Optical adhesive sheet

The optical adhesive sheet addresses peeling and stress issues in foldable display panels by optimizing shear modulus and loss tangent, improving bendability and adhesion through reduced stress.

JP2024169235APending Publication Date: 2024-12-05NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023086540
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional optical adhesive sheets for foldable display panels tend to peel off at bending points due to differences in curvature radius and generate excessive elongation stress during high-speed bending, affecting the device's bendability and functionality.

Method used

An optical adhesive sheet with a shear storage modulus of 200 kPa or less at 25°C and 1000 Hz, a loss tangent tan δ of 0.2 or more at 1 to 100 Hz, and specific adhesive properties to prevent peeling and elongation stress.

Benefits of technology

The adhesive sheet effectively reduces shear stress and elongation stress, enhancing the bendability and adhesion of foldable display panels by suppressing peeling and ensuring high-speed bending performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169235000001_ABST
    Figure 2024169235000001_ABST
Patent Text Reader

Abstract

To provide an optical adhesive sheet suitable for foldable display panels.SOLUTION: An adhesive sheet 10 is an optical adhesive sheet, has a shear storage elastic modulus of 200 kPa or less at 25°C and a frequency of 1000 Hz, and has a loss tangent tanδ of 0.2 or more at 25°C and a frequency of 1-100 Hz.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical pressure-sensitive adhesive sheet. [Background technology]

[0002] A display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. In the manufacturing process of such a display panel, for example, an optically transparent adhesive sheet (optical adhesive sheet) is used to bond the elements included in the laminated structure.

[0003] Meanwhile, development of repeatedly foldable display panels for smartphones and tablet terminals is progressing. Specifically, a foldable display panel can be repeatedly deformed between a bent shape and a flat non-bent shape. In such a foldable display panel, each element in a laminated structure is made to be repeatedly foldable, and a thin optical adhesive sheet is used for bonding between such elements. An optical adhesive sheet for flexible devices such as a foldable display panel is described, for example, in the following Patent Document 1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-111754 A Summary of the Invention [Problem to be solved by the invention]

[0005] Conventionally, at the folding portion of a foldable display panel, the optical adhesive sheet is easily peeled off from the element as the adherend. When the display panel is folded, the optical adhesive sheet and the element (adherend) have different curvature radii in the curved shape at the folding portion, and a shear force acts on the optical adhesive sheet attached to the element (adherend). Peeling of the optical adhesive sheet is undesirable because it causes a malfunction of the device. There is a high demand for the optical adhesive sheet for the foldable display panel to be less likely to peel off from the element (adherend) when the display panel is bent.

[0006] In addition, when the foldable display panel is folded, the folded portion of the optical adhesive sheet in the panel is substantially elongated, and an elongation stress is generated locally in the folded portion. Since the optical adhesive sheet is a viscoelastic body, the higher the folding speed (folding speed), the greater the elongation stress generated. The greater the elongation stress during folding, the more difficult it becomes to fold the foldable display panel (deterioration of foldability). In conventional optical adhesive sheets, the elongation stress generated during folding at high speed is relatively large.

[0007] The present invention provides an optical adhesive sheet suitable for use in foldable display panels. [Means for solving the problem]

[0008] The present invention [1] includes an optical adhesive sheet having a shear storage modulus of 200 kPa or less at 25°C and a frequency of 1000 Hz, and a loss tangent tanδ at 25°C of 0.2 or more at a frequency of 1 to 100 Hz.

[0009] The present invention [2] includes the optical adhesive sheet according to the above [1], in which the loss tangent tan δ at 25° C. has a minimum value in the frequency range of 1 to 10 Hz.

[0010] The present invention [3] includes an optical adhesive sheet according to the above [1] or [2], in which the loss tangent tanδ at 25°C has a minimum value Vmin in the frequency range of 1 to 10 Hz and a maximum value Vmax in the frequency range of 0.01 to 1 Hz, and the ratio of the maximum value Vmax to the minimum value Vmin is 1.2 or more and 1.7 or less.

[0011] The present invention [4] includes an optical adhesive sheet according to any one of [1] to [3] above, which has a relative dielectric constant of 4.0 or less at 100 kHz.

[0012] The present invention [5] includes an optical adhesive sheet according to any one of [1] to [4] above, which has an adhesive strength of 2.0 N / 10 mm or more in a peel test under conditions of 25°C, a peel angle of 180° and a tensile speed of 60 mm / min. Effect of the Invention

[0013] As described above, the optical adhesive sheet of the present invention has a shear storage modulus of 200 kPa or less at 25 ° C and a frequency of 1000 Hz. Such a soft optical adhesive sheet is suitable for alleviating the shear stress generated in the optical adhesive sheet when the adherend to which the adhesive sheet is attached is deformed. This alleviation of the shear stress is suitable for suppressing the peeling of the optical adhesive sheet from the adherend. In addition, as described above, the optical adhesive sheet of the present invention has a loss tangent tan δ at 25 ° C of 0.2 or more at a frequency of 1 to 100 Hz. Such an optical adhesive sheet is suitable for suppressing the elongation stress generated when bending at high speed, and therefore is suitable for realizing good high-speed bending properties in a foldable display panel. The optical adhesive sheet as described above is suitable for use in a foldable display panel. [Brief description of the drawings]

[0014] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of an optical adhesive sheet of the present invention. [Diagram 2]Fig. 2 shows an example of a method for using the optical adhesive sheet of the present invention. Fig. 2A shows a step of attaching the optical adhesive sheet to a first adherend, Fig. 2B shows a step of joining the first adherend and the second adherend via the optical adhesive sheet, and Fig. 2C shows an aging step. [Diagram 3] 3 shows a schematic diagram of the frequency dependence of loss tangent tan δ in the pressure-sensitive adhesive sheets of Examples 1 to 4. [Figure 4] FIG. 4A shows the test piece in a flat state during the repeated bending test, and FIG. 4B shows the test piece in a curved state during the repeated bending test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] As shown in Fig. 1, an adhesive sheet 10 as one embodiment of the optical adhesive sheet of the present invention has a sheet shape of a predetermined thickness and extends in a direction (plane direction) perpendicular to the thickness direction H. The adhesive sheet 10 has an adhesive surface 11 on one side in the thickness direction H, and an adhesive surface 12 on the other side in the thickness direction H. Fig. 1 exemplarily shows a state in which release liners L1, L2 are bonded to the adhesive surfaces 11, 12 of the adhesive sheet 10. The release liner L1 is disposed on the adhesive surface 11. The release liner L2 is disposed on the adhesive surface 12. The release liners L1, L2 are each peeled off at a predetermined timing when the adhesive sheet 10 is used.

[0016] The adhesive sheet 10 is an optically transparent adhesive sheet disposed at a light passing portion in a flexible device. An example of the flexible device is a flexible display panel. An example of the flexible display panel is a foldable display panel and a rollable display panel. The flexible display panel has a laminated structure including elements such as a pixel panel, a polarizing film, a touch panel, and a cover film. The adhesive sheet 10 is used, for example, in the manufacturing process of the flexible display panel to bond elements included in the laminated structure.

[0017] The pressure-sensitive adhesive sheet 10 has a shear storage modulus G' of 200 kPa or less at 25° C. and a frequency of 1000 Hz, and a loss tangent tanδ of 0.2 or more at 25° C. and a frequency of 1 to 100 Hz. The shear storage modulus G' and loss tangent tanδ (=shear loss modulus G" / shear storage modulus G') of the pressure-sensitive adhesive sheet 10 are determined by dynamic viscoelasticity measurement described later in the examples.

[0018] As described above, the adhesive sheet 10 has a shear storage modulus G' of 200 kPa or less at 25°C and a frequency of 1000 Hz. Such a soft adhesive sheet 10 is suitable for alleviating the shear stress generated in the adhesive sheet 10 when the adherend to which the adhesive sheet 10 is attached is deformed. This alleviation of the shear stress is suitable for suppressing the peeling of the adhesive sheet 10 from the adherend. In addition, as described above, the adhesive sheet 10 has a loss tangent tanδ of 0.2 or more at 25°C at a frequency of 1 to 100 Hz. Such an adhesive sheet 10 is suitable for suppressing the elongation stress generated when bending at high speed, and therefore is suitable for realizing good high-speed bending properties in a foldable display panel. The above-mentioned adhesive sheet 10 is suitable for use in a foldable display panel.

[0019] The shear storage modulus G' (25°C, frequency 1000Hz) of the adhesive sheet 10 is preferably 195kPa or less, more preferably 190kPa or less, even more preferably 180kPa or less, even more preferably 160kPa or less, and even more preferably 150kPa or less, from the viewpoint of the above-mentioned stress relaxation in the adhesive sheet 10. The shear storage modulus G' (25°C, frequency 1000Hz) is preferably 50kPa or more, more preferably 80kPa or more, and even more preferably 100kPa or more, from the viewpoint of ensuring good adhesion and handleability in the adhesive sheet 10. Methods for adjusting the shear storage modulus G' of the adhesive sheet 10 include, for example, selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, and adjusting the blending amount, and selecting the type of crosslinking agent and adjusting the blending amount.

[0020] From the viewpoint of realizing the above-mentioned good high-speed bending property, the loss tangent tan δ (25°C) of the pressure-sensitive adhesive sheet 10 is preferably 0.25 or more, more preferably 0.28 or more, at a frequency of 1 to 100 Hz. From the viewpoint of the handleability and processability of the pressure-sensitive adhesive sheet 10, the loss tangent tan δ (25°C) of the pressure-sensitive adhesive sheet 10 is preferably 1 or less, more preferably 0.9 or less, even more preferably 0.8 or less, and even more preferably 0.7 or less, at a frequency of 1 to 100 Hz. Methods for adjusting the loss tangent tan δ of the pressure-sensitive adhesive sheet 10 include, for example, selecting the type of base polymer in the pressure-sensitive adhesive sheet 10, adjusting the molecular weight and the amount of the base polymer, and selecting the type of crosslinking agent and adjusting the amount of the crosslinking agent.

[0021] The loss tangent tan δ of the pressure-sensitive adhesive sheet 10 at 25° C. preferably has a minimum value within a frequency range of 1 to 10 Hz. Such a configuration is preferable for suppressing the elongation stress generated in the pressure-sensitive adhesive sheet 10 when an adherend to which the pressure-sensitive adhesive sheet 10 is attached is bent at a normal speed.

[0022] The loss tangent tanδ of the pressure-sensitive adhesive sheet 10 at 25°C has a minimum value Vmin in the frequency range of 1 to 10 Hz and a maximum value Vmax in the frequency range of 0.01 to 1 Hz, and the ratio of the maximum value Vmax to the minimum value Vmin (Vmax / Vmin) is preferably 1.2 or more and preferably 1.7 or less, more preferably 1.5 or less. Such a configuration is preferable for ensuring stable viscoelastic properties of the pressure-sensitive adhesive sheet 10 over a wide frequency range (deformation speed range), and is therefore suitable for achieving good foldability in a foldable display panel.

[0023] The thickness of the adhesive sheet 10 is preferably 45 μm or more, more preferably 48 μm or more, and even more preferably 50 μm or more, from the viewpoint of ensuring a good stress relaxation function in the adhesive sheet 10. The thickness of the adhesive sheet 10 is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 70 μm or less, from the viewpoint of thinning the flexible device.

[0024] The moisture permeability of the pressure-sensitive adhesive sheet 10, measured under conditions of 40° C. and a relative humidity of 92%, is preferably 400 g / m 2 24h or less, preferably 395g / m 2 24h or less, preferably 390g / m 2 24h or less, more preferably 380g / m 2 ·24h or less. The moisture permeability of the adhesive sheet 10 means the moisture permeability when the thickness of the adhesive sheet 10 is 50 μm. The adhesive sheet 10 with low moisture permeability is suitable for suppressing partial swelling of the end of the adhesive sheet 10 when the adhesive sheet 10 is used to bond adherends together (swelling occurs due to penetration of moisture into the end). Suppressing partial swelling at the end of the adhesive sheet 10 is suitable for suppressing peeling of the end from the adherend. Methods for adjusting the moisture permeability of the adhesive sheet 10 include, for example, selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, and adjusting the amount of the base polymer. The selection of the type of base polymer includes selecting the type of side chain of the base polymer and adjusting the amount of the base polymer. The selection of the type of side chain of the base polymer includes adjusting the length of the alkyl portion in the side chain, and selecting the type of functional group contained in the side chain and adjusting the amount of the functional group. Methods for adjusting the moisture permeability of the adhesive sheet 10 also include selecting the type of additive other than the base polymer and adjusting the amount of the additive. The method for measuring the moisture permeability of the pressure-sensitive adhesive sheet 10 is as described below in the examples.

[0025] The dielectric constant D1 of the adhesive sheet 10 at 100 kHz (dielectric constant before humidification described later) is preferably 4.0 or less, more preferably 3.8 or less, and even more preferably 3.6 or less, from the viewpoint of realizing good sensing sensitivity in the touch sensor equipped in the display panel. The dielectric constant D1 is, for example, 3.0 or more, 3.3 or more, or 3.5 or more. The method of adjusting the dielectric constant D1 includes, for example, selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, and adjusting the blending amount. The selection of the type of base polymer includes selecting the type of side chain of the base polymer and adjusting the amount. The selection of the type of side chain of the base polymer includes adjusting the length of the alkyl part in the side chain, and selecting the type of functional group contained in the side chain and adjusting the amount. The method of adjusting the dielectric constant D1 also includes selecting the type of additive other than the base polymer and adjusting the blending amount (the same applies to the dielectric constant D2 described later). The measurement method of the dielectric constant is specifically as described later in the examples.

[0026] The dielectric constant D2 of the adhesive sheet 10 after 24 hours in an environment of 40°C and 92% relative humidity (after humidification) is preferably 4.0 or less, preferably 3.8 or less, and more preferably 3.6 or less, from the viewpoint of realizing good sensing sensitivity in a humidified environment in a touch sensor provided in a display panel. The dielectric constant D2 is, for example, 2.8 or more, 3.0 or more, or 3.2 or more.

[0027] From the viewpoint of obtaining stable dielectric properties in the adhesive sheet 10, the ratio of the relative dielectric constant D2 to the relative dielectric constant D1 (D2 / D1) is preferably 0.80 or more, more preferably 0.85 or more, and is preferably 1.1 or less, more preferably 1.05 or less.

[0028] The adhesive strength F1 of the adhesive sheet 10 in a peel test (first peel test) under the conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 2.0 N / 10 mm or more, more preferably 2.2 N / 10 mm or more, from the viewpoint of suppressing peeling of the adhesive sheet 10 from the adherend in the normal temperature region. The adhesive strength F1 means the adhesive strength to a polyimide (PI) film at 25°C. The measurement method of the adhesive strength F1 is specifically as described later in the Examples. The method of adjusting the adhesive strength F1 includes, for example, selecting the type of base polymer in the adhesive sheet 10, adjusting the molecular weight, and adjusting the blending amount. The selection of the type of base polymer includes adjusting the composition of the monomer that forms the base polymer. The method of adjusting the adhesive strength F1 also includes selecting the type of components other than the base polymer in the adhesive sheet 10, and adjusting the blending amount of the components. The components include a crosslinking agent, a silane coupling agent, and an oligomer. The above-mentioned adhesive strength adjustment method is also applicable to the adhesive strength F2 described later.

[0029] The adhesive strength F2 of the adhesive sheet 10 in a peel test (second peel test) under conditions of 65°C, a peel angle of 180°, and a tensile speed of 60 mm / min is preferably 1.3 N / 10 mm or more, preferably 1.5 N / 10 mm or more, and more preferably 1.7 N / 10 mm or more, from the viewpoint of suppressing peeling of the adhesive sheet 10 from the adherend in a high temperature region. The adhesive strength F2 means the adhesive strength to a PI film at 65°C. The method for measuring the adhesive strength F2 is specifically as described below in relation to the examples.

[0030] The adhesive sheet 10 is a sheet-like pressure-sensitive adhesive formed from an adhesive composition. The adhesive sheet 10 (adhesive composition) contains at least a base polymer.

[0031] The base polymer is an adhesive component that imparts adhesiveness to the adhesive sheet 10. Examples of the base polymer include acrylic polymers, silicone polymers, polyester polymers, polyurethane polymers, polyamide polymers, polyvinyl ether polymers, vinyl acetate / vinyl chloride copolymers, modified polyolefin polymers, epoxy polymers, fluoropolymers, and rubber polymers. The base polymers may be used alone or in combination of two or more kinds. From the viewpoint of ensuring good transparency and adhesiveness in the adhesive sheet 10, the base polymer is preferably an acrylic polymer.

[0032] An acrylic polymer is a copolymer of monomer components containing 50% by mass or more of (meth)acrylic acid ester. "(Meth)acrylic" means acrylic and / or methacrylic.

[0033] As the (meth)acrylic acid ester, preferably, a (meth)acrylic acid alkyl ester is used, and more preferably, a (meth)acrylic acid alkyl ester in which the alkyl group has a carbon number of 1 to 20. The (meth)acrylic acid alkyl ester may have a linear or branched alkyl group, or may have an alicyclic alkyl group.

[0034] Examples of (meth)acrylic acid alkyl esters having a linear or branched alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, and isooctyl (meth)acrylate. , nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (i.e., lauryl (meth)acrylate), isotridecyl (meth)acrylate, tetradecyl (meth)acrylate, isotetradecyl (meth)acrylate, pentadecyl (meth)acrylate, cetyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, and nonadecyl (meth)acrylate.

[0035] Examples of the (meth)acrylic acid alkyl ester having an alicyclic alkyl group include (meth)acrylic acid cycloalkyl ester, (meth)acrylic acid ester having a bicyclic aliphatic hydrocarbon ring, and (meth)acrylic acid ester having a tricyclic or higher aliphatic hydrocarbon ring. Examples of the (meth)acrylic acid cycloalkyl ester include (meth)acrylic acid cyclopentyl, (meth)acrylic acid cyclohexyl, (meth)acrylic acid cycloheptyl, and (meth)acrylic acid cyclooctyl. Examples of the (meth)acrylic acid ester having a bicyclic aliphatic hydrocarbon ring include (meth)acrylic acid isobornyl. Examples of (meth)acrylic acid esters having three or more aliphatic hydrocarbon rings include dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, tricyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, and 2-ethyl-2-adamantyl (meth)acrylate.

[0036] As the (meth)acrylic acid alkyl ester, from the viewpoint of balancing the softness and adhesive strength required for an adhesive sheet for flexible device applications with the low moisture permeability of the adhesive sheet in the adhesive sheet 10, preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group with 6 to 14 carbon atoms is used, more preferably at least one selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms is used, and even more preferably at least two selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms are used. As the (meth)acrylic acid alkyl esters having an alkyl group with 6 to 14 carbon atoms, 2-ethylhexyl acrylate (2EHA), n-octyl acrylate (NOAA), isononyl acrylate (INAA), and lauryl acrylate (LA) are preferred.

[0037] The proportion of the (meth)acrylic acid alkyl ester in the monomer component is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 97% by mass or more, from the viewpoint of appropriately exhibiting softness, adhesive strength, and low moisture permeability in the pressure-sensitive adhesive sheet 10. The proportion is, for example, 99.9% by mass or less, 99.5% by mass or less, or 99% by mass or less. When a first (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms is used in combination with another second (meth)acrylic acid alkyl ester selected from (meth)acrylic acid alkyl esters having an alkyl group with 8 to 12 carbon atoms, the proportion of the first (meth)acrylic acid alkyl ester in the monomer component is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and also preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% ​​by mass or less. The proportion of the second (meth)acrylic acid alkyl ester in the monomer component is preferably 20 mass% or more, more preferably 30 mass% or more, even more preferably 35 mass% or more, and is preferably 80 mass% or less, more preferably 70 mass% or less, even more preferably 65 mass% or less.

[0038] The monomer component may include a copolymerizable monomer that is copolymerizable with the (meth)acrylic acid alkyl ester. The copolymerizable monomer may include, for example, a monomer having a polar group. The polar group-containing monomer may include, for example, a hydroxy group-containing monomer, a monomer having a nitrogen atom-containing ring, and a carboxy group-containing monomer. The polar group-containing monomer is useful for modifying the acrylic polymer, such as introducing a crosslinking point into the acrylic polymer and ensuring the cohesive force of the acrylic polymer. The monomer component preferably includes a hydroxy group-containing monomer, and does not include a monomer having a nitrogen atom-containing ring and a carboxy group-containing monomer.

[0039] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. As the hydroxyl group-containing monomer, at least one selected from the group consisting of 2-hydroxyethyl acrylate (2HEA) and 4-hydroxybutyl acrylate (4HBA) is preferably used.

[0040] The proportion of the hydroxy group-containing monomer in the monomer components is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring cohesive strength in the pressure-sensitive adhesive sheet 10. From the viewpoint of adjusting the polarity of the acrylic polymer (related to the compatibility between the acrylic polymer and various additive components in the pressure-sensitive adhesive sheet 10), the proportion is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less.

[0041] Examples of monomers having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, and N-vinylisothiazole.

[0042] When a monomer having a nitrogen atom-containing ring is used, the proportion of the monomer having a nitrogen atom-containing ring in the monomer components is preferably 0.1 mass % or more, more preferably 0.2 mass % or more, and even more preferably 0.5 mass % or more, from the viewpoints of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10 and ensuring the adhesive strength to the adherend in the pressure-sensitive adhesive sheet 10. This proportion is preferably 10 mass % or less, more preferably 5 mass % or less, and even more preferably 3 mass % or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and adjusting the polarity of the acrylic polymer (related to the compatibility of various additive components in the pressure-sensitive adhesive sheet 10 with the acrylic polymer).

[0043] Examples of carboxy group-containing monomers include acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.

[0044] When a carboxyl group-containing monomer is used, the proportion of the carboxyl group-containing monomer in the monomer components is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.8 mass% or more, from the viewpoints of introducing a crosslinked structure into the acrylic polymer, ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10, and ensuring the adhesive strength to the adherend in the pressure-sensitive adhesive sheet 10. The proportion is preferably 10 mass% or less, more preferably 5 mass% or less, and even more preferably 3 mass% or less, from the viewpoints of adjusting the glass transition temperature of the acrylic polymer and avoiding the risk of corrosion of the adherend by acid.

[0045] The proportion of the polar group-containing monomer in the monomer component (when multiple polar group-containing monomers are included, the proportion of the total amount of the multiple polar group-containing monomers) is preferably 7% by mass or less, more preferably 5% by mass or less, even more preferably 3.5% by mass or less, and particularly preferably 3% by mass or less, from the viewpoint of lowering the glass transition temperature of the base polymer and ensuring the softness of the adhesive sheet 10. The proportion is, for example, 0.1% by mass or more, 0.5% by mass or more, or 0.8% by mass or more.

[0046] The monomer component may contain other copolymerizable monomers. Examples of the other copolymerizable monomers include acid anhydride monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, alkoxy group-containing monomers, and aromatic vinyl compounds. These other copolymerizable monomers may be used alone or in combination of two or more.

[0047] The monomer components forming the base polymer preferably include an alkyl (meth)acrylate ester and a polar group-containing monomer, and more preferably include an alkyl (meth)acrylate ester having an alkyl group with 8 to 12 carbon atoms and a hydroxyl group-containing monomer. In this case, the ratio of the hydroxyl group-containing monomer in the total amount of the alkyl (meth)acrylate ester and the hydroxyl group-containing monomer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 0.8% by mass or more, from the viewpoint of introducing a crosslinked structure into the acrylic polymer and ensuring the cohesive force in the pressure-sensitive adhesive sheet 10. The ratio is preferably 5% by mass or less, more preferably 3.5% by mass or less, even more preferably 3% by mass or less, even more preferably 2% by mass or less, and even more preferably 1.5% by mass or less, from the viewpoint of lowering the glass transition temperature of the base polymer and ensuring the softness of the pressure-sensitive adhesive sheet 10. When the monomer components forming the base polymer include an alkyl (meth)acrylate ester having an alkyl group with 8 to 12 carbon atoms and a hydroxyl group-containing monomer, it preferably does not include a monomer having a nitrogen atom-containing ring and a carboxyl group-containing monomer.

[0048] The base polymer preferably has a crosslinked structure. Examples of methods for introducing a crosslinked structure into the base polymer include the following first and second methods. In the first method, a base polymer having a functional group capable of reacting with a crosslinking agent and a crosslinking agent are blended into an adhesive composition, and the base polymer and the crosslinking agent are reacted in an adhesive sheet. In the second method, a polyfunctional compound is included as a crosslinking agent in the monomer components forming the base polymer, and a base polymer having a branched structure (crosslinked structure) introduced into the polymer chain is formed by polymerization of the monomer components. These methods may be used in combination.

[0049] The crosslinking agent used in the first method includes, for example, a compound that reacts with functional groups (such as hydroxyl groups and carboxyl groups) contained in the base polymer. Examples of such crosslinking agents include isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, and carbodiimide crosslinking agents. The crosslinking agents in the first method may be used alone or in combination of two or more. As the crosslinking agent in the first method, an isocyanate crosslinking agent is preferably used because it has high reactivity with hydroxyl groups and carboxyl groups in the base polymer and is easy to introduce a crosslinked structure.

[0050] Examples of isocyanate crosslinking agents include tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, tetramethylxylylene diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, and polymethylene polyphenylisocyanate. In addition, examples of isocyanate crosslinking agents include derivatives of these isocyanates. Examples of the isocyanate derivatives include isocyanurate modified products and polyol modified products. Commercially available isocyanate crosslinking agents include, for example, Coronate L (trimethylolpropane adduct of tolylene diisocyanate, manufactured by Tosoh), Coronate HL (trimethylolpropane adduct of hexamethylene diisocyanate, manufactured by Tosoh), Coronate HX (isocyanurate of hexamethylene diisocyanate, manufactured by Tosoh), Takenate D110N (trimethylolpropane adduct of xylylene diisocyanate, manufactured by Mitsui Chemicals), and Takenate 600 (1,3-bis(isocyanatomethyl)cyclohexane, manufactured by Mitsui Chemicals).

[0051] Peroxide crosslinking agents include dibenzoyl peroxide, di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, and t-butylperoxypivalate.

[0052] Epoxy crosslinkers include bisphenol A, epichlorohydrin type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidyl aniline, diamine glycidyl amine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane.

[0053] The amount of the crosslinking agent in the first method is, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and more preferably 0.1 parts by mass or more, per 100 parts by mass of the base polymer, from the viewpoint of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10. From the viewpoint of ensuring good tackiness in the pressure-sensitive adhesive sheet 10, the amount of the crosslinking agent in the first method is, for example, 5 parts by mass or less, preferably 1 part by mass or less, and more preferably 0.2 parts by mass or less, per 100 parts by mass of the base polymer.

[0054] In the second method, the monomer components (including the polyfunctional compound and the monofunctional monomer for introducing a crosslinked structure) may be polymerized at once or in multiple stages. In the multi-stage polymerization method, first, the monofunctional monomer for forming the base polymer is polymerized (preliminary polymerization), thereby preparing a prepolymer composition containing a partial polymer (a mixture of a polymer with a low degree of polymerization and an unreacted monofunctional monomer). Next, a polyfunctional compound is added as a crosslinking agent to the prepolymer composition, and then a polymerization reaction is allowed to proceed in a reaction system containing the partial polymer and the polyfunctional compound (main polymerization).

[0055] Examples of the polyfunctional compound include polyfunctional monomers and polyfunctional oligomers that contain two or more ethylenically unsaturated double bonds in one molecule. Examples of the polyfunctional monomer include polyfunctional (meth)acrylates.

[0056] Examples of the polyfunctional (meth)acrylate include difunctional (meth)acrylate, trifunctional (meth)acrylate, and tetrafunctional or higher polyfunctional (meth)acrylate.

[0057] Examples of bifunctional (meth)acrylates include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, glycerin di(meth)acrylate, ethoxylated bisphenol A diacrylate (BPAEODE), and neopentyl glycol di(meth)acrylate.

[0058] Examples of trifunctional (meth)acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and tris(acryloyloxyethyl)isocyanurate.

[0059] Examples of tetrafunctional or higher polyfunctional (meth)acrylates include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, alkyl-modified dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0060] Examples of polyfunctional oligomers include urethane (meth)acrylate oligomers, polyester (meth)acrylate oligomers, polyether (meth)acrylate oligomers, polyol (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate.

[0061] The polyfunctional compound as the crosslinking agent in the second method may be used alone or in combination of two or more kinds. As the polyfunctional compound, a polyfunctional monomer is preferably used, and more preferably at least one selected from the group consisting of dipentaerythritol hexaacrylate (DPHA), 1,6-hexanediol diacrylate (HDDA), and trimethylolpropane triacrylate (TMPTA) is used.

[0062] The amount of the polyfunctional compound as a crosslinking agent in the monomer components is preferably 0.02 parts by mass or more, more preferably 0.04 parts by mass or more, and even more preferably 0.06 parts by mass or more, per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring the cohesive strength of the pressure-sensitive adhesive sheet 10. The amount of the polyfunctional compound is preferably 3 parts by mass or less, more preferably 2 parts by mass or less, and even more preferably 1 part by mass or less, per 100 parts by mass of the monofunctional monomer, from the viewpoint of ensuring good tackiness in the pressure-sensitive adhesive sheet 10.

[0063] The acrylic polymer (base polymer) can be formed by polymerizing the above-mentioned monomer components. Examples of the polymerization method include solution polymerization, emulsion polymerization, and solvent-free photopolymerization (e.g., ultraviolet polymerization). For example, ethyl acetate and toluene are used as the solvent for solution polymerization. In the polymerization, a chain transfer agent may be used. For example, a thermal polymerization initiator and a photopolymerization initiator are used as the polymerization initiator. The polymerization initiator may be used alone or in combination of two or more kinds. The amount of the polymerization initiator used is preferably 0.03 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.07 parts by mass or more, and is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.3 parts by mass or less, per 100 parts by mass of the monomer components.

[0064] Examples of the thermal polymerization initiator include azo polymerization initiators and peroxide polymerization initiators. Examples of the azo polymerization initiator include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionate)dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, and 2,2'-azobis(2-amidinopropane)dihydrochloride. Examples of the peroxide polymerization initiator include dibenzoyl peroxide, t-butyl permaleate, and lauroyl peroxide.

[0065] Examples of the photopolymerization initiator include a radical photopolymerization initiator, a cationic photopolymerization initiator, and an anionic photopolymerization initiator.

[0066] Examples of the radical photopolymerization initiator include an acylphosphine oxide photopolymerization initiator, a benzoin ether photopolymerization initiator, and an acetophenone photopolymerization initiator.

[0067] Examples of the acylphosphine oxide photopolymerization initiator include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. Examples of the benzoin ether photopolymerization initiator include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone.

[0068] The weight average molecular weight of the base polymer is preferably 100,000 or more, more preferably 300,000 or more, and even more preferably 500,000 or more, from the viewpoint of ensuring the cohesive force in the pressure-sensitive adhesive sheet 10. The weight average molecular weight of the base polymer is measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.

[0069] The glass transition temperature (Tg) of the base polymer is preferably 0° C. or lower, more preferably −10° C. or lower, and even more preferably −20° C. or lower. The glass transition temperature is, for example, −80° C. or higher.

[0070] The glass transition temperature (Tg) of the base polymer can be determined by the following Fox formula (theoretical value). The Fox formula is a relational expression between the glass transition temperature Tg of a polymer and the glass transition temperature Tgi of a homopolymer of a monomer constituting the polymer. In the following Fox formula, Tg represents the glass transition temperature (°C) of a polymer, Wi represents the weight fraction of a monomer i constituting the polymer, and Tgi represents the glass transition temperature (°C) of a homopolymer formed from the monomer i. The glass transition temperature of a homopolymer can be determined by a literature value. For example, the glass transition temperatures of various homopolymers are listed in "Polymer Handbook" (4th edition, John Wiley & Sons, Inc., 1999). On the other hand, the glass transition temperature of a homopolymer of a monomer can also be determined by a method specifically described in JP-A-2007-51271.

[0071] Fox formula 1 / (273+Tg)=Σ[Wi / (273+Tgi)]

[0072] The pressure-sensitive adhesive composition may contain a silane coupling agent. The content of the silane coupling agent in the pressure-sensitive adhesive composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, based on 100 parts by mass of the base polymer. The content is preferably 5 parts by mass or less, more preferably 3 parts by mass or less.

[0073] The adhesive composition may contain other components as necessary. Examples of the other components include solvents, tackifiers, plasticizers, softeners, antioxidants, fillers, colorants, UV absorbers, surfactants, and antistatic agents. Examples of the solvent include polymerization solvents that are used as necessary during polymerization of acrylic polymers, and solvents that are added to the polymerization reaction solution after polymerization. Examples of the solvent include ethyl acetate and toluene.

[0074] The pressure-sensitive adhesive sheet 10 can be produced, for example, by applying the above-mentioned pressure-sensitive adhesive composition onto a release liner L1 (first release liner) to form a coating film, and then drying the coating film. The pressure-sensitive adhesive sheet 10 may also be produced by applying the above-mentioned pressure-sensitive adhesive composition onto a release liner L1 (first release liner) to form a coating film, laminating a release liner L2 (second release liner) onto the coating film, and then drying the coating film between the release liners.

[0075] The release liner L1 may be, for example, a flexible plastic film. Examples of the plastic film include polyester films such as polyethylene terephthalate films, polyethylene films, and polypropylene films. The thickness of the release liner L1 is, for example, 3 μm or more and, for example, 200 μm or less. The surface of the release liner L1 is preferably subjected to a release treatment.

[0076] Examples of the method for applying the pressure-sensitive adhesive composition include roll coating, kiss roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, and die coating. The drying temperature for the coating film is, for example, 50° C. to 200° C. The drying time is, for example, 5 seconds to 20 minutes.

[0077] The release liner L2 is preferably a flexible plastic film whose surface has been subjected to a release treatment. As the release liner L2, the plastic films described above with respect to the release liner L1 can be used.

[0078] In this manner, adhesive sheet 10 having adhesive surfaces 11, 12 covered and protected by release liners L1, L2 can be manufactured.

[0079] The haze of the pressure-sensitive adhesive sheet 10 is preferably 3% or less, more preferably 2% or less, and more preferably 1% or less. The haze of the pressure-sensitive adhesive sheet 10 can be measured using a haze meter in accordance with JIS K7136 (2000). Examples of haze meters include "NDH2000" manufactured by Nippon Denshoku Industries Co., Ltd. and "HM-150 type" manufactured by Murakami Color Research Laboratory Co., Ltd.

[0080] The total light transmittance of the pressure-sensitive adhesive sheet 10 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. The total light transmittance of the pressure-sensitive adhesive sheet 10 is, for example, 100% or less. The total light transmittance of the pressure-sensitive adhesive sheet 10 can be measured in accordance with JIS K 7375 (2008).

[0081] 2A to 2C show an example of a method of using the adhesive sheet 10. FIG.

[0082] In this method, first, as shown in FIG. 2A, the adhesive sheet 10 is attached to one surface in the thickness direction H of a first member 21 (adherend). The first member 21 is, for example, one element in a laminated structure of a flexible display panel. Examples of the element include a pixel panel, a polarizing film, a touch panel, and a cover film (the same applies to the second member 22 described below). Through this process, the adhesive sheet 10 for bonding to other members is provided on the first member 21.

[0083] 2B, one surface side in the thickness direction H of the first member 21 is joined to the other surface side in the thickness direction H of the second member 22 via the adhesive sheet 10 on the first member 21. The second member 22 is, for example, another element in the laminated structure of the flexible display panel.

[0084] Next, as shown in FIG. 2C, the adhesive sheet 10 between the first member 21 and the second member 22 is aged. Aging enhances the bonding strength between the adhesive sheet 10 and the members 21, 22. The aging temperature is, for example, 20° C. to 160° C. The aging time is, for example, 1 minute to 21 days. When the aging is performed by autoclaving (heating and pressurizing), the temperature is, for example, 30° C. to 80° C., the pressure is, for example, 0.1 to 0.8 MPa, and the treatment time is, for example, 15 minutes or longer. EXAMPLES

[0085] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".

[0086] Example 1 Preparation of Prepolymer Composition In a flask, 0.05 parts by mass of 2,2-dimethoxy-1,2-diphenylethan-1-one (product name "Omnirad651", manufactured by IGM Resins) as a first photopolymerization initiator and 0.05 parts by mass of 1-hydroxycyclohexyl phenyl ketone (product name "Omnirad184", manufactured by IGM Resins) as a second photopolymerization initiator were added to a monomer mixture containing 51 parts by mass of 2-ethylhexyl acrylate (2EHA), 48 parts by mass of lauryl acrylate (LA), and 1 part by mass of 4-hydroxybutyl acrylate (4HBA). The mixture was then irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a first prepolymer composition (containing monomer components that had not undergone a polymerization reaction) with a polymerization rate of approximately 10%.

[0087] Preparation of Pressure-Sensitive Adhesive Composition A first adhesive composition was obtained by mixing 100 parts by mass of the first prepolymer composition, 0.06 parts by mass of dipentaerythritol hexaacrylate (DPHA) as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.).

[0088] <Formation of Adhesive Layer> A first adhesive composition was applied onto the release-treated surface of a first release liner (product name "Diafoil MRF#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side to form a coating film. Next, the release-treated surface of a second release liner (product name "Diafoil MRE#75", thickness 75 μm, manufactured by Mitsubishi Chemical Corporation) having a release-treated surface on one side was attached onto the coating film on the first release liner. Next, the coating film between the release liners was irradiated with ultraviolet light to photocure the coating film and form an adhesive layer (thickness 50 μm). For ultraviolet light irradiation, a black light was used as the irradiation light source, and the irradiation intensity was 5 mW / cm. 2 It was decided.

[0089] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) with double-sided release liners was prepared for Example 1. The composition of the pressure-sensitive adhesive sheet for Example 1 is shown in Table 1 in units of "parts by mass" (the same applies to the examples and comparative examples described below).

[0090] Example 2 First, 0.05 parts by mass of a first photopolymerization initiator (Omnirad651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad184) were added to a monomer mixture containing 29 parts by mass of n-octyl acrylate (NOAA), 70 parts by mass of 2EHA, and 1 part by mass of 4HBA in a flask, and then the mixture was irradiated with ultraviolet light under a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a second prepolymer composition with a polymerization rate of approximately 10%.

[0091] Next, 100 parts by mass of the second prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a second pressure-sensitive adhesive composition.

[0092] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in the formation of the adhesive layer in Example 1, except that the second adhesive composition was used instead of the first adhesive composition.

[0093] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) with double-sided release liners of Example 2 was produced.

[0094] Example 3 First, 0.05 parts by mass of a first photopolymerization initiator (Omnirad651) and 0.05 parts by mass of a second photopolymerization initiator (Omnirad184) were added to a monomer mixture containing 70 parts by mass of isononyl acrylate (INAA), 29 parts by mass of LA, and 1 part by mass of 4HBA in a flask, and then the mixture was irradiated with ultraviolet light in a nitrogen atmosphere to polymerize a portion of the monomer components in the mixture, thereby obtaining a third prepolymer composition with a polymerization rate of approximately 10%.

[0095] Next, 100 parts by mass of the third prepolymer composition, 0.06 parts by mass of DPHA as a crosslinking agent, and 0.3 parts by mass of a silane coupling agent (KBM-403) were mixed together to obtain a third pressure-sensitive adhesive composition.

[0096] Next, an adhesive layer (thickness 50 μm) was formed between the first and second release liners in the same manner as in the formation of the adhesive layer in Example 1, except that the third adhesive composition was used instead of the first adhesive composition.

[0097] In this manner, a pressure-sensitive adhesive sheet (thickness: 50 μm) with double-sided release liners of Example 3 was produced.

[0098] Example 4 The adhesive sheet of Example 4 with double-sided release liner was produced in the same manner as the adhesive sheet of Example 2, except that in preparing the prepolymer composition, the amount of 2EHA was 50 parts by mass and the amount of NOAA was 49 parts by mass.

[0099] Comparative Example 1 A pressure-sensitive adhesive sheet of Comparative Example 1 with a double-sided release liner was prepared in the same manner as the pressure-sensitive adhesive sheet of Example 1, except for the following: In preparing the prepolymer composition, 56 parts by mass of 2EHA, 34 parts by mass of LA, 7 parts by mass of 4HBA, and 2 parts by mass of N-vinyl-2-pyrrolidone (NVP) were blended. In preparing the pressure-sensitive adhesive composition, 1 part by mass of the following acrylic oligomer was further blended.

[0100] Preparation of Oligomers First, in a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, a mixture containing 60 parts by mass of dicyclopentanyl methacrylate (DCPMA), 40 parts by mass of methyl methacrylate (MMA), 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a solvent was stirred under a nitrogen atmosphere at 70°C for 1 hour. Next, 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added to the mixture to prepare a reaction solution, which was reacted under a nitrogen atmosphere at 70°C for 1 hour and then at 80°C for 2 hours (polymerization reaction). Next, the reaction solution was heated to 130°C to volatilize and remove toluene, the chain transfer agent, and unreacted monomers. As a result, an acrylic oligomer (solid form) was obtained as a hydrophobic oligomer without a polar group. The weight average molecular weight of this acrylic oligomer was 5100.

[0101] <Moisture permeability> The moisture permeability was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 4 and Comparative Example 1. Specifically, the results are as follows.

[0102] First, the pressure-sensitive adhesive sheet with double-sided release liners was left to stand for 3 days in an atmosphere with a temperature of 23°C and a relative humidity of 55%. This adjusted the condition of the pressure-sensitive adhesive sheet. Next, one of the release liners was peeled off from the pressure-sensitive adhesive sheet, and the exposed surface was then covered with a 25 μm-thick triacetyl cellulose (TAC) film (moisture permeability: 1070 g / m 2 The other release liner was then peeled off from the pressure sensitive adhesive sheet on the TCA film, yielding a sample film for moisture permeability measurement.

[0103] Next, the moisture permeability in the thickness direction of the adhesive sheet was measured in accordance with the moisture permeability test (cup method) of JIS Z0208. Specifically, first, a predetermined amount of calcium chloride weighed in advance was placed in a test cup (an aluminum cup with a circular opening of 30 mm in diameter, used in the cup method of JIS Z0208), and the opening of the cup was blocked with a sample film. The area of ​​the sample film blocking the opening of the cup corresponds to the area of ​​a circle with a diameter of 30 mm. Next, the cup with the sample film was placed in a constant temperature and humidity chamber at a temperature of 40°C and a relative humidity of 90%, and left for 24 hours. Next, the calcium chloride taken out of the cup was weighed. The increased mass (g) of calcium chloride was multiplied by the area (m 2 The value was divided by the moisture permeability (g / m 2 The moisture permeability obtained in this manner is that of the pressure-sensitive adhesive sheet with the TAC film, but since the moisture permeability of the TAC film is significantly greater than that of the pressure-sensitive adhesive sheet, the moisture permeability of the sample film was regarded as that of the pressure-sensitive adhesive sheet.

[0104] <Dielectric constant> The relative dielectric constant was examined for each of the pressure-sensitive adhesive sheets of Examples 1 to 4 and Comparative Example 1. Specifically, the results are as follows.

[0105] First, a measurement sample was prepared by sandwiching the adhesive sheet between copper foil and an electrode. Next, the dielectric constant of the measurement sample was measured at a frequency of 100 kHz under the following conditions in accordance with JIS K6911 using Agilent Technologies' Precision Impedance Analyzer 4294A (first dielectric constant measurement). The measurement results are shown in Table 1 as the dielectric constant D1 of the adhesive sheet at 100 kHz.

[0106] [Conditions for measuring dielectric constant] Electrode configuration: Aluminum plate with a diameter of 12.1 mm and a thickness of 0.5 mm Counter electrode: 3oz copper plate Measurement environment: Temperature 25℃, relative humidity 50%

[0107] In addition, the adhesive sheet was subjected to a humidification treatment, and then the dielectric constant of the adhesive sheet was measured (second dielectric constant measurement). In the humidification treatment, the adhesive sheet was stored for 24 hours in an environment of 40°C and a relative humidity of 92%. The method for measuring the second dielectric constant was the same as the above-mentioned first dielectric constant measurement method. The measurement results are shown in Table 1 as the dielectric constant D2 at 100 kHz after humidification of the adhesive sheet. The ratio (D2 / D1) of the dielectric constant D2 to the above-mentioned dielectric constant D1 is also shown in Table 1.

[0108] Dynamic Viscoelasticity Measurement For each of the pressure-sensitive adhesive sheets of Examples 1 to 4 and Comparative Example 1, the dynamic viscoelasticity was measured.

[0109] First, a required number of samples for measurement were prepared for each adhesive sheet. Specifically, first, a plurality of pieces of adhesive sheet cut out from the adhesive sheet were pasted together to prepare a sample sheet with a thickness of about 1.5 mm. Next, this sheet was punched out to obtain cylindrical pellets (diameter 7.9 mm) as the measurement samples.

[0110] Next, dynamic viscoelasticity measurements were performed on the measurement sample using a dynamic viscoelasticity measuring device (name: "Advanced Rheometric Expansion System (ARES) G2", manufactured by TA Instruments). Specifically, the measurement sample was fixed to a parallel plate jig with a diameter of 7.9 mm on the same device, and then the measurement was performed. In this measurement, the measurement mode was shear mode, the strain amount was 0.3%, the measurement temperature was in the range of -20°C to 60°C in 10°C increments, and the actual measured angular frequency (ω) range was 0.1 to 100 rad / s. Next, using the analysis software built into the dynamic viscoelasticity measuring device, the reference temperature was set to 25°C, and the frequency range was 1.0 x 10 -5 Hz~1×10 3A master curve (a composite curve based on the temperature-time conversion rule) spanning 1000 to 2000 Hz was synthesized from the measurement data (frequency f (Hz) was calculated by the formula f=ω / (2π)). This resulted in frequency-dependent data of the shear storage modulus G' and loss tangent tan δ (=shear loss modulus G" / shear storage modulus G'). From the obtained data, the shear storage modulus G' and loss tangent tan δ at predetermined frequencies (0.1 Hz, 1 Hz, 10 Hz, 100 Hz, 1000 Hz) were read. These values ​​are shown in Table 1. The maximum value Vmax of the loss tangent tan δ in the frequency range of 0.01 to 1 Hz, and the minimum value Vmin of the loss tangent tan δ in the frequency range of 1 to 10 Hz are also shown in Table 1. The ratio (Vmax / Vmin) of the maximum value Vmax to the minimum value Vmin is also shown in Table 1. In addition, for each of Examples 1 to 4, A graph showing the frequency dependency of loss tangent tan δ (25°C) in a pressure-sensitive adhesive sheet (an example of measurement results obtained by dynamic viscoelasticity measurement) is shown typically in Fig. 3. In the graph of Fig. 3, the horizontal axis represents frequency (Hz) and the vertical axis represents loss tangent tan δ. As shown in the graph of Fig. 3, the pressure-sensitive adhesive sheets of Examples 1 to 4 have a loss tangent tan δ at 25°C of 0.2 or more at frequencies of 1 to 100 Hz, a minimum value Vmin of the loss tangent tan δ at 25°C in the frequency range of 1 to 10 Hz, and a maximum value Vmax of the loss tangent tan δ at 25°C in the frequency range of 0.01 to 1 Hz.

[0111] <180° peel test> For each of the pressure-sensitive adhesive sheets of Examples 1 to 4 and Comparative Example 1, the adhesive strength to an adherend was examined by a 180° peel test.

[0112] Specifically, first, a required number of measurement samples were prepared for each adhesive sheet. In preparing the measurement samples, first, the first release liner was peeled off from the adhesive sheet, and the exposed surface was attached to a polyethylene terephthalate (PET) film (product name "Lumirror S10", thickness 50 μm, manufactured by Toray) whose surface had been plasma-treated to obtain a laminate. In the plasma treatment, a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Kogyo Co., Ltd.) was used, and the voltage was set to 160 V, the frequency was set to 10 kHz, and the treatment speed was set to 5000 mm / min. Next, a test piece (width 10 mm x length 100 mm) was cut out from the laminate (PET film / adhesive sheet / second release liner). Next, the second release liner was peeled off from the adhesive sheet in this test piece, and the exposed surface was attached to a polyimide (PI) film (product name "GV200", thickness 80 μm, manufactured by Kolon Co., Ltd.) whose surface had been plasma-treated. Next, the PI film with the adhesive sheet (test piece) was subjected to a heating and pressurizing treatment under the conditions of a temperature of 50°C, a pressure of 0.5 MPa, and a time of 15 minutes. This caused the test piece to be pressure-bonded to the PI film. In this manner, a measurement sample was prepared.

[0113] Next, the test sample was left to stand at room temperature for 30 minutes, and then a 180° peel test was performed to peel the test piece from the PI film in the test sample, and the force required for peeling (peel strength) was measured (first peel test). A tensile tester (product name "Autograph AG-50NX plus", manufactured by Shimadzu Corporation) was used for this measurement. In this measurement, the measurement temperature was 25°C, the relative humidity was 55%, the peel angle of the test piece from the PI film was 180°, the pulling speed of the test piece was 60 mm / min, and the peel length was 50 mm. The average value of the measured peel strength is shown in Table 1 as adhesive strength F1 (N / 10 mm).

[0114] On the other hand, a peel test was carried out under the same conditions as the first peel test except that the measurement temperature was changed to 65° C. (second peel test). The measurement results are shown in Table 1 as adhesive strength F2 (N / 10 mm).

[0115] <Bending test> For each of the pressure-sensitive adhesive sheets of Examples 1 to 4 and Comparative Example 1, a bending test was carried out as follows.

[0116] First, the second release liner was peeled off from the pressure-sensitive adhesive sheet with double-sided release liner, and the exposed surface was plasma-treated. Meanwhile, both sides (first side, second side) of a polarizing film with a thickness of 51 μm were also plasma-treated. In addition, the surface of a transparent polyimide film with a thickness of 80 μm and the surface of a polyethylene terephthalate (PET) film with a thickness of 125 μm were also plasma-treated. In each plasma treatment, a plasma irradiation device (product name "AP-TO5", manufactured by Sekisui Kogyo Co., Ltd.) was used, and the voltage was set to 160 V, the frequency was set to 10 kHz, and the treatment speed was set to 5000 mm / min. Then, the above-mentioned exposed surface of the pressure-sensitive adhesive sheet and the first side of the polarizing film were bonded together. In this bonding, the pressure-sensitive adhesive sheet with the first release liner and the polarizing film were pressure-bonded together by moving a 2 kg roller back and forth once in an environment of 23°C. Next, the first release liner was peeled off from the adhesive sheet with the polarizing film, and the transparent polyimide film was attached to the exposed surface of the adhesive sheet. Next, the PET film was attached to the second surface of the polarizing film via a thin and strong adhesive sheet having a thickness of 15 μm. In this attachment, the polarizing film and the PET film were pressed together by a 2 kg roller going back and forth once in an environment of 23°C. As a result, a laminated film having a laminated structure of a PET film (thickness 125 μm), a thin and strong adhesive sheet (thickness 15 μm), a polarizing film (thickness 51 μm), an adhesive sheet (thickness 50 μm), and a transparent polyimide film (thickness 80 μm) was obtained.

[0117] Next, a test piece for evaluation was cut out from the laminated film thus prepared. Specifically, a rectangular test piece of 35 mm x 100 mm was cut out from the laminated film so that the absorption axis direction of the polarizing film was parallel to the long side direction in the test piece to be cut out. Next, the test piece was autoclaved for 15 minutes under the conditions of 35°C and 0.50 MPa.

[0118] Next, a bending test was performed on the test piece using a planar body unloaded U-shaped expansion and contraction tester (manufactured by Yuasa System Co., Ltd.) (first bending test). In this test, as shown in FIG. 4A, bending jigs 201 and 202 of the test machine were attached to both ends of the long side direction of the test piece 100, respectively, and the test piece 100 was fixed to the test machine. Each of the bending jigs 201 and 202 holds a range of 20 mm from the edge of the test piece 100. A central 60 mm region in the long side direction of the test piece 100 is not fixed to the bending jigs 201 and 202. In this test, the test piece 100 was repeatedly deformed (bent) 200,000 times at a bending speed of 60 rpm between a bent form (FIG. 4B) in which the surface on the PET film side is on the inside and a non-bent form (FIG. 4A) in a thermostatic chamber at a temperature of −20° C. Specifically, the bent shape in this test is a shape in which the axial direction of the bending moment acting on the test piece 100 is perpendicular to the absorption axis direction of the polarizing film. In this bent shape, the bending radius of the test piece 100 was 1.3 mm, and the bending angle was 180°. The repeatedly bent bent portion 100a of the test piece 100 was observed, and the adhesiveness of the pressure-sensitive adhesive sheet to the adherend in the bending test was evaluated as "good" when no peeling occurred between the pressure-sensitive adhesive sheet and the adherend (transparent polyimide film, polarizing film), and evaluated as "poor" when peeling occurred. The evaluation results are shown in Table 1.

[0119] On the other hand, a bending test was carried out on a test piece that had not been subjected to the first bending test under the same conditions as the first bending test except that the temperature was changed to 25° C. (second bending test). The evaluation results are shown in Table 1.

[0120] Each of the pressure-sensitive adhesive sheets of Examples 1 to 4 has a shear storage modulus G' (25°C) of 200 kPa or less at a frequency of 1000 Hz, and a loss tangent tanδ (25°C) of 0.2 or more at frequencies of 1 to 100 Hz. Each of the pressure-sensitive adhesive sheets of Examples 1 to 4 exhibited good adhesion to the adherend in both the first bending test (-20°C) and the second bending test (25°C). In contrast, the pressure-sensitive adhesive sheet of Comparative Example 1 did not have a good balance between adhesive strength and modulus compared to the pressure-sensitive adhesive sheets of Examples 1 to 4, and did not exhibit good adhesion to the adherend in the second bending test (25°C).

[0121] [Table 1] [Explanation of symbols]

[0122] 10 Adhesive sheet (optical adhesive sheet) 11,12 Adhesive surface H Thickness direction L1, L2 Release liner 21 First member 22 Second member

Claims

1. An optical adhesive sheet, The shear storage modulus at 25° C. and a frequency of 1000 Hz is 200 kPa or less; An optical adhesive sheet having a loss tangent tanδ at 25°C of 0.2 or more at a frequency of 1 to 100 Hz.

2. The optical adhesive sheet according to claim 1, wherein the loss tangent tan δ at 25 ° C. has a minimum value in the frequency range of 1 to 10 Hz.

3. The loss tangent tan δ at 25 ° C. has a minimum value Vmin in the frequency range of 1 to 10 Hz and a maximum value Vmax in the frequency range of 0.01 to 1 Hz, and the ratio of the maximum value Vmax to the minimum value Vmin is 1.2 or more and 1.7 or less. The optical adhesive sheet according to claim 1.

4. The optical adhesive sheet according to claim 1 , having a relative dielectric constant of 4.0 or less at 100 kHz.

5. 5. The optical adhesive sheet according to claim 1, which has an adhesive strength of 2.0 N / 10 mm or more in a peel test under conditions of 25°C, a peel angle of 180°, and a tensile speed of 60 mm / min.

Citation Information

Patent Citations

  • Laminate, touch panel, laminate formation kit, and, method of improving bending resistance of transparent conductive film

    JP2017065217A

  • Photocurable adhesive sheet, photocurable adhesive sheet with release sheet, optical film with photocurable adhesive sheet, laminate for constituting image display device and image display device

    JP2020125370A

  • Optical adhesive sheet having release liners

    JP2023069650A

  • Adhesive sheet for image display device, method for manufacturing image display device, and image display device

    WO2013161666A1

  • Optical adhesive sheet for foldable device

    WO2022163637A1