Polyvinyl alcohol film and optical film produced from the same

By controlling the elution amount and storage modulus of polyvinyl alcohol films, the issues of film breakage and red light leakage in polarizing films are addressed, achieving high transmittance and low leakage rates.

JP2024169407AActive Publication Date: 2024-12-05CHANG CHUN PETROCHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024084382
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-22
Filing Date
2024-05-23
Publication Date
2024-12-05
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

Conventional polyvinyl alcohol films are prone to breakage during the production of polarizing films due to excessive stretching tension, and the resulting polarizing films often have low single transmittance and high red light leakage rates.

Method used

Control the elution amount of polyvinyl alcohol in water at specific conditions and adjust the storage modulus versus temperature curve to achieve a specific absolute value of slope, ensuring the polyvinyl alcohol film has a thickness of 45-75 μm and specific storage modulus ranges at 45°C and 55°C.

Benefits of technology

The modified polyvinyl alcohol film exhibits reduced stretching tension, resulting in polarizing films with high single transmittance and low red light leakage rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169407000001_ABST
    Figure 2024169407000001_ABST
Patent Text Reader

Abstract

To provide a polyvinyl alcohol film, and an optical film produced from the same.SOLUTION: A polyvinyl alcohol film contains a polyvinyl alcohol resin, wherein when the polyvinyl alcohol film is immersed in water at 40°C for one minute, an elution amount of the polyvinyl alcohol is 0.20 to 9.00 ppm / m2, when the polyvinyl alcohol film is raised from 30°C to 65°C at a temperature-rising rate of 1°C / min in the water and a storage elastic modulus (E')-versus-temperature curve is measured, the curve has an inclination value between 45°C to 55°C, and an absolute value of the inclination is 0.20 to 0.70 MPa / °C. The polyvinyl alcohol film has low drawing tension, therefore has characteristics that the film is difficult to be cut in drawing, and an optical film produced from the same has characteristics such as a high single transmittance and a low leakage rate of red light.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polyvinyl alcohol (PVA) products, and in particular, but not exclusively, to polyvinyl alcohol films and optical films made therefrom. [Background technology]

[0002] Polyvinyl alcohol (PVA) film is a hydrophilic material obtained by coating and drying an aqueous solution containing polyvinyl alcohol polymer and plasticizer. It has properties such as high transparency, mechanical strength, water solubility, and good processability, and is therefore widely used in packaging materials and various optical films for electronic devices, such as polarizing films.

[0003] The polarizing film obtained by processing the polyvinyl alcohol film through the polarizing process has the property of blocking only light from a specific direction, so that the brightness of the light that passes through can be controlled. Based on this property, the polarizing film is applied to various displays, glasses, and wearable terminals, and has become an indispensable component. The polarizing process generally includes processes such as swelling, stretching, and dyeing. Specifically, the polyvinyl alcohol film is placed in a solution and the above-mentioned process is carried out to diffuse the dye molecules into the molecules in the polyvinyl alcohol film, and a relatively regular arrangement is obtained by stretching, so that the polarizing film can absorb the light component parallel to the arrangement direction and pass the light component perpendicular to the arrangement direction to produce the property of polarizing light. However, conventional polyvinyl alcohol films are often prone to film breakage during the manufacture of polarizing films due to excessive stretching tension.

[0004] With regard to prior art such as the polyvinyl alcohol thin film disclosed in Patent Document 1, the average value of the detection intensity of positive silicon fragment ions obtained by cation analysis based on time-of-flight secondary ion mass spectrometry on at least one side of the polyvinyl alcohol thin film is 0.001 to 0.01, and the average value of the detection intensity of positive silicon fragment ions is the average value of the detection intensity of positive silicon fragment ions obtained by cation analysis based on a time-of-flight secondary ion mass spectrometry on any line parallel to the TD direction of the polyvinyl alcohol thin film at five points that divide the polyvinyl alcohol thin film into six equal parts in the TD direction. This technical means has realized that stretching breaks are unlikely to occur during uniaxial stretching.

[0005] In addition, the prior art also discloses that the properties of a polarizing film can be improved by modifying the structure of polyvinyl alcohol and adjusting the manufacturing process of a polyvinyl alcohol film or a polarizing film. For example, Patent Document 2 discloses a polarizing film that has excellent polarization performance and has little leakage of red light in a crossed Nicol state. In addition, prior art such as Patent Document 3 also discloses that a polarizing film with high polarization properties can be obtained by stretching at a high stretch ratio because the polyvinyl alcohol-based thin film has good stretchability and is not easily cut during the manufacturing of the polarizing film, and the elution and precipitation of the polyvinyl alcohol-based resin during the manufacturing of the polarizing film can be suppressed, thereby suppressing contamination of the polarizing film manufacturing equipment and enabling the manufacture with a high yield. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Taiwan Patent Publication No. 202233739 [Patent Document 2] Taiwan Patent Publication No. 201719207 [Patent Document 3] Taiwan Patent Publication No. 202400694 Summary of the Invention [Problem to be solved by the invention]

[0007] In the prior art, when a polarizing film is manufactured using a polyvinyl alcohol film, the polyvinyl alcohol film is often prone to breakage during the manufacture of the polarizing film due to excessive stretching tension, and the polarizing film made from this polyvinyl alcohol film often has the problems of low single-piece transmittance and high red light leakage. In this regard, the present inventors have found that by adjusting the polyvinyl alcohol film to have a specific amount of polyvinyl alcohol elution when immersed in water at a specific temperature and time, and that the curve of storage modulus (E') vs. temperature measured under specific conditions has a specific absolute value of slope in a specific temperature range, thereby improving the problem that the polyvinyl alcohol film is prone to breakage during stretching, and further improving the problems of low single-piece transmittance and high red light leakage of the polarizing film manufactured thereafter. [Means for solving the problem]

[0008] Specifically, one embodiment of the present invention contains a polyvinyl alcohol resin, and when immersed in water at 40° C. for 1 minute, the amount of polyvinyl alcohol eluted is 0.20 to 9.00 ppm / m 2 The polyvinyl alcohol film is heated in water from 30°C to 65°C at a heating rate of 1°C / min, and a storage modulus (E') vs. temperature curve is measured, the curve having a slope between 45°C and 55°C, and the absolute value of the slope is 0.20 to 0.70 MPa / °C.

[0009] According to some embodiments of the present invention, the amount of elution of the polyvinyl alcohol is 1.60 to 7.20 ppm / m 2 and the absolute value of the slope is 0.20 to 0.60 MPa / °C.

[0010] According to some embodiments of the present invention, the absolute value of the slope is 0.25 to 0.60 MPa / °C.

[0011] According to some embodiments of the present invention, the absolute value of the slope is 0.35 to 0.55 MPa / °C.

[0012] According to some embodiments of the present invention, the polyvinyl alcohol film has a storage modulus (E') at 45°C of 5.00 to 14.00 MPa, and a storage modulus (E') at 55°C of 3.00 to 7.00 MPa.

[0013] According to some embodiments of the present invention, the polyvinyl alcohol film has a storage modulus (E') at 45°C of 8.00 to 11.50 MPa, and a storage modulus (E') at 55°C of 4.00 to 6.00 MPa.

[0014] According to some embodiments of the present invention, the polyvinyl alcohol film has a compressive strength of 13.0 to 30.0 N / mm when immersed in a 2 wt % aqueous boric acid solution at 50° C. for 30 seconds. 2 The stretching tension is

[0015] According to some embodiments of the present invention, the polyvinyl alcohol resin has an average degree of polymerization of 1,500-3,500.

[0016] According to some embodiments of the present invention, the polyvinyl alcohol resin has a Polydispersity Index (PDI) of 3.5 or less.

[0017] According to some embodiments of the present invention, the polyvinyl alcohol film has a thickness of 45 to 75 μm.

[0018] Another aspect of the present invention provides an optical film made from the polyvinyl alcohol film described above.

[0019] According to some embodiments of the present invention, the optical film is a polarizing film.

[0020] According to some embodiments of the present invention, the polarizing film has a single-piece transmittance of 42.5% or more and a red light leakage rate of less than 5.0%. Effect of the Invention

[0021] The polyvinyl alcohol film of the present invention is suitable for use in various applications, particularly as an optical film such as a polarizing film. The polyvinyl alcohol film obtained based on the technical content of the present invention is less likely to break due to the small stretching tension during the manufacture of the polarizing film. The polarizing film made of the polyvinyl alcohol film has a low red light leakage rate and a high single transmittance.

[0022] Furthermore, the inventors have also discovered that the red light leakage rate of a polarizing film made of the polyvinyl alcohol film can be further improved by controlling the polyvinyl alcohol film so that it has a specific range of storage modulus (E') under temperature conditions of 45°C and 55°C, respectively.

[0023] In order to make the above and other objects, features, advantages and embodiments of the present invention more comprehensible, reference is made to the following drawings. [Brief description of the drawings]

[0024] [Figure 1] FIG. 2 is a schematic diagram showing an analysis of the absolute value of the slope of the storage modulus (E′) vs. temperature curve of a polyvinyl alcohol film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an analysis of the absolute value of the slope of the storage modulus (E′) vs. temperature curve of a polyvinyl alcohol film according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing an analysis of the absolute value of the slope of the storage modulus (E′) vs. temperature curve of a polyvinyl alcohol film according to one embodiment of the present invention. [Figure 4] FIG. 2 is a schematic diagram showing an analysis of the absolute value of the slope of the storage modulus (E′) vs. temperature curve of a polyvinyl alcohol film according to one embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing the analysis of the single transmittance and red light leakage rate of a polarizing film corresponding to a polyvinyl alcohol film according to one embodiment of the present invention. [Figure 6] 6A and 6B are schematic diagrams illustrating the analysis of the single transmittance and red light leakage rate of a polarizing film equivalent to a polyvinyl alcohol film according to one embodiment of the present invention. [Figure 7] FIG. 2 is a schematic diagram showing sampling for analyzing the red light leakage rate of a polarizing film corresponding to a polyvinyl alcohol film according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] In order to make the description of the present invention more detailed and complete, the following provides an illustrative description of the embodiments and specific examples of the present invention, which are not the only ways of implementing or operating the specific examples of the present invention. In this specification and the appended claims, "a" and "the" may also be interpreted as plural unless the context dictates otherwise.

[0026] The numerical ranges and parameters specifying the present invention are approximate, but the relevant numerical values ​​in the specific examples are presented as precisely as possible. However, any numerical value necessarily contains standard deviations inherent in each individual testing method. As used herein, the term "about" indicates that the actual value is within an acceptable standard error of the mean and is within the belief of one of ordinary skill in the art to which the present invention pertains.

[0027] [Polyvinyl alcohol film] One embodiment of the present invention contains a polyvinyl alcohol resin, and when immersed in water at 40° C. for 1 minute, the amount of polyvinyl alcohol eluted is 0.20 to 9.00 ppm / m 2and a storage modulus (E') vs. temperature curve is measured in water at a heating rate of 1°C / min from 30°C to 65°C, the curve having a slope between 45°C and 55°C, and the absolute value of the slope is 0.20 to 0.70 MPa / °C. According to some embodiments of the present invention, the polyvinyl alcohol film has a thickness of 45 to 75 μm. Specifically, the thickness is the following value or a value within a range between any two of these values, for example, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, and 75 μm, and the aforementioned values ​​are merely examples and are not limited thereto.

[0028] The "elastic modulus" mentioned in this specification is a physical property used to analyze the relationship between stress and strain in material mechanics, and is the ratio of stress to strain. The elastic modulus obtained when the stress applied to the material is a normal force is represented by E. The "storage modulus (E')" is the component that the material absorbs and converts the applied energy and stores it inside the material, and is usually used to recover from deformation and maintain the original appearance of the material, and is related to the elastic properties of the material.

[0029] The polyvinyl alcohol film is heated in water from 30°C to 65°C at a heating rate of 1°C / min, and a storage modulus (E') vs. temperature curve (hereinafter referred to as storage modulus vs. temperature curve) is measured. The curve has a double slope characteristic as shown in Figure 1, and the absolute value of the slope (dashed line in Figure 1) after the inflection point temperature is exceeded represents the dissolution rate of crystals in the polyvinyl alcohol film in water during the heating process. Since the heating rate during analysis is constant, the larger the absolute value of the slope, the faster the dissolution rate of crystals in the same time period is, and the smaller and more uniform the crystals in the polyvinyl alcohol film are. Without being bound by any particular theory, it is believed that the appropriate size and uniformity of the crystals in the polyvinyl alcohol film makes it easier to stretch and dye during the production of the polarizing film, and a polarizing film with high single-piece transmittance and low red light leakage rate is produced. Furthermore, the appropriate crystals reduce the tension during stretching, reducing the occurrence of film breakage. The inventors have found that if the absolute value of the slope is too large, the polyvinyl alcohol film will be prone to breakage due to insufficient mechanical strength, and if the absolute value of the slope is too small, the polyvinyl alcohol film will have too many undissolved crystals (i.e., crystals that remain without being completely dissolved), and the stretching tension will become too large, making the film prone to breakage.

[0030] Therefore, in order to improve the problem that the polyvinyl alcohol film is easily broken due to excessive stretching tension during stretching, and the single transmittance of the polarizing film obtained thereafter is low and the red light leakage rate is high, it is necessary to control the absolute value of the slope within a specific range. Specifically, the polyvinyl alcohol film is heated in water from 30°C to 65°C at a heating rate of 1°C / min, and the storage modulus (E') vs. temperature curve is measured, and the curve has a slope value between 45°C and 55°C, and the absolute value of the slope is 0.20 to 0.70 MPa / °C. Specifically, the analytical temperature is the following value or a value within a range between any two of these values, for example, 0.20 MPa / °C, 0.25 MPa / °C, 0.30 MPa / °C, 0.35 MPa / °C, 0.40 MPa / °C, 0.45 MPa / °C, 0.50 MPa / °C, 0.55 MPa / °C, 0.60 MPa / °C, 0.65 MPa / °C, and 0.70 MPa / °C, preferably 0.20 MPa / °C to 0.60 MPa / °C, more preferably 0.25 MPa / °C to 0.60 MPa / °C, and particularly preferably 0.35 MPa / °C to 0.60 MPa / °C. When the analytical temperature exceeds 55°C, the crystallization of the polyvinyl alcohol film may completely disappear and the physical properties may change suddenly. Therefore, when analyzing the absolute value of the slope, it is important to set the analytical temperature range not to exceed 55°C.

[0031] As for the method of analyzing the absolute value of the slope, since the polyvinyl alcohol film absorbs moisture (including moisture in the air) and may affect the state of its crystal form, molecular arrangement, etc., the moisture content of each polyvinyl alcohol film to be measured can be adjusted to the same by pretreatment before measuring the storage modulus (E') vs. temperature curve of the polyvinyl alcohol film, thereby making the state of each polyvinyl alcohol film to be measured the same. The moisture content can usually be adjusted to about 8 to 9% by weight, but is not limited thereto in the present specification.

[0032] The "amount of polyvinyl alcohol eluted" mentioned in this specification means that after the polyvinyl alcohol film is immersed in water, the phenomenon of polyvinyl alcohol elution occurs, and as the temperature of the water rises and the immersion time becomes longer, the amount of polyvinyl alcohol eluted increases. Since the temperature of the dye bath in the dyeing tank is generally about 20 to 45°C, the phenomenon of polyvinyl alcohol elution also occurs during dyeing of the polyvinyl alcohol film. Without being bound by a specific theory, the amount of polyvinyl alcohol eluted is probably related to the amount of polyvinyl alcohol that can be freely diffused in the amorphous region in the polyvinyl alcohol film. In other words, the higher the amount of polyvinyl alcohol eluted, the more polyvinyl alcohol that can be freely diffused, which indicates that the structure of the amorphous region in the polyvinyl alcohol film is loose but not tight, and relatively speaking, the dyeing solution can easily diffuse into the polyvinyl alcohol film through the loose structure and adsorb around the polyvinyl alcohol. The present inventors have found that if the amount of polyvinyl alcohol eluted is too large, the polyvinyl alcohol film is likely to excessively adsorb dye solution, and the color of the polarized film produced thereafter becomes too dark, resulting in an excessively low single-unit transmittance, and if the amount of polyvinyl alcohol eluted is too small, it becomes difficult to stretch or dye the polyvinyl alcohol film, and the polarized film produced thereafter may have an excessively low single-unit transmittance.

[0033] Therefore, in order to improve the single-piece transmittance of the polarizing film made of the polyvinyl alcohol film, it is necessary to control the amount of polyvinyl alcohol eluted within a specific range. Specifically, the amount of polyvinyl alcohol eluted after the polyvinyl alcohol film is immersed in water at 40° C. for 1 minute is 0.20 to 9.00 ppm / m 2 Specifically, the following values ​​or values ​​within a range between any two of these values, for example 0.20 ppm / m 2 , 1.00 ppm / m 2 , 1.60 ppm / m 2 , 2.40 ppm / m 2 , 3.20 ppm / m 2 , 4.00 ppm / m2 , 4.80 ppm / m 2 , 5.60 ppm / m 2 , 6.40 ppm / m 2 , 7.20 ppm / m 2 ppm / m 2 , 8.00 ppm / m 2 and 9.00 ppm / m 2 and preferably 1.60 ppm / m 2 ~7.20ppm / m 2 It is.

[0034] The "storage modulus (E') of a polyvinyl alcohol film at 45°C (hereinafter referred to as the storage modulus at 45°C)" described in this specification can represent the degree of undissolved crystals of the polyvinyl alcohol film in water at a temperature of 45°C. Without being bound by a specific theory, it is believed that the degree of dye adsorption in the dyeing process in the polarizing film manufacturing process is related to the storage modulus at 45°C. The inventors have found that the higher the storage modulus at 45°C, the higher the degree of undissolved crystals of the polyvinyl alcohol film in water at 45°C, and therefore the lower the degree of dye adsorption, i.e., the smaller the amount of dye adsorption. When the amount of dye adsorption of a polyvinyl alcohol film is small, the I5 generated after stretching in a stretching tank is likely to be large. - If the amount of produced is too low, the final polarizing film is likely to have red light leakage problems.

[0035] Therefore, by controlling the storage modulus of the polyvinyl alcohol film at 45°C within a specific range, the red light leakage rate of the manufactured polarized film can be improved. Specifically, the storage modulus (E') of the polyvinyl alcohol film at 45°C is 5.00 to 14.00 MPa, specifically, the following values ​​or values ​​within a range between any two of these values, for example, 5.00 MPa, 5.5 MPa, 6.00 MPa, 6.5 MPa, 7.00 MPa, 7.5 MPa, 8.00 MPa, 8.5 MPa, 9.00 MPa, 9.5 MPa, 10.00 MPa, 10.5 MPa, 11.00 MPa, 11.5 MPa, 12.00 MPa, 12.5 MPa, 13.00 MPa, 13.5 MPa and 14.00 MPa, and preferably 8.00 to 11.50 MPa.

[0036] The term "storage modulus (E') of the polyvinyl alcohol film at 55°C (hereinafter referred to as storage modulus at 55°C)" described in this specification can represent the degree of insoluble crystals of the polyvinyl alcohol film in water at a temperature of 55°C. During the production of a polarizing film, the film is usually stretched at 55°C and immersed in a boric acid solution. Without being bound by a specific theory, it is believed that the degree of insoluble crystals of the raw film in the stretching process in the polarizing film production process is probably related to the storage modulus at 55°C. The inventors have found that the higher the storage modulus at 55°C, the higher the degree of insoluble crystals of the raw polyvinyl alcohol film and the smaller the amount of boric acid crosslinking. If the amount of boric acid crosslinking is small, the dye adsorbed on the polyvinyl alcohol film is easily washed away and lost, and the I5 generated after stretching is likely to be reduced. - If the yield is too low, the final polarizing film will be prone to red light leakage problems.

[0037] Therefore, by controlling the storage modulus of the polyvinyl alcohol film at 55°C within a specific range, the red light leakage rate of the manufactured polarized film can be improved. Specifically, the storage modulus (E') of the polyvinyl alcohol film at 55°C is 3.00 to 7.00 MPa, specifically, the following values ​​or values ​​within a range between any two of these values, for example, 3.00 MPa, 3.50 MPa, 4.00 MPa, 4.50 MPa, 5.00 MPa, 5.50 MPa, 6.00 MPa, 6.50 MPa and 7.00 MPa, and preferably 4.00 to 6.00 MPa.

[0038] According to some preferred embodiments of the present invention, the polyvinyl alcohol film has a lower stretching tension, which can reduce the possibility of film breakage due to excessive stretching tension when it is manufactured as a polarizing film. Specifically, when immersed in a 2 wt % boric acid aqueous solution at 50° C. for 30 seconds, the stretching tension of the polyvinyl alcohol film is 13.0 to 30.0 N / mm 2 Specifically, the following values ​​or values ​​within a range between any two of these values, for example, 13.0 N / mm 2 , 15.0N / mm 2 , 17.0N / mm 2 , 19.0N / mm 2 , 21.0N / mm 2 , 23.0N / mm 2 , 25.0N / mm 2 , 27.0N / mm 2 , 29.0N / mm 2 , 30.0N / mm 2 It is.

[0039] The "average degree of polymerization" referred to in this specification means a measured value obtained by the test method described in the JIS K 6726 (1994) standard. Without being bound by any particular theory, it is believed that the average degree of polymerization of the polyvinyl alcohol film is probably related to the size of the crystal particles produced. The inventors have found that if the average degree of polymerization is too high, the chain segments of the polyvinyl alcohol become long and difficult to move, the size of the crystal particles produced becomes non-uniform, and polyvinyl alcohol is difficult to dissolve, and if the average degree of polymerization is too low, crystals are difficult to form and the crystal particles are relatively non-uniform, so polyvinyl alcohol is easily dissolved. Therefore, they have found that in order to form crystal particles of uniform size, it is necessary to control the average degree of polymerization of the polyvinyl alcohol film within a specific range. Specifically, the average degree of polymerization of the polyvinyl alcohol resin is 1500 to 3500, specifically, the following values ​​or values ​​within a range between any two of these values, for example, 1500, 1700, 1900, 2100, 2300, 2500, 2700, 2900, 3100, 3300, and 3500.

[0040] The term "Polymer Dispersity Index (PDI)" used in this specification is used to describe the molecular weight distribution of a polyvinyl alcohol resin, and is the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn). According to some preferred embodiments of the present invention, the polyvinyl alcohol resin has a polydispersity index of 3.5 or less, specifically, for example, 3.5 or less, 3.3 or less, 3.1 or less, 2.9 or less, 2.7 or less, 2.5 or less, or 2.3 or less. Without being bound by a particular theory, the inventors have found that if the polydispersity index is too high, the polyvinyl alcohol film is more likely to dissolve low molecular weight polyvinyl alcohol, and the amount of polyvinyl alcohol dissolved becomes too large.

[0041] As described above, the polyvinyl alcohol film of the present invention is a film obtained by processing and molding a film-forming material containing a polyvinyl alcohol resin. During the production of the film, a plasticizer, a surfactant, or other known additives may be added as a film-forming material.

[0042] The polyvinyl alcohol resin used is polymerized from a vinyl ester resin monomer to form a polyvinyl ester resin having a degree of polymerization of 1500 to 3500 and a polydispersity index of 3.5 or less, and then undergoes a saponification reaction to obtain a polyvinyl alcohol resin. Examples of the vinyl ester resin monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl octoate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, 2,2,4,4-tetramethyl vinyl valerate, and ethenyl 2,2-dimethylpropanoate, but the present invention is not limited thereto, and examples thereof include ethylene acetate. The vinyl ester polymer is preferably a polymer obtained by using one or more vinyl ester monomers as a monomer, and more preferably a polymer obtained by using one vinyl ester monomer as a monomer. The vinyl ester polymer may be a copolymer of one or more vinyl ester monomers and other copolymerizable monomers.

[0043] The amount of the copolymerization monomer to be added may be, for example, 2 to 4 mol %, but is not limited thereto, and may be, for example, 2.0, 2.5, 3.0, 3.5, or 4.0 mol %. Olefin compounds having 3 to 30 carbon atoms, such as ethylene, propylene, 1-butene, and isobutylene; acrylic acid or a salt thereof; methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, octadecyl acrylate, etc. methacrylic acid or its salts; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, 2-ethylhexyl acrylate, dodecyl methacrylate, methacrylic acid, and methacrylic acid; acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, and acrylamidopropanesulfonic acid. or its salt, acrylamide derivatives such as acrylamidopropyldimethylamine or its salt, and N-hydroxymethylacrylamide or its derivative; methacrylamide derivatives such as methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidepropylsulfonic acid or its salt, methacrylamidepropyldimethylamine or its salt, and N-hydroxymethylmethacrylamide or its derivative; N-vinylamides such as N-vinylformamide, N-vinylacetamide, and N-vinylpyrrolidone; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, tert-butyl vinyl ether, dodecyl vinyl ether, and stearyl vinyl ether; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride; allyl compounds such as allyl acetate and allyl chloride; maleic acid or its salts, esters, or anhydrides;Examples of the monomer include itaconic acid or its salt, ester, or anhydride, maleic acid or its salt or ester, propargyl acetate, etc.; vinyl silicon compounds such as vinyltrimethoxysilane; and isopropenyl acetate. The vinyl ester polymer may have one or more structural units derived from these copolymerization monomers.

[0044] The saponification degree of the polyvinyl alcohol resin used is 95 mol% or more, and the "saponification degree" is a measured value obtained by a test method described in the JIS K 6726 (1994) standard. In one or more embodiments, the saponification degree is, for example, 95 mol% or more, 96 mol% or more, 97 mol% or more, 98 mol% or more, 99 mol% or more, or 99.5 mol% or more. Preferably, the saponification degree is 99.95 mol% or more, more preferably 99.97 mol% or more, for example, 99.97 mol% or more, 99.98 mol% or more, or 99.99 mol% or more.

[0045] According to some embodiments of the present invention, the "plasticizer" described herein is specifically, but not limited to, glycerin, ethylene glycol, propylene glycol, diethylene glycol, diglycerol, triethylene glycol, tetraethylene glycol, trimethylolpropane, etc., or a combination thereof. In the present invention, glycerin is preferred. In one or more embodiments, the amount of the plasticizer added is 5 to 15% by weight relative to the weight of the polyvinyl alcohol resin, specifically, for example, 6% by weight, 7% by weight, 8% by weight, 9% by weight, 10% by weight, 11% by weight, 12% by weight, 13% by weight, 14% by weight, and 15% by weight, but not limited thereto. In a preferred embodiment, the amount of the plasticizer added is 10% by weight relative to the weight of the polyvinyl alcohol resin.

[0046] In addition to the plasticizer, other additives including, but not limited to, surfactants may be added as necessary in the dissolving step. The surfactants include, but are not limited to, cationic, anionic or nonionic surfactants, and specifically include carboxylate type such as potassium laurate, sulfate type such as sodium lauryl sulfate, sulfonate type such as dodecylbenzenesulfonate, alkylphenyl ether type such as polyoxyethylene octylphenyl ether, alcohol phenyl ether type such as polyethylene glycol monooctylphenyl ether, alkyl ester type such as polyethylene glycol monolaurate, alkylamine type such as polyoxyethylene laurylamino ether, alkylamide type such as polyoxyethylene lauramide, polypropylene glycol ether type such as polyoxyethylene polyoxypropylene ether, alkanolamide type such as lauric acid diethanolamide, oleic acid diethanolamide, allyl phenyl ether type such as polyoxyallyl phenyl ether, or sodium lauryl alcohol polyoxyethylene ether sulfate. The amount of surfactant added is 600 to 3000 ppm relative to the weight of the polyvinyl alcohol resin, but is not limited thereto.

[0047] Furthermore, the polyvinyl alcohol film may further contain components such as a water-soluble polymer, a defoamer, an antioxidant, an ultraviolet absorber, a lubricant, other polymer compounds, or combinations thereof, as long as the effects of the present invention are not impaired.

[0048] [Method of manufacturing polyvinyl alcohol film] The method for producing a polyvinyl alcohol film of the present invention includes: (a) a dissolving step of heating and dissolving a polyvinyl alcohol-based resin and adjusting the concentration of the polyvinyl alcohol-based resin to form a polyvinyl alcohol casting solution; (b) a casting step of casting the polyvinyl alcohol casting solution onto a casting drum and peeling it off from the casting drum to obtain a preformed film; (c) a heating roller step of contacting the polyvinyl alcohol preformed film with a plurality of heating rollers to obtain a polyvinyl alcohol film preform; (d) a heat treatment step of placing the polyvinyl alcohol film preformed product in a heat treatment device to heat treat it, and then obtaining a polyvinyl alcohol film semi-formed product; and (e) a temperature and humidity adjustment step of placing the polyvinyl alcohol film molded product in a temperature and humidity regulator and adjusting the temperature and humidity to obtain a polyvinyl alcohol film molded product.

[0049] <Dissolution process> According to some embodiments of the present invention, the dissolving step is performed by stirring the film-forming materials, such as polyvinyl alcohol-based resin having a degree of polymerization of 1500-3500 and a polydispersity index of 3.5 or less, solvent, plasticizer, etc., while raising the temperature to 140°C-160°C (e.g., 140°C, 150°C or 160°C, but not limited thereto), for 1-3 hours, e.g., 1 hour, 2 hours or 3 hours. After the materials are uniformly dissolved, a polyvinyl alcohol aqueous solution is formed, and the concentration of the polyvinyl alcohol aqueous solution is adjusted to 25-35 wt% (e.g., 25 wt%, 30 wt%, or 35 wt%, but not limited thereto), to obtain a polyvinyl alcohol casting solution.

[0050] According to some embodiments of the present invention, the solvent used in the dissolving step is not particularly limited in the present invention, as long as it can dissolve polyvinyl alcohol resin. Examples of the solvent include, but are not limited to, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylenediamine, diethylenetriamine, etc., and the above solvents can be used alone or in combination of two or more. Considering environmental and economic aspects, it is preferable to use water as the solvent in the present invention.

[0051] <Casting process> According to some embodiments of the present invention, the casting process mainly involves sending the polyvinyl alcohol casting liquid to an extruder to be mixed uniformly again, degassed (for example, but not limited to, degassed with a double screw extruder), and then discharging the liquid from a T-die lip and casting it onto a rotating cast drum (also called a casting drum) at a temperature of 88°C to 98°C (for example, but not limited to, 90°C, 93°C, or 96°C) to form a film, thereby obtaining a polyvinyl alcohol preformed film. According to some embodiments of the present invention, in the casting process, the temperature of the polyvinyl alcohol casting liquid after being mixed uniformly again in the extruder and degassed must be controlled to at least 90°C (for example, but not limited to, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, or 98°C). According to another embodiment of the present invention, when the polyvinyl alcohol casting solution is cast onto a rotating high-temperature casting drum, the temperature of the casting drum is preferably 85 to 95°C, and the residence time of the polyvinyl alcohol on the casting drum is preferably 0.6 to 1.2 minutes.

[0052] <Heating roller process> According to some embodiments of the present invention, the heating roller process mainly involves contacting and drying the upper and lower surfaces of the polyvinyl alcohol preformed film peeled off from the casting drum with multiple heating rollers, and then obtaining a polyvinyl alcohol film preform. The temperature of the multiple heating rollers (for example, 13 heating rollers) gradually decreases from high to low, with the first heating roller being the roller with the highest temperature among all the heating rollers (for example, 90 to 99 ° C, but not limited thereto, specifically, for example, 90 ° C, 91 ° C, 92 ° C, 93 ° C, 94 ° C, 95 ° C, 96 ° C, 97 ° C, 98 ° C, or 99 ° C, but not limited thereto, preferably 95 ° C), and the temperature of the last heating roller being the lowest among all the heating rollers (for example, 30 to 40 ° C, but not limited thereto).

[0053] <Heat treatment process> According to some embodiments of the present invention, the heat treatment step is a step of heating and drying the polyvinyl alcohol film preform peeled off from the heating roller in the film thickness direction by heat radiation to obtain a polyvinyl alcohol film semi-formed product. The heat treatment is preferably performed by using infrared rays, and the film surface temperature of the polyvinyl alcohol film preform when heated by infrared rays is 80°C to 120°C, specifically, the following values ​​or values ​​within any two of these ranges, for example, 80°C, 90°C, 100°C, 110°C, and 120°C, and the heating time is 25 to 35 seconds, specifically, the following values ​​or values ​​within any two of these ranges, for example, 25 seconds, 27 seconds, 29 seconds, 31 seconds, 33 seconds, and 35 seconds. Without being bound by any particular theory, the inventors have found that if the surface temperature of the polyvinyl alcohol film preform during heating is too high, the size of the crystal particles produced will be large and the crystal distribution will be non-uniform, and if the surface temperature is too low, the size of the crystal particles will be too small or it will be even more difficult to form crystals, and the above two situations will have a negative effect on the absolute value of the slope of the storage modulus vs. temperature curve of the polyvinyl alcohol film produced thereafter.

[0054] <Temperature and humidity adjustment process> According to some embodiments of the present invention, the polyvinyl alcohol film semi-formed product is placed in a temperature and humidity controller at a specific time, and the temperature and relative humidity are adjusted to promote recrystallization. The temperature of the temperature and humidity controller can be controlled to 60°C to 80°C, specifically, the following values ​​or any two values ​​within the ranges thereof, for example, 60°C, 70°C, and 80°C, the relative humidity can be controlled to 60% to 80%, specifically, the following values ​​or any two values ​​within the ranges thereof, for example, 60%, 70%, and 80%, and the time can be controlled to 3 to 8 minutes, specifically, the following values ​​or any two values ​​within the ranges thereof, for example, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, and 8 minutes. Without being bound by any theory, the inventors have found that by increasing the high temperature and relative humidity, the recrystallization action and the rearrangement of polyvinyl alcohol are accelerated, the denseness of the structure in the polyvinyl alcohol film is improved, and the absolute value of the slope and the amount of polyvinyl alcohol eluted are affected.

[0055] [Optical film and its manufacturing method] Another object of the present invention is to provide an optical film made from said polyvinyl alcohol film. The "optical film" mentioned in this specification can be a polarizing film, a retardation film, a viewing angle widening film, a brightness enhancing film, etc., and is particularly a polarizing film.

[0056] According to some embodiments of the present invention, the single-layer transmittance of the polarizing film is 42.5% or more, for example 42.5% or more, 43.0% or more, or 43.5% or more, and the red light leakage rate of the polarizing film is less than 5.0%, for example less than 5.0%, less than 4.5%, less than 4.0%, less than 3.5%, less than 3.0%, less than 2.5%, less than 2.0%, less than 1.5%, or less than 1.0%.

[0057] According to some embodiments of the present invention, the "method of manufacturing an optical film" of the present application refers to a method of manufacturing a polarizing film, and further includes manufacturing a polyvinyl alcohol film into a polarizing film. The manufacturing method includes a dyeing step of adsorbing iodide ions, a boric acid treatment step, and a water washing step, and a stretching step of uniaxial stretching can be performed in the boric acid treatment step or a step before this. Preferably, a swelling step of swelling the polyvinyl alcohol film with water can be provided before the dyeing step. Note that a final drying step is usually provided after the water washing step.

[0058] In the swelling step, the polyvinyl alcohol film is immersed in a treatment bath (e.g., pure water) at a temperature of 30°C to 55°C, for example, to wash the film surface and perform a swelling treatment. The swelling treatment time is usually 5 to 300 seconds, preferably 20 to 240 seconds. According to some embodiments, a plurality of guide rollers are arranged in a swelling tank containing the treatment bath in order to transport the polyvinyl alcohol film. Next, the polyvinyl alcohol film is stretched in the machine direction (MD) to 1.05 to 2.5 times its original length, and then a dyeing step is performed.

[0059] In the dyeing process, the polyvinyl alcohol film that has been through the swelling process is immersed in a dyeing tank containing a dye bath. The dyeing conditions can be determined within a range in which iodine is adsorbed onto the polyvinyl alcohol film and does not cause defects such as extreme dissolution or devitrification of the film. The dye bath in the dyeing process can be, for example, an aqueous solution containing iodine and potassium iodide, and the concentration of iodine in the dye bath is preferably 0.01 to 0.5% by weight, and the concentration of potassium iodide is preferably 0.01 to 10% by weight. A specific example is an aqueous solution containing 0.037% by weight of iodine and 1.85% by weight of potassium iodide, but is not limited thereto. In place of potassium iodide, other iodides such as zinc iodide may be used, or other iodides may be used in addition to potassium iodide. The dye bath temperature is usually 20 to 45° C., for example, 40° C., and the dyeing time (dyeing time) is usually 10 to 600 seconds, preferably 30 to 200 seconds. Next, the polyvinyl alcohol film is stretched in the machine direction to 2 to 4 times its original length, and then a boric acid treatment and a stretching step are carried out.

[0060] In the boric acid treatment and stretching process, the polyvinyl alcohol film dyed with iodine is treated with a boric acid-containing aqueous solution to crosslink, and the adsorbed iodine is fixed to the resin. The process is usually carried out by immersing the polyvinyl alcohol film that has been subjected to the dyeing process in a fixing tank containing a boric acid-containing treatment bath. The boric acid treatment bath preferably contains iodide in addition to boric acid, and examples of the iodide used here include potassium iodide or zinc iodide, and examples of the iodide include aqueous solutions containing boric acid and potassium iodide at a concentration of 5.5% by weight each. In addition, compounds other than iodide, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, sodium sulfite, potassium sulfate, sodium sulfate, etc. may also be present in the boric acid treatment bath. The boric acid treatment and stretching process are usually carried out at 50 to 70°C, for example at a temperature of 55°C, and the treatment time is usually 10 to 600 seconds, preferably 20 to 300 seconds, and more preferably 20 to 100 seconds. Next, the polyvinyl alcohol film is stretched in the machine direction to 3 times or more of the original length, and the subsequent process is carried out. The upper limit of the stretching ratio is not particularly limited, but is preferably less than 8 times, for example. The stretching ratio includes, but is not limited to, 3.3 times or more, for example, 3.3 to 8.0 times, more preferably 3.5 to 6.0 times, and particularly preferably 4.0 to 5.5 times.

[0061] After the polyvinyl alcohol film is subjected to the above process and the subsequent washing and drying processes, a polarizing film is formed. In the washing and drying processes, the iodine solution and boric acid remaining on the film surface are washed with water or an aqueous solution containing iodide (for example, but not limited to, an aqueous solution of potassium iodide with a concentration of 5.5% by weight). Next, after a drying process (for example, but not limited to, drying in an oven at a temperature of 60°C for 5 minutes), a polarizing film is formed.

[0062] Furthermore, the polarizing film includes a protective layer attached to at least one surface of the polarizing film. The protective layer is preferably a component having a function such as preventing abrasion of the surface of the polarizing film. According to different embodiments, the protective layer may be provided on only one surface of the polarizing film, or on both surfaces of the polarizing film. The protective layer may be a protective film made of a transparent resin material. The transparent resin may be an acrylic resin such as a methyl methacrylate resin, an olefin resin, a polyvinyl chloride resin, a cellulose resin, a styrene resin, an acrylonitrile-butadiene-styrene copolymer resin, an acrylonitrile-styrene copolymer resin, a polyvinyl acetate resin, a polyvinylidene chloride resin, a polyamide resin, a polyacetal resin, a polycarbonate resin, a modified polyphenylene ether resin, a polyester resin (such as a polybutylene terephthalate resin or a polyethylene terephthalate resin), a polysulfone resin, a polyethersulfone resin, a polyarylate resin, a polyimideimide resin, a polyimide resin, an epoxy resin, an oxetane resin, or the like, with a cellulose resin such as cellulose triacetate (TAC) being preferred. EXAMPLES

[0063] The present invention will be described in detail below with reference to specific examples. However, it will be understood that these specific examples are intended to aid in the understanding of the present invention and are not intended to limit the scope of the present invention in any way.

[0064] 1. Preparation of Polyvinyl Alcohol Film Here, the present invention provides a non-limiting method for preparing polyvinyl alcohol films. The polyvinyl alcohol films of the non-limiting examples (Examples 1-16) and the polyvinyl alcohol films of the comparative examples (Comparative Examples 1-6) are prepared in a manner similar to that disclosed below.

[0065] The following are the main steps of producing polyvinyl alcohol films in this embodiment and the comparative example, and the following Table 1 details the differences in one or more process parameters between this embodiment and the comparative example.

[0066] Dissolving step: First, 1800 kg of polyvinyl alcohol resin with a specific degree of polymerization and polydispersity index (specific degree of polymerization and polydispersity index are shown in Table 1), 4000 kg of water, and 180 kg of glycerin were added to a dissolving barrel, and the dissolving temperature was raised to 150°C while stirring, and the mixture was dissolved for 2 hours. After the mixture was dissolved uniformly, the concentration of the polyvinyl alcohol aqueous solution was adjusted to 30% by weight to obtain a polyvinyl alcohol casting liquid. The polyvinyl alcohol resin in the examples and comparative examples was a polyvinyl alcohol resin that was polymerized by vinyl acetate, was not modified (i.e., did not contain other comonomers), and had a saponification degree of 99.95 mol%.

[0067] Casting process: the polyvinyl alcohol casting solution was transported to an extruder, where it was uniformly mixed again and degassed. The temperature of the polyvinyl alcohol casting solution was then controlled to 98°C, after which the casting solution was discharged from a T-die lip and cast onto a rotating cast drum at a temperature of 96°C to form a film, thereby forming a polyvinyl alcohol preformed film.

[0068] Heating roller process: After the polyvinyl alcohol preformed film was peeled off from the casting drum, the upper and lower surfaces of the polyvinyl alcohol preformed film were dried by contact with 13 heating rollers while the temperature was lowered one by one. The first heating roller was the roller with the highest temperature (95°C) among all the heating rollers, and the 13th heating roller was the roller with the lowest temperature (30°C) among all the heating rollers, and a polyvinyl alcohol film preformed product was obtained.

[0069] Heat treatment step: Next, the polyvinyl alcohol film preform was heated and dried with infrared rays for 30 seconds, and the film surface temperature during infrared heating was controlled within a specific range (the specific film surface temperature during heating is shown in Table 1), to obtain a semi-formed polyvinyl alcohol film.

[0070] Temperature and humidity adjustment process: Next, the polyvinyl alcohol film semi-molded product was placed in a temperature and humidity controller and recrystallized at a specific temperature and relative humidity for a specific time (the specific temperature, relative humidity and time are shown in Table 1) to obtain a polyvinyl alcohol film molded product, and the polyvinyl alcohol film molded product had a specific thickness (the specific thickness is shown in Table 1).

[0071] [Table 1]

[0072] 2. Manufacturing of polarizing film Here, the present invention provides a non-limiting method for producing a polarizing film from a polyvinyl alcohol film. According to the method disclosed below, the polyvinyl alcohol films of the non-limiting examples (Examples 1-11) and the polyvinyl alcohol films of the comparative examples (Comparative Examples 1-6) are prepared into corresponding polarizers.

[0073] The following are the main steps common to the manufacture of polarizers from the vinyl alcohol films of the examples and comparative examples of the present invention. After unwinding the polyvinyl alcohol film, it is put into a swelling tank filled with pure water at 30°C to wash and swell the film surface, and the polyvinyl alcohol film is stretched to 1.2 times its original length in the machine direction, and then the temperature is controlled to 45°C and the film is dyed in a dyeing tank containing 0.037 wt% iodine and 1.85 wt% potassium iodide aqueous solution, and the polyvinyl alcohol film is stretched to 3.4 times its original length in the machine direction. After dyeing, the temperature is controlled to 55°C and the film is placed in a stretching tank containing an aqueous potassium iodide solution with a concentration of 5.5 wt% each of boric acid and potassium iodide, and the polyvinyl alcohol film is stretched to 6 times its original length along the machine direction, and then washed with iodine water and an aqueous solution containing 5.5 wt% potassium iodide of boric acid remaining on the film surface. Next, the film was dried in an oven at 60° C. for 5 minutes, and cellulose triacetate protective films were attached to the upper and lower surfaces and dried to produce a polarizing film.

[0074] 3.Analysis method Here, the present invention provides methods for analyzing and testing the polyvinyl alcohol films of Examples 1 to 11 and Comparative Examples 1 to 6 above.

[0075] Average degree of polymerization The average degree of polymerization in the present invention is measured by the test method described in JIS K 6726 (1994).

[0076] Polydispersity Index (PDI) Gel Permeation Chromatography (GPC) is used to test the peak molecular weight and polydispersity index of the polyvinyl alcohol resin.

[0077] Equipment and its brand (1) Waters 515 HPLC pump, (2) Waters 717plus autosampler, (3) A Waters 2414 refractive index detector with a detection temperature of 36°C. (4) Analytical column Waters Ultrahydrogel Guard Column, 125Å, 6μm, 6mm*40Mm, 1K~500K, Waters Ultrahydrogel 120 Column, 120Å, 6μm, 7.8mm*300Mm, 100~5K, Waters Ultrahydrogel 250 Column, 250Å, 6μm, 7.8mm*300Mm, 1K~80K, Waters Ultrahydrogel 500 Column, 500Å, 10μm, 7.8mm*300Mm, 5K~400K, Waters Ultrahydrogel 1000 Column, 1000Å, 12μm, 7.8mm*300Mm, 10K~1M.

[0078] Test conditions (1) Analysis flow rate: 0.413mL / min, (2) Flow liquor: 0.85% by weight sodium nitrate aqueous solution; (3) Column oven temperature: 36°C; (4) Standard: Polyethylene glycol (PEG), with peak molecular weight (Mp) of 1,608,000 / 1,039,000 / 545,000 / 117,900 / 66,200 / 28,330 / 16,100 / 3,860 / 1,450 / 610 / 194; (5) Analysis sample composition: 0.08 g of polyvinyl alcohol resin to be measured, 17 g of 0.85 wt% sodium nitrate aqueous solution, and 0.45 μm PTFE syringe filter, (6) Sample injection volume: 210 μL, (7)Exam duration: 106 minutes.

[0079] Data processing: The number average molecular weight (Mw) and weight average molecular weight (Mn) of the polyvinyl alcohol resin were calculated, and the polydispersity index (PDI) was calculated according to the following formula.

[0080] PDI=Mw / Mn

[0081] Storage modulus (E') and absolute value of the slope of its curve versus temperature Equipment and brand: TA Instruments DMA 850 Sample preparation method: A polyvinyl alcohol film is cut into a rectangle of 5 cm in the machine direction (MD) and 5 mm in the transverse direction (TD), and the moisture content of the polyvinyl alcohol film is adjusted to 8-9% by weight before being set in the machine to make the state of the polyvinyl alcohol film consistent. Next, referring to FIG. 2, one end of the polyvinyl alcohol film 2 is fixed with a dovetail clip 3 of about 1.11 g, and the other end is inserted into the immersion stretching jig 1, and a part of the polyvinyl alcohol film 2 is placed between the upper fixed shaft 1a and the lower fixed shaft 1b, and the bottom end 3a of the dovetail clip 3 is 1 cm away from the immersion stretching jig 1 (distance a shown in FIG. 2), and a space is provided between the upper end 2a of the polyvinyl alcohol film 2 and the upper end of the immersion stretching jig 1. Next, the upper fixed shaft 1a is tightened to fix the polyvinyl alcohol film 2. 3, the entire immersion stretching jig 1, the polyvinyl alcohol film 2 held therein, and the dovetail clip 3 are placed vertically in a 100 mL beaker 4 filled with pure water so that the liquid level of the beaker is located at the upper fixed shaft 1a, the beaker 4 is temperature-controlled in a thermostatic water bath (not shown) at 30° C., and a load (weight of the dovetail clip 3) is applied to the polyvinyl alcohol film 2 to cause it to swell for 20 minutes. Finally, referring to FIG. 4, the immersion stretching jig 1 is removed from the beaker 4 and held vertically, and the polyvinyl alcohol film 2 is stretched by the weight of the dovetail clip 3. After confirming that the polyvinyl alcohol film 2 is in the center, the lower fixed shaft 1b of the immersion stretching jig 1 is tightened, and the excess polyvinyl alcohol film 2c (the mesh-like portion in FIG. 4) is cut off, and the sample is the polyvinyl alcohol film 2b clamped to the immersion stretching jig 1 and subjected to the load and swelling.

[0082] Test conditions: When the above sample is still fixed in the immersion and stretching fixture, select the vibration heating mode, place the sample and the immersion stretching fixture 1 holding the sample together in an immersion bath filled with deionized water, set the frequency to 1Hz, the amplitude to 200μm, the force track to 200%, set the temperature to measure from 30℃ to 65℃, stretch the film with a static force of 0.15N before analysis, then start analyzing with a heating rate of 1℃ / min, and draw a storage modulus (E') vs. temperature change curve. Here, the detection end of the thermocouple is placed at a height of 5mm from the bottom of the water bath.

[0083] Data processing: Transform the coordinate axis of the storage modulus (E') into a linear coordinate axis and use the slope analysis built into the software provided with the instrument. Set the analysis temperature range to 30-45 °C. The software will auto-enter the calculated slope value and take the absolute value of the slope.

[0084] Storage modulus (E') at 45°C and 55°C: The storage modulus (E') values ​​were obtained at 45°C and 55°C on the linear coordinate storage modulus (E') vs. temperature curve described above.

[0085] Amount of polyvinyl alcohol eluted Reagent composition (1) Boric acid solution: 20.00 g of boric acid was weighed into a 500 mL transparent measuring bottle, and first dissolved in a small amount of deionized water (DI water), then added deionized water up to the 500 mL horizontal scale line. (2) Iodine solution: 1.27 g of solid iodine and 2.50 g of potassium iodide were weighed into a 100 mL brown measuring bottle and first dissolved in a small amount of deionized water (DI water), then added up to the 100 mL horizontal scale line.

[0086] Preparation of calibration curve: Polyvinyl alcohol resin with a degree of polymerization of 2400, a degree of saponification of 99.9 mol%, and a polydispersity index of 2.2 was dried at 105 ° C for 3 hours until completely dried, and then standards with polyvinyl alcohol resin concentrations of 100 ppm, 50 ppm, 25 ppm, 12.5 ppm, 6.25 ppm, 3.125 ppm, 1.5625 ppm, and 0.78125 ppm were prepared, and the absorbance at 670 nm was analyzed to prepare a calibration curve. 20 g of the standard was taken and placed in a grinding serum bottle, and 15 mL of boric acid solution, 3 mL of iodine solution, and 12 mL of deionized water were added in that order, shaken to mix uniformly, and then left for 15 minutes.

[0087] Test conditions: 1L of deionized water was placed in a serum bottle, and the serum bottle was placed in a thermostatic water bath at a temperature of 40°C. A polyvinyl alcohol film was cut into 20 test pieces with a machine direction (MD) of 5 cm and a transverse direction (TD) of 5 cm, and each test piece was immersed in the deionized water in the serum bottle, and after immersion for 1 minute, it was removed, and a total of 20 test pieces were continuously immersed. Next, the serum bottle was removed from the thermostatic bath, the serum bottle was cooled to 25°C, and the weight of the solution in the serum bottle was recorded. 20g of the solution in the serum bottle was weighed into a grinding serum bottle, and 15mL of boric acid solution, 3mL of iodine solution, and 12mL of deionized water were added in order, shaken to mix uniformly, and then left for 15 minutes. Next, the absorbance of the solution at 670 nm was analyzed using an ultraviolet-visible spectroscopy (UV-vis), and the result was applied to a calibration curve to back-calculate the concentration, thereby determining the amount of polyvinyl alcohol eluted.

[0088] Polyvinyl alcohol film thickness Equipment and brand: Mitutoyo 543-391B Test method: Before analysis, confirm that the scale of the contact probe on the stage is 0, then place the polyvinyl alcohol film to be tested flat on the stage, lift up the probe and gently place it on the polyvinyl alcohol film, and read the thickness value.

[0089] 4. Evaluation method and results Here, the present invention provides evaluation methods for polyvinyl alcohol films and polarizers in Examples and Comparative Examples, and the results of correlation with the above-mentioned analysis contents.

[0090] Evaluation of stretching tension Equipment and brand: HT-9102 tensile testing machine manufactured by Koda Sample preparation method: Cut the polyvinyl alcohol film into a rectangular test piece with a machine direction (MD) of 150 mm and a transverse direction (TD) of 12.7 mm. Place the test piece in an environment with a temperature of 23°C and a relative humidity of 50%, and after adjusting the temperature and humidity for 20 hours, immerse it in an aqueous solution of boric acid with a temperature of 50°C and a concentration of 2% by weight for 30 seconds. Immediately after immersion, set it in the equipment and test it.

[0091] Test conditions: the distance between the fixtures is 5 cm, the pulling speed is controlled at 240 mm / min, the thickness of the sample and the length along the machine direction and width direction are input into the computer, and the system automatically converts the stretching tension.

[0092] Film breakage evaluation Test conditions: A polyvinyl alcohol film is stretched continuously for 10,000 m to produce a polarizer.

[0093] Evaluation criteria ○: No breaks during manufacturing process ×: One or more tears occurred during the manufacturing process.

[0094] Single unit transmittance Equipment and brand: JASCO spectrophotometer V-7100 How to prepare samples: Cut the polarizing film into two square samples measuring 2 cm in the machine direction (MD) and 2 cm in the transverse direction (TD) at the center of its width.

[0095] Test conditions: Using a spectrophotometer V-7100 equipped with an integrating sphere, perform luminosity correction in the visible light region with a C light source and a 2° field of view according to the test method described in the JIS Z 8722 (2009) standard. As shown in Figure 5, overlapping samples are taken, and the machine direction MD1 of one sample is perpendicular to the machine direction MD2 of the other sample. As shown in Figure 6A, one of the samples is rotated clockwise so that the machine directions MD1 and MD2 of the two samples form an angle A of +45°, and the light transmittance T1 at a wavelength of 550 nm is measured, and as shown in Figure 6B, one of the samples is rotated counterclockwise so that the mechanical directions MD1 and MD2 of the two samples form an angle B of -45°, and the light transmittance T2 at a wavelength of 550 nm is measured. Next, calculate the single transmittance according to the following formula.

[0096] Ts(%) = (Ts1 + Ts2) / 2

[0097] Red light leakage rate Equipment and brand: JASCO spectrophotometer V-7100 How to prepare samples: Three locations were taken from the polarizing film: 5 cm from the left edge in the width direction (distance x shown in Figure 7), 5 cm from the center, and 5 cm from the right edge (distance x shown in Figure 7). Two square samples measuring 2 cm in the machine direction (MD) and 2 mm in the transverse direction (TD) were cut out from each of the three locations (Figure 7).

[0098] Test conditions Single piece transmittance Ts (%): According to the above-mentioned method for measuring single piece transmittance, the single piece transmittance Ts (%) is measured at three locations, the left end, the center, and the right end.

[0099] Transmittance T700⊥(%): Two samples were taken from the same location and stacked on top of each other. As shown in Figure 5, the machine direction MD1 of one sample is perpendicular to the machine direction MD2 of the other sample. As shown in Figure 6A, one of the samples was rotated clockwise so that the machine directions MD1 and MD2 of the two samples form an angle A of +45°. The light transmittance T 45Then, as shown in Figure 6B, one of the samples was rotated counterclockwise so that the mechanical directions MD1 and MD2 of the two samples form an angle B of 45°, and the optical transmittance T at a wavelength of 700 nm was measured. -45 Measure the T 45 and T -45 The average value is taken as the transmittance T700⊥(%) at the position.

[0100] Red light leakage rate: With single transmittance Ts (%) on the horizontal axis and transmittance T700⊥ (%) on the vertical axis, an approximation line is drawn from the analysis values ​​of three points, and the transmittance T700⊥ (%) when the single transmittance Ts is 44% (i.e. the orthogonal transmittance of light with a wavelength of 700 Nm) is determined from said approximation line, and this is the red light leakage rate.

[0101] Evaluation criteria: Red light leakage rate is preferably less than 5%.

[0102] Furthermore, Table 2 shows the results of the stretching tension evaluation and film breakage evaluation of the polyvinyl alcohol films of Examples 1 to 11 and Comparative Examples 1 to 6 of the present application, the single transmittance and red light leakage rate of the corresponding polarizing films, the absolute value of the slope of the storage modulus vs. temperature curve of the polyvinyl alcohol films (abbreviated as the absolute value of the slope in Table 2), and the amount of polyvinyl alcohol eluted.

[0103] [Table 2]

[0104] As can be seen from Table 2, the absolute value of the slope of the polyvinyl alcohol films of Examples 1 to 11 was in the range of 0.20 to 0.70 MPa / °C, and the amount of polyvinyl alcohol eluted was 0.20 to 9.00 ppm / m 2 The strength of these polyvinyl alcohol films ranges from 13.0 to 30.0 N / mm 2It was observed that the polyvinyl alcohol films had low stretching tension and good film breakage evaluation, and the polarizing films manufactured from these polyvinyl alcohol films all had high single-unit transmittance of 42.5% or more and low red light leakage rate of less than 5.0%. In contrast, the polyvinyl alcohol films of Comparative Examples 1 to 6 have absolute values ​​of the slope and the amount of polyvinyl alcohol eluted that are not within the ideal range, so these polyvinyl alcohol films and the corresponding polarizing films cannot simultaneously have the above-mentioned technical features. Therefore, only by simultaneously controlling the absolute value of the slope of the polyvinyl alcohol film and the amount of polyvinyl alcohol eluted within the ideal range, the problem of film breakage occurring easily when stretched by excessive stretching tension and the problems of low single-unit transmittance and high red light leakage rate of the polarizing films manufactured from the polyvinyl alcohol films can be improved.

[0105] Furthermore, Table 3 shows the results of red light leakage rate of the polarizing films corresponding to the polyvinyl alcohol films of Examples 1 to 11 and Comparative Examples 1 to 6 of the present application, and the storage modulus of the polyvinyl alcohol films at 45° C. and 55° C.

[0106] [Table 3]

[0107] As can be seen from Table 3, when the storage modulus of the polyvinyl alcohol film at 45°C is controlled to 5.00 to 14.00 MPa and the storage modulus at 55°C is controlled to 3.00 to 7.00 MPa, the polarizing film manufactured from the polyvinyl alcohol film has a low red light leakage rate of less than 5.0% as in Examples 1 to 11 and Comparative Examples 1, 3, 4 and 6. In contrast, when the storage modulus of the polyvinyl alcohol film at 45°C and the storage modulus at 55°C are not simultaneously controlled within the ideal range, the polarizing film manufactured from the polyvinyl alcohol film has a high red light leakage rate as in Comparative Examples 2 and 5. Therefore, the problem of high red light leakage rate of the polarizing film manufactured from the polyvinyl alcohol film can be improved only by simultaneously controlling the storage modulus of the polyvinyl alcohol film at 45°C and the storage modulus at 55°C within the ideal range.

[0108] All ranges provided herein are intended to include each specific range within the stated range, and combinations of subranges between the stated ranges. Also, any range explicitly stated herein includes the endpoints unless otherwise indicated. Thus, the range 1-5 specifically includes 1, 2, 3, 4, and 5, as well as subranges 2-5, 3-5, 2-3, 2-4, 1-4, etc.

[0109] All publications and patent applications cited in this specification are herein incorporated by reference and for all purposes are to the same extent as if each individual publication or patent application was specifically and individually indicated to be incorporated by reference herein. In the event of a conflict between the specification and a publication or patent application incorporated by reference herein, the specification shall control. [Explanation of symbols]

[0110] 1. Immersion stretching jig 1a Upper fixed shaft 1b Lower fixed shaft 2 Polyvinyl alcohol film 2a top end 2b Polyvinyl alcohol film after loading and swelling 2c Extra polyvinyl alcohol film 3 Dovetail Clips 3a bottom edge 4 Beaker a, x distance A, B angle MD1, MD2 machine direction

Claims

1. Contains polyvinyl alcohol resin, When immersed in water at 40°C for 1 minute, the amount of polyvinyl alcohol eluted was 0.20 to 9.00 ppm / m 2 and the storage modulus (E') vs. temperature curve is measured at a temperature rise rate of 1°C / min from 30°C to 65°C in water, the curve having a slope between 45°C and 55°C, and the absolute value of the slope is 0.20 to 0.70 MPa / °C. Polyvinyl alcohol film.

2. The amount of polyvinyl alcohol eluted is 1.60 to 7.20 ppm / m 2 and the absolute value of the slope is 0.20 to 0.60 MPa / °C.

3. The polyvinyl alcohol film according to claim 2, wherein the absolute value of the slope is 0.25 to 0.60 MPa / °C.

4. The polyvinyl alcohol film according to claim 3, wherein the absolute value of the slope is 0.35 to 0.55 MPa / °C.

5. 2. The polyvinyl alcohol film according to claim 1, having a storage modulus (E') of 5.00 to 14.00 MPa at 45°C and a storage modulus (E') of 3.00 to 7.00 MPa at 55°C.

6. 3. The polyvinyl alcohol film according to claim 2, having a storage modulus (E') of 8.00 to 11.50 MPa at 45°C and a storage modulus (E') of 4.00 to 6.00 MPa at 55°C.

7. When immersed in a 2% by weight aqueous solution of boric acid at 50°C for 30 seconds, the resistance is 13.0 to 30.0 N / mm 2 The polyvinyl alcohol film according to any one of claims 1 to 6, having a stretching tension of

8. The polyvinyl alcohol film according to any one of claims 1 to 6, wherein the polyvinyl alcohol resin has an average degree of polymerization of 1,500 to 3,500.

9. The polyvinyl alcohol film according to any one of claims 1 to 6, wherein the polyvinyl alcohol resin has a polydispersity index (Polymer Dispersity Index, PDI) of 3.5 or less.

10. The polyvinyl alcohol film according to any one of claims 1 to 6, having a thickness of 45 to 75 µm.

11. An optical film produced from the polyvinyl alcohol film according to any one of claims 1 to 10.

12. The optical film of claim 11 which is a polarizing film.

13. The optical film of claim 12 , wherein the polarizing film has a single-piece transmittance of 42.5% or more and a red light leakage rate of less than 5.0%.

Citation Information

Patent Citations

  • Polyvinyl alcohol-based film and method for producing the same

    JP2006219638A

  • Polyvinyl alcohol film and method for producing polarizing film

    JP2022033365A

  • Polyvinyl alcohol resin for production of polarizing film, method for producing same, polyvinyl alcohol film, method for producing polyvinyl alcohol film, polarizing film and polyvinyl alcohol resin

    WO2017033552A1

  • Adhesive and polarizing plate

    WO2020184657A1

  • Polyvinyl alcohol-based film for polarizing film production use, method for producing same, and polarizing film using same

    WO2024143239A1