Optical adhesive sheet
The optical adhesive sheet with specific thickness, moisture permeability, and shear storage modulus addresses peeling issues in flexible display panels by providing stress relaxation and peeling suppression, enhancing device reliability.
Patent Information
- Application Number
- JP2023086538
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Optical adhesive sheets used in foldable and rollable display panels tend to peel off from adherends due to high tensile stress during deformation, leading to device malfunction.
An optical adhesive sheet with a thickness of 45 μm or more, moisture permeability of 400 g/m² in 24 hours at 40°C and 92% relative humidity, shear storage modulus of 70 kPa or less at -20°C, and a ratio of shear storage modulus G2 to G1 of 2.0 or less, providing stress relaxation and suppressing peeling.
The adhesive sheet effectively relieves stress and suppresses peeling, ensuring durability and reliability in flexible devices by preventing adhesive separation from adherends during bending and rolling.
Smart Images

Figure 2024169233000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical pressure-sensitive adhesive sheet. [Background technology]
[0002] A display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. In the manufacturing process of such a display panel, for example, an optically transparent adhesive sheet (optical adhesive sheet) is used to bond the elements included in the laminated structure.
[0003] Meanwhile, development of repeatedly foldable display panels for smartphones and tablet terminals is progressing. Specifically, a foldable display panel can be repeatedly deformed between a bent shape and a flat non-bent shape. In such a foldable display panel, each element in a laminated structure is made to be repeatedly foldable, and a thin optical adhesive sheet is used for bonding between such elements. An optical adhesive sheet for flexible devices such as a foldable display panel is described, for example, in the following Patent Document 1. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-111754 A Summary of the Invention [Problem to be solved by the invention]
[0005] Conventionally, at the folding portion of a foldable display panel, the optical adhesive sheet is easily peeled off from the element as the adherend. This is because, when the display panel is folded, a relatively large tensile stress is locally generated at the folding portion of the optical adhesive sheet. At the folding portion of the optical adhesive sheet, the greater the tensile stress in the shear direction, for example, on the element (adherend), the more likely peeling occurs between the optical adhesive sheet and the element. The occurrence of such peeling is undesirable, as it causes a malfunction of the device. There is a high demand for the optical adhesive sheet for the foldable display panel to be less likely to peel off from the element (adherend) when the display is bent.
[0006] On the other hand, as a flexible device, development of a rollable display panel is also progressing. A rollable display panel can be repeatedly deformed, for example, between a rolled shape after being entirely or partially rolled up and a flat shape after being entirely unrolled. In such a rollable display panel, each element in the laminated structure is made to be repeatedly deformable, and a thin optical adhesive sheet is used for bonding between such elements. When the rollable display panel is in a rolled shape, the optical adhesive sheet bonded to the rolled element continues to receive tensile stress from the element. Such an optical adhesive sheet is required to be highly unlikely to peel off from the element (adherend) when the display is in a rolled shape.
[0007] The present invention provides an optical adhesive sheet suitable for flexible device applications. [Means for solving the problem]
[0008] The present invention [1] is an optical pressure-sensitive adhesive sheet having a thickness of 45 μm or more and a moisture permeability of 400 g / m measured under conditions of 40° C. and a relative humidity of 92%. 2The optical adhesive sheet includes an optical adhesive sheet having a shear storage modulus G1 of 70 kPa or less at -20°C and a shear storage modulus G2 of -30°C, the ratio of the shear storage modulus G2 to the shear storage modulus G1 being 2.0 or less.
[0009] The present invention [2] includes the optical adhesive sheet according to the above [1], in which the shear storage modulus G2 is 120 kPa or less.
[0010] The present invention [3] includes the optical adhesive sheet according to the above [1] or [2], which has a relative dielectric constant of 4.0 or less at 100 kHz.
[0011] The present invention [4] includes an optical adhesive sheet described in any one of [1] to [3] above, in which the ratio of the dielectric constant after 24 hours in an environment of 40°C and a relative humidity of 92% to the dielectric constant at 100 kHz is 1.1 or less.
[0012] The present invention [5] includes an optical adhesive sheet according to any one of [1] to [4] above, which has an adhesive strength of 2.0 N / 10 mm or more in a peel test under conditions of 25°C, a peel angle of 180° and a tensile speed of 60 mm / min. Effect of the Invention
[0013] As described above, the optical adhesive sheet of the present invention has a shear storage modulus G1 of 70 kPa or less at -20°C, and the ratio of the shear storage modulus G2 at -30°C to the shear storage modulus G1 is 2.0 or less. Such a soft optical adhesive sheet is suitable for relaxing the stress generated in the optical adhesive sheet and the adherend when the adherend to which the adhesive sheet is attached is deformed (stress relaxation function). The stress relaxation in the optical adhesive sheet is suitable for suppressing peeling of the optical adhesive sheet from the adherend. The stress relaxation in the adherend is suitable for suppressing damage such as cracking of the adherend. In addition, as described above, the optical adhesive sheet of the present invention has a thickness of 45 μm or more, and a moisture permeability of 400 g / m2 measured under conditions of 40°C and a relative humidity of 92%. 224h or less. A thick optical adhesive sheet with a thickness of 45μm or more is suitable for ensuring the above-mentioned stress relaxation function. Moisture permeability 400g / m 2 An optical adhesive sheet with low moisture permeability of 24 hours or less is suitable for suppressing partial swelling of the ends of the optical adhesive sheet when the optical adhesive sheet is used to bond adherends (swelling occurs due to penetration of moisture into the ends). Suppressing partial swelling at the ends of the optical adhesive sheet is suitable for suppressing peeling of the ends from the adherend. In a thick optical adhesive sheet with a thickness of 45 μm or more, the increase in thickness of the ends of the adhesive sheet due to swelling is suppressed, suppressing peeling of the ends from the adherend. Such optical adhesive sheets are suitable for flexible device applications. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of an optical adhesive sheet of the present invention. [Diagram 2] Fig. 2 shows an example of a method for using the optical adhesive sheet of the present invention. Fig. 2A shows a step of attaching the optical adhesive sheet to a first adherend, Fig. 2B shows a step of joining the first adherend and the second adherend via the optical adhesive sheet, and Fig. 2C shows an aging step. [Diagram 3] FIG. 3A shows the test piece in a flat state during the repeated bending test, and FIG. 3B shows the test piece in a curved state during the repeated bending test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] As shown in Fig. 1, an adhesive sheet 10 as one embodiment of the optical adhesive sheet of the present invention has a sheet shape of a predetermined thickness and extends in a direction (plane direction) perpendicular to the thickness direction H. The adhesive sheet 10 has an adhesive surface 11 on one side in the thickness direction H, and an adhesive surface 12 on the other side in the thickness direction H. Fig. 1 exemplarily shows a state in which release liners L1, L2 are bonded to the adhesive surfaces 11, 12 of the adhesive sheet 10. The release liner L1 is disposed on the adhesive surface 11. The release liner L2 is disposed on the adhesive surface 12. The release liners L1, L2 are each peeled off at a predetermined timing when the adhesive sheet 10 is used.
[0016] The adhesive sheet 10 is an optically transparent adhesive sheet disposed at a light passing portion in a flexible device. An example of the flexible device is a flexible display panel. An example of the flexible display panel is a foldable display panel and a rollable display panel. The flexible display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. The adhesive sheet 10 is used, for example, in the manufacturing process of the flexible display panel to bond elements included in the laminated structure.
[0017] The pressure-sensitive adhesive sheet 10 has a shear storage modulus G1 of 70 kPa or less at -20°C, and a shear storage modulus G2 at -30°C, with the ratio of the shear storage modulus G2 to the shear storage modulus G1 being 2.0 or less. The pressure-sensitive adhesive sheet 10 also has a thickness of 45 μm or more. In addition, the pressure-sensitive adhesive sheet 10 has a moisture permeability of 400 g / m2 measured under conditions of 40°C and a relative humidity of 92%. 2 Less than 24 hours.
[0018] As described above, the adhesive sheet 10 has a shear storage modulus G1 of 70 kPa or less at -20°C, and the ratio of the shear storage modulus G2 at -30°C to the shear storage modulus G1 is 2.0 or less. Such a soft adhesive sheet 10 is suitable for relaxing the stress that occurs in the adhesive sheet 10 and the adherend when the adherend to which the adhesive sheet 10 is attached is deformed (stress relaxation function). The stress relaxation in the adhesive sheet 10 is suitable for preventing the adhesive sheet 10 from peeling off from the adherend. The stress relaxation in the adherend is suitable for preventing damage such as cracking of the adherend.
[0019] As described above, the pressure-sensitive adhesive sheet 10 has a thickness of 45 μm or more and a moisture permeability of 400 g / m2 measured under conditions of 40° C. and a relative humidity of 92%. 2 24 hours or less. A thick adhesive sheet 10 having a thickness of 45 μm or more is suitable for ensuring the above-mentioned stress relaxation function. Moisture permeability 400 g / m 2 The adhesive sheet 10 with low moisture permeability of 24 hours or less is suitable for suppressing partial swelling of the edge of the adhesive sheet 10 when the adhesive sheet 10 is used to bond adherends together (swelling occurs due to penetration of moisture into the edge). Suppressing partial swelling at the edge of the adhesive sheet 10 is suitable for suppressing peeling of the edge from the adherend. In a thick adhesive sheet 10 with a thickness of 45 μm or more, the increase in thickness of the edge of the adhesive sheet 10 caused by swelling is suppressed, suppressing peeling of the edge from the adherend.
[0020] The pressure-sensitive adhesive sheet 10 as described above is suitable for use in flexible devices that are repeatedly deformed.
[0021] The shear storage modulus G1 (-20°C) is preferably 60 kPa or less, more preferably 50 kPa or less, and even more preferably 45 kPa or less, from the viewpoint of stress relaxation at the deformed portion when the pressure-sensitive adhesive sheet 10 is deformed (bent, curved, etc.). The shear storage modulus G1 is preferably more than 40 kPa, more preferably 45 kPa or more, from the viewpoint of ensuring good adhesion and handling properties in the pressure-sensitive adhesive sheet 10. The shear storage modulus G1 of the pressure-sensitive adhesive sheet 10 is determined by dynamic viscoelasticity measurement described later in the examples (the same applies to the shear storage moduli G2 to G4 described later). Methods for adjusting the shear storage modulus G1 of the pressure-sensitive adhesive sheet 10 include, for example, selection of the type of base polymer in the pressure-sensitive adhesive sheet 10, adjustment of the molecular weight, and adjustment of the blending amount, and selection of the type of crosslinking agent and adjustment of the blending amount (the same applies to the shear storage moduli G2 to G4 described later).
[0022] The shear storage modulus G2 (-30°C) is preferably 120 kPa or less, more preferably 100 kPa or less, even more preferably 80 kPa or less, and particularly preferably 70 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the adhesive sheet 10. From the viewpoint of ensuring good adhesiveness and handleability in the adhesive sheet 10, the shear storage modulus G2 is preferably 45 kPa or more, more preferably 50 kPa or more, and even more preferably 55 kPa or more.
[0023] The ratio (G2 / G1) of the shear storage modulus G2 to the shear storage modulus G1 is preferably 1.8 or less, more preferably 1.7 or less, and even more preferably 1.6 or less, from the viewpoint of ensuring a stable stress relaxation function of the pressure-sensitive adhesive sheet 10 in the low temperature range. The ratio (G2 / G1) is, for example, 0.9 or more, 1.0 or more, or 1.1 or more.
[0024] The shear storage modulus G3 of the pressure-sensitive adhesive sheet 10 at 25°C is preferably 50 kPa or less, more preferably 40 kPa or less, even more preferably 30 kPa or less, and particularly preferably 23 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the pressure-sensitive adhesive sheet 10. From the viewpoint of ensuring good adhesiveness and handleability in the pressure-sensitive adhesive sheet 10, the shear storage modulus G3 is preferably more than 18 kPa, more preferably 19 kPa or more, and even more preferably 20 kPa or more.
[0025] The shear storage modulus G4 of the pressure-sensitive adhesive sheet 10 at 60°C is preferably 50 kPa or less, more preferably 40 kPa or less, even more preferably 30 kPa or less, and particularly preferably 23 kPa or less, from the viewpoint of the above-mentioned stress relaxation in the pressure-sensitive adhesive sheet 10. From the viewpoint of ensuring good adhesion, cohesive strength, and handleability in the pressure-sensitive adhesive sheet 10, the shear storage modulus G4 is preferably 13 kPa or more, more preferably 15 kPa or more, and even more preferably 17 kPa or more.
[0026] The thickness of the adhesive sheet 10 is preferably 48 μm or more, and more preferably 50 μm or more, from the viewpoint of ensuring a good stress relaxation function in the adhesive sheet 10. The thickness of the adhesive sheet 10 is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 70 μm or less, from the viewpoint of thinning the flexible device.
[0027] The moisture permeability of the pressure-sensitive adhesive sheet 10 is preferably 395 g / m from the viewpoint of suppressing swelling of the pressure-sensitive adhesive sheet 10 in a humid environment. 2 24h or less, preferably 390g / m 2 24h or less, more preferably 380g / m 2·24h or less. The moisture permeability of the adhesive sheet 10 means the moisture permeability when the thickness of the adhesive sheet 10 is 50 μm. Methods for adjusting the moisture permeability of the adhesive sheet 10 include, for example, selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, and adjusting the amount of the base polymer. Selection of the type of base polymer includes selection of the type of side chain of the base polymer and adjustment of the amount of the side chain. Selection of the type of side chain of the base polymer includes adjustment of the length of the alkyl portion in the side chain, and selection of the type of functional group contained in the side chain and adjustment of the amount of the side chain. Methods for adjusting the moisture permeability of the adhesive sheet 10 include selection of the type of additive other than the base polymer and adjustment of the amount of the additive. The method for measuring the moisture permeability of the adhesive sheet 10 is as described below in relation to the examples.
[0028] The dielectric constant D1 of the adhesive sheet 10 at 100 kHz (dielectric constant before humidification described later) is preferably 4.0 or less, preferably 3.8 or less, and more preferably 3.6 or less, from the viewpoint of realizing good sensing sensitivity in the touch sensor equipped in the display panel. The dielectric constant D1 is, for example, 3.0 or more, 3.3 or more, or 3.5 or more. The method of adjusting the dielectric constant D1 includes, for example, selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, and adjusting the blending amount. The selection of the type of base polymer includes selecting the type of side chain of the base polymer and adjusting the amount. The selection of the type of side chain of the base polymer includes adjusting the length of the alkyl part in the side chain, and selecting the type of functional group contained in the side chain and adjusting the amount. The method of adjusting the dielectric constant D1 also includes selecting the type of additive other than the base polymer and adjusting the blending amount (the same applies to the dielectric constant D2 described later). The measurement method of the dielectric constant is specifically as described later in the examples.
[0029] The dielectric constant D2 of the adhesive sheet 10 after 24 hours in an environment of 40°C and 92% relative humidity (after humidification) is preferably 4.0 or less, preferably 3.8 or less, and more preferably 3.6 or less, from the viewpoint of realizing good sensing sensitivity in a humidified environment in a touch sensor provided in a display panel. The dielectric constant D2 is, for example, 2.8 or more, 3.0 or more, or 3.2 or more.
[0030] From the viewpoint of obtaining stable dielectric properties in the adhesive sheet 10, the ratio of the relative dielectric constant D2 to the relative dielectric constant D1 (D2 / D1) is preferably 0.80 or more, more preferably 0.85 or more, and is preferably 1.1 or less, more preferably 1.05 or less.
[0031] The adhesive strength F1 of the adhesive sheet 10 in a peel test (first peel test) under the conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 2.0 N / 10 mm or more, more preferably 2.2 N / 10 mm or more, from the viewpoint of suppressing peeling of the adhesive sheet 10 from the adherend in the normal temperature region. The adhesive strength F1 means the adhesive strength to a polyimide (PI) film at 25°C. The measurement method of the adhesive strength F1 is specifically as described later in the Examples. The method of adjusting the adhesive strength F1 includes, for example, selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, and adjusting the blending amount. The selection of the type of base polymer includes adjusting the composition of the monomer that forms the base polymer. The method of adjusting the adhesive strength F1 also includes selecting the type of components other than the base polymer in the adhesive sheet 10, and adjusting the blending amount of the components. The components include a crosslinking agent, a silane coupling agent, and an oligomer. The above-mentioned adhesive strength adjustment method is also applicable to the adhesive strength F2 described later.
[0032] The adhesive strength F2 of the adhesive sheet 10 in a peel test (second peel test) under conditions of 65°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 1.3 N / 10 mm or more, preferably 1.5 N / 10 mm or more, and more preferably 1.7 N / 10 mm or more, from the viewpoint of suppressing peeling of the adhesive sheet 10 from the adherend in a high temperature region. The adhesive strength F2 means the adhesive strength to a PI film at 65°C. The method for measuring the adhesive strength F2 is specifically as described below in relation to the examples.
[0033] The adhesive sheet 10 is a sheet-like pressure-sensitive adhesive formed from an adhesive composition. The adhesive sheet 10 (adhesive composition) contains at least a base polymer.
[0034] The base polymer is an adhesive component that imparts adhesiveness to the adhesive sheet 10. Examples of the base polymer include acrylic polymers, silicone polymers, polyester polymers, polyurethane polymers, polyamide polymers, polyvinyl ether polymers, vinyl acetate / vinyl chloride copolymers, modified polyolefin polymers, epoxy polymers, fluoropolymers, and rubber polymers. The base polymers may be used alone or in combination of two or more kinds. From the viewpoint of ensuring good transparency and adhesiveness in the adhesive sheet 10, the base polymer is preferably an acrylic polymer.
[0035] An acrylic polymer is a copolymer of monomer components containing 50% by mass or more of (meth)acrylic acid ester. "(Meth)acrylic" means acrylic and / or methacrylic.
[0036] As the (meth)acrylic acid ester, preferably, a (meth)acrylic acid alkyl ester is used, and more preferably, a (meth)acrylic acid alkyl ester in which the alkyl group has a carbon number of 1 to 20. The (meth)acrylic acid alkyl ester may have a linear or branched alkyl group, or may have an alicyclic alkyl group.
[0037] Examples of (meth)acrylic acid alkyl esters having a linear or branched alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, and isooctyl (meth)acrylate. , nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (i.e., lauryl (meth)acrylate), isotridecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, and nonadecyl (meth)acrylate.
[0038] Examples of the (meth)acrylic acid alkyl ester having an alicyclic alkyl group include (meth)acrylic acid cycloalkyl ester, (meth)acrylic acid ester having a bicyclic aliphatic hydrocarbon ring, and (meth)acrylic acid ester having a tricyclic or higher aliphatic hydrocarbon ring. Examples of the (meth)acrylic acid cycloalkyl ester include (meth)acrylic acid cyclopentyl, (meth)acrylic acid cyclohexyl, (meth)acrylic acid cycloheptyl, and (meth)acrylic acid cyclooctyl. Examples of the (meth)acrylic acid ester having a bicyclic aliphatic hydrocarbon ring include (meth)acrylic acid isobornyl. Examples of (meth)acrylic acid esters having three or more aliphatic hydrocarbon rings include dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.
[0039] As the (meth)acrylic acid alkyl ester, from the viewpoint of balancing the softness and adhesive strength required for an adhesive sheet for flexible device applications with the low moisture permeability of the adhesive sheet in the adhesive sheet 10, preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group with 6 to 14 carbon atoms is used, more preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms is used, and even more preferably at least two selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms are used. As the (meth)acrylic acid alkyl esters having an alkyl group with 6 to 14 carbon atoms, 2-ethylhexyl acrylate (2EHA), n-octyl acrylate (NOAA), isononyl acrylate (INAA), and lauryl acrylate (LA) are preferred.
[0040] The proportion of the (meth)acrylic acid alkyl ester in the monomer component is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 97% by mass or more, from the viewpoint of appropriately exhibiting softness, adhesive strength, and low moisture permeability in the pressure-sensitive adhesive sheet 10. The proportion is, for example, 99.9% by mass or less, 99.5% by mass or less, or 99% by mass or less. When a first (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms is used in combination with another second (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms, the proportion of the first (meth)acrylic acid alkyl ester in the monomer component is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and also preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% by mass or less. The proportion of the second (meth)acrylic acid alkyl ester in the monomer component is preferably 20 mass% or more, more preferably 30 mass% or more, even more preferably 35 mass% or more, and is preferably 80 mass% or less, more preferably 70 mass% or less, even more preferably 65 mass% or less.
[0041] The monomer component may include a copolymerizable monomer that is copolymerizable with the (meth)acrylic acid alkyl ester. The copolymerizable monomer may include, for example, a monomer having a polar group. The polar group-containing monomer may include, for example, a hydroxy group-containing monomer, a monomer having a nitrogen atom-containing ring, and a carboxy group-containing monomer. The polar group-containing monomer is useful for modifying the acrylic polymer, such as introducing a crosslinking point into the acrylic polymer and ensuring the cohesive force of the acrylic polymer.
[0042] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. As the hydroxyl group-containing monomer, at least one selected from the group consisting of 2-hydroxyethyl acrylate (2HEA) and 4-hydroxybutyl acrylate (4HBA) is preferably used.
[0043] The proportion of the hydroxy group-containing monomer in the monomer components is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring cohesive strength in the pressure-sensitive adhesive sheet 10. From the viewpoint of adjusting the polarity of the acrylic polymer (related to the compatibility between the acrylic polymer and various additive components in the pressure-sensitive adhesive sheet 10), the proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.
[0044] Examples of monomers having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, and N-vinylisothiazole.
[0045] When a monomer having a nitrogen atom-containing ring is used, the proportion of the monomer having a nitrogen atom-containing ring in the monomer components is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more, from the viewpoints of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10 and ensuring the adhesive strength to the adherend in the pressure-sensitive adhesive sheet 10. This proportion is preferably 20% by mass or less, more preferably 10% by mass or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and adjusting the polarity of the acrylic polymer (related to the compatibility of various additive components in the pressure-sensitive adhesive sheet 10 with the acrylic polymer).
[0046] Examples of carboxy group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.
[0047] When a carboxyl group-containing monomer is used, the proportion of the carboxyl group-containing monomer in the monomer components is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.8 mass% or more, from the viewpoints of introducing a crosslinked structure into the acrylic polymer, ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10, and ensuring the adhesive strength to the adherend in the pressure-sensitive adhesive sheet 10. The proportion is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 3 mass% or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and avoiding the risk of corrosion of the adherend by acid.
[0048] The proportion of the polar group-containing monomer in the monomer component (when multiple polar group-containing monomers are included, the proportion of the total amount of the multiple polar group-containing monomers) is preferably 7% by mass or less, more preferably 5% by mass or less, even more preferably 3.5% by mass or less, and particularly preferably 3% by mass or less, from the viewpoint of lowering the glass transition temperature of the base polymer and ensuring the softness of the adhesive sheet 10. The proportion is, for example, 0.1% by mass or more, 0.5% by mass or more, or 0.8% by mass or more.
[0049] The monomer component may contain other copolymerizable monomers. Examples of the other copolymerizable monomers include acid anhydride monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, alkoxy group-containing monomers, and aromatic vinyl compounds. These other copolymerizable monomers may be used alone or in combination of two or more.
[0050] The monomer components forming the base polymer preferably include an alkyl (meth)acrylate ester and a polar group-containing monomer, and more preferably include an alkyl (meth)acrylate ester having an alkyl group with 8 to 12 carbon atoms and a hydroxyl group-containing monomer. In this case, the ratio of the hydroxyl group-containing monomer in the total amount of the alkyl (meth)acrylate ester and the hydroxyl group-containing monomer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.8% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring the cohesive force of the pressure-sensitive adhesive sheet 10. From the viewpoint of lowering the glass transition temperature of the base polymer and ensuring the softness of the pressure-sensitive adhesive sheet 10, the ratio is preferably 5% by mass or less, more preferably 3.5% by mass or less, even more preferably 3% by mass or less, even more preferably 2% by mass or less, and even more preferably 1.5% by mass or less.
[0051] The base polymer preferably has a crosslinked structure. Examples of methods for introducing a crosslinked structure into the base polymer include the following first and second methods. In the first method, a base polymer having a functional group capable of reacting with a crosslinking agent and a crosslinking agent are blended into an adhesive composition, and the base polymer and the crosslinking agent are reacted in an adhesive sheet. In the second method, a polyfunctional compound is included as a crosslinking agent in the monomer components forming the base polymer, and a base polymer having a branched structure (crosslinked structure) introduced into the polymer chain is formed by polymerization of the monomer components. These methods may be used in combination.
[0052] The crosslinking agent used in the first method includes, for example, a compound that reacts with functional groups (such as hydroxyl groups and carboxyl groups) contained in the base polymer. Examples of such crosslinking agents include isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, and carbodiimide crosslinking agents. The crosslinking agents in the first method may be used alone or in combination of two or more. As the crosslinking agent in the first method, an isocyanate crosslinking agent is preferably used because it has high reactivity with hydroxyl groups and carboxyl groups in the base polymer and is easy to introduce a crosslinked structure.
[0053] Examples of isocyanate crosslinking agents include tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, tetramethylxylylene diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, and polymethylene polyphenylisocyanate. In addition, examples of isocyanate crosslinking agents include derivatives of these isocyanates. Examples of the isocyanate derivatives include isocyanurate modified products and polyol modified products. Commercially available isocyanate crosslinking agents include, for example, Coronate L (trimethylolpropane adduct of tolylene diisocyanate, manufactured by Tosoh), Coronate HL (trimethylolpropane adduct of hexamethylene diisocyanate, manufactured by Tosoh), Coronate HX (isocyanurate of hexamethylene diisocyanate, manufactured by Tosoh), Takenate D110N (trimethylolpropane adduct of xylylene diisocyanate, manufactured by Mitsui Chemicals), and Takenate 600 (1,3-bis(isocyanatomethyl)cyclohexane, manufactured by Mitsui Chemicals).
[0054] Peroxide crosslinking agents include dibenzoyl peroxide, di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, and t-butylperoxypivalate.
[0055] Epoxy crosslinkers include bisphenol A, epichlorohydrin type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidyl aniline, diamine glycidyl amine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.
[0056] The amount of the crosslinking agent in the first method is, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and more preferably 0.1 parts by mass or more, per 100 parts by mass of the base polymer, from the viewpoint of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10. From the viewpoint of ensuring good tackiness in the pressure-sensitive adhesive sheet 10, the amount of the crosslinking agent in the first method is, for example, 5 parts by mass or less, preferably 1 part by mass or less, and more preferably 0.2 parts by mass or less, per 100 parts by mass of the base polymer.
[0057] In the second method, the monomer components (including the polyfunctional compound and the monofunctional monomer for introducing a crosslinked structure) may be polymerized at once or in multiple stages. In the multi-stage polymerization method, first, the monofunctional monomer for forming the base polymer is polymerized (preliminary polymerization), thereby preparing a prepolymer composition containing a partial polymer (a mixture of a polymer with a low degree of polymerization and an unreacted monofunctional monomer). Next, a polyfunctional compound is added as a crosslinking agent to the prepolymer composition, and then a polymerization reaction is allowed to proceed in a reaction system containing the partial polymer and the polyfunctional compound (main polymerization).
[0058] Examples of the polyfunctional compound include polyfunctional monomers and polyfunctional oligomers that contain two or more ethylenically unsaturated double bonds in one molecule. Examples of the polyfunctional monomer include polyfunctional (meth)acrylates.
[0059] Examples of the polyfunctional (meth)acrylate include difunctional (meth)acrylate, trifunctional (meth)acrylate, and tetrafunctional or higher polyfunctional (meth)acrylate.
[0060] Examples of bifunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, glycerin di(meth)acrylate, ethoxylated bisphenol A diacrylate (BPAEODE), and neopentyl glycol di(meth)acrylate.
[0061] Examples of trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(acryloyloxyethyl)isocyanurate.
[0062] Examples of tetrafunctional or higher polyfunctional (meth)acrylates include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0063] Examples of polyfunctional oligomers include urethane (meth)acrylate oligomers, polyester (meth)acrylate oligomers, polyether (meth)acrylate oligomers, polyol (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate.
[0064] The polyfunctional compound as the crosslinking agent in the second method may be used alone or in combination of two or more kinds. As the polyfunctional compound, a polyfunctional monomer is preferably used, and more preferably at least one selected from the group consisting of dipentaerythritol hexaacrylate (DPHA), 1,6-hexanediol diacrylate (HDDA), and trimethylolpropane triacrylate (TMPTA) is used.
[0065] The amount of the polyfunctional compound as a crosslinking agent in the monomer components is preferably 0.02 parts by mass or more, more preferably 0.04 parts by mass or more, and even more preferably 0.06 parts by mass or more, per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10. The amount of the polyfunctional compound is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring good tackiness in the pressure-sensitive adhesive sheet 10.
[0066] The acrylic polymer (base polymer) can be formed by polymerizing the above-mentioned monomer components. Examples of the polymerization method include solution polymerization, emulsion polymerization, and solvent-free photopolymerization (e.g., ultraviolet polymerization). For example, ethyl acetate and toluene are used as the solvent for solution polymerization. In the polymerization, a chain transfer agent may be used. For example, a thermal polymerization initiator and a photopolymerization initiator are used as the polymerization initiator. The polymerization initiator may be used alone or in combination of two or more kinds. The amount of the polymerization initiator used is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.07 parts by mass or more, and is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less, per 100 parts by mass of the monomer components.
[0067] Examples of the thermal polymerization initiator include azo polymerization initiators and peroxide polymerization initiators. Examples of the azo polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate)dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, and 2,2'-azobis(2-amidinopropane)dihydrochloride. Examples of the peroxide polymerization initiator include dibenzoyl peroxide, t-butyl permaleate, and lauroyl peroxide.
[0068] Examples of the photopolymerization initiator include a radical photopolymerization initiator, a cationic photopolymerization initiator, and an anionic photopolymerization initiator.
[0069] Examples of the radical photopolymerization initiator include an acylphosphine oxide photopolymerization initiator, a benzoin ether photopolymerization initiator, and an acetophenone photopolymerization initiator.
[0070] Examples of the acylphosphine oxide photopolymerization initiator include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. Examples of the benzoin ether photopolymerization initiator include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone.
[0071] The weight average molecular weight of the base polymer is preferably 100,000 or more, more preferably 300,000 or more, and even more preferably 500,000 or more, from the viewpoint of ensuring the cohesive force in the pressure-sensitive adhesive sheet 10. The weight average molecular weight of the base polymer is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.
[0072] The glass transition temperature (Tg) of the base polymer is preferably 0° C. or lower, more preferably −10° C. or lower, and even more preferably −20° C. or lower. The glass transition temperature is, for example, −80° C. or higher.
[0073] The glass transition temperature (Tg) of the base polymer can be determined by the following Fox formula (theoretical value). The Fox formula is a relational expression between the glass transition temperature Tg of a polymer and the glass transition temperature Tgi of a homopolymer of a monomer constituting the polymer. In the following Fox formula, Tg represents the glass transition temperature (°C) of a polymer, Wi represents the weight fraction of a monomer i constituting the polymer, and Tgi represents the glass transition temperature (°C) of a homopolymer formed from the monomer i. The glass transition temperature of a homopolymer can be determined by a literature value. For example, the glass transition temperatures of various homopolymers are listed in "Polymer Handbook" (4th edition, John Wiley & Sons, Inc., 1999). On the other hand, the glass transition temperature of a homopolymer of a monomer can also be determined by a method specifically described in JP-A-2007-51271.
[0074] Fox formula 1 / (273+Tg)=Σ[Wi / (273+Tgi)]
[0075] The pressure-sensitive adhesive composition may contain a silane coupling agent. The content of the silane coupling agent in the pressure-sensitive adhesive composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, based on 100 parts by mass of the base polymer. The content is preferably 5 parts by mass or less, more preferably 3 parts by mass or less.
[0076] The adhesive composition may contain other components as necessary. Examples of the other components include solvents, tackifiers, plasticizers, softeners, antioxidants, fillers, colorants, UV absorbers, surfactants, and antistatic agents. Examples of the solvent include polymerization solvents that are used as necessary during polymerization of acrylic polymers, and solvents that are added to the polymerization reaction solution after polymerization. Examples of the solvent include ethyl acetate and toluene.
[0077] The pressure-sensitive adhesive sheet 10 can be produced, for example, by applying the above-mentioned pressure-sensitive adhesive composition onto a release liner L1 (first release liner) to form a coating film, and then drying the coating film. The pressure-sensitive adhesive sheet 10 may also be produced by applying the above-mentioned pressure-sensitive adhesive composition onto a release liner L1 (first release liner) to form a coating film, laminating a release liner L2 (second release liner) onto the coating film, and then drying the coating film between the release liners.
[0078] The release liner L1 may be, for example, a flexible plastic film. Examples of the plastic film include polyester films such as polyethylene terephthalate films, polyethylene films, and polypropylene films. The thickness of the release liner L1 is, for example, 3 μm or more and, for example, 200 μm or less. The surface of the release liner L1 is preferably subjected to a release treatment.
[0079] Examples of the method for applying the pressure-sensitive adhesive composition include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating. The drying temperature for the coating film is, for example, 50° C. to 200° C. The drying time is, for example, 5 seconds to 20 minutes.
[0080] The release liner L2 is preferably a flexible plastic film whose surface has been subjected to a release treatment. As the release liner L2, the plastic films described above with respect to the release liner L1 can be used.
[0081] In this manner, adhesive sheet 10 can be manufactured in which adhesive surfaces 11, 12 are covered and protected by release liners L1, L2.
[0082] The haze of the pressure-sensitive adhesive sheet 10 is preferably 3% or less, more preferably 2% or less, and more preferably 1% or less. The haze of the pressure-sensitive adhesive sheet 10 can be measured using a haze meter in accordance with JIS K7136 (2000). Examples of haze meters include "NDH2000" manufactured by Nippon Denshoku Industries Co., Ltd. and "HM-150 type" manufactured by Murakami Color Research Laboratory Co., Ltd.
[0083] The total light transmittance of the pressure-sensitive adhesive sheet 10 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. The total light transmittance of the pressure-sensitive adhesive sheet 10 is, for example, 100% or less. The total light transmittance of the pressure-sensitive adhesive sheet 10 can be measured in accordance with JIS K 7375 (2008).
[0084] 2A to 2C show an example of a method of using the adhesive sheet 10. FIG.
[0085] In this method, first, as shown in FIG. 2A, the adhesive sheet 10 is attached to one surface in the thickness direction H of a first member 21 (adherend). The first member 21 is, for example, one element in a laminated structure of a flexible display panel. Examples of the element include a pixel panel, a polarizing film, a touch panel, and a cover film (the same applies to the second member 22 described below). Through this process, the adhesive sheet 10 for bonding to other members is provided on the first member 21.
[0086] 2B, one surface side in the thickness direction H of the first member 21 is joined to the other surface side in the thickness direction H of the second member 22 via the adhesive sheet 10 on the first member 21. The second member 22 is, for example, another element in the laminated structure of the flexible display panel.
[0087] Next, as shown in FIG. 2C, the adhesive sheet 10 between the first member 21 and the second member 22 is aged. Aging enhances the bonding strength between the adhesive sheet 10 and the members 21, 22. The aging temperature is, for example, 20° C. to 160° C. The aging time is, for example, 1 minute to 21 days. When the aging is performed by autoclaving (heating and pressurizing), the temperature is, for example, 30° C. to 80° C., the pressure is, for example, 0.1 to 0.8 MPa, and the treatment time is, for example, 15 minutes or longer. EXAMPLES
[0088] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".
[0089] Example 1 Preparation of Prepolymer Composition In a flask, 0.05 parts by mass of 2,2-dimethoxy-1,2-diphenylethan-1-one (trade name "Omnirad651", manufactured by IGM Resins) as a first photopolymerization initiator and 0.05 parts by mass of 1-hydroxycyclohexyl phenyl ketone (trade name "Omnirad184", manufactured by IGM Resins) as a second photopolymerization initiator were added to a monomer mixture containing 60 parts by mass of 2-ethylhexyl acrylate (2EHA), 39 parts by mass of lauryl acrylate (LA), and 1 part by mass of 4-hydroxybutyl acrylate (4HBA) in a flask. The mixture was then irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a first prepolymer composition (containing monomer components that had not undergone a polymerization reaction) with a polymerization rate of approximately 10%.
[0090] Preparation of Pressure-Sensitive Adhesive Composition A first adhesive composition was obtained by mixing 100 parts by mass of the first prepolymer composition, 0.06 parts by mass of dipentaerythritol hexaacrylate (DPHA) as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.).
[0091] <Formation of Pressure-Sensitive Adhesive Layer> A first adhesive composition was applied onto the release-treated surface of a first release liner (product name "Diafoil MRF#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side to form a coating film. Next, the release-treated surface of a second release liner (product name "Diafoil MRE#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side was attached onto the coating film on the first release liner. Next, the coating film between the release liners was irradiated with ultraviolet light to photocure the coating film and form an adhesive layer (thickness 50 μm). For ultraviolet light irradiation, a black light was used as the irradiation light source, and the irradiation intensity was 5 mW / cm. 2 It was decided.
[0092] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) with double-sided release liners was prepared for Example 1. The composition of the pressure-sensitive adhesive sheet for Example 1 is shown in Table 1 in units of "parts by mass" (the same applies to the examples and comparative examples described below).
[0093] Example 2 An adhesive sheet of Example 2 with double-sided release liner was produced in the same manner as the adhesive sheet of Example 1, except that in preparing the prepolymer composition, the amount of 2EHA was 51 parts by mass and the amount of LA was 48 parts by mass.
[0094] Example 3 An adhesive sheet of Example 3 with double-sided release liner was produced in the same manner as the adhesive sheet of Example 1, except that in preparing the prepolymer composition, the amount of 2EHA was 58 parts by mass and the amount of 4HBA was 3 parts by mass.
[0095] Example 4 First, 0.05 parts by mass of a first photopolymerization initiator (Omnirad651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad184) were added to a monomer mixture containing 29 parts by mass of n-octyl acrylate (NOAA), 70 parts by mass of 2EHA, and 1 part by mass of 4HBA in a flask, and then the mixture was irradiated with ultraviolet light under a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a second prepolymer composition with a polymerization rate of approximately 10%.
[0096] Next, 100 parts by mass of the second prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a second pressure-sensitive adhesive composition.
[0097] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in the formation of the adhesive layer in Example 1, except that the second adhesive composition was used instead of the first adhesive composition.
[0098] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) with double-sided release liners of Example 4 was produced.
[0099] Example 5 First, 0.05 parts by mass of a first photopolymerization initiator (Omnirad651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad184) were added to a monomer mixture containing 70 parts by mass of isononyl acrylate (INAA), 29 parts by mass of LA, and 1 part by mass of 4HBA in a flask, and then the mixture was irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a third prepolymer composition with a polymerization rate of approximately 10%.
[0100] Next, 100 parts by mass of the third prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a third pressure-sensitive adhesive composition.
[0101] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in the formation of the adhesive layer in Example 1, except that the third adhesive composition was used instead of the first adhesive composition.
[0102] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) with double-sided release liners of Example 5 was produced.
[0103] Comparative Example 1 A pressure-sensitive adhesive sheet of Comparative Example 1 with a double-sided release liner was prepared in the same manner as the pressure-sensitive adhesive sheet of Example 1, except for the following: In preparing the prepolymer composition, 56 parts by mass of 2EHA, 34 parts by mass of LA, 7 parts by mass of 4HBA, and 2 parts by mass of N-vinyl-2-pyrrolidone (NVP) were blended. In preparing the pressure-sensitive adhesive composition, 1 part by mass of the following acrylic oligomer was further blended.
[0104] Preparation of Oligomers First, in a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, a mixture containing 60 parts by mass of dicyclopentanyl methacrylate (DCPMA), 40 parts by mass of methyl methacrylate (MMA), 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a solvent was stirred under a nitrogen atmosphere at 70°C for 1 hour. Next, 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was reacted under a nitrogen atmosphere at 70°C for 1 hour and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove toluene, the chain transfer agent, and unreacted monomers. As a result, an acrylic oligomer (solid form) was obtained as a hydrophobic oligomer without a polar group. The weight average molecular weight of this acrylic oligomer was 5100.
[0105] Comparative Example 2 An adhesive sheet of Comparative Example 2 with double-sided release liner was produced in the same manner as the adhesive sheet of Example 5, except that in preparing the prepolymer composition, the amount of INAA was 50 parts by mass and the amount of LA was 49 parts by mass.
[0106] <Moisture permeability> The moisture permeability was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 and 2. Specifically, the results are as follows.
[0107] First, the pressure-sensitive adhesive sheet with double-sided release liners was left to stand for 3 days in an atmosphere with a temperature of 23°C and a relative humidity of 55%. This adjusted the condition of the pressure-sensitive adhesive sheet. Next, one of the release liners was peeled off from the pressure-sensitive adhesive sheet, and the exposed surface was then covered with a 25 μm-thick triacetyl cellulose (TAC) film (moisture permeability: 1070 g / m 2 The other release liner was then peeled off from the adhesive sheet on the TAC film. This gave a sample film for measuring moisture permeability.
[0108] Next, the moisture permeability in the thickness direction of the adhesive sheet was measured in accordance with the moisture permeability test (cup method) of JIS Z0208. Specifically, first, a predetermined amount of calcium chloride weighed in advance was placed in a test cup (an aluminum cup with a circular opening of 30 mm in diameter, used in the cup method of JIS Z0208), and the opening of the cup was blocked with a sample film. The area of the sample film blocking the opening of the cup corresponds to the area of a circle with a diameter of 30 mm. Next, the cup with the sample film was placed in a constant temperature and humidity chamber at a temperature of 40°C and a relative humidity of 92%, and left for 24 hours. Next, the calcium chloride taken out of the cup was weighed. The increased mass (g) of calcium chloride was multiplied by the area (m 2 The value was divided by the moisture permeability (g / m 2The moisture permeability obtained in this manner is that of the pressure-sensitive adhesive sheet with the TAC film, but since the moisture permeability of the TAC film is significantly greater than that of the pressure-sensitive adhesive sheet, the moisture permeability of the sample film was regarded as that of the pressure-sensitive adhesive sheet.
[0109] <Dielectric constant> The relative dielectric constant was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 and 2. Specifically, the results are as follows.
[0110] First, a measurement sample was prepared by sandwiching the adhesive sheet between copper foil and an electrode. Next, the dielectric constant of the measurement sample was measured at a frequency of 100 kHz under the following conditions in accordance with JIS K6911 using Agilent Technologies' Precision Impedance Analyzer 4294A (first dielectric constant measurement). The measurement results are shown in Table 1 as the dielectric constant D1 of the adhesive sheet at 100 kHz.
[0111] [Conditions for measuring dielectric constant] Electrode configuration: Aluminum plate with a diameter of 12.1 mm and a thickness of 0.5 mm Counter electrode: 3oz copper plate Measurement environment: Temperature 25℃, relative humidity 50%
[0112] In addition, the adhesive sheet was subjected to a humidification treatment, and then the dielectric constant of the adhesive sheet was measured (second dielectric constant measurement). In the humidification treatment, the adhesive sheet was stored for 24 hours in an environment of 40°C and a relative humidity of 92%. The method for measuring the second dielectric constant was the same as the above-mentioned first dielectric constant measurement method. The measurement results are shown in Table 1 as the dielectric constant D2 at 100 kHz after humidification of the adhesive sheet. The ratio (D2 / D1) of the dielectric constant D2 to the above-mentioned dielectric constant D1 is also shown in Table 1.
[0113] <Shear storage modulus> For each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 and 2, the dynamic viscoelasticity was measured.
[0114] For each adhesive sheet, the required number of samples for measurement were prepared. Specifically, first, a plurality of pieces of adhesive sheet cut out from the adhesive sheet were pasted together to prepare a sample sheet with a thickness of about 1.5 mm. Next, this sheet was punched out to obtain cylindrical pellets (diameter 7.9 mm) as the measurement samples.
[0115] Then, the measurement sample was fixed to a parallel plate jig with a diameter of 7.9 mm using a dynamic viscoelasticity measuring device (name: "Discovery Hybrid Reometeter-2 (DHR-2)", manufactured by TA Instruments), and then dynamic viscoelasticity measurement was performed. In this measurement, the measurement mode was shear mode, the measurement temperature range was -50°C to 150°C, the heating rate was 5°C / min, and the frequency was 1Hz. From the measurement results, the shear storage modulus at a predetermined temperature (-30°C, -20°C, 25°C, 60°C) was read. Table 1 shows the shear storage modulus G1 (kPa) at -20°C, the shear storage modulus G2 (kPa) at -30°C, the shear storage modulus G3 (kPa) at 25°C, and the shear storage modulus G4 (kPa) at 60°C. Table 1 also shows the ratio of the shear storage modulus G2 to the shear storage modulus G1 (G2 / G1).
[0116] <180° peel test> For each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 and 2, the adhesive strength to an adherend was examined by a 180° peel test.
[0117] Specifically, first, a required number of measurement samples were prepared for each adhesive sheet. In preparing the measurement samples, first, the first release liner was peeled off from the adhesive sheet, and the exposed surface was attached to a polyethylene terephthalate (PET) film (product name "Lumirror S10", thickness 50 μm, manufactured by Toray) whose surface had been plasma-treated to obtain a laminate. In the plasma treatment, a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Kogyo Co., Ltd.) was used, and the voltage was set to 160 V, the frequency was set to 10 kHz, and the treatment speed was set to 5000 mm / min. Next, a test piece (width 10 mm x length 100 mm) was cut out from the laminate (PET film / adhesive sheet / second release liner). Next, the second release liner was peeled off from the adhesive sheet in this test piece, and the exposed surface was attached to a polyimide (PI) film (product name "GV200", thickness 80 μm, manufactured by Kolon Co., Ltd.) whose surface had been plasma-treated. Next, the PI film with the adhesive sheet (test piece) was subjected to a heating and pressurizing treatment under the conditions of a temperature of 50°C, a pressure of 0.5 MPa, and a time of 15 minutes. This caused the test piece to be pressure-bonded to the PI film. In this manner, a measurement sample was prepared.
[0118] Next, the test sample was left to stand at room temperature for 30 minutes, and then a 180° peel test was performed to peel the test piece from the PI film in the test sample, and the force required for peeling (peel strength) was measured (first peel test). A tensile tester (product name "Autograph AG-50NX plus", manufactured by Shimadzu Corporation) was used for this measurement. In this measurement, the measurement temperature was 25°C, the relative humidity was 55%, the peel angle of the test piece from the PI film was 180°, the pulling speed of the test piece was 60 mm / min, and the peel length was 50 mm. The average value of the measured peel strength is shown in Table 1 as adhesive strength F1 (N / 10 mm).
[0119] On the other hand, a peel test was carried out under the same conditions as the first peel test except that the measurement temperature was changed to 65° C. (second peel test). The measurement results are shown in Table 1 as adhesive strength F2 (N / 10 mm).
[0120] <Bending test> For each of the pressure-sensitive adhesive sheets of Examples 1 to 5 and Comparative Examples 1 and 2, a bending test was carried out as follows.
[0121] First, the second release liner was peeled off from the pressure-sensitive adhesive sheet with double-sided release liner, and the exposed surface was plasma-treated. Meanwhile, both sides (first side, second side) of a polarizing film with a thickness of 51 μm were also plasma-treated. In addition, the surface of a transparent polyimide film with a thickness of 80 μm and the surface of a polyethylene terephthalate (PET) film with a thickness of 125 μm were also plasma-treated. In each plasma treatment, a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Kogyo Co., Ltd.) was used, and the voltage was set to 160 V, the frequency was set to 10 kHz, and the treatment speed was set to 5000 mm / min. Then, the above-mentioned exposed surface of the pressure-sensitive adhesive sheet and the first side of the polarizing film were bonded together. In this bonding, the pressure-sensitive adhesive sheet with the first release liner and the polarizing film were pressure-bonded together by moving a 2 kg roller back and forth once in an environment of 23°C. Next, the first release liner was peeled off from the adhesive sheet with the polarizing film, and the transparent polyimide film was attached to the exposed surface of the adhesive sheet. Next, the PET film was attached to the second surface of the polarizing film via a thin and strong adhesive sheet having a thickness of 15 μm. In this attachment, the polarizing film and the PET film were pressed together by a 2 kg roller going back and forth once in an environment of 23°C. As a result, a laminated film having a laminated structure of a PET film (thickness 125 μm), a thin and strong adhesive sheet (thickness 15 μm), a polarizing film (thickness 51 μm), an adhesive sheet (thickness 50 μm), and a transparent polyimide film (thickness 80 μm) was obtained.
[0122] Next, a test piece for evaluation was cut out from the laminated film thus prepared. Specifically, a rectangular test piece of 35 mm x 100 mm was cut out from the laminated film so that the absorption axis direction of the polarizing film was parallel to the long side direction in the test piece to be cut out. Next, the test piece was autoclaved for 15 minutes under the conditions of 35°C and 0.50 MPa.
[0123] Next, a bending test was performed on the test piece using a planar body unloaded U-shaped expansion and contraction tester (manufactured by Yuasa System Co., Ltd.) (first bending test). In this test, as shown in FIG. 3A, bending jigs 201 and 202 of the test machine were attached to both ends of the long side direction of the test piece 100, respectively, and the test piece 100 was fixed to the test machine. Each of the bending jigs 201 and 202 holds a range of 20 mm from the edge of the test piece 100. A central 60 mm region in the long side direction of the test piece 100 is not fixed to the bending jigs 201 and 202. In this test, the test piece 100 was repeatedly deformed (bent) 200,000 times at a bending speed of 60 rpm between a bent form (FIG. 3B) in which the surface on the PET film side is on the inside and a non-bent form (FIG. 3A) in a thermostatic chamber at a temperature of −20° C. Specifically, the bent shape in this test is a shape in which the axial direction of the bending moment acting on the test piece 100 is perpendicular to the absorption axis direction of the polarizing film. In this bent shape, the bending radius of the test piece 100 was 1.3 mm, and the bending angle was 180°. The repeatedly bent bent portion 100a of the test piece 100 was observed, and the adhesiveness of the pressure-sensitive adhesive sheet to the adherend in the bending test was evaluated as "good" when no peeling occurred between the pressure-sensitive adhesive sheet and the adherend (transparent polyimide film, polarizing film), and evaluated as "poor" when peeling occurred. The evaluation results are shown in Table 1.
[0124] On the other hand, a bending test was carried out on a test piece that had not been subjected to the first bending test under the same conditions as the first bending test except that the temperature was changed to -30°C (second bending test). The evaluation results are shown in Table 1.
[0125] Each of the pressure-sensitive adhesive sheets in Examples 1 to 5 has a shear storage modulus G1 (-20°C) of 70 kPa or less, and a ratio (G2 / G1) of the shear storage modulus G2 (-30°C) to the shear storage modulus G1 of 2.0 or less. Each of the pressure-sensitive adhesive sheets in Examples 1 to 5 also has a thickness of 45 μm or more, and a moisture permeability under specified conditions of 400 g / m 2·24h or less. Each of the pressure-sensitive adhesive sheets of Examples 1 to 5 exhibited good adhesion to the adherend in both the first bending test (-20°C) and the second bending test (-30°C). In contrast, the pressure-sensitive adhesive sheet of Comparative Example 1 had a shear storage modulus G1 of not 70 kPa or less, a ratio (G2 / G1) of not 2.0 or less, and a moisture permeability under specified conditions of not 400 g / m 2 The pressure-sensitive adhesive sheet of Comparative Example 2 did not exhibit good adhesion to the adherend in the second flex test (-30°C) because the ratio (G2 / G1) was not 2.0 or less.
[0126] [Table 1] [Explanation of symbols]
[0127] 10 Adhesive sheet (optical adhesive sheet) 11,12 Adhesive surface H Thickness direction L1, L2 Release liner 21 First member 22 Second member
Claims
1. An optical adhesive sheet, Has a thickness of 45 μm or more, Moisture permeability measured at 40°C and 92% relative humidity is 400g / m 2 ・24 hours or less, Has a shear storage modulus G1 of 70 kPa or less at -20 ° C.; Has a shear storage modulus G2 at -30°C; An optical adhesive sheet, wherein the ratio of the shear storage modulus G2 to the shear storage modulus G1 is 2.0 or less.
2. The optical adhesive sheet according to claim 1 , wherein the shear storage modulus G2 is 120 kPa or less.
3. The optical adhesive sheet according to claim 1 , having a relative dielectric constant of 4.0 or less at 100 kHz.
4. 2. The optical adhesive sheet according to claim 1, wherein the ratio of the dielectric constant after 24 hours in an environment of 40°C and a relative humidity of 92% to the dielectric constant at 100 kHz is 1.1 or less.
5. 5. The optical adhesive sheet according to claim 1, which has an adhesive strength of 2.0 N / 10 mm or more in a peel test under conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min.
Citation Information