Nonaqueous electrolyte secondary battery

By using a compound LPFO additive and adhesive-layered separators, the cycle characteristics of wide electrode bodies in non-aqueous electrolyte secondary batteries are improved, ensuring high capacity retention through enhanced adhesion and electrolyte circulation management.

JP2024170036AActive Publication Date: 2024-12-06PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023086955
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-12-06
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

Wide electrode bodies in non-aqueous electrolyte secondary batteries experience deterioration in cycle characteristics due to electrolyte circulation between the electrode plate and separator during repeated charging and discharging, leading to decreased performance.

Method used

Incorporating a compound LPFO additive in the electrolyte at specific concentrations and using a separator with adhesive layers to bond the electrode plates to the separator, along with housing the electrode body under pressure, to maintain adhesion and improve cycle characteristics.

Benefits of technology

The solution effectively suppresses deterioration in cycle characteristics, maintaining high capacity retention rates even with wide electrode bodies, achieving over 92% capacity retention after 500 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024170036000001_ABST
    Figure 2024170036000001_ABST
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte secondary battery which is capable of suppressing deterioration in cycle characteristics and includes a wide electrode body, and a method for manufacturing the same.SOLUTION: A nonaqueous electrolyte secondary battery includes an electrode body and an electrolytic solution. The electrode body is a wound type electrode body in which a positive electrode plate and a negative electrode plate are wound around a winding axis through a separator. The positive electrode plate and the negative electrode plate are bonded to the separator. The positive electrode plate includes a positive electrode active material layer, and the negative electrode plate includes a negative electrode active material layer. At least any one of the positive electrode active material layer and the negative electrode active material layer has a size in a winding axis direction of the electrode body of 150 mm or more. The electrolytic solution contains a solvent, an electrolyte, and an additive. The additive includes a compound LPFO represented by formula (1), and the content of the compound LPFO in the electrolytic solution is 0.15 mass% or more and 3.0 mass% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery and a method for manufacturing the same. [Background technology]

[0002] Japanese Patent Laid-Open Publication No. 2010-198858 (Patent Document 1) discloses that the use of a non-aqueous electrolyte solution containing 0.1% by weight or more and 5% by weight or less of a compound PFO suppresses capacity deterioration and output reduction due to charge-discharge cycles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2010-198858 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the case of a wide electrode assembly (e.g., a dimension of 15 cm or more in the longitudinal direction of the active material layer), the electrode plate and the separator are often bonded together to facilitate insertion into a can, prevent miswinding, and prevent springback. In a nonaqueous electrolyte secondary battery (hereinafter also referred to as a battery) including such an electrode assembly, the circulation of the electrolyte between the electrode plate and the separator may deteriorate during repeated charging and discharging, and the cycle characteristics may deteriorate.

[0005] An object of the present disclosure is to provide a non-aqueous electrolyte secondary battery having wide electrode plates in which deterioration of cycle characteristics is suppressed, and a method for manufacturing the same. [Means for solving the problem]

[0006] The present invention provides the following nonaqueous electrolyte secondary battery and method for producing the same. [1] A battery comprising an electrode body and an electrolyte solution, The electrode body is a wound electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween, The positive electrode plate and the negative electrode plate are bonded to a separator, The positive electrode plate includes a positive electrode active material layer, The negative electrode plate includes a negative electrode active material layer, At least one of the positive electrode active material layer and the negative electrode active material layer has a dimension of 150 mm or more in the winding axis direction of the electrode body, The electrolytic solution contains a solvent, an electrolyte, and an additive, The additive has the following formula (1): [ka] and a content of the compound LPFO in the electrolyte solution is 0.15% by mass or more and 3.0% by mass or less. [2] The nonaqueous electrolyte secondary battery according to [1], wherein the separator has a resin film and an adhesive layer disposed on at least one side of the resin film. [3] The nonaqueous electrolyte secondary battery according to [1] or [2], further comprising an outer casing, wherein the electrode assembly is housed in the outer casing while being subjected to pressure in a thickness direction. [4] The nonaqueous electrolyte secondary battery according to any one of [1] to [3], wherein the electrode body has a dimension in the winding axis direction of 180 mm or more. [5] The method includes a housing step of housing the electrode body in an outer casing and a liquid injection step of injecting an electrolyte, The electrode body is a wound electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween, The positive electrode plate and the negative electrode plate are bonded to a separator, The positive electrode plate includes a positive electrode active material layer, The negative electrode plate includes a negative electrode active material layer, At least one of the positive electrode active material layer and the negative electrode active material layer has a dimension of 150 mm or more in the winding axis direction of the electrode body, The electrolytic solution contains a solvent, an electrolyte, and an additive, The additive has the following formula (1): [ka] wherein the content of the compound LPFO in the electrolyte solution is 0.15% by mass or more and 3.0% by mass or less. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a nonaqueous electrolyte secondary battery including a wide electrode assembly in which deterioration of cycle characteristics is suppressed, and a method for manufacturing the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram showing an example of the configuration of a nonaqueous electrolyte secondary battery according to this embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the configuration of the electrode body in this embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing an example of the configuration of the electrode body in this embodiment. [Figure 4] FIG. 4 is a schematic diagram for explaining the preparation of the electrode body in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings, but the present invention is not limited to the following embodiment. In all of the drawings, the scale of each component is appropriately adjusted to make it easier to understand, and the scale of each component shown in the drawings does not necessarily match the scale of the actual component.

[0010] In this specification, elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."

[0011] FIG. 1 is a schematic diagram showing an example of the configuration of a battery in this embodiment. The battery 100 can be used for any purpose. For example, the battery 100 may be used as a main power source or a power source for power assist in an electric vehicle or the like. A battery module or a battery pack may be formed by connecting a plurality of batteries 100. The battery 100 may have a rated capacity of, for example, 1 to 200 Ah.

[0012] The battery 100 includes an electrode assembly 50 and an electrolyte. As shown in FIG. 1, the battery 100 may further include an exterior body 90. The exterior body 90 houses the electrode assembly 50 and an electrolyte (not shown). The exterior body 90 is rectangular (flattened rectangular parallelepiped). The exterior body 90 may be made of, for example, an aluminum (Al) alloy. The electrode assembly 50 may be housed in the exterior body 90 with pressure applied in the thickness direction (the D-axis direction in FIG. 1).

[0013] The exterior body 90 may include, for example, a sealing plate 91 and an exterior can 92. The sealing plate 91 closes the opening of the exterior can 92. For example, the sealing plate 91 and the exterior can 92 may be joined by laser processing or the like. The exterior body 90 may have any shape. The exterior body 90 may be, for example, in a pouch shape. That is, the exterior body 90 may be a pouch made of an Al laminate film or the like.

[0014] The sealing plate 91 is provided with a positive electrode terminal 81 and a negative electrode terminal 82. The sealing plate 91 may further be provided with an injection port (not shown), a gas exhaust valve (not shown), and the like. An electrolyte may be injected into the exterior body 90 from the injection port. The injection port may be closed by, for example, a sealing plug. The positive electrode current collecting member 71 connects the positive electrode terminal 81 and the electrode body 50. The positive electrode current collecting member 71 may be, for example, an Al plate. The negative electrode current collecting member 72 connects the negative electrode terminal 82 and the electrode body 50. The negative electrode current collecting member 72 may be, for example, a copper (Cu) plate.

[0015] The electrode body 50 may be a wound electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween. Each of the positive electrode plate, the negative electrode plate, and the separator may be, for example, a laminate having a band-like planar shape. A wound body may be formed by spirally winding the band-like laminate. The wound body may be, for example, cylindrical. A flat electrode body 50 may be formed by radially compressing the cylindrical wound body. The dimension of the electrode body 50 in the winding axis direction (hereinafter also referred to as the width direction) (W-axis direction in FIG. 1) may be, for example, 180 mm or more, or may be 180 mm or more and 300 mm or less.

[0016] FIG. 2 is a schematic diagram showing an example of the configuration of the electrode body in this embodiment. The electrode body 50 in FIG. 2 is a wound type electrode body having a winding axis R parallel to the W-axis direction. The electrode body 50 includes a laminate 40. The electrode body 50 may be substantially composed of the laminate 40. The laminate 40 includes a positive electrode plate 10, a negative electrode plate 20, and a separator 30. At least a part of the separator 30 is interposed between the positive electrode plate 10 and the negative electrode plate 20. The separator 30 separates the positive electrode plate 10 and the negative electrode plate 20. The positive electrode plate 10 and the negative electrode plate 20 are each bonded to the separator 30. The separator 30 may have an adhesive layer described later on one side or both sides. When the separator 30 has an adhesive layer described later, the positive electrode plate 10 and the negative electrode plate 20 can each be bonded to the separator 30 via the adhesive layer. The laminate 40 may include only one separator 30. The laminate 40 may include two separators 30. For example, the positive electrode plate 10 may be sandwiched between two separators 30. For example, the negative electrode plate 20 may be sandwiched between two separators 30. The laminate 40 may be formed by stacking, for example, a separator 30 (first separator), a negative electrode plate 20, a separator 30 (second separator), and a positive electrode plate 10 in this order.

[0017] FIG. 3 is a schematic cross-sectional view showing an example of the configuration of the electrode body in this embodiment. FIG. 3 shows a cross section perpendicular to the winding axis. The electrode body 50 includes a curved portion 51 and a flat portion 52. At the curved portion 51, the laminate 40 is curved. At the curved portion 51, the laminate 40 may be arc-shaped. At the flat portion 52, the laminate 40 is flat. The flat portion 52 is sandwiched between the two curved portions 51. The flat portion 52 connects the two curved portions 51. The thickness of the laminate 40 indicates the total thickness of the positive electrode plate 10, the negative electrode plate 20, and the separator 30 included in the laminate 40. The laminate 40 may have a thickness of, for example, 100 to 200 μm, or may have a thickness of 1 to 100 mm.

[0018] In the electrode body 50, the positive electrode plates 10 may have any number of layers. The number of layers of the positive electrode plates 10 indicates the number of times that a straight line that cuts the electrode body 50 in the layering direction intersects with the positive electrode plates 10. The layering direction indicates the direction in which the positive electrode plates 10, the negative electrode plates 20, and the separators 30 are layered in the electrode body 50. The layering direction in the wound electrode body 50 is parallel to the thickness direction of the positive electrode plates 10, the negative electrode plates 20, and the separators 30 in the flat portion 52 (the D-axis direction in FIG. 3).

[0019] As shown in FIG. 4, the electrode body 50 can be produced by stacking a positive electrode plate 10 and a negative electrode plate 20 with a separator 30 between them so that the aluminum foil of the positive electrode plate and the copper foil of the negative electrode plate are exposed at both ends, and then winding the laminate around one end of the laminate as the winding axis R.

[0020] The positive electrode plate 10 may have a number of laminations of, for example, 2 to 100. The negative electrode plate 20 may have a number of laminations of, for example, 2 to 100. The separator 30 may have a number of laminations of, for example, 4 to 200. The number of laminations of the negative electrode plate 20 and the separator 30 may be counted in the same manner as the number of laminations of the positive electrode plate 10.

[0021] The positive electrode plate 10 includes a positive electrode active material layer. In Fig. 1, the dimension of the positive electrode active material layer in a direction parallel to the winding axis direction (W axis direction) of the electrode body 50 is 150 mm or more, and may be, for example, 180 mm or more, 200 mm or more, or 220 mm or more, or may be 300 mm or less. The positive electrode active material layer will be described later.

[0022] The negative electrode plate 20 includes a negative electrode active material layer. In Fig. 1, the dimension of the negative electrode active material layer in a direction parallel to the winding axis direction (W-axis direction) of the electrode body 50 is 150 mm or more, and may be, for example, 180 mm or more, 200 mm or more, or 220 mm or more, or may be 300 mm or less. The negative electrode active material layer will be described later.

[0023] The positive electrode plate 10 includes a positive electrode core material 11 and a positive electrode active material layer 12 (see FIG. 2). The positive electrode active material layer 12 may be disposed on the surface of the positive electrode core material 11. The positive electrode active material layer 12 may be disposed on only one side of the positive electrode core material 11. The positive electrode active material layer 12 may be disposed on both the front and back sides of the positive electrode core material 11. The positive electrode core material 11 is a conductive sheet. The positive electrode core material 11 may include, for example, pure Al foil, Al alloy foil, or the like. The positive electrode core material 11 may have a thickness of, for example, 10 to 30 μm. The positive electrode core material 11 may be exposed at one end in the width direction (W-axis direction in FIG. 2) of the electrode body 50. A positive electrode current collecting member 71 may be joined to the exposed portion of the positive electrode core material 11 (see FIG. 1). The thickness of the positive electrode plate 10 may be, for example, 20 to 290 μm, 50 to 250 μm, or 100 to 200 μm. The longitudinal dimension of the positive electrode plate 10 may be, for example, 0.5 to 5 m, or 1 to 3 m.

[0024] The thickness of the positive electrode active material layer 12 indicates the total thickness of the positive electrode active material layers 12 included in the laminate 40. For example, when the positive electrode active material layers 12 are formed on both sides of the positive electrode plate 10, the thickness of the positive electrode active material layer 12 indicates the total thickness of the positive electrode active material layers 12 on both sides (two). The positive electrode active material layer 12 may have a thickness of, for example, 10 to 260 μm, may have a thickness of 20 to 60 μm, or may have a thickness of 30 to 50 μm. The thickness of the positive electrode active material layer 12 on one side (one) may be, for example, 10 to 30 μm, or may be 15 to 25 μm.

[0025] The positive electrode active material layer 12 may contain a lithium transition metal composite oxide. The lithium transition metal composite oxide may contain at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. For example, in the composition formula of "Li(NiCoMn)O2", the sum of the composition ratios in parentheses is 1. That is, "C Ni +C Co +C Mn =1" relationship is satisfied. For example, "C Ni " indicates the composition ratio of Ni. The composition ratio of each component is arbitrary as long as the sum of the composition ratios is 1. The positive electrode active material layer 12 may contain positive electrode active material particles. The positive electrode active material particles may contain any component. The positive electrode active material particles may contain the above-mentioned lithium transition metal composite oxide.

[0026] The positive electrode active material layer 12 may further contain, for example, a conductive material, a binder, and the like, in addition to the positive electrode active material particles. For example, the positive electrode active material layer 12 may be substantially composed of, by mass fraction, 0.1 to 10% of a conductive material, 0.1 to 10% of a binder, and the remainder being positive electrode active material particles. The conductive material may contain, for example, a carbon material, and the like. The binder may contain any component. The binder may contain, for example, polyvinylidene fluoride (PVdF), and the like. The filling density (after compression) of the positive electrode active material layer 12 is, for example, 3.0 g / cm. 3 More than 4.0g / cm 3 It may be the following:

[0027] The negative electrode plate 20 includes a negative electrode core material 21 and a negative electrode active material layer 22 (see FIG. 2). The negative electrode active material layer 22 may be disposed on the surface of the negative electrode core material 21. The negative electrode active material layer 22 may be disposed on only one side of the negative electrode core material 21. The negative electrode active material layer 22 may be disposed on both the front and back sides of the negative electrode core material 21. The negative electrode core material 21 is a conductive sheet. The negative electrode core material 21 may include, for example, a pure Cu foil, a Cu alloy foil, or the like. The negative electrode core material 21 may have a thickness of, for example, 5 to 30 μm. In the width direction (W-axis direction in FIG. 2) of the negative electrode plate 20, the negative electrode core material 21 may be exposed at one end. A negative electrode current collecting member 72 may be joined to the exposed portion of the negative electrode core material 21 (see FIG. 1). The thickness of the negative electrode plate 20 may be, for example, 20 to 290 μm, 50 to 250 μm, or 100 to 200 μm. The longitudinal dimension of the negative electrode plate 20 may be, for example, 0.5 to 5 m, or 1 to 3 m.

[0028] The thickness of the negative electrode active material layer 22 indicates the total thickness of the negative electrode active material layers 22 included in the laminate 40. For example, when the negative electrode active material layers 22 are formed on both sides of the negative electrode plate 20, the thickness of the negative electrode active material layers 22 indicates the total thickness of the negative electrode active material layers 22 on both sides (two). The negative electrode active material layers 22 may have a thickness of, for example, 10 to 260 μm, may have a thickness of 40 to 80 μm, or may have a thickness of 50 to 70 μm. The thickness of the negative electrode active material layer 22 on one side (one) may be, for example, 20 to 40 μm, or may be 25 to 35 μm. The packing density (after compression) of the negative electrode active material layers 22 is, for example, 1.3 g / cm. 3 More than 1.8g / cm 3 It may be the following:

[0029] The negative electrode active material layer 22 is made of, for example, graphite, silicon, silicon oxide, tin, tin oxide, and Li4Ti5O 12The negative electrode active material layer 22 may contain at least one selected from the group consisting of the negative electrode active material. The negative electrode active material layer 22 may contain negative electrode active material particles. The negative electrode active material particles may contain the above-mentioned negative electrode active material. The negative electrode active material layer 22 may be substantially composed of negative electrode active material particles. The negative electrode active material particles may be, for example, composite particles. The negative electrode active material particles may contain, for example, a substrate particle and a coating. The coating may cover the surface of the substrate particle. The substrate particle may contain, for example, graphite, etc. The coating may contain, for example, amorphous carbon, etc.

[0030] The negative electrode active material layer 22 may further contain a conductive material, a binder, and the like in addition to the negative electrode active material particles. For example, the negative electrode active material layer 22 may be substantially composed of 0 to 10% by mass of a conductive material, 0.1 to 10% by mass of a binder, and the remainder being negative electrode active material particles. The conductive material may contain any component. The conductive material may contain, for example, a carbon material, etc. The binder may contain any component. For example, the binder may contain at least one selected from the group consisting of carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR).

[0031] The separator 30 includes a resin film. The separator 30 may be substantially made of a resin film. The resin film may be substantially made of, for example, a polyolefin-based material. The polyolefin-based material may include, for example, at least one selected from the group consisting of polyethylene (PE) and polypropylene (PP). The resin film may have a thickness of, for example, 10 to 50 μm, may have a thickness of 10 to 30 μm, or may have a thickness of 10 to 20 μm. The resin film may be porous. The separator may have an air permeability of, for example, 100 to 300 sec / cc.

[0032] The separator 30 may have an adhesive layer on one side or both sides. The separator 30 may have a resin film and an adhesive layer disposed on at least one side of the resin film. The adhesive layer may have a function of bonding the positive electrode plate 10 and the separator 30, and bonding the negative electrode plate 20 and the separator 30. The separator 30 may preferably have an adhesive layer disposed on both sides from the viewpoint of ease of can insertion, prevention of winding slippage, and prevention of springback. The adhesive layer may contain, for example, an acrylic resin and a fluorine-based polymer. The fluorine polymer may contain, for example, PVdF, etc. The adhesive layer may further contain a filler. The filler may contain, for example, ceramic particles, etc. When the adhesive layer contains a filler, the content of the filler may be, for example, 70 mass% or more. The thickness of the adhesive layer may be, for example, 1 to 10 μm, or 1 to 5 μm. The thickness of the adhesive layer indicates the total thickness of the adhesive layers contained in the separator 30. For example, when the separator 30 has an adhesive layer on both sides, the total thickness of the adhesive layers on both sides (two) is indicated. The basis weight of the adhesive layer on the separator 30 (the total basis weight when two adhesive layers are included) is, for example, 6.0 to 10.0 g / m 2 It may be.

[0033] The separator 30 may have a heat-resistant layer on the side facing the positive electrode plate. When the separator 30 has an adhesive layer and a heat-resistant layer, the heat-resistant layer and the adhesive layer may be disposed in this order from the resin film side. The heat-resistant layer may contain, for example, an acrylic resin and a filler. The filler may contain, for example, ceramic particles. When the heat-resistant layer contains a filler, the content of the filler may be, for example, 90 mass % or more. The thickness of the heat-resistant layer may be, for example, 1 to 10 μm, or 1 to 5 μm.

[0034] The electrolyte is a liquid electrolyte. The electrolyte includes a solvent, an electrolyte, and an additive. The solvent is aprotic. The solvent may include any component. The solvent may include at least one selected from the group consisting of carbonate-based solvents, 1,2-dimethoxyethane (DME), methyl formate (MF), methyl acetate (MA), methyl propionate (MP), and γ-butyrolactone (GBL). The solvent preferably includes a carbonate-based solvent. Examples of carbonate-based solvents include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC).

[0035] The electrolyte is dissolved in a solvent. The electrolyte includes, for example, a lithium salt (hereinafter, also referred to as a Li salt). The Li salt may include, for example, at least one selected from the group consisting of LiPF6, LiBF4, and LiN(FSO2)2. The Li salt may have a molar concentration of, for example, 0.2 to 2.0 M (mol / L).

[0036] The additive has the following formula (1): [ka] The content of the compound LPFO in the electrolyte is 0.15% by mass or more and 3.0% by mass or less. When the content of the compound LPFO in the electrolyte is less than 0.15% by mass, it tends to be difficult to suppress the deterioration of the cycle characteristics. When the content of the compound LPFO in the electrolyte is more than 3.0% by mass, the amount of gas generated increases and it tends to be difficult to maintain the adhesion between the electrode assembly and the separator. From the viewpoint of cycle characteristics, the content of the compound LPFO in the electrolyte is preferably 0.2 to 1.2% by mass, more preferably 0.3 to 1.0% by mass. It is believed that by setting the content of LPFO, a compound that generates a relatively large amount of gas in the electrolyte, to between 0.15% by mass and 3.0% by mass, gas is generated during initial activation, causing localized peeling of the adhesion between the separator and the electrode plate, forming microscopic liquid-containing paths (paths through which liquid can flow) while maintaining adhesion throughout the wound body as a whole, improving circulation of the liquid during subsequent charging and discharging, and maintaining cycle performance (capacity retention rate during rapid charging cycles) even in wide electrode bodies.

[0037] The additive may further contain at least one selected from the group consisting of vinylene carbonate (VC) and vinyl ethylene carbonate (VEC) as a compound other than the compound LPFO. When the additive contains other compounds, the content of the other compounds in the electrolytic solution may be, for example, 0.01% by mass or more and 5% by mass or less.

[0038] The battery of the present disclosure can have a capacity retention rate of more than 92% in an evaluation of cycle characteristics. The evaluation of cycle characteristics is carried out according to the method described in the Examples section below.

[0039] The method for manufacturing a battery may include, for example, an accommodation step of accommodating the electrode body in an exterior body, and an electrolyte injection step. In the accommodation step, the aluminum foil of the positive current collecting member and the aluminum plate for external current collection of the electrode body are welded, and the copper foil of the negative current collecting member and the copper plate for external current collection of the electrode body are welded, and the battery is inserted into the outer case of the aluminum laminate film. In the electrolyte injection step, the above-mentioned electrolyte can be injected. After the electrolyte injection, the battery can be obtained by sealing and welding the can. EXAMPLES

[0040] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0041] [Separator] The following separators A and B were prepared. Both had an air permeability of 200 sec / cc. Separator A: A substrate (thickness: 12 μm) made of polyethylene resin, on both sides of which is an adhesive layer (thickness on one side: 2 μm, total thickness on both sides: 4 μm, basis weight: 4.0 g / m) made of acrylic resin (PVdF) containing 75% by mass of ceramic particles. 2 ) A separator with an adhesive layer. Separator B: A heat-resistant layer (thickness: 4 μm, basis weight: 8.0 g / m) made of an acrylic binder containing 90% by mass of ceramic particles on one side (positive electrode side) of a substrate (thickness: 12 μm) made of polyethylene resin. 2 ) A separator comprising:

[0042] [Positive plate] A positive electrode plate was prepared with a positive electrode active material layer containing a lithium transition metal composite oxide as a positive electrode active material, PVdF as a positive electrode binder, and a carbon material as a conductive material on both sides of an aluminum foil. The positive electrode plate had a thickness of 0.15 mm, a longitudinal dimension of 2.5 m, a packing density of the positive electrode active material layer of 3.5 g / cc, and a width of 220 mm.

[0043] [Negative plate] A negative electrode plate was prepared with a negative electrode active material layer containing graphite as a negative electrode active material, SBR and CMC as a negative electrode binder, and a carbon material as a conductive material on both sides of a copper foil. The thickness of the negative electrode plate was 0.18 mm, the dimension in the longitudinal direction was 2.75 m, the packing density of the negative electrode active material layer was 1.5 g / cc, and the width of the negative electrode active material layer was 224 mm.

[0044] [Electrolyte] Electrolyte A was prepared, which contained a solvent containing EC and EMC (volume ratio of EC:EMC=1:3), an electrolyte (1M LiPF6), a first additive (VC 0.8% by mass), and a second additive containing LPFO with the content shown in Table 1. Electrolytes B and C were also prepared, which contained LiPF2O2 and LiBOB, respectively, as the second additive. Furthermore, electrolyte D was prepared, which contained a solvent containing EC and EMC (volume ratio of EC:EMC=1:3), an electrolyte (1M LiPF6), a first additive (VC 0.8% by mass), and no second additive.

[0045] [Evaluation of cycle characteristics] The battery was repeatedly charged at 4.2 V at a current value of 1 C in a 25° C. environment and discharged to 3 V at a current value of 1 C as one cycle. The capacity retention rate was determined as the retention rate of the discharge capacity at the 500th cycle relative to the discharge capacity at the first cycle. The capacity retention rate was calculated using the following formula: Capacity retention rate = (500th cycle discharge capacity / 1st cycle discharge capacity) x 100 (%) The evaluation criteria are shown below. ○: Capacity retention rate of over 91%. △: Capacity retention rate of 87 to 91%. ×: Capacity retention rate less than 87%.

[0046] <Example 1> A laminate was prepared by stacking the positive and negative plates with separator A between them so that the aluminum foil of the positive plate and the copper foil of the negative plate were exposed at both ends, and the laminate was wound around one end of the laminate as a winding axis to prepare a wound electrode body (width: 300 mm). After pressing this wound body with 150 kN, the aluminum foil of the positive plate of the electrode body and the aluminum plate of the positive electrode current collector were welded, and the copper foil of the negative plate of the electrode body and the copper plate of the negative electrode current collector were welded, and the electrode body was inserted into an Al exterior can of a specified size, and 150 cc of electrolyte A was poured in, and the can was sealed and welded to prepare a battery cell. The evaluation results of the cycle characteristics are shown in Table 1.

[0047] <Comparative Examples 1 to 7> A battery cell was produced in the same manner as in Example 1, except that the electrolyte, second additive, and separator shown in Table 1 were used. When separator B was used, the positive and negative plates were not bonded to the separator. The evaluation results of the cycle characteristics are shown in Table 1.

[0048] [Table 1]

[0049] <Reference examples 1~5> Battery cells of Reference Examples 1 to 5 were produced in the same manner as in Example 1, Comparative Example 3, Comparative Example 4, Comparative Example 6, and Comparative Example 8, except that the widths of the positive electrode active material layer and the negative electrode active material layer were set to 110 mm and 112 mm, respectively. The evaluation results of the cycle characteristics are shown in Table 2.

[0050] [Table 2]

[0051] In Example 1 according to the present disclosure, superior cycle characteristics were obtained compared to Comparative Examples 1 to 7 not according to the present disclosure. Reference Examples 1 to 5 all had good cycle characteristics, which is believed to be because the electrolyte circulation is improved in the case of an electrode body with a narrow active material layer. It can be seen that the present disclosure provides a nonaqueous electrolyte secondary battery with a wide electrode body in which the deterioration of cycle characteristics is suppressed. [Explanation of symbols]

[0052] 10 positive electrode plate, 11 positive electrode core material, 12 positive electrode active material layer, 20 negative electrode plate, 21 negative electrode core material, 22 negative electrode active material layer, 30 separator, 40 laminate, 50 electrode body, 51 curved portion, 52 flat portion, 71 positive electrode current collector, 72 negative electrode current collector, 81 positive electrode terminal, 82 negative electrode terminal, 90 exterior body, 91 sealing plate, 92 exterior can, 100 battery, W width direction, R winding axis.

Claims

1. An electrode assembly and an electrolyte solution are included. The electrode body is a wound electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween, The positive electrode plate and the negative electrode plate are bonded to a separator, The positive electrode plate includes a positive electrode active material layer, The negative electrode plate includes a negative electrode active material layer, At least one of the positive electrode active material layer and the negative electrode active material layer has a dimension of 150 mm or more in a winding axis direction of the electrode body, The electrolytic solution contains a solvent, an electrolyte, and an additive, The additive has the following formula (1): 【Chemistry 1】 and a content of the compound LPFO in the electrolyte solution is 0.15% by mass or more and 3.0% by mass or less.

2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the separator comprises a resin film and an adhesive layer disposed on at least one side of the resin film.

3. The nonaqueous electrolyte secondary battery according to claim 1 , further comprising an outer casing, the electrode assembly being housed in the outer casing with pressure being applied in a thickness direction of the electrode assembly.

4. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrode body has a dimension of 180 mm or more in the direction of the winding axis.

5. The method includes a housing step of housing the electrode body in an outer casing and a liquid injection step of injecting an electrolyte, The electrode body is a wound electrode body in which a positive electrode plate and a negative electrode plate are wound with a separator interposed therebetween, The positive electrode plate and the negative electrode plate are bonded to a separator, The positive electrode plate includes a positive electrode active material layer, The negative electrode plate includes a negative electrode active material layer, At least one of the positive electrode active material layer and the negative electrode active material layer has a dimension of 150 mm or more in a winding axis direction of the electrode body, The electrolytic solution contains a solvent, an electrolyte, and an additive, The additive has the following formula (1): 【Chemistry 2】 and a content of the compound LPFO in the electrolyte solution is 0.15% by mass or more and 3.0% by mass or less.

Citation Information

Patent Citations

  • Nonaqueous electrolyte battery, electrode for nonaqueous electrolyte battery, and manufacturing method of this electrode for nonaqueous electrolyte battery

    JP2007123237A

  • Nonaqueous electrolyte secondary battery, manufacturing method of nonaqueous electrolyte secondary battery, and nonaqueous electrolyte

    JP2013145724A

  • Lithium ion secondary battery

    JP2014107222A

  • Electrochemical device

    JP2014116237A

  • Battery separator, electrode body, nonaqueous electrolyte secondary battery, and method for manufacturing battery separator

    JP2022064377A