700°C, a pressure of 100 Torr, and monosilane of 1200 sccm. After that, it was removed from the device and left in the atmosphere for 1 hour to form a second δ-doped layer 3-2 of oxygen on the surface side, and a high mobility substrate 1 was obtained.
[0052] For the high mobility substrate obtained here, the first δ-doped layer, the thin film (silicon) layer, and the second δ-doped layer all had a thickness of 3 nm and a mobility of 100 cm 2 / V s.
[0053] [Example 2] Example 2 is different from Example 1 in that the steps of forming the δ-doped layer and the silicon layer are added.
[0054] A boron-doped p-type silicon (110) single crystal substrate with a diameter of 300 mm and a resistivity of 10 Ω·cm was prepared as a semiconductor substrate (support substrate). This was immersed in a 1% concentration hydrofluoric acid solution for 3 minutes, and after removing the native oxide film, it was left in the air (temperature 23°C ± 1°C, humidity 39% ± 3%) for 3 hours to form a first δ-doped layer of oxygen. It was then placed in a low-pressure epitaxial growth apparatus, and a silicon layer was grown for 2 seconds under the conditions of a temperature of 700°C, a pressure of 100 Torr, and monosilane of 1200 sccm. It was then removed from the apparatus and left in the air for 1 hour to form a third δ-doped layer of oxygen, and then placed in a low-pressure epitaxial growth apparatus, and a silicon layer was grown for 2 seconds under the conditions of a temperature of 700°C, a pressure of 100 Torr, and monosilane of 1200 sccm. The substrate was then removed from the apparatus and left in the atmosphere for 1 hour to form a second δ-doped layer of oxygen on the surface side. The substrate was then placed in a reduced-pressure epitaxial growth apparatus, where a silicon layer was grown in 2 seconds under conditions of a temperature of 700°C, a pressure of 100 Torr, and 1200 sccm of monosilane, yielding a high-mobility substrate.
[0055] For the high mobility substrate obtained here, the first δ-doped layer, the silicon layer, the third δ-doped layer, the thin film (silicon) layer, and the second δ-doped layer all had a thickness of 3 nm and a mobility of 100 cm 2 / V s.
[0056] [Example 3] Example 3 is different from Example 1 in that the process of forming the δ-doped layer and silicon layer is added, the film formation conditions are different, and a second δ-doped layer is formed by thermally oxidizing a thin film (silicon) in a heat treatment furnace.
[0057] A boron-doped p-type silicon (110) single crystal substrate with a diameter of 300 mm and a resistivity of 10 Ω·cm was prepared as a semiconductor substrate (support substrate). This was immersed in a 1% concentration hydrofluoric acid solution for 3 minutes, and after removing the native oxide film, it was left in the air (temperature 23°C ± 1°C, humidity 39% ± 3%) for 3 hours to form a first δ-doped layer of oxygen. It was then placed in a low-pressure epitaxial growth apparatus, and a silicon layer was grown for 2 seconds under the conditions of a temperature of 700°C, a pressure of 100 Torr, and monosilane of 1200 sccm. It was then removed from the apparatus and left in the air for 1 hour to form a third δ-doped layer of oxygen, and then placed in a low-pressure epitaxial growth apparatus, and a thin film (silicon) layer was grown for 120 seconds under the conditions of a temperature of 700°C, a pressure of 100 Torr, and monosilane of 1200 sccm. The substrate was then removed from the apparatus and placed in a heat treatment furnace where it was heat treated in an oxygen atmosphere at 600° C. for 5 minutes, forming a second δ-doped layer of oxygen on the surface side and obtaining a high mobility substrate.
[0058] For the high mobility substrate obtained here, the first δ-doped layer, the silicon layer, the third δ-doped layer, the thin film (silicon) layer, and the second δ-doped layer all had a thickness of 3 nm and a mobility of 100 cm 2 / V s.
[0059] We will now add some further consideration to the above results. In particular, regarding mobility, according to Non-Patent Document 3, the mobility of conventional two-dimensional material MoS2 is 50 to 100 cm 2 / V s, and the mobility of the high mobility substrates obtained in Examples 1 to 3 was 100 cm 2 / V·s, Examples 1 to 3 were able to achieve mobilities that were comparable to those of two-dimensional materials.
[0060] As described above, it has been demonstrated that the high mobility substrate and the manufacturing method of the high mobility substrate of the present invention are capable of realizing high mobility while uniformly forming the entire surface of a large-area substrate (substrate with a large diameter), and are therefore practical. Furthermore, by using a thin film layer that mimics such a two-dimensional material, it becomes possible to form a high-mobility channel material over the entire surface of a large-area substrate. Furthermore, it is inexpensive because it can be realized using common semiconductor materials such as silicon, without using expensive two-dimensional materials such as MoS2.
[0061] The present invention includes the following aspects. [1]: A semiconductor substrate; a first δ-doped layer on the semiconductor substrate, the first δ-doped layer having a band gap larger than that of the semiconductor substrate; a thin film of the same material as the semiconductor substrate on the first δ-doped layer; a second δ-doped layer on the thin film, the second δ-doped layer having a band gap larger than that of the semiconductor substrate; A high mobility substrate characterized in that said thin film is sandwiched between said first δ-doped layer and said second δ-doped layer. [2]: the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers; the semiconductor substrate and the thin film are silicon; The high mobility substrate according to the above-mentioned [1], wherein the thickness of the thin film is 2 nm or more and 3 nm or less. [3]: On a semiconductor substrate, forming a first δ-doped layer having a band gap larger than that of the semiconductor substrate; forming a thin film made of the same material as the semiconductor substrate thereon; forming a second δ-doped layer thereon, the second δ-doped layer having a band gap larger than that of the semiconductor substrate; A method for producing a high mobility substrate, comprising sandwiching the thin film between the first δ-doped layer and the second δ-doped layer. [4]: the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers; The semiconductor substrate and the thin film are made of silicon; The method for producing a high mobility substrate according to the above item [3], wherein the thin film has a thickness of 2 nm or more and 3 nm or less. [5]: When forming the thin film, the thin film is formed to a thickness that takes into account the fact that the thin film will become thinner due to oxidation, The method for producing a high mobility substrate according to the above [3] or [4], wherein the second δ-doped layer is formed by oxidizing the thin film. [6]: on said first δ-doped layer, After forming silicon to a thickness of 1 nm to 3 nm and then forming an oxygen delta-doped layer several times, The method for producing a high mobility substrate according to any one of the above [3] to [5], further comprising forming the thin film of silicon thereon to a thickness of 2 nm to 3 nm.
[0062] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0063] 1...high mobility substrate, 2...semiconductor substrate (support substrate), 3-1, 6-1...first δ-doped layer (first oxide layer), 3-2...second δ-doped layer (second oxide layer), 4, 5...thin film (silicon), 5-1...portion that is oxidized to form second δ-doped layer, 5-2...portion that is not oxidized and remains as thin film (silicon), 6-2, 6-3...δ-doped layer, 7-1, 7-2...silicon.
Claims
1. A semiconductor substrate; a first δ-doped layer on the semiconductor substrate, the first δ-doped layer having a band gap larger than that of the semiconductor substrate; a thin film of the same material as the semiconductor substrate on the first δ-doped layer; a second δ-doped layer on the thin film, the second δ-doped layer having a band gap larger than that of the semiconductor substrate; A high mobility substrate characterized in that said thin film is sandwiched between said first δ-doped layer and said second δ-doped layer.
2. the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers; the semiconductor substrate and the thin film are silicon; 2. The high mobility substrate according to claim 1, wherein the thin film has a thickness of 2 nm to 3 nm.
3. On a semiconductor substrate, forming a first δ-doped layer having a band gap larger than that of the semiconductor substrate; forming a thin film made of the same material as the semiconductor substrate thereon; forming a second δ-doped layer thereon, the second δ-doped layer having a band gap larger than that of the semiconductor substrate; A method for producing a high mobility substrate, comprising sandwiching the thin film between the first δ-doped layer and the second δ-doped layer.
4. the first δ-doped layer and the second δ-doped layer are oxygen δ-doped layers; The semiconductor substrate and the thin film are made of silicon; 4. The method for producing a high mobility substrate according to claim 3, wherein the thickness of the thin film is set to 2 nm or more and 3 nm or less.
5. When forming the thin film, the thin film is formed to a thickness that takes into account the fact that the thin film will become thinner due to oxidation, 4. The method for producing a high mobility substrate according to claim 3, wherein the second .delta.-doped layer is formed by oxidizing the thin film.
6. on said first δ-doped layer, After forming silicon to a thickness of 1 nm to 3 nm and then forming an oxygen δ-doped layer several times, 6. The method for producing a high mobility substrate according to claim 3, further comprising forming the thin silicon film thereon to a thickness of 2 nm to 3 nm.
Citation Information
Patent Citations
Method of manufacturing semiconductor wafer
JP2005005490A
Method of manufacturing semiconductor substrate
JP2009016637A
Method for manufacturing laminated wafer
JP2015177150A
Method for manufacturing SOI wafer having thin film SOI layer
JP2019087617A
Manufacturing method for epitaxial wafer, and epitaxial wafer
JP2021111696A