Marine biodegradable polymer compound having aliphatic unsaturated carbon-carbon bond and method for producing the same
A marine biodegradable polymer compound with aliphatic unsaturated bonds and specific side-chain substituents addresses the challenge of biodegradability in low microorganism environments by promoting ion exchange and microbial decomposition in seawater, enhancing the degradation of resin materials.
Patent Information
- Application Number
- JP2023087000
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
AI Technical Summary
Existing biodegradable resins face challenges in degrading effectively in marine environments with low microorganism concentrations, such as oceans, and often require combinations with non-biodegradable materials to maintain physical properties, leading to reduced biodegradability.
A marine biodegradable polymer compound with aliphatic unsaturated carbon-carbon bonds and specific substituents in the side chain, which promotes biodegradation through ion exchange with seawater ions, forming pores and increasing the resin's surface area, facilitating microbial decomposition.
The polymer compound enhances biodegradability in seawater by dissolving and forming pores, accelerating the decomposition of resin materials, thereby reducing marine pollution and maintaining physical properties.
Smart Images

Figure 2024170052000001 
Figure 2024170052000002 
Figure 2024170052000003
Abstract
Description
[Technical field]
[0001] The present invention relates to marine biodegradable polymeric compounds having aliphatic unsaturated carbon-carbon bonds and a method for producing the same. [Background technology]
[0002] In recent years, environmental pollution (marine pollution) and adverse effects on ecosystems caused by microplastics have become a problem, and various efforts have been launched to reduce the environmental burden. Among these, the development and popularization of biodegradable resins has been attracting attention.
[0003] On the other hand, although general biodegradable resins show high biodegradability in environments such as soil and sludge where there are many microorganisms responsible for decomposition, they have the disadvantage of being difficult to decompose in environments with extremely low microbial concentrations, such as in the ocean (Non-Patent Document 1).In addition, it has been found that the decomposition rate of resins that have been reported to be biodegradable in the ocean, such as polycaprolactone (PCL) and polyhydroxyalkanoic acid (PHA), varies greatly depending on the type of seawater, and it has been reported that this is influenced by various factors, such as the presence or absence of decomposing bacteria in the seawater, the number of bacteria, salt concentration, pH, water temperature, dissolved oxygen concentration, and amount of dissolved organic carbon (Non-Patent Document 2).
[0004] In addition, starch-based resins have also been put to practical use as biodegradable resins and are on the market, but because the physical properties of starch alone are significantly inferior, most of them are mixed with polyester-based resins such as polybutylene adipate / terephthalate (PBAT) and polylactic acid (PLA), which are difficult to biodegrade in the ocean. Therefore, even starch-based resins tend to have significantly reduced biodegradability in the ocean.
[0005] Under these circumstances, there is a demand for the development of materials that can be decomposed reliably in any type of seawater while maintaining their physical properties, as well as materials that can promote the decomposition of resins that are difficult to biodegrade in seawater and that also reduce the environmental impact. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] Hideshige Takada, "Current Status of Microplastic Pollution, International Trends and Countermeasures," Journal of Japan Society for Material Cycle Management, Vol. 29, No. 4, pp. 261-269, 2018 [Non-Patent Document 2] Akira Ebisui and 4 others, "Decomposition of biodegradable plastics in seawater," Fisheries Engineering, Vol. 40, No. 2, pp. 143-149, 2003 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above circumstances, and provides a polymer compound that induces biodegradability in the ocean, and a marine biodegradable resin composition using the same. [Means for solving the problem]
[0008] As a result of intensive research conducted by the present inventors to solve the above problems, it has been found that a polyolefin resin containing a repeating unit having at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, having an aliphatic unsaturated carbon-carbon bond in the main chain, and having one or more -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R +is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation.) in its side chain, it has been found that it exhibits high marine biodegradability. In particular, it has been found that a polymer compound in which a prepolymer compound having an anionic group contained in the marine biodegradable polymer compound is bonded via a divalent or higher metal cation has high strength because the side chains are bonded together via the metal cation, and that the molecules of the polymer compound are cut by ion exchange with monovalent cations such as sodium and potassium in seawater, accelerating marine degradation.
[0009] Furthermore, the inventors discovered that by using this material in combination with a resin, particularly a biodegradable resin, the material undergoes primary decomposition in seawater first, and that (1) pores are formed in the resin material, increasing the specific surface area of the resin and promoting the growth of microorganisms responsible for decomposition, and (2) the primary decomposition has the effect of promoting secondary decomposition, i.e., biodegradation by microorganisms, thereby ultimately promoting the biodegradation of resin materials in the ocean, thereby completing the present invention.
[0010] That is, the present invention provides the following marine biodegradable polymer compound and a method for producing the same. 1. A polymer having a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, an aliphatic unsaturated carbon-carbon bond in the main chain, and one or more -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation. 2. A marine biodegradable polymer compound having two or more acidic groups in its side chain. 3. The marine biodegradable polymer compound of 1 or 2, wherein the repeating unit contains an ester bond. 4. A marine biodegradable polymer compound according to any one of 1 to 3, having a number average molecular weight of 300 to 100,000. 5. In addition, -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation. 6. A marine biodegradable polymer compound according to any one of 1 to 5, having an average of 0.1 to 50 aliphatic unsaturated carbon-carbon bonds per molecule. 7. The marine biodegradable polymer compound according to any one of 1 to 6, wherein the substituent is bonded to the main chain via a linking group having 1 to 50 atoms. 8. The substituent is -COO - R + 8. A marine biodegradable polymer compound according to any one of 1 to 7. 9. Any of the marine biodegradable polymer compounds of 1 to 8 having maleic acid residues in the main chain. 10.R + is a monovalent metal cation or a monovalent organic cation. 11. A marine biodegradable polymer compound in which a polymeric polyvalent anion derived from any one of the marine biodegradable polymer compounds 1 to 10 is bound via a divalent or higher metal cation. 12. The content of the metal cation is 1 to 100 eq / 10 5 g of 11 marine biodegradable polymer compounds. 13. The marine biodegradable polymer compound according to 11 or 12, wherein the divalent or higher metal cation is a calcium ion, a magnesium ion or an aluminum ion. 14. A marine biodegradation promoter comprising any one of the marine biodegradable polymer compounds of 1 to 13. A marine biodegradable resin composition comprising the marine biodegradation promoter of 15.14 and a resin. 16. The marine biodegradable resin composition of 15, wherein the resin is a biodegradable resin. 17. The marine biodegradable resin composition of 16, wherein the content of the marine biodegradation promoter is 1 to 50 mass % and the content of the biodegradable resin is 50 to 99 mass %. 18. A molded article obtained from the marine biodegradable resin composition according to any one of 15 to 17. 19. A method for producing a marine biodegradable polymer compound, comprising a step of reacting a polymer compound having a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, and having an aliphatic unsaturated carbon-carbon bond in its main chain, with a compound having a reactive group reactive to an aliphatic unsaturated carbon-carbon bond and a substituent selected from -COOH, -SO3H, -O-SO3H, and -P(=O)(OH)-OH. 20. A method for producing a marine biodegradable polymer compound, the method comprising the step of neutralizing, with a monovalent base, a substituent of a marine biodegradable polymer compound, the substituent comprising a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, an aliphatic unsaturated carbon-carbon bond in the main chain, and one or more substituents selected from -COOH, -SO3H, -O-SO3H, and -P(=O)(OH)-OH in a side chain. 21. A method for producing a marine biodegradable polymer compound according to claim 20, wherein the base is lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate or potassium bicarbonate. 22. A polymer having a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, an aliphatic unsaturated carbon-carbon bond in the main chain, and one or more -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R +is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation.) A method for producing a marine biodegradable polymer compound, comprising a step of crosslinking a marine biodegradable polymer compound having a substituent selected from the group consisting of a hydrogen ion, a monovalent metal cation, and a monovalent organic cation, at a side chain thereof, with a polyvalent metal salt. 23. A method for producing a marine biodegradable polymer compound according to claim 22, wherein the polyvalent metal salt is a calcium salt, a magnesium salt or an aluminum salt. Effect of the Invention
[0011] The marine biodegradable polymer compound of the present invention has marine biodegradability and exhibits characteristic physical properties derived from the substituents and unsaturated bonds in the side chains. Furthermore, the marine biodegradable polymer compound gradually dissolves in seawater or exhibits hydrophilicity upon contact with seawater, so that resin compositions and molded articles containing the same are accelerated in the ocean and are useful for marine pollution countermeasures. The marine biodegradable polymer compound has marine biodegradability, so that compositions and molded articles containing the same are accelerated in the ocean and are useful for marine pollution countermeasures. By using a marine biodegradation promoter consisting of the marine biodegradable polymer compound of the present invention, environmentally friendly compositions and molded articles can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Marine biodegradable polymer compound A] A first aspect of the marine biodegradable polymer compound of the present invention includes a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond (hereinafter, also simply referred to as an aliphatic unsaturated bond) in the main chain, and has one or more -COO - R + , -SO3 - R + , -O-SO3 - R + and -P(=O)(OH)-O - R + (In the formula, R +is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation.) (hereinafter, also referred to as marine biodegradable polymer compound A). The aliphatic unsaturated bond may be a double bond or a triple bond, but is preferably a double bond in consideration of the stability and reactivity of the structure.
[0013] The marine biodegradable polymer compound A may have two or more of the above-mentioned substituents on the side chain. When the compound A has two or more of the above-mentioned substituents, the respective substituents may be the same or different from each other.
[0014] From the viewpoints of mechanical properties and biodegradability, the repeating units constituting the marine biodegradable polymer compound A preferably contain an ester bond or an amide bond, more preferably contain an ester bond, and most preferably contain an ester bond generated by polycondensation of a dicarboxylic acid and a diol in the repeating unit.
[0015] The marine biodegradable polymer compound A preferably has a molecular weight of 300 to 100,000, and in consideration of biodegradability and mechanical properties in seawater, more preferably 300 to 10,000, even more preferably 500 to 5,000, even more preferably 700 to 4,000, and most preferably 900 to 3,000. If the molecular weight is within the above range, it is preferable because the biodegradability and mechanical properties are good. In the present invention, the molecular weight means the number average molecular weight obtained by the terminal group quantitative analysis.
[0016] The marine biodegradable polymer compound A must have the above-mentioned substituent on the side chain, but may also have the above-mentioned substituent on the end of the main chain. In that case, the substituent may be on both ends, or only on one end, but this can be adjusted according to the desired physical properties, biodegradability, and water solubility. The substituent on the end of the main chain may be the same as or different from the substituent on the side chain.
[0017] In the marine biodegradable polymer compound A, the number of the substituents is preferably an appropriate number of acidic groups relative to the number average molecular weight in consideration of physical properties, biodegradability, and water solubility. Specifically, the value obtained by dividing the number average molecular weight by the average number of acidic groups per molecule is preferably 100 to 10,000, more preferably 200 to 5,000, even more preferably 300 to 5,000, and most preferably 500 to 1,000.
[0018] The marine biodegradable polymer compound A has an aliphatic unsaturated carbon-carbon bond in the main chain, and in order to achieve both strength and biodegradability, the number of aliphatic unsaturated carbon-carbon bonds is preferably 0.1 to 50 per molecule on average, more preferably 0.5 to 25, and even more preferably 1 to 10.
[0019] The substituents on the side chains may be directly bonded to the main chain or may be bonded via a linking group, but in consideration of mechanical properties, the substituents are preferably bonded via a linking group having 1 to 50 atoms, more preferably bonded via a linking group having 2 to 30 atoms, and even more preferably bonded via a linking group having 5 to 25 atoms. The structure of the linking group may be linear, branched, or cyclic, but is preferably linear or branched, and more preferably linear. In addition, the atoms constituting the linking group are not particularly limited, but the linking group preferably contains at least one selected from carbon atoms, oxygen atoms, nitrogen atoms, boron atoms, sulfur atoms, phosphorus atoms, and silicon atoms, and more preferably contains at least one selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms.
[0020] Considering the environmental load and ease of handling, the substituent is preferably -COO - R + , -SO3 - R + Preferably, -COO - R + It is particularly preferred that:
[0021] The aliphatic unsaturated bond in the marine biodegradable polymer compound A may be derived from any monomer, but in consideration of ease of introduction, cost, and risk of side reactions, it is preferable that the aliphatic unsaturated bond is derived from a polyol compound having an aliphatic unsaturated bond or a polycarboxylic acid compound having an aliphatic unsaturated bond, and it is more preferable that the aliphatic unsaturated bond is derived from a dicarboxylic acid compound having an aliphatic unsaturated bond.
[0022] Specific examples of the polyol compound having an aliphatic unsaturated bond are preferably diol compounds having an aliphatic unsaturated bond such as 2-butene-1,4-diol, 3-hexene-1,6-diol, 4-hydroxy-2-(hydroxymethyl)-2-cyclopenten-1-one, etc. As the polyol compound having an aliphatic unsaturated bond, a commercially available product or a synthesized product may be used.
[0023] Specific examples of the polycarboxylic acid compound having an aliphatic unsaturated bond include dicarboxylic acids having an aliphatic unsaturated bond such as maleic acid, fumaric acid, citraconic acid, mesaconic acid, 2-pentenedioic acid, methylenesuccinic acid, allylmalonic acid, isopropylidenesuccinic acid, 2,4-hexadienedioic acid, and acetylenedicarboxylic acid, and in consideration of reactivity, solubility, and physical properties of the product, fumaric acid and maleic acid are preferred, and maleic acid is more preferred. The polycarboxylic acid compound having an aliphatic unsaturated bond may be a commercially available product or a synthesized product.
[0024] The marine biodegradable polymer compound A preferably has a relative cellulose biodegradability of 40% or more. In the present invention, the relative cellulose biodegradability is the degree of decomposition of cellulose after 60 days of immersion in seawater. The marine biodegradable polymer compound A more preferably has a relative cellulose biodegradability of 50% or more, even more preferably 60% or more, and most preferably 80% or more. The relative cellulose biodegradability can be measured by ASTM D6691, known marine biodegradation test methods, etc., or BOD modified with reference to these methods.
[0025] The marine biodegradable polymer compound A preferably has a softening point or melting point suitable for the melting temperature of the resin. The polymer compound is solid or liquid at room temperature, and more specifically, the lower limit of the softening point or melting point is preferably 0°C or more, 25°C or more, 40°C or more, 80°C or more, and 100°C or more, in that order, and the upper limit is preferably 180°C or less, 150°C or less, and 120°C or less, in that order. In consideration of handling, it is preferable that the softening point or melting point is preferably within the range of 0 to 180°C, more preferably 25 to 120°C.
[0026] [Production method of marine biodegradable polymer compound A] In the marine biodegradable polymer compound A, the R + is a hydrogen ion (i.e., the substituent is selected from -COOH, -SO3H, -O-SO3H, and -P(=O)(OH)-OH (hereinafter also referred to as marine biodegradable polymer compound A1) can be produced by a method including a step of reacting a polymer compound (hereinafter also referred to as polymer compound P) containing a repeating unit including at least one bond selected from ester bond, amide bond, carbonate bond, urethane bond, and urea bond, and having an aliphatic unsaturated carbon-carbon bond in the main chain, with a compound (hereinafter also referred to as compound Q) having a reactive group reactive to an aliphatic unsaturated carbon-carbon bond and a substituent selected from -COOH, -SO3H, -O-SO3H, and -P(=O)(OH)-OH (hereinafter these are collectively referred to as acidic group A).
[0027] Examples of the polymer compound P include an unsaturated polyester compound, an unsaturated polyamide compound, an unsaturated polycarbonate compound, an unsaturated polyurethane compound, an unsaturated polyurea compound, and the like. An unsaturated polyester compound or an unsaturated polyamide compound is preferable, and an unsaturated polyester compound is more preferable.
[0028] The unsaturated polyester compound can be produced, for example, by polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond and a polyol compound containing a polyol compound having no aliphatic unsaturated bond, polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having no aliphatic unsaturated bond and a polyol compound containing a polyol compound having an aliphatic unsaturated bond, or polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond and a polyol compound containing a polyol compound having an aliphatic unsaturated bond. When producing an unsaturated polyester, a known polyester polymerization method can be referred to, for example, the method described in Sen to Kogyo, Vol. 40, No. 4.5, pp. 259-261, 1984 can be referred to. In addition, a commercially available product can be used as the unsaturated polyester compound.
[0029] Specific examples of the polyvalent carboxylic acid compound having an aliphatic unsaturated bond and the polyol compound having an aliphatic unsaturated bond include those mentioned above.
[0030] Specific examples of the polyol compound having no aliphatic unsaturated bond include saturated diol compounds such as ethylene glycol, 1,3-propanediol, and 1,4-butanediol, and 1,4-butanediol is preferred in terms of reactivity, solubility, and physical properties of the product. The polyol compound having no aliphatic unsaturated bond may be a commercially available product or a synthesized product.
[0031] Specific examples of the polycarboxylic acid compound having no aliphatic unsaturated bond include saturated polycarboxylic acids and aromatic polycarboxylic acids such as succinic acid, glutaric acid, adipic acid, sebacic acid, terephthalic acid, isophthalic acid, trimellitic acid, pyromellitic acid, etc. The polycarboxylic acid compound having no aliphatic unsaturated bond may be a commercially available product or a synthesized product.
[0032] The unsaturated polyester compound is preferably produced by polycondensation of a polycarboxylic acid compound containing a dicarboxylic acid compound having an aliphatic unsaturated bond and a polyol compound containing a diol compound having no aliphatic unsaturated bond.
[0033] At this time, the polycarboxylic acid compound as the raw material may contain a polycarboxylic acid compound without an aliphatic unsaturated bond in addition to the dicarboxylic acid compound with an aliphatic unsaturated bond. Specific examples of the polycarboxylic acid compound without an aliphatic unsaturated bond include succinic acid, glutaric acid, adipic acid, sebacic acid, terephthalic acid, isophthalic acid, trimellitic acid, pyromellitic acid, etc., but in consideration of reactivity, solubility, and physical properties of the product, succinic acid or adipic acid is preferable, and succinic acid is more preferable. The content of the polycarboxylic acid compound without an aliphatic unsaturated bond in the carboxylic acid compound as the raw material is preferably 0 to 80 mol%, more preferably 10 to 40 mol%, and most preferably 30 to 60 mol%.
[0034] The polyol compound as a raw material may contain a polyol compound having a triol or more in addition to the diol compound. Specific examples of the polyol compound include monosaccharides such as glycerin, trimethylolpropane, pentaerythritol, and glucose, and the like. Considering reactivity, solubility, and physical properties of the product, glycerin or trimethylolpropane is preferred, and glycerin is more preferred. The content of the polyol compound having a triol or more in the polyol compound as a raw material is preferably 0.01 to 5 mol%, more preferably 0.05 to 3 mol%, and most preferably 0.1 to 1 mol%.
[0035] In the polymerization reaction of the unsaturated polyester compound, a polycondensation catalyst such as antimony trioxide, a germanium catalyst, or a titanium catalyst; or a catalyst generally used for ester exchange such as magnesium acetate or manganese acetate may be used as needed to promote the reaction. Considering the environmental load, a catalyst that does not contain a metal is preferable. The amount of the catalyst used is preferably about 0.01 to 5 parts by mass relative to 100 parts by mass of the raw material compound.
[0036] The unsaturated polyamide compound can be produced, for example, by polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond and a polyamine compound containing a polyamine compound having no aliphatic unsaturated bond, polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having no aliphatic unsaturated bond and a polyamine compound containing a polyamine compound having an aliphatic unsaturated bond, or polycondensation of a polycarboxylic acid compound containing a polycarboxylic acid compound having an aliphatic unsaturated bond and a polyamine compound containing a polyamine compound having an aliphatic unsaturated bond. The polycarboxylic acid can be the above-mentioned compound, and the polyamine having an aliphatic unsaturated bond can be a diamine compound having an aliphatic unsaturated bond such as 2-butene-1,4-diamine or 3-hexene-1,6-diamine. When producing a polyamide having an aliphatic unsaturated bond, a known polyamide polymerization method can be referred to, for example, the methods described in JP-B-52-12233 and JP-B-5-71056. As the polyamide compound having an aliphatic unsaturated bond, a commercially available product may be used.
[0037] In the polymerization reaction of the unsaturated polyamide, a polycondensation catalyst such as a metal salt, an ammonium salt, or an ester of phosphoric acid, phosphorous acid, or hypophosphorous acid may be used as needed to promote the reaction. The amount of the catalyst used is preferably about 0.01 to 5.0 parts by mass based on 100 parts by mass of the raw material compound.
[0038] The unsaturated polycarbonate compound can be produced, for example, by polycondensing a carbonate ester such as diphenyl carbonate or phosgene or a carbonate chloride with a polyol compound having an aliphatic unsaturated bond. As the polyol compound having an aliphatic unsaturated bond, for example, a diol compound having an aliphatic unsaturated bond such as 2-butene-1,4-diol or 3-hexene-1,6-diol can be used. When producing the unsaturated polycarbonate compound, a known polycarbonate polymerization method can be referred to, for example, the methods described in JP-A-2013-010948 and JP-A-2016-94589. In addition, a commercially available product may be used as the unsaturated polycarbonate compound.
[0039] In the polymerization reaction of the unsaturated polycarbonate, a polycondensation catalyst such as antimony trioxide, a germanium catalyst, a titanium catalyst, etc., or a catalyst generally used for ester exchange such as magnesium acetate, manganese acetate, etc. may be used for the purpose of promoting the reaction, if necessary. The amount of the catalyst used is preferably about 0.01 to 1.0 part by mass relative to 100 parts by mass of the raw material compound.
[0040] The unsaturated polyurethane compound can be produced, for example, by polyaddition of a polyisocyanate such as hexamethylene diisocyanate or diphenylmethane diisocyanate with a diol compound having an aliphatic unsaturated bond, an unsaturated polyester compound having a hydroxyl group prepared by the above-mentioned method, or a polyol compound including an unsaturated polycarbonate compound having a hydroxyl group, a polyisocyanate including a polyisocyanate having an aliphatic unsaturated bond such as 2-butene-1,4-diisocyanate or 3-hexene-1,6-diisocyanate, and a polyol compound, or a polyisocyanate including a polyisocyanate having an aliphatic unsaturated bond with a diol compound having an aliphatic unsaturated bond or a polyol including a polyol compound having an aliphatic unsaturated bond. When producing the unsaturated polyurethane compound, known polyurethane polymerization methods can be referred to, for example, the methods described in JP-B-52-12233 and JP-B-5-71056 can be referred to.
[0041] In the reaction between a polyol compound having an aliphatic unsaturated bond and a polyisocyanate, an amine catalyst such as 1,4-diazabicyclo[2.2.2]-octane (DABCO) or 1,8-diazabicyclo-[5.4.0]-undec-7-ene (DBU) or a tin catalyst such as dibutyltin dilaurate may be used in order to shorten the reaction time or lower the reaction temperature by improving the reactivity. In addition, zinc complexes, iron complexes, bismuth complexes and zirconium complexes similar to the tin complexes are also useful as catalysts. The amount of the catalyst used is preferably about 0.01 to 5 parts by mass relative to 100 parts by mass of the raw material compound.
[0042] The unsaturated polyurea compound can be produced, for example, by polycondensation of the polyisocyanate described above with the polyamine compound containing the polyamine compound having the aliphatic unsaturated bond or the polyamine containing the unsaturated polyamide compound having an amino group prepared by the method described above, polycondensation of the polyisocyanate containing the polyisocyanate having the aliphatic unsaturated bond and the polyamine compound, or polycondensation of the polyisocyanate containing the polyisocyanate having the aliphatic unsaturated bond and the polyamine compound containing the polyamine compound having the aliphatic unsaturated bond or the unsaturated polyamide compound having an amino group prepared by the method described above.When producing the unsaturated polyurea compound, it is possible to refer to the known polymerization method of polyurea, for example, the method described in JP-A-2004-27148.
[0043] In the polymerization reaction of the unsaturated polyurea compound, a catalyst such as a salt of a metal such as lithium, sodium, magnesium, aluminum, potassium, titanium, cobalt, germanium, zinc, rubidium, strontium, tin, antimony, cesium, barium, lead, etc., an alkoxide, an organometallic compound, etc. may be used for the purpose of promoting the reaction as necessary. The amount of the catalyst used is preferably about 0.0001 to 1 part by mass relative to 100 parts by mass of the raw material compound.
[0044] In the reaction between the polymer compound P and the compound Q, the amount of the compound Q used is preferably 5 to 200 mol % based on the aliphatic unsaturated bonds in the unsaturated polyester compound. At 5 to 20 mol %, the physical properties derived from the double bonds are strongly expressed, while at more than 20 mol % and 200 mol % or less, the physical properties derived from the side chain acidic group A are strongly expressed, so the amount may be adjusted according to the purpose.
[0045] The reaction between the polymer compound P and the compound Q is not particularly limited, and may be, for example, a conjugate addition reaction, a radical reaction, a Diels-Alder reaction, or a photocycloaddition reaction, but in consideration of reactivity, selectivity, and the physical properties of the product, a conjugate addition reaction is preferred. Particularly preferred examples of the reaction include the addition reaction of mercaptocarboxylic acid, amino acid, malonic acid derivative, etc. to an aliphatic unsaturated bond of a polyester compound having a maleic acid residue.
[0046] In the reaction between polymer compound P and compound Q, a commonly used catalyst may be used as necessary. Examples of such catalysts include base catalysts such as DBU and TEA in conjugate addition reactions, transition metal catalysts such as organoruthenium complexes and organotitanium complexes in radical reactions, Lewis acid catalysts such as ytterbium triflate and scandium triflate in Diels-Alder reactions, and photosensitizers such as thiophene and benzophenone in photocycloaddition reactions.
[0047] Compound Q can be appropriately selected according to the intended reaction. For example, examples of compound Q include mercaptocarboxylic acids such as 3-mercaptopropionic acid, amino acids such as 5-aminovaleric acid and 6-aminohexanoic acid, aminosulfonic acids such as 2-aminoethanesulfonic acid, aminophosphoric acids such as ethanolamine phosphoric acid, malonic acid, organic copper ate complexes, and other nucleophilic organic acids and derivatives thereof in the case of conjugate addition reactions, carboxylic acids and sulfonic acids having unsaturated bonds such as acrylic acid, 3-pentenoic acid, carboxystyrene, and styrenesulfonic acid in the case of radical reactions, pyrrole carboxylic acids such as 1-methyl-2-pyrrole carboxylic acid in the case of Diels-Alder reactions, and carboxylic acids having unsaturated bonds such as acrylic acid and 3-pentenoic acid in the case of photocycloaddition reactions. Considering reactivity, selectivity, physical properties of the product, and safety, it is preferable to use 3-mercaptopropionic acid, 5-aminovaleric acid, 6-aminohexanoic acid, and malonic acid derivatives in conjugate addition reactions, and it is most preferable to use 3-mercaptopropionic acid in conjugate addition reactions. The compound Q may be a commercially available product or a synthesized product.
[0048] The compound Q may be used with the acidic group A as it is, or the acidic group A may be protected by esterification or the like as necessary, and then deprotected to give the acidic group A after the reaction between the polymer compound P and the compound Q.
[0049] In the marine biodegradable polymer compound A, the R + A marine biodegradable polymer compound A2, in which some or all of the acidic groups A in the marine biodegradable polymer compound A1 are monovalent metal cations or monovalent organic cations, can be synthesized by neutralizing some or all of the acidic groups A in the marine biodegradable polymer compound A1.
[0050] In the marine biodegradable polymer compound A2, the substituent R + As the cation, a lithium ion, a sodium ion, a potassium ion, a rubidium ion, a cesium ion, a francium ion, an ammonium ion, a methylammonium ion, an ethylammonium ion, an anilinium ion, a pyridinium ion, a dimethylammonium ion, a diethylammonium ion, a trimethylammonium ion, a triethylammonium ion, and the like are preferred, and from the viewpoints of safety, environmental load, and operability, a sodium ion, a potassium ion, and an ammonium ion are more preferred, and a sodium ion and a potassium ion are even more preferred.
[0051] The neutralization reaction is not particularly limited, and can be carried out using, for example, an inorganic base and / or an organic base that can react with an acidic group. Examples of the base include lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, trisodium phosphate, tripotassium phosphate, lithium methoxide, sodium methoxide, potassium methoxide, lithium tert-butoxide, sodium tert-butoxide, potassium tert-butoxide, ammonia, methylamine, ethylamine, TEA, DBU, and the like. Among these, lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, or potassium hydrogen carbonate is preferred, and in consideration of safety and environmental load, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium hydrogen carbonate, or potassium hydrogen carbonate is particularly preferred.
[0052] [Marine biodegradable polymer compound B] A second embodiment of the marine biodegradable polymer compound of the present invention is a marine biodegradable polymer compound (hereinafter also referred to as marine biodegradable polymer compound B) obtained by crosslinking marine biodegradable polymer compound A with a divalent or higher metal cation. That is, marine biodegradable polymer compound B contains a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond in the main chain, and has one or more -COO - , -SO3 - , -O-SO3 - and -P(=O)(OH)-O - The anionic polymer compound has a structure in which the anionic polymer compound has, at its side chain, a monovalent anionic substituent selected from the group consisting of the above, and is bonded by an ionic bond via a divalent or higher metal cation.
[0053] The divalent or higher metal cation is not particularly limited, but may be calcium ion, beryllium ion, magnesium ion, strontium ion, barium ion, zinc ion, aluminum ion, iron ion, copper ion, platinum ion, gold ion, titanium ion, nickel ion, cobalt ion, manganese ion, zirconium ion, ruthenium ion, rhodium ion, palladium ion, scandium ion, gallium ion, indium ion, radium ion, etc. Among these, calcium ion, beryllium ion, magnesium ion, strontium ion, barium ion, zinc ion, aluminum ion, etc. are preferred, and calcium ion, magnesium ion, aluminum ion, etc. are more preferred. The divalent or higher metal cation may be used alone or in combination of multiple types.
[0054] The metal ion equivalent in the marine biodegradable polymer compound is 1 to 100 eq / 10 5 g is preferable, but considering biodegradability in seawater and mechanical properties, 2 to 80 eq / 10 5 g is more preferable, and 10 to 50eq / 10 5 g is more preferable. If the metal ion equivalent is within the above range, it is preferable because it has good biodegradability and mechanical properties are not impaired. The metal ion equivalent is a value measured by inductively coupled plasma mass spectrometry (ICP-MS).
[0055] The marine biodegradable polymer compound B is a compound in which at least two marine biodegradable polymer compounds A2 are bonded via metal cations, and the marine biodegradable polymer compound A2 may contain only one type, or may contain multiple different types, and may further contain other anionic compounds at the same time. Examples of such anionic compounds include carboxylate anions, sulfonate anions, and polymer compounds having an anionic group at the end and a number average molecular weight of 500 to 10,000.
[0056] The marine biodegradable polymer compound B may have a structure such as a linear, branched, or crosslinked network structure. In the case of a linear or branched structure, the molecular weight is preferably 600 to 1,000,000, more preferably 1,000 to 500,000, even more preferably 5,000 to 300,000, and most preferably 10,000 to 100,000. A typical biodegradable resin, which will be described later, exhibits high biodegradability in an environment in which many microorganisms responsible for decomposition, such as soil or sludge, but has the disadvantage that it is difficult to decompose in an environment in which the concentration of microorganisms is extremely low, such as in the ocean. The present inventors have focused on metal ions that are abundant in seawater and stable salinity in the ocean. It is speculated that the marine biodegradable polymer compound B is decomposed by ion exchange in seawater (reduced to low molecular weight by cleavage) and chemically reduced to low molecular weight, so that decomposition proceeds efficiently even in an environment in which there are few microorganisms responsible for biodegradation. By setting the molecular weight of the marine biodegradable polymer compound B within the above range, biodegradability in the ocean can be promoted more efficiently, while the resin composition used during normal use is also physically useful.
[0057] The marine biodegradable polymer compound B preferably has a softening point or melting point suitable for the melting temperature of the resin. The polymer compound is solid at room temperature, and more specifically, the lower limit of the softening point or melting point is preferably 40°C or more, 50°C or more, and 60°C or more, in that order, and the upper limit is preferably 250°C or less, 180°C or less, 160°C or less, and 140°C or less, in that order. When the resin is a biodegradable resin, it is preferable that the softening point or melting point is preferably within the range of 40 to 200°C, more preferably 50 to 160°C, and even more preferably 60 to 140°C.
[0058] The marine biodegradable polymer compound B preferably has a relative cellulose biodegradability of 40% or more. In the present invention, the relative cellulose biodegradability is the degree of decomposition of cellulose after 60 days of immersion in seawater. The marine biodegradable polymer compound B more preferably has a relative cellulose biodegradability of 50% or more, even more preferably 60% or more, and most preferably 80% or more. The relative cellulose biodegradability can be measured by ASTM D6691, known marine biodegradation test methods, etc., or BOD modified with reference to these methods.
[0059] [Production method of marine biodegradable polymer compound B] The marine biodegradable polymer compound B can be produced by a method including a step of crosslinking the marine biodegradable polymer compound A with a polyvalent metal salt.
[0060] Examples of the crosslinking treatment method include a method in which a powder or solution of a polyvalent metal salt is dropped into a medium in which the marine biodegradable polymer compound A is dissolved, and precipitation or precipitating is performed while a bonding treatment is performed; a method in which a powder or solution of a polyvalent metal salt is dropped into a molten liquid of the marine biodegradable polymer compound A, and a method in which a solution in which the marine biodegradable polymer compound A is dissolved is dropped into a powder of a polyvalent metal salt or a solution in which the polyvalent metal salt is dissolved, and precipitation or precipitating is performed while a bonding treatment is performed.
[0061] As a preferred example, a solution in which the marine biodegradable polymer compound A2 is dissolved in water, an organic solvent, or a mixed solvent thereof, or a melt in which the marine biodegradable polymer compound A2 is heated and dissolved is prepared. At this time, heating may be performed as necessary to improve the solubility or to reduce the viscosity of the melt. Next, a solution containing a divalent or higher metal salt is added to the obtained solution or melt and stirred. Alternatively, a solution in which the marine biodegradable polymer compound A2 is dissolved in a solution containing a divalent or higher metal salt may be added and stirred.
[0062] Examples of the polyvalent metal salt include calcium salt, strontium salt, magnesium salt, barium salt, radium salt, lead salt, zinc salt, nickel salt, iron salt, copper salt, cadmium salt, cobalt salt, manganese salt, aluminum salt, gallium salt, indium salt, and thallium salt. However, calcium salt, magnesium salt, and aluminum salt are preferred from the viewpoints of being metals contained in seawater, environmental aspects, safety, and versatility, and calcium salt and magnesium salt are more preferred in consideration of the seawater environment. Specific examples of the polyvalent metal salt include calcium chloride, calcium sulfate, calcium carbonate, calcium hydroxide, calcium oxide, magnesium chloride, magnesium sulfate, magnesium carbonate, magnesium hydroxide, magnesium oxide, aluminum sulfate, sodium aluminum sulfate (sodium alum), and potassium aluminum sulfate (potassium alum), and calcium chloride, magnesium chloride, and aluminum sulfate are preferred from the viewpoints of solubility in water, ease of handling, and cost.
[0063] Furthermore, neutralization and binding via a divalent or higher metal cation can be carried out simultaneously by neutralizing the acidic group A of the marine biodegradable polymer compound A1 with a base containing a divalent or higher metal.
[0064] As a preferred example, a solution in which the marine biodegradable polymer compound A1 is dissolved in water, an organic solvent, or a mixed solvent thereof, or a melt in which the marine biodegradable polymer compound A1 is heated and dissolved is prepared. At this time, heating may be performed as necessary to improve the solubility or to reduce the viscosity of the melt. Next, a solution of a base containing a divalent or higher metal is added to the obtained solution or melt and stirred. Alternatively, a solution or melt in which the marine biodegradable polymer compound A1 is dissolved may be added to a solution of a base containing a divalent or higher metal and stirred.
[0065] Examples of the base containing a divalent or higher metal include magnesium hydride, strontium hydride, calcium hydride, barium hydride, magnesium methoxide, calcium methoxide, strontium methoxide, barium methoxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium oxide, strontium oxide, calcium oxide, barium oxide, magnesium carbonate, strontium carbonate, calcium carbonate, barium carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium hydrogen carbonate, barium hydrogen carbonate, and the like. From the viewpoints of solubility in water, reactivity, cost, and the like, calcium hydride, calcium methoxide, calcium hydroxide, and barium hydroxide are preferred, and calcium hydroxide is more preferred.
[0066] The concentration of the polyvalent metal salt in the solution containing the polyvalent metal salt or the concentration of the base in the solution containing a base containing a divalent or higher metal is preferably 1 to 40% by mass, more preferably 10 to 30% by mass. The solvent of the solution is preferably water, lower alcohol solvents such as methanol, ethanol, 1-propanol, and 2-propanol, amphipathic solvents such as acetone, acetonitrile, THF, DMF, DMSO, and NMP, and mixed solvents thereof, but may be a mixed solvent with other organic solvents as long as it can dissolve the salt to a desired concentration without dissolving the particles.
[0067] Furthermore, if the polyvalent metal salt or the base containing a divalent or higher metal has a good reactivity and reacts even in a solid state, it may be used in a powder form without using a medium, or it may be dispersed in a small amount of medium.
[0068] In this way, the marine biodegradable polymer compound A can be bound via the metal cation, and the target marine biodegradable polymer compound B, which gradually becomes insoluble, is obtained as a precipitate or a bulk. The treatment time is preferably 0.5 to 24 hours, more preferably 1 to 12 hours.
[0069] At this time, in order to control the particle size and shape (e.g., spherical) of the precipitate or sediment, a surfactant or a polymer stabilizer may be dissolved in at least one of the solution in which the marine biodegradable polymer compound A1 or A2 is dissolved and the solution containing a base containing a divalent or higher metal or a polyvalent metal salt.
[0070] Heating may be performed when precipitating or precipitating the desired marine biodegradable polymer compound B. Heating may be performed when mixing the solution in which the marine biodegradable polymer compound A1 or A2 is dissolved or the molten liquid of the marine biodegradable polymer compound A1 or A2 with the solution containing a polyvalent metal salt or a base containing a divalent or higher metal, or when stirring after mixing, or both of these. The heating temperature is preferably 15 to 150°C, more preferably 20 to 100°C, and more preferably 40 to 80°C.
[0071] After the treatment, the particles can be washed and dried as necessary to obtain the marine biodegradable polymer compound B. Washing can be performed by a conventional method, for example, removing the solvent after the binding treatment, adding water and centrifuging. Drying can be performed by a conventional method, for example, spray drying, vacuum drying, freeze drying, etc. The obtained marine biodegradable polymer compound B may be surface-treated or pulverized to adjust the particle size, using known equipment as necessary.
[0072] The marine biodegradable polymer compound B may be one in which at least one end of the anionic polymer compound that is not bonded to itself via a divalent metal cation is blocked with a blocking segment group.
[0073] By selecting the blocking segment group, in a single material and a composite material (marine biodegradable resin composition) using this material, it is possible to incorporate multiple effects such as adjustment of melting temperature and melt viscosity, adjustment of crystallinity, adjustment of microbial adhesion and biodegradability, adjustment of physical properties such as resin tensile strength, bending strength, and elasticity, improvement of compatibility with resin, adjustment of hydrophobicity, adjustment of water repellency, adjustment of adhesion, and adjustment of plasticity, and it is possible to improve both the biodegradability and physical properties of the marine biodegradable resin composition. Since it is desirable for the organic anion to be the blocking segment to have a structure having marine biodegradability, it is desirable to select a blocking segment group having marine biodegradability with a molecular weight of 5000 or less. For example, when emphasis is placed on the biodegradability rate in the ocean and the maintenance of average physical properties, a molecular weight of 2500 or less is preferable, and a molecular weight of 1000 or less is more preferable.
[0074] Specifically, the blocking segment group preferably has a monovalent hydrocarbon group having 3 or more carbon atoms, more preferably has a monovalent hydrocarbon group having 6 or more carbon atoms, even more preferably has a monovalent hydrocarbon group having 10 or more carbon atoms, and most preferably has a monovalent hydrocarbon group having 12 or more carbon atoms. There are no particular limitations on the upper limit of the number of carbon atoms in the monovalent hydrocarbon group, but it is preferably 30 or less, more preferably 25 or less, and even more preferably 20 or less.
[0075] The blocking segment group is preferably a monovalent organic anion selected from a carboxylate anion having a monovalent hydrocarbon group with 3 or more carbon atoms, a sulfonate anion having a monovalent hydrocarbon group with 3 or more carbon atoms, a sulfate ester anion having a monovalent hydrocarbon group with 3 or more carbon atoms, and a phosphate ester anion having a monovalent hydrocarbon group with 3 or more carbon atoms. Among these, a monovalent organic anion derived from a carboxylic acid having a monovalent hydrocarbon group with 3 or more carbon atoms is preferred, and a monovalent organic anion derived from a fatty acid having a monovalent hydrocarbon group with 3 or more carbon atoms or an amino acid derivative having a monovalent hydrocarbon group with 3 or more carbon atoms is more preferred.
[0076] Terminal blocking can be carried out using at least one terminal blocking agent selected from a carboxylic acid having a monovalent hydrocarbon group having 3 or more carbon atoms, a salt of the carboxylic acid, a sulfonic acid having a monovalent hydrocarbon group having 3 or more carbon atoms, a salt of the sulfonic acid, a sulfate having a monovalent hydrocarbon group having 3 or more carbon atoms, a salt of the sulfate ester, a phosphate having a monovalent hydrocarbon group having 3 or more carbon atoms, and a salt of the phosphate ester. Terminal blocking can be carried out by adding the terminal blocking agent to a solution containing polymer compound A or B, and then performing a bonding treatment with a polyvalent metal ion.
[0077] As the terminal blocking agent, the acid compounds or salt compounds described in paragraphs
[0029] to
[0044] of JP2021-191810A are preferable.
[0078] [Marine biodegradable resin composition] The marine biodegradable resin composition of the present invention contains the marine biodegradable polymer compound.
[0079] The marine biodegradable polymer compound may be used as a main raw material, or may be used in combination with other resins as additives. The other resins are not particularly limited, but are preferably biodegradable resins. When used in combination with other resins as additives, the marine biodegradable polymer compound functions as a marine biodegradation promoter. In this case, the composite resin becomes a resin composition in which biodegradation in the ocean is promoted. In addition, in order to adjust the physical properties and handling properties of the resin composition, multiple types of resins can be used in combination as the other resins.
[0080] Examples of the other resins include polyethylene, polyester, polypropylene, polyethylene terephthalate, polystyrene, polyurethane, epoxy resin, chlorinated polyethylene resin, chlorinated polypropylene resin, modified nylon resin, phenol resin, silicone resin, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyvinyl chloride, polyvinylidene chloride, styrene-maleic acid resin, styrene-butadiene resin, butadiene resin, acrylonitrile-butadiene resin, poly(meth)acrylonitrile resin, (meth)acrylamide resin, bio-PET, bio-polyamide, bio-polycarbonate, bio-polyurethane, polyvinyl alcohol, polybutylene adipate / terephthalate, polyethylene terephthalate succinate, bio-polybutylene succinate, polylactic acid blend, starch blend polyester resin, polybutylene terephthalate succinate, polylactic acid, and polyhydroxyalkanoic acid. In consideration of the effect of reducing the burden on the environment and promoting marine biodegradability, resins with high biodegradability are particularly preferred.
[0081] In addition, examples of the biodegradable resin include polycaprolactone, poly(caprolactone / butylene succinate), polybutylene succinate (PBS), poly(butylene succinate / adipate) (PBSA), poly(butylene adipate / terephthalate) (PBAT), poly(butylene succinate / carbonate), polyethylene terephthalate copolymer, poly(ethylene terephthalate / succinate), poly(tetramethylene adipate / terephthalate), polyethylene succinate, and the like. Resins made from petroleum-derived raw materials such as poly(lactic acid / polybutylene succinate), poly(glycolic acid / caprolactone copolymer, glycolic acid / trimethylene carbonate copolymer; (polylactic acid / polybutylene succinate) block copolymer, (polylactic acid / polycaprolactone) copolymer, (polylactic acid / polyether) copolymer, polylactic acid blend PBAT, lactic acid / glycolic acid copolymer, biopolybutylene succinate, poly(butylene succinate / adipate), starch blend Resins whose raw materials are partly derived from biomass, such as polyester resins and poly(butylene terephthalate succinate); resins whose raw materials are 100% derived from biomass, such as polyhydroxyalkanoates such as polyhydroxybutyrate / hydroxyhexanoate (PHBH), poly(3-hydroxybutyrate / 4-hydroxybutyrate) (P3HB4HB), and poly(hydroxybutyrate / hydroxyvalerate) (PHBV), and polylactic acid (PLA); and resins derived from natural polymers, such as cellulose, cellulose acetate, cellulose ester resins, starch, esterified starch, and chitosan.
[0082] Among these, it is preferable to combine the marine biodegradable polymer compound with a biodegradable resin selected from resins that are biodegradable in soil or compost but poorly biodegradable in the ocean, such as polycaprolactone, (bio)PBS, PBSA, PBAT, poly(tetramethylene adipate / terephthalate), poly(butylene succinate / carbonate), polyhydroxyalkanoic acids such as PHBH and PHBV, PLA, cellulose, starch, chitosan, and other natural polymer-derived resins. As the biodegradable resin, particularly preferred are resins derived from PBSA, PBS, PBAT, PLA, and starch.
[0083] In addition, in consideration of reducing the environmental load, the raw material for the resin to be combined is preferably derived from biomass, and most preferably is 100% derived from biomass.
[0084] The marine biodegradable resin composition of the present invention may contain a solvent. The solvent may dissolve the resin that serves as a matrix while leaving the marine biodegradable polymer compound as particles, or may dissolve both the resin and the marine biodegradable polymer compound. By appropriately adjusting these, the composition can be used as a molded body formed into a film by casting or the like, as a paint, ink, surface treatment agent, etc. Examples of preferred solvents include water, formic acid, hexane, heptane, acetonitrile, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethylsulfoxide, dimethylsulfone, acetone, methyl ethyl ketone, diethyl ketone, acetophenone, dimethyl ether, dipropyl ether, tetrahydrofuran, chloroform, methylene chloride, trichloroethylene, ethylene dichloride, tetrachloroethane, chlorobenzene, methanol, ethanol, n-propanol, isopropanol, butanol, pentanol, hexafluoroisopropanol, methyl glycol, methyl triglycol, hexyl glycol, phenyl glycol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, benzene, toluene, xylene, etc. These may be used alone or in combination of two or more.
[0085] When a solvent is used, the total concentration of the resin and the marine biodegradable polymer compound in the resin composition is preferably 0.5 to 90% by mass, more preferably 1 to 80% by mass, even more preferably 5 to 60% by mass, and most preferably 10 to 50% by mass. The ratio of the marine biodegradable polymer compound to the resin is preferably 99:1 to 10:90, more preferably 97:3 to 40:60, even more preferably 95:5 to 50:50, and most preferably 90:10 to 60:40, by mass.
[0086] The marine biodegradable resin composition of the present invention may not contain a solvent. In this case, the resin may be thermally melted and a non-melting marine biodegradable polymer compound may be added thereto and mixed, or the resin and the marine biodegradable polymer compound may be melted together and mixed.
[0087] In the marine biodegradable resin composition of the present invention, the content of the marine biodegradable polymer compound is preferably 1 to 50 mass%, more preferably 3 to 50 mass%, more preferably 5 to 45 mass%, even more preferably 7 to 40 mass%, and most preferably 10 to 35 mass%. On the other hand, the content of the resin is preferably 50 to 99 mass%, more preferably 50 to 97 mass%, even more preferably 55 to 95 mass%, even more preferably 60 to 93 mass%, and most preferably 65 to 90 mass%. By containing the marine biodegradable polymer compound in the above range, it can be utilized as a marine biodegradation promoter that promotes the progress of biodegradation in seawater while maintaining the physical properties of the biodegradable resin. The marine biodegradable polymer compound may be used alone or in combination of two or more.
[0088] The marine biodegradable resin composition of the present invention may contain additives such as antioxidants, release agents, peeling agents, surface modifiers, hydrophobic agents, water repellents, hydrophilizing agents, dyes and pigments, colorants, heat stabilizers, light stabilizers, weather resistance improvers, antistatic agents, antifogging agents, lubricants, antiblocking agents, hardeners, softeners, compatibilizers, flame retardants, flow improvers, plasticizers, dispersants, antibacterial agents, fillers, metal deactivators, etc. The content of these additives is not particularly limited as long as it does not impair the effects of the present invention, but is preferably about 0.1 to 50 parts by mass relative to 100 parts by mass of the resin.
[0089] When the marine biodegradable resin composition contains a solvent, it can be prepared, for example, by adding the resin, the marine biodegradable polymer compound, and the additives, if necessary, to a solvent simultaneously or in any order, and mixing them. When the marine biodegradable resin composition does not contain a solvent, it can be prepared, for example, by melting the resin, adding the marine biodegradable polymer compound and the additives, if necessary, to the solvent simultaneously or in any order, and mixing them, or by heating the resin and the marine biodegradable polymer compound to melt them together and mix them, and adding the additives, if necessary, and mixing them.
[0090] [Molded body] By molding the resin composition, a molded article in which the marine biodegradable polymer compound is dispersed or dissolved in the resin can be obtained. When the resin composition contains a solvent, the resin composition can be used as is for molding, and when the resin composition does not contain a solvent, the resin or the resin and the marine biodegradable polymer compound in the resin composition can be melted by heat and then molded.
[0091] The shape of the molded product may be, for example, a film, a fiber, a plate, a foam molded product, or any other shape depending on the application. The molding method is not particularly limited, and any of the conventionally known molding methods may be used. Specific examples of such methods include blow molding, injection molding, extrusion molding, compression molding, melt extrusion molding, solution casting molding, and calendar molding.
[0092] The marine biodegradable resin composition of the present invention can be used as a raw material for plastic molded products, and as various additives for molded products such as liquids, coatings, films, plates, paper, etc. When used as a raw material for plastic molded products, it can be used as a raw material for general-purpose applications such as films, packaging, containers, trays, laminating materials, adhesives, coating materials, medical materials, fibers for clothing, shoes, belts, tires, tubes, shock absorbing materials, fishing lines, fishing nets, etc., and materials for marine applications, etc., and is particularly suitable for use as a raw material for marine applications, etc. In addition, when used as an additive, for example, light scattering agents and optical filter materials, colorants, cosmetics, absorbents, adsorbents, inks, adhesives, electromagnetic wave shielding materials, fluorescent sensors, biomarkers, recording materials, recording elements, polarizing materials, drug carriers for drug delivery systems (DDS), biosensors, DNA chips, test agents, baked voided molded products, antiblocking agents, screen printing, offset printing, process printing, gravure printing, pad printing, coaters, inkjet printing, etc., additives for printing inks used in marking pens, ballpoint pens, fountain pens, brush pens, markers, and other writing instrument ink additives, crayons, paints, erasers, and other stationery additives, paint additives used in brush painting, spray painting, electrostatic painting, electrocoating, flow painting, roller painting, dip painting, etc., and especially paints used for marine applications such as hull paints. It can be widely used as an additive. EXAMPLES
[0093] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0094] In the following examples and comparative examples, the metal ion equivalent was measured by heating and decomposing the target substance with nitric acid or aqua regia, and using an ICP-MS (ICPE-9820 manufactured by Shimadzu Corporation) by emission spectrometry. The melting temperature was measured using a differential scanning calorimeter (DSC6200 manufactured by Seiko Instruments Inc.). Specifically, 5 mg of the measurement sample was precisely weighed, and the precisely weighed measurement sample was placed in an aluminum pan. Using an empty aluminum pan as a reference, the temperature was raised at a rate of 10°C / min in the measurement temperature range of 20 to 300°C at normal temperature and humidity. The melting temperature was calculated from the endothermic (melting) peak point of the obtained curve.
[0095] [1] Synthesis of marine biodegradable polymer compound A [Example 1-1] Synthesis of marine biodegradable polymer compound A-1 43.2 g of 1,4-butanediol and 53.7 g of maleic acid were added to a 300 mL recovery flask and stirred at 160°C for 6 hours under a nitrogen atmosphere. Then, 2.26 g of 3-mercaptopropionic acid, 1.33 g of triethylamine and 100 g of acetonitrile were added and stirred at 70°C for 3 hours to obtain marine biodegradable polymer compound A-1. Marine biodegradable polymer compound A-1 is 1 H-NMR measurement confirmed that the copolymer had a number average molecular weight of 2100, an average of eight aliphatic unsaturated bonds, and an average of two acidic groups.
[0096] [Example 1-2] Synthesis of marine biodegradable polymer compound A-2 41.6 g of 1,4-butanediol, 50.8 g of dimethyl maleate, 16.8 g of dimethyl terephthalate, and 0.96 g of titanium tetraisopropoxide were added to a 300 mL recovery flask and stirred at 160°C for 5 hours under a nitrogen atmosphere. After that, 37.1 g of 3-mercaptopropionic acid and 18.2 g of acetonitrile were added and stirred at 130°C for 4 hours to obtain marine biodegradable polymer compound A-2. Marine biodegradable polymer compound A-2 is 1 H-NMR measurement confirmed that the copolymer had a number average molecular weight of 2000, an average of three aliphatic unsaturated bonds, and an average of four acidic groups.
[0097] [Example 1-3] Synthesis of marine biodegradable polymer compound A-3 39.7 g of 1,4-butanediol, 25.2 g of succinic acid, and 25.0 g of maleic acid were added to a 300 mL recovery flask and stirred at 160°C for 6 hours under a nitrogen atmosphere. Then, 25.7 g of 3-mercaptopropionic acid and 11.4 g of acetonitrile were added and stirred at 130°C for 3 hours to obtain marine biodegradable polymer compound A-3. Marine biodegradable polymer compound A-3 is 1 H-NMR measurement confirmed that the copolymer had a number average molecular weight of 1,800, an average of two aliphatic unsaturated bonds, and an average of two acidic groups.
[0098] [Examples 1-4] Synthesis of marine biodegradable polymer compound A-4 43.5 g of 1,4-butanediol, 52.9 g of maleic acid, and 0.53 g of fumaric acid were added to a 300 mL recovery flask and stirred at 160°C under a nitrogen atmosphere for 6 hours. After that, 1.25 g of 5-aminovaleric acid was added and stirred at 160°C under a nitrogen atmosphere for 3 hours to obtain marine biodegradable polymer compound A-4. Marine biodegradable polymer compound A-4 is 1 H-NMR measurement confirmed that the copolymer had a number-average molecular weight of 1,900, an average of seven aliphatic unsaturated bonds, and an average of two acidic groups.
[0099] [Examples 1-5] Synthesis of marine biodegradable polymer compound A-5 46.9g of 1,4-butanediol, 39.5g of adipic acid, and 31.3g of maleic acid were added to a 500mL recovery flask and stirred at 160℃ for 6 hours under a nitrogen atmosphere, then 8.45g of di-tert-butyl malonate, 4.00g of potassium carbonate, and 100g of acetonitrile were added and stirred at 70℃ for 3 hours. Then, 174mL of 3N hydrochloric acid was added and stirred for 1 hour. Next, an aqueous sodium hydroxide solution was added to adjust the pH to 7, and the mixture was extracted with ethyl acetate and dried under reduced pressure to obtain marine biodegradable polymer compound A-5. Marine biodegradable polymer compound A-5 is 1H-NMR measurement confirmed that the copolymer had a number-average molecular weight of 3,600, an average of eight aliphatic unsaturated bonds, and an average of three acidic groups.
[0100] [Comparative Example 1-1] As the comparative polymer compound AX-1, sodium polyacrylate (degree of polymerization: 2700 to 7500) (FUJIFILM Wako Pure Chemical Industries, Ltd.) was used.
[0101] Table 1 below shows the marine biodegradable polymer compounds A-1 to A-5 and polymer compound AX-1. [Table 1]
[0102] [2] Synthesis of marine biodegradable polymer compound B [Example 2-1] Synthesis of marine biodegradable polymer compound B-1 60.0g of marine biodegradable polymer compound A-1 and 21.1g of 10% by mass sodium bicarbonate aqueous solution were added to a 300mL eggplant flask and stirred, then 20.1g of 30% by mass calcium chloride aqueous solution was added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-1. The melting point of marine biodegradable polymer compound B-1 was 51°C.
[0103] [Example 2-2] Synthesis of marine biodegradable polymer compound B-2 59.8g of marine biodegradable polymer compound A-2 and 40.8g of 10% by mass potassium bicarbonate aqueous solution were added to a 300mL eggplant flask and stirred, then 39.9g of 30% by mass magnesium chloride aqueous solution was added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-2. The melting point of marine biodegradable polymer compound B-2 was 107°C.
[0104] [Example 2-3] Synthesis of marine biodegradable polymer compound B-3 30.4g of marine biodegradable polymer compound A-3 and 78.2g of 10% by mass potassium bicarbonate aqueous solution were added to a 300mL eggplant flask and stirred, then 25.1g of 30% by mass calcium chloride aqueous solution was added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-3. The melting point of marine biodegradable polymer compound B-3 was 95°C.
[0105] [Example 2-4] Synthesis of marine biodegradable polymer compound B-4 61.1g of marine biodegradable polymer compound A-4 and 50.0g of 2.5% by mass sodium hydroxide aqueous solution were added to a 300mL eggplant flask and stirred, then 15.2g of 30% by mass aluminum sulfate aqueous solution was added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-4. The melting point of marine biodegradable polymer compound B-4 was 58°C.
[0106] [Example 2-5] Synthesis of marine biodegradable polymer compound B-5 60g of marine biodegradable polymer compound A-5 and 35.1g of 2% by mass sodium hydroxide aqueous solution were added to a 300mL eggplant flask and stirred, then 12.0g of 30% by mass calcium chloride aqueous solution and 2.6g of 30% by mass magnesium chloride aqueous solution were added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain marine biodegradable polymer compound B-5. The melting point of marine biodegradable polymer compound B-5 was 61°C.
[0107] [Comparative Example 2-1] Synthesis of ionically cross-linked polymer compound BX-1 In a 300 mL recovery flask, 30.0 g of sodium polyacrylate (polymerization degree 2500-7500) (FUJIFILM Wako Pure Chemical Industries, Ltd.) and 100 g of ion-exchanged water were added and stirred, and then 35.1 g of 30 mass% calcium chloride aqueous solution was added and stirred. The precipitate was washed with water and then dried under reduced pressure to obtain ion-crosslinked polymer compound BX-1. Polymer compound BX-1 did not melt by heat.
[0108] Table 2 below shows the marine biodegradable polymer compounds B-1 to B-5 and the ionically cross-linked polymer compound BX-1. [Table 2]
[0109] [3] Biodegradability testing of compounds and powders [Examples 3-1 to 3-10, Comparative Examples 3-1 to 3-2] Marine biodegradable polymer compounds A-1 to A-5, marine biodegradable polymer compounds B-1 to B-5, compound AX-1, and polymer compound BX-1 were subjected to seawater biodegradation tests using the following method. As a control material, microcrystalline cellulose (Sigma-Aldrich Avicel PH-101) was used and evaluated based on the relative biodegradability of cellulose. The results are shown in Table 3.
[0110] <Test method and conditions> Biodegradability measurement method: Measurement of oxygen consumption using a closed respirometer (ASTM D6691 reference) Test equipment: OxiTop IDS (WTW) Culture temperature: 30±1℃, dark place Biodegradation (%)=(BOD O -BOD B ) / ThOD×100 BOD O : Biochemical oxygen demand for testing or inoculum activity confirmation (measured value: mg) BOD B : Average biochemical oxygen demand in blank test (measured value: mg) ThOD: required when the test or control material is completely oxidized Theoretical oxygen demand (calculated value: mg) Relative biodegradability of cellulose (%) = (maximum biodegradability of test particles / maximum biodegradability of cellulose) x 100 Seawater (collected from Tokyo Bay [Chiba Prefecture: Chiba Port])] The collected seawater was aerated at room temperature of 25 degrees Celsius after removing foreign matter with a 10 μm filter. In addition, ammonium chloride and potassium dihydrogen phosphate were added as inorganic nutrients at 0.05 g / L and 0.1 g / L, respectively.
[0111] [Table 3]
[0112] The results shown in Table 3 indicate that the particles of the present invention had biodegradability approximately equivalent to that of cellulose within a culture period of 60 days.
[0113] [4] Preparation of marine biodegradable resin composition and confirmation test in seawater-1 (1) Surface changes [Examples 4-1 to 4-5, Comparative Examples 4-1 to 4-2] Marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1, which were crushed with a crusher (Osaka Chemical Co., Ltd. Wonder Blender WB-1) and classified with a stainless steel sieve (26 μm mesh), were mixed with biodegradable resin PBSA (Mitsubishi Chemical Co., Ltd. FD-92) at 140 ° C. to a concentration of 20 mass%, and press molded at 150 ° C. to prepare a film with a thickness of 200 μm (Examples 4-1 to 4-5, Comparative Example 4-1). In addition, PBSA itself (not containing marine biodegradable polymer compounds) was press molded at 150 ° C. to prepare a film with a thickness of 200 μm (Comparative Example 4-2). The obtained films were cut into 10 mm square pieces and placed in 200 mL of ion-exchanged water and 200 mL of seawater (collected from Tokyo Bay (Chiba Port, Chiba Prefecture)) at 25°C for 7 and 30 days, respectively, and then the films were taken out and the surface and appearance of the films were observed under a scanning electron microscope. The results are shown in Table 4.
[0114] [Table 4]
[0115] From the results shown in Table 4, it is believed that biodegradability is promoted not only by the breakdown in seawater but also by the presence of microorganisms in seawater.
[0116] (2) Weight loss of composite resin [Examples 5-1 to 5-5, Comparative Examples 5-1 to 5-2] Using the same method as in (1), films were prepared by adding marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 to PBSA, and a film of PBSA alone. The obtained films were processed into 20 mm squares, sandwiched between stainless steel nets, and immersed in seawater (collected from Tokyo Bay [Chiba Prefecture: Chiba Port]) in a 15 L tank, and the progress of weight loss after immersion for 30, 60, and 90 days was observed. The results are shown in Table 5.
[0117] [Table 5]
[0118] (3) Tensile strength measurement [Examples 6-1 to 6-5, Comparative Example 6-1] In the same manner as in (1), films were prepared by adding marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 to PBSA at concentrations of 10 mass%, 20 mass%, or 30 mass%, respectively, and a film of PBSA alone. According to JIS K 7139-A22, dumbbells were prepared from the various films, and the tensile stress (yield point) was measured using a universal testing machine (MCT-2150, manufactured by A&D Co., Ltd.). Each sample was measured five times, and the average value was taken as the tensile stress. The results are shown in Table 6.
[0119] [Table 6]
[0120] [5] Preparation of marine biodegradable resin composition and confirmation test in seawater-2 (1) Surface changes [Examples 7-1 to 7-5, Comparative Examples 7-1 to 7-2] Marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1, which were crushed with a crusher (Wonder Blender WB-1 manufactured by Osaka Chemical Co., Ltd.) and classified with a stainless steel sieve (26 μm mesh size), were mixed with a biodegradable starch-based resin (Mater-Bi EF05B, manufactured by Novamont) at 140 ° C. to a concentration of 20 mass%, and press molded at 150 ° C. to prepare a film with a thickness of 200 μm (Examples 7-1 to 7-5, Comparative Example 7-1). In addition, the starch-based resin itself (not including particle groups) was press molded at 150 ° C. to prepare a film with a thickness of 200 μm (Comparative Example 7-2). The obtained films were cut into 10 mm square pieces and placed in 200 mL of ion-exchanged water and 200 mL of seawater (collected from Tokyo Bay (Chiba Prefecture: Chiba Port)) at 25°C for 7 and 30 days, respectively, and then the films were taken out and the surface and appearance of the films were observed under a scanning electron microscope. The results are shown in Table 7.
[0121] [Table 7]
[0122] From the results shown in Table 5, it is believed that biodegradability is promoted not only by the breakdown in seawater but also by the presence of microorganisms in seawater.
[0123] (2) Weight loss of composite resin [Examples 8-1 to 8-5, Comparative Examples 8-1 to 8-2] Using the same method as in (1), films were prepared in which marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 were added to starch-based resin, and a film of starch-based resin alone was also prepared. The obtained film was cut into 20 mm squares, sandwiched between stainless steel netting, and immersed in seawater (collected from Tokyo Bay [Chiba Prefecture: Chiba Port]) in a 15 L tank. The weight loss after immersion for 30, 60, and 90 days was observed. The results are shown in Table 8.
[0124] [Table 8]
[0125] (3) Tensile strength measurement [Examples 9-1 to 9-5, Comparative Example 9-1] Using a method similar to that used in (1), films were prepared in which marine biodegradable polymer compounds B-1 to B-5 and polymer compound BX-1 were added to starch-based resin at concentrations of 10 mass%, 20 mass%, or 30 mass%, respectively, and films of starch-based resin alone. According to JIS K 7139-A22, dumbbells were made from various films and the tensile stress (yield point) was measured using a universal testing machine (MCT-2150, manufactured by A&D Co., Ltd.). Five measurements were made for each sample, and the average value was taken as the tensile stress. The results are shown in Table 9.
[0126] [Table 9]
[0127] From the above results, the marine biodegradable polymer compound of the present invention is easily dissolved or hydrophilic in seawater by being decomposed into lower molecular weight or salt-substituted by biodegradation prior to the biodegradable resin. Therefore, by adding a marine biodegradation promoter consisting of the marine biodegradable polymer compound of the present invention to a resin composition that is biodegradable in soil or compost or a resin composition that is poorly biodegradable in the sea, it becomes possible to form irregularities in seawater, aid the attachment of microorganisms, and promote biodegradation, which ultimately makes it possible to improve the overall marine biodegradability and reduce the environmental burden. By combining the marine biodegradation promoter consisting of the marine biodegradable polymer compound of the present invention with a resin that is biodegradable in soil or compost, it is possible to improve the seawater biodegradability, and by appropriately modifying the structure of the organic anion, it is possible to incorporate a number of effects, such as adjustment of the melting temperature and viscosity, adjustment of the degree of crystallinity, adjustment of microbial adhesion and biodegradability, adjustment of physical properties such as the resin tensile strength, flexural strength, and elasticity, improvement of compatibility with the resin, adjustment of the degree of hydrophobicity, adjustment of hydrophobicity, adjustment of adhesion and plasticity, etc., and it is possible to improve both the biodegradability and physical properties of the marine biodegradable resin composition.
Claims
1. The compound has a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond in the main chain, and has one or more -COO - R + , -SO 3 - R + , -O-SO 3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation or a monovalent organic cation.
2. The marine biodegradable polymer compound according to claim 1, having two or more acidic groups in the side chain.
3. The marine biodegradable polymer compound according to claim 1 , wherein the repeating unit contains an ester bond.
4. 2. The marine biodegradable polymer compound according to claim 1, which has a number average molecular weight of 300 to 100,000.
5. Furthermore, the main chain has a —COO - R + , -SO 3 - R + , -O-SO 3 - R + and -P(=O)(OH)-O - R + (In the formula, R + The marine biodegradable polymer compound according to claim 1, which has a substituent selected from the group consisting of hydrogen ions, monovalent metal cations and monovalent organic cations.
6. 2. The marine biodegradable polymer compound according to claim 1, wherein the number of aliphatic unsaturated carbon-carbon bonds in one molecule is from 0.1 to 50 on average.
7. The marine biodegradable polymer compound according to claim 1, wherein the substituent is bonded to the main chain via a linking group having 1 to 50 atoms.
8. The substituent is -COO - R + 2. The marine biodegradable polymer compound according to claim 1,
9. 2. The marine biodegradable polymer compound according to claim 1, having maleic acid residues in the main chain.
10. R + The marine biodegradable polymer compound according to claim 1, wherein is a monovalent metal cation or a monovalent organic cation.
11. A marine biodegradable polymer compound comprising a polymeric polyvalent anion derived from the marine biodegradable polymer compound according to claim 1 bound via a divalent or higher metal cation.
12. The content of the metal cation is 1 to 100 eq / 10 5 The marine biodegradable polymer compound according to claim 11, wherein
13. The marine biodegradable polymer compound according to claim 11, wherein the divalent or higher metal cation is a calcium ion, a magnesium ion or an aluminum ion.
14. A marine biodegradation promoter comprising the marine biodegradable polymer compound according to any one of claims 1 to 13.
15. A marine biodegradable resin composition comprising the marine biodegradation promoter according to claim 14 and a resin.
16. The marine biodegradable resin composition according to claim 15, wherein the resin is a biodegradable resin.
17. The marine biodegradable resin composition according to claim 16, wherein the content of the marine biodegradation promoter is 1 to 50 mass% and the content of the biodegradable resin is 50 to 99 mass%.
18. A molded article obtained from the marine biodegradable resin composition according to claim 15.
19. A polymer compound containing a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, and having an aliphatic unsaturated carbon-carbon bond in the main chain, and a reactive group reactive with an aliphatic unsaturated carbon-carbon bond, and -COOH, -SO 3 H, -O-SO 3 A method for producing a marine biodegradable polymer compound, comprising the step of reacting a compound having a substituent selected from H and -P(=O)(OH)-OH with a compound having a substituent selected from H and -P(=O)(OH)-OH.
20. The polymer contains a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond in the main chain, and has one or more -COOH, -SO 3 H, -O-SO 3 A method for producing a marine biodegradable polymer compound, comprising a step of neutralizing a substituent of a marine biodegradable polymer compound having a substituent selected from H and -P(=O)(OH)-OH in a side chain thereof with a monovalent base.
21. The method for producing a marine biodegradable polymer compound according to claim 20, wherein the base is lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate or potassium bicarbonate.
22. The compound has a repeating unit containing at least one bond selected from an ester bond, an amide bond, a carbonate bond, a urethane bond, and a urea bond, has an aliphatic unsaturated carbon-carbon bond in the main chain, and has one or more -COO - R + , -SO 3 - R + , -O-SO 3 - R + and -P(=O)(OH)-O - R + (In the formula, R + is a hydrogen ion, a monovalent metal cation, or a monovalent organic cation.) A method for producing a marine biodegradable polymer compound, comprising a step of crosslinking a marine biodegradable polymer compound having a substituent selected from the group consisting of a hydrogen ion, a monovalent metal cation, and a monovalent organic cation, at a side chain, with a polyvalent metal salt.
23. The method for producing a marine biodegradable polymer compound according to claim 22, wherein the polyvalent metal salt is a calcium salt, a magnesium salt or an aluminum salt.