Melt-blown nonwoven fabric, sanitary material, waterproof sheet, and medical sheet
A blend of thermoplastic non-elastomer and elastomer fibers in melt-blown nonwoven fabrics addresses the limitations of tensile strength and resistance, enhancing their suitability for high filtration and deformable applications.
Patent Information
- Application Number
- JP2023087311
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Melt-blown nonwoven fabrics disclosed in existing technologies lack sufficient tensile strength, elongation, toughness, water pressure resistance, and abrasion resistance, limiting their applications in high filtration pressure and deformable applications such as sanitary materials and medical clothing.
A melt-blown nonwoven fabric composed of thermoplastic non-elastomer fibers (A) and thermoplastic elastomer fibers (B) with a melting point difference, blended in a ratio of 60/40 to 99/1, enhancing fiber fusion and integration, resulting in improved tensile strength, elongation, toughness, and water pressure resistance.
The blended fabric exhibits excellent tensile strength, elongation, toughness, and water pressure resistance, making it suitable for applications requiring high filtration pressure and deformability, such as sanitary materials and medical clothing.
Smart Images

Figure 2024170251000002 
Figure 2024170251000003 
Figure 2024170251000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to meltblown nonwoven fabrics, sanitary materials, waterproof sheets, and medical sheets. [Background technology]
[0002] Meltblown nonwoven fabrics are made of ultrafine fibers and are superior in flexibility, uniformity, and density to general spunbond nonwoven fabrics, and are therefore widely used in filters (e.g., liquid filters, air filters, etc.), sanitary materials, etc.
[0003] Patent Document 1 discloses a long fiber nonwoven fabric (hereinafter also referred to as "meltblown nonwoven fabric") manufactured by the meltblowing method. The meltblown nonwoven fabric disclosed in Patent Document 1 is made by mixing specific adhesive fibers and specific non-adhesive fibers in a ratio of 30 / 70 weight % to 95 / 5 weight %. Specifically, Patent Document 1 discloses a meltblown nonwoven fabric in which polypropylene fibers and ethylene-octene copolymer fibers are mixed in a weight ratio of 30 / 70. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-197291 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the meltblown nonwoven fabric disclosed in Patent Document 1 may not have sufficient tensile strength. Therefore, the meltblown nonwoven fabric disclosed in Patent Document 1 may not be suitable for applications requiring high filtration pressure (e.g., high flow rate filtration, fine particle capture, etc.) or applications requiring conformability to the human body and abrasion resistance (e.g., sanitary materials, medical clothing, etc.). In order to expand the applications of meltblown nonwoven fabrics, there is a demand for meltblown nonwoven fabrics that are excellent in resistance to breakage (i.e., tensile strength, elongation, and toughness), water pressure resistance, and abrasion resistance.
[0006] The present disclosure has been made in light of the above. An object of one embodiment of the present disclosure is to provide a meltblown nonwoven fabric, a sanitary material, a waterproof sheet, and a medical sheet that are excellent in tensile strength, elongation, toughness, water pressure resistance, and abrasion resistance. [Means for solving the problem]
[0007] Means for solving the above problems include the following embodiments. <1> The fiber (A) includes a thermoplastic non-elastomer (a) and a fiber (B) includes a thermoplastic elastomer (b), The melting point of the thermoplastic elastomer (b) is lower than the melting point of the thermoplastic non-elastomer (a); The meltblown nonwoven fabric has a blend ratio (A / B) of the fibers (A) and the fibers (B) of 60 / 40 to 99 / 1 in terms of mass ratio. <2> The thermoplastic non-elastomer (a) comprises a propylene homopolymer, The thermoplastic elastomer (b) includes a polyolefin-based elastomer. <1> The meltblown nonwoven fabric according to claim 1. <3> The blend ratio (A / B) is 65 / 35 to 72 / 28. <1> or <2> The meltblown nonwoven fabric according to claim 1. <4> Tensile strength in machine direction (MD) per unit weight is 0.28N·m 2 / 25mm·g or more, <1> ~ <3> 13. The meltblown nonwoven fabric according to any one of claims 1 to 12. <5> Machine direction (MD) toughness is 12.5N / in 2 The above <1> ~ <4> 13. The meltblown nonwoven fabric according to any one of claims 1 to 12. <6> The water pressure resistance is 320mmH2O or more. <1> ~ <5> 13. The meltblown nonwoven fabric according to any one of claims 1 to 12. <7> Tensile strength in machine direction (MD) per unit weight is 0.28N·m 2 / 25mm·g or more, The elongation in the machine direction (MD) is 120% or more, Machine direction (MD) toughness is 10N / in 2 That's all. The water pressure resistance is 320mmH2O or more. <1> ~ <6> 13. The meltblown nonwoven fabric according to any one of claims 1 to 12. <8> The above <1> ~ <7> A sanitary material comprising the meltblown nonwoven fabric according to any one of claims 1 to 5. <9> The above <1> ~ <7> A water-resistant sheet comprising the meltblown nonwoven fabric according to any one of claims 1 to 5. <10> The above <1> ~ <7> A medical sheet comprising the meltblown nonwoven fabric according to any one of claims 1 to 5. Effect of the Invention
[0008] According to one embodiment of the present disclosure, there are provided a meltblown nonwoven fabric, a sanitary material, a waterproof sheet, and a medical sheet that are excellent in tensile strength, elongation, toughness, water pressure resistance, and abrasion resistance. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram showing an apparatus for producing a meltblown fiber nonwoven fabric according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a front view of a die according to an embodiment of the present disclosure. [Diagram 3] FIG. 3 is a graph showing the MD tensile strength versus the POE blend ratio for the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In the present disclosure, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit. In the present disclosure, in the ranges described stepwise, the upper or lower limit value described in one range may be replaced with the upper or lower limit value of another range described stepwise. In the ranges described in the present disclosure, the upper or lower limit value of the range may be replaced with the value shown in the examples. In the present disclosure, the term "step" refers not only to an independent step, but also to a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In this disclosure, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, it means the total amount of multiple substances present in the composition, unless otherwise specified. In this disclosure, "nonwoven fabric" refers to a flat assembly of fibers that has a certain level of structural strength achieved by physical and / or chemical processes, excluding weaving, knitting, and papermaking.
[0011] (1) Meltblown nonwoven fabric The meltblown nonwoven fabric (hereinafter also referred to as "MB nonwoven fabric") of the present disclosure includes fiber (A) containing a thermoplastic non-elastomer (a) and fiber (B) containing a thermoplastic elastomer (b). The melting point of the thermoplastic elastomer (b) is lower than the melting point of the thermoplastic non-elastomer (a). The blend ratio (A / B) of the fiber (A) and the fiber (B) is 60 / 40 to 99 / 1 in mass ratio.
[0012] In the present disclosure, the term "thermoplastic non-elastomer" refers to a thermoplastic resin that does not have rubber-like elasticity at room temperature. In more detail, the term "thermoplastic non-elastomer" refers to a thermoplastic resin that has a tensile modulus of elasticity of 6.0×10 at 25° C. 8 This indicates a thermoplastic resin with a thermal expansion coefficient of 10 Pa or more. "Thermoplastic elastomer" refers to a thermoplastic resin that has rubber-like elasticity at room temperature. Thermoplastic elastomers are partially crosslinked thermoplastic resins. In detail, a thermoplastic elastomer has a tensile modulus of elasticity of 6.0×10 at 25°C. 8 This indicates a thermoplastic resin having a compressive strength of less than Pa. "Meltblown nonwoven" refers to a nonwoven fabric made by extruding molten polymer into a high velocity hot gas stream to form fibers that are then laid down on a moving screen. The average fiber diameter of meltblown nonwoven fabrics is typically less than 10 μm.
[0013] Since the meltblown nonwoven fabric of the present disclosure has the above-described configuration, it has excellent tensile strength, elongation, toughness, water pressure resistance and abrasion resistance. Meltblown nonwoven fabrics are obtained by extruding molten polymer from a nozzle into a high-speed, high-temperature gas stream to produce multiple fibers, which are then layered on a moving screen. In this process, the fibers extruded from the nozzle into the high-temperature gas stream are stretched and thinned by the high-temperature gas stream, and move through the air toward the screen while gradually cooling as the high-temperature gas stream mixes with the surrounding air. The fibers are then deposited on the screen by the suction action of the air suction installed at the bottom of the screen, and are collected while fused together by the residual heat. Fibers deposited closer to the screen are subject to a stronger suction action of the air suction. As a result, the fibers tend to be more strongly fused together than those deposited farther from the screen. When the fibers constituting the meltblown nonwoven fabric are composed only of fibers (A) containing a thermoplastic non-elastomer (a), the fibers (A) are likely to solidify the resin on the fiber surface as they are stretched and thinned and cooled, and require a strong air suction action to fuse them. For this reason, the fibers (A) on the opposite side to the screen side of the meltblown nonwoven fabric laminated on the screen (hereinafter also referred to as the "nozzle side") are unlikely to fuse together. Therefore, the fibers (A) on the nozzle side of the meltblown nonwoven fabric are likely to unravel. In other words, the meltblown nonwoven fabric is unlikely to be integrated as a whole. As a result, the tensile strength of the meltblown nonwoven fabric and the wear resistance of the nozzle side surface may not be sufficient. On the other hand, in the meltblown nonwoven fabric of the present disclosure, the thermoplastic elastomer (b) contained in the fiber (B) has a lower melting point than the thermoplastic non-elastomer (a) contained in the fiber (A) and exhibits adhesion. As a result, the fiber (B) is less likely to undergo solidification of the fiber surface resin accompanying stretching and thinning and cooling than the fiber (A) under the same condition of the distance from the nozzle to the screen, and can be fused to the fiber (A) or the fiber (B) without the suction action of air suction. In other words, in the meltblown nonwoven fabric of the present disclosure, the fibers are fused to each other throughout the entire thickness direction. In other words, the meltblown nonwoven fabric of the present disclosure is more likely to be integrated as a whole than a meltblown nonwoven fabric made only of the fiber (A) produced under the same condition of the distance from the nozzle to the screen. Furthermore, the mixed fiber ratio (A / B) is 60 / 40 to 99 / 1 in mass ratio. In other words, the fiber (A) having a relatively high strength is contained in a larger amount than the fiber (B) having a relatively low strength. As a result, it is presumed that the meltblown nonwoven fabric of the present disclosure has excellent tensile strength, elongation, toughness, water pressure resistance and abrasion resistance.
[0014] In the meltblown lamination, the direction parallel to the moving direction of the screen among the surface directions of the movable screen on which the fibers are laminated is also referred to as the "machine direction (MD)". The direction perpendicular to the moving direction of the screen among the surface directions of the movable screen on which the long fibers are laminated is also referred to as the "cross direction (CD)".
[0015] The machine direction (MD) of a meltblown nonwoven can be determined from the meltblown nonwoven itself by measuring the tensile strength of the meltblown nonwoven. Generally, in the production of meltblown nonwoven fabrics, the moving speed of the screen is set to be fast from the viewpoint of productivity. Therefore, the fibers contained in the meltblown nonwoven fabric tend to be oriented in a direction parallel to the machine direction (MD) when stacked on the screen. As a result, the tensile strength of the meltblown nonwoven fabric in the machine direction (MD) is higher than the tensile strength of the meltblown nonwoven fabric in the cross direction (CD). Therefore, by measuring the tensile strength of the meltblown nonwoven fabric, the machine direction (MD) of the meltblown nonwoven fabric can be determined from the meltblown nonwoven fabric itself.
[0016] The MB nonwoven fabric is a mixed fiber nonwoven fabric containing fiber (A) and fiber (B). The MB nonwoven fabric may further contain known fibers in addition to fiber (A) and fiber (B).
[0017] The mixed fiber ratio (A / B) is, in mass ratio, 60 / 40 to 99 / 1. The mixed fiber ratio (A / B) is preferably 65 / 35 to 72 / 28. This provides the meltblown nonwoven fabric with an excellent balance between strength and elongation. The method for measuring the mixed fiber ratio (A / B) is the same as that described in the Examples.
[0018] The average fiber diameter of the MB nonwoven fabric is usually less than 10 μm and is appropriately selected depending on the application of the MB nonwoven fabric. From the viewpoint of filter performance and water pressure resistance, the average fiber diameter of the MB nonwoven fabric is preferably 6.5 μm or less, more preferably 6.0 μm or less, and even more preferably 5.5 μm or less. The average fiber diameter of the MB nonwoven fabric may be 2.5 μm or more, more preferably 5.0 μm or more, or may be 5.3 μm or more. From these viewpoints, the average fiber diameter of the MB nonwoven fabric is preferably 2.5 μm to 6.5 μm. The method for measuring the average fiber diameter of the MB nonwoven fabric is the same as that described in the Examples.
[0019] The MB nonwoven fabric is a sheet-like material. The structure of the MB nonwoven fabric is appropriately selected depending on the application of the MB nonwoven fabric, and may be, for example, a single-layer structure or a multi-layer structure of two or more layers.
[0020] The thickness of the MB nonwoven fabric is not particularly limited and is appropriately selected depending on the application. The thickness of the MB nonwoven fabric is preferably 0.005 mm to 10 mm, more preferably 0.01 mm to 2 mm. When the thickness is 0.005 mm or more, when the MB nonwoven fabric is used as a filter, a good balance between the dust collection efficiency and the pressure loss is ensured, and the filtration performance tends to be further improved. The thickness of the MB nonwoven fabric was measured as follows: Ten samples (size: 100 mm lengthwise × 100 mm widthwise) were taken from the MB nonwoven fabric. The thickness of the samples was measured at five points, namely, the center and four corners, using a thickness meter (PEACOCK, product number "R1-250", measuring probe 25 mmφ) with a load of 7 g / m 2 The thickness is measured by the average of the 10 samples.
[0021] The basis weight of the MB nonwoven fabric is not particularly limited and is appropriately selected depending on the application. The basis weight of the MB nonwoven fabric is preferably 0.001 g / m 2 ~30g / m 2 , more preferably 0.002 g / m 2 ~20g / m 2 The basis weight is 0.001g / m 2 When the weight per unit area is 30 g / m or more, the strength of the MB nonwoven fabric is improved, and the MB nonwoven fabric tends to be easier to manufacture. 2 When the pressure loss of the MB nonwoven fabric is not too high, the MB nonwoven fabric tends to be suitable for use as a filter. The method for measuring the basis weight of the MB nonwoven fabric is the same as that described in the Examples.
[0022] The tensile strength in the machine direction (MD) (hereinafter simply referred to as "MD") per unit weight (hereinafter simply referred to as "MD tensile strength") is 0.28 N·m 2 / 25mm·g or more. MD tensile strength is used as one of the indicators to evaluate the resistance to breakage of meltblown nonwoven fabric. MD tensile strength is 0.28N·m 2 / 25 mm g or more indicates that the MB nonwoven fabric has excellent tensile strength, making it suitable for use in applications that require high filtration pressure (e.g., high-flow filtration, capture of fine particles, etc.). MD tensile strength is 0.29N·m 2 / 25mm·g or more. MD tensile strength is 0.35N·m 2 From this viewpoint, the MD tensile strength may be 0.28 N m 2 / 25mm g~0.35N m 2 / 25mm·g may also be used. The method for measuring the MD tensile strength is the same as that described in the Examples.
[0023] The elongation in the machine direction (MD) (hereinafter also referred to as "MD elongation") is preferably 120% or more. The MD elongation is used as one of the indices for evaluating the resistance to breakage of meltblown nonwoven fabrics. An MD elongation of 120% or more indicates that the MB nonwoven fabric has excellent elongation. This makes it suitable for use in applications requiring deformation conforming to the human body (e.g., sanitary materials, medical clothing, etc.). The MD elongation may be 160% or more. The MD elongation may be 190% or less, or 175% or less. The MD elongation may be 120% to 190%. The method for measuring the MD elongation is the same as that described in the Examples.
[0024] Machine direction (MD) toughness (hereinafter referred to as "MD toughness") is 12.5N / in 2 It is preferable that the MD toughness is 12.5 N / in or more. The MD toughness is used as one of the indices for evaluating the resistance of meltblown nonwoven fabric to breakage. The MD toughness is expressed as a parameter that takes into account the MD tensile strength and the MD elongation. The higher the MD toughness, the stronger the tenacity of the meltblown nonwoven fabric and the less likely it is to tear. 2The above indicates that MB nonwoven fabric has excellent toughness, which makes it suitable for use in applications requiring high filtration pressure (e.g., high flow rate filtration, fine particle capture, etc.) and applications requiring conformity to the human body (e.g., sanitary materials, medical clothing, etc.). MD toughness is 13.0N / in 2 The MD toughness can be more than 14.0N / in 2 It may be less than 13.5N / in 2 The MD toughness may be 12.5N / in 2 ~14.0N / in 2 It may be the following. The method for measuring the MD toughness is the same as that described in the Examples.
[0025] The water pressure resistance is preferably 320 mmH2O or more. A water pressure resistance of 320 mmH2O or more indicates that the MB nonwoven fabric has excellent water pressure resistance. This makes it suitable for use in applications requiring high water barrier properties (e.g., sanitary materials, medical clothing, etc.). The water resistance may be 340 mmH2O or more, or 350 mmH2O or more. The water resistance may be 400 mmH2O or less. From these viewpoints, the water resistance may be 320 mmH2O to 400 mmH2O. The method for measuring the water pressure resistance is the same as that described in the examples.
[0026] Tensile strength in machine direction (MD) is 0.28N·m 2 / 25mm·g or more, elongation in the machine direction (MD) is 120% or more, and toughness in the machine direction (MD) is 10N / in 2 It is preferable that the water pressure resistance is 320 mmH2O or more. This makes the MB nonwoven fabric excellent in tensile strength, elongation, toughness, and water pressure resistance.
[0027] The MB nonwoven fabric may be subjected to post-treatment or secondary processing depending on the application. Examples of post-treatment include heat treatment, calendaring, and electrostatic charging for the purpose of improving mechanical strength. Examples of secondary processing include folding and cutting.
[0028] (1.1) Fibers (A) The fiber (A) contains a thermoplastic non-elastomer (a). The fiber (A) may consist of only the thermoplastic non-elastomer (a), or may further contain a known resin in addition to the thermoplastic non-elastomer (a). The details of the thermoplastic non-elastomer (a) will be described later.
[0029] The average fiber diameter of the fiber (A) is usually less than 10 μm. The preferred range of the average fiber diameter of the fiber (A) is the same as the preferred range of the average fiber diameter of the MB nonwoven fabric. The average fiber diameter of the fiber (A) is the same as the method described in the Examples.
[0030] The fibers (A) may be long fibers or short fibers. The cross-sectional shape of the fibers (A) is not particularly limited, and examples thereof include circular, elliptical, and irregular cross sections.
[0031] The fiber (A) may be a composite fiber or a monocomponent fiber. The composite fiber is preferably composed of two or more thermoplastic resins. Examples of the composite fiber include a core-sheath type, a side-by-side type, an island-in-the-sea type, and a side-by-side type.
[0032] The fiber (A) may contain known additives as necessary, such as antioxidants, weather stabilizers, heat stabilizers, light stabilizers, antistatic agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, etc.
[0033] (1.1.1) Thermoplastic non-elastomers (a) Examples of the thermoplastic non-elastomer (a) include olefin-based resins, polyamide-based resins, polyester-based resins, polycarbonate-based resins, polystyrene-based resins, polyurethane-based resins, vinyl chloride-based resins, fluorine-based resins, etc. The thermoplastic non-elastomer (a) may be used alone or in combination of two or more kinds. Among them, the thermoplastic non-elastomer (a) preferably contains an olefin-based resin, and more preferably is an olefin-based resin. By containing the olefin-based resin, the nonwoven fabric can be obtained inexpensively.
[0034] The melting point of the thermoplastic non-elastomer (a) is not particularly limited and is appropriately selected depending on the application of the meltblown nonwoven fabric, etc. The melting point of the thermoplastic non-elastomer (a) is preferably 140°C or higher, more preferably 150°C or higher, even more preferably 155°C or higher, and particularly preferably 160°C to 170°C. The melting point of the thermoplastic non-elastomer (a) is defined as the peak top of the peak observed on the highest temperature side of a melting endothermic curve obtained by holding a sample at -40°C for 5 minutes under a nitrogen atmosphere and then heating at 10°C / min using a differential scanning calorimeter (DSC). Specifically, the melting point can be determined as the peak top of the peak observed on the highest temperature side of a melting endothermic curve obtained by holding a sample of 5 mg under a nitrogen atmosphere at -40°C for 5 minutes and then heating at 10°C / min using a differential scanning calorimeter (manufactured by Perkin-Elmer, product name: DSC-7).
[0035] (1.1.2) Olefin resins Examples of the olefin resin include a propylene polymer, an ethylene polymer, polymethylpentene, an ethylene-cyclic olefin copolymer, etc. The olefin resin may be one type, or two or more types having different melting points, molecular weights, crystal structures, etc. Among them, the olefin-based resin preferably contains a propylene-based polymer, and more preferably is a propylene-based polymer. By containing the propylene-based polymer, the olefin-based resin can provide a nonwoven fabric having high heat resistance at low cost.
[0036] (1.1.3) Propylene polymers The propylene-based polymer contains structural units derived from propylene. The propylene-based polymer is a propylene homopolymer or a propylene copolymer. The propylene copolymer is preferably a copolymer of propylene and one or more α-olefins. The α-olefin has 2 or more carbon atoms (excluding 3 carbon atoms), and preferably 2 to 8 (excluding 3 carbon atoms). Specific examples of the α-olefin in the propylene copolymer include ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene. Among them, the propylene-based polymer preferably contains a propylene homopolymer, and more preferably is a propylene homopolymer. When the propylene-based polymer contains a propylene homopolymer, a nonwoven fabric having high strength and high heat resistance can be obtained at low cost.
[0037] The melting point of the propylene polymer is preferably 140°C or higher, more preferably 150°C or higher, further preferably 155°C or higher, and particularly preferably 160°C to 170°C. The method for measuring the melting point of the propylene-based polymer is the same as the method for measuring the melting point of the thermoplastic non-elastomer (a).
[0038] The melt flow rate (MFR) of the propylene polymer is not particularly limited, and is preferably 1 g / 10 min to 1000 g / 10 min, more preferably 5 g / 10 min to 500 g / 10 min, and even more preferably 10 g / 10 min to 100 g / 10 min. The MFR of the propylene polymer is measured in accordance with ASTM D-1238 under the conditions of 230° C. and a load of 2.16 kg.
[0039] Hereinafter, the melt flow rate measured in accordance with ASTM D-1238 at 230°C and a load of 2.16 kg will also be referred to as "MFR (230°C)".
[0040] The proportion of the propylene-based polymer in the total amount of the fibers (A) is preferably from 90% by mass to 100% by mass, and more preferably from 98% by mass to 100% by mass.
[0041] The propylene-based polymer may be a commercially available product.
[0042] (1.1.4) Thermoplastic non-elastomers derived from biomass (a) The thermoplastic non-elastomer (a) (e.g., ethylene-based polymer, propylene-based polymer, polyester-based polymer, etc.) may be a raw material derived from biomass. Since the raw material derived from biomass is a carbon-neutral material, the environmental load in the production of MB nonwoven fabric can be reduced. The monomers used as raw materials for biomass-derived thermoplastic resins are obtained by cracking biomass naphtha or by synthesis from biomass-derived ethylene. The biomass-derived thermoplastic non-elastomer (a) is obtained by polymerizing the biomass-derived monomers thus synthesized in the same manner as in the case of using conventionally known petroleum-derived thermoplastic resins. A thermoplastic resin polymer synthesized using a bio-derived monomer as a raw material is a biomass-derived thermoplastic non-elastomer (a). The content of the bio-derived thermoplastic non-elastomer (a) in the raw material monomer is more than 0 mass% and may be 100 mass% or less, based on the total amount of the raw material monomer. The "biomass degree" indicates the content of carbon derived from biomass, and is calculated by measuring radioactive carbon (C14). Carbon dioxide in the atmosphere contains a certain percentage of C14 (approximately 105.5 pMC). Therefore, it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere (such as corn) is also about 105.5 pMC. It is also known that fossil fuels contain very little C14. Therefore, the content of carbon derived from biomass in the raw material can be calculated by measuring the proportion of C14 in the total carbon atoms in the polymer. The thermoplastic non-elastomer (a) may contain a thermoplastic polymer obtained by recycling, that is, a so-called recycled polymer. The term "recycled polymer" includes polymers obtained by recycling waste polymer products, and can be produced, for example, by the method described in DE 102019127827 (A1). The recycled polymer may contain a marker that identifies it as having been obtained by recycling.
[0043] (1.1) Fiber (B) The fiber (B) contains a thermoplastic elastomer (b). The fiber (B) may be composed of only the thermoplastic non-elastomer (b), or may further contain a known resin in addition to the thermoplastic elastomer (b). Details of the thermoplastic elastomer (b) will be described later.
[0044] The average fiber diameter of the fiber (B) is usually less than 10 μm. The preferred range of the average fiber diameter of the fiber (B) is the same as the preferred range of the average fiber diameter of the MB nonwoven fabric. The average fiber diameter of the fiber (B) is the same as the method described in the Examples.
[0045] The fibers (B) may be long fibers or short fibers. The cross-sectional shape of the fibers (B) is not particularly limited, and examples thereof include a circular, elliptical, irregular cross section, and the like.
[0046] The fiber (B) may be a composite fiber or a monocomponent fiber. The composite fiber is preferably composed of two or more thermoplastic resins. Examples of the composite fiber include a core-sheath type, a side-by-side type, an island-in-the-sea type, and a side-by-side type.
[0047] The fiber (B) may contain known additives as necessary, such as antioxidants, weather stabilizers, heat stabilizers, light stabilizers, antistatic agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, etc.
[0048] (1.2.1) Thermoplastic elastomer (b) Examples of the thermoplastic elastomer (b) include olefin-based elastomers (hereinafter also referred to as "POE") such as α-olefin copolymers, polyurethane-based elastomers, polystyrene-based elastomers, polyvinyl chloride-based elastomers, polyester-based elastomers, polyamide-based elastomers, fluorine-based elastomers, etc. The thermoplastic elastomers may be used alone or in combination of two or more. Among them, the thermoplastic elastomer (b) preferably contains an α-olefin copolymer, and more preferably is an α-olefin copolymer. When the thermoplastic elastomer (b) contains an α-olefin copolymer, a nonwoven fabric having high heat resistance can be obtained inexpensively.
[0049] The melting point of the thermoplastic elastomer (b) is lower than that of the thermoplastic non-elastomer (a). The value obtained by subtracting the melting point of the thermoplastic elastomer (b) from the melting point of the thermoplastic non-elastomer (a) (hereinafter also referred to as "melting point difference") is preferably 3°C or more, more preferably 5°C or more, from the viewpoint of enhancing the fiber fusion effect of the fiber (B) containing the thermoplastic elastomer (b). The melting point difference (resin) is preferably 100°C or less, more preferably 10°C or less, from the viewpoint of preventing the occurrence of temperature unevenness in the die (spinneret) when the extrusion temperatures of the thermoplastic non-elastomer (a) and the thermoplastic elastomer (b) are the same. The method for measuring the melting point of the thermoplastic elastomer (b) is the same as the method for measuring the melting point of the thermoplastic non-elastomer (a).
[0050] (1.2.1.1) α-Olefin copolymers The α-olefin copolymer is a copolymer in which two or more copolymerization components having an α-olefin skeleton are copolymerized. Examples of the copolymerization component having an α-olefin skeleton include α-olefins, etc. Examples of the α-olefins include ethylene, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.
[0051] The α-olefin copolymer may be in the form of an alternating copolymer, a graft copolymer, a block copolymer or a random copolymer.
[0052] The block copolymer is preferably a block copolymer of a polyolefin block forming a highly crystalline polymer that serves as the hard portion and a monomer copolymer exhibiting amorphous properties that serves as the soft portion.Specific examples of the block copolymer include olefin (crystalline)-ethylene-butylene-olefin block copolymer, polypropylene-polyolefin (amorphous)-polypropylene block copolymer, etc.
[0053] The MFR (230°C) of the α-olefin copolymer is not particularly limited, and is preferably 1 g / 10 min to 100 g / 10 min, more preferably 10 g / 10 min to 80 g / 10 min, further preferably 15 g / 10 min to 70 g / 10 min, and particularly preferably 15 g / 10 min to 50 g / 10 min.
[0054] The proportion of the α-olefin copolymer in the total amount of the fibers (B) is preferably from 90% by mass to 100% by mass, and more preferably from 98% by mass to 100% by mass.
[0055] (1.3) Preferred embodiments From the viewpoint of enhancing the fusion effect between fiber (A) and fiber (B), it is preferable that the thermoplastic non-elastomer (a) contained in fiber (A) and the thermoplastic elastomer (b) contained in fiber (B) contain a common monomer. This creates affinity between the partial structure common to the thermoplastic non-elastomer (a) and the thermoplastic elastomer (b), improving the compatibility between fiber (A) and fiber (B). As a result, the MB nonwoven fabric has excellent tensile strength, elongation, toughness, water pressure resistance, and abrasion resistance. The main monomer of the thermoplastic non-elastomer (a) contained in the fiber (A) is preferably the same as the main monomer of the thermoplastic elastomer (b) contained in the fiber (B). The term "main monomer" refers to a monomer having the highest content (mass%) among the monomer components constituting the resin. This increases the ratio of partial structures that are common to the thermoplastic non-elastomer (a) and the thermoplastic elastomer (b) and have affinity with each other, and the compatibility between the fiber (A) and the fiber (B) is further improved. As a result, the tensile strength, elongation, toughness, water pressure resistance, and abrasion resistance of the MB nonwoven fabric are more excellent. When the thermoplastic non-elastomer (a) contains a propylene homopolymer, it is preferable that the thermoplastic elastomer (b) contains a propylene-based elastomer. This makes it possible to obtain a nonwoven fabric with high strength and high heat resistance at low cost. Examples of commercially available propylene-based elastomers (main monomer: propylene) include Toughmer PN20300 (registered trademark) (Mitsui Chemicals, Inc.).
[0056] (1.4) Purpose The MB nonwoven fabric is not particularly limited, and examples thereof include clothing (e.g., interlining, adhesive interlining, etc.), medical (e.g., surgical gown, covering cloth, etc.), construction (e.g., roofing material, tufted carpet base material, etc.), civil engineering (e.g., drain material, filtration material, etc.), vehicles (e.g., automobile interior, automobile parts, etc.), hygiene (e.g., diapers, sanitary products, first aid products, cleaning products, etc.), interior (e.g., carpet, furniture parts, fittings, wall coverings, decorative items, etc.), bedding (e.g., futon bags, pillow covers, sheets, etc.), agriculture (e.g., vinyl greenhouse sheets, seedbed sheets, etc.), leather (e.g., artificial leather base fabric, synthetic leather base fabric, etc.), living materials (e.g., storage products, packaging materials, bags, etc.), industrial materials (e.g., industrial materials, electrical materials, product base materials, etc.), etc. Specifically, the MB nonwoven fabric is suitable for use in filters (for example, gas filters (air filters), liquid filters, etc.), sanitary materials, waterproof sheets, medical sheets, etc.
[0057] (1.5) Meltblown nonwoven fabric manufacturing equipment The meltblown nonwoven fabric of the present disclosure is produced using a meltblown nonwoven fabric production apparatus.
[0058] Hereinafter, an example of a meltblown nonwoven fabric production apparatus used for producing the meltblown nonwoven fabric of the present disclosure will be described with reference to FIGS. 1 and 2.
[0059] (1.5.1) Composition As shown in Fig. 1, the meltblown nonwoven fabric production apparatus 1 according to this embodiment includes an extruder 10, a gear pump 20, an extruder 30, a gear pump 40, a die (spinneret) 50, a gas heating device 60, and a collection mechanism 70. The extruder 10 is connected to the die 50 via the gear pump 20. The extruder 30 is connected to the die 50 via the gear pump 40.
[0060] Hereinafter, the raw material of fiber (A) is also referred to as "resin composition (A)", and the raw material of fiber (B) is also referred to as "resin composition (B)".
[0061] (1.5.2) Extruder The extruder 10 melts the solid matter of the resin composition (A) and supplies the molten matter of the resin composition (A) to the gear pump 20 . As shown in Fig. 1, the extruder 10 has a hopper 11 and a barrel 12. The hopper 11 and the barrel 12 are connected. A solid material of the resin composition (A) is charged into the hopper 11. The barrel 12 plasticizes and kneads the solid material of the resin composition (A) charged from the hopper 11 while moving it. The extruder 10 may be a single screw extruder or a multi-screw extruder (for example, a twin screw extruder, etc.).
[0062] The gear pump 20 continuously supplies the molten resin composition (A) to the die 50. The volume of the molten resin composition (A) supplied to the die 50 per unit time can be controlled by changing the rotation speed of the gear pump 20. The gear pump 20 may remove foreign matter from the molten resin composition (A). The gear pump 20 may be a known gear pump.
[0063] The extruder 30 melts the solid matter of the resin composition (B) and supplies the molten matter of the resin composition (B) to the gear pump 20. As shown in Fig. 1, the extruder 30 has a hopper 31 and a barrel 32. The hopper 31 and the barrel 32 are connected. A solid material of the resin composition (B) is charged into the hopper 31. The barrel 32 plasticizes and kneads the solid material of the resin composition (B) charged from the hopper 31 while moving it. The extruder 30 may be a single screw extruder or a multi-screw extruder (for example, a twin screw extruder, etc.).
[0064] The gear pump 40 continuously supplies the molten resin composition (B) to the die 50. The volume of the molten resin composition (B) supplied to the die 50 per unit time can be controlled by changing the rotation speed of the gear pump 40. The gear pump 40 may remove foreign matter from the molten resin composition (B). The gear pump 40 may be a known gear pump.
[0065] (1.5.4) The die 50 extrudes each of the melted resin composition (A) and the melted resin composition (B) into a high-velocity flow of high-temperature gas G to form a plurality of fibers.
[0066] 1, the die 50 has a plurality of spinning nozzles 51 and two gas nozzles 52. The two gas nozzles 52 are formed so as to sandwich the plurality of spinning nozzles 51 in the machine direction (MD).
[0067] The temperature of the die 50 (hereinafter also referred to as the "die temperature") is not particularly limited as long as it is a temperature at which the molten resin composition (A) and the molten resin composition (B) can be extruded, and is appropriately selected depending on the types of resin composition (A) and resin composition (B), etc.
[0068] (1.5.4.1) Spinning nozzle As shown in Figure 2, the multiple spinning nozzles 51 are arranged in a row at equal intervals along the cross direction (CD). The diameter L1 (see Figure 2) of the spinning nozzle 51 is appropriately selected depending on the application of the MB nonwoven fabric, etc., and may be 0.08 mm to 0.60 mm. The nozzle distance L2 (see Figure 2) between adjacent spinning nozzles 51 is appropriately selected depending on the application of the MB nonwoven fabric, etc., and may be 0.5 mm to 3.0 mm. The number of multiple spinning nozzles 51 is not particularly limited and is appropriately selected depending on the application of the MB nonwoven fabric, etc.
[0069] The multiple spinning nozzles 51 include multiple spinning nozzles 51A that discharge a melt of the resin composition (A) and multiple spinning nozzles 51B that discharge a melt of the resin composition (B). The multiple spinning nozzles 51A are connected to the extruder 10 via a first flow path (not shown) of the die 50. The multiple spinning nozzles 51B are connected to the extruder 30 via a second flow path (not shown) of the die 50. The first flow path and the second flow path are independent of each other.
[0070] The discharge amount per one spinning nozzle 51 of each of the multiple spinning nozzles 51A and the multiple spinning nozzles 51B (hereinafter also referred to as the "single-hole discharge amount") is appropriately selected according to the above-mentioned mixed fiber ratio (A / B). The above-mentioned mixed fiber ratio (A / B) can be adjusted by adjusting the single-hole discharge amount of each of the spinning nozzles 51A and the spinning nozzles 51B.
[0071] In this embodiment, as shown in Figure 2, a first group in which three spinning nozzles 51A are arranged in succession and a second group in which three spinning nozzles 51B are arranged in succession are arranged alternately along the cross direction (CD).
[0072] However, the present disclosure is not limited thereto, and the first group may be composed of one, two, or four or more spinning nozzles 51A, and the second group may be composed of one, two, or four or more spinning nozzles 51B. In addition, in this embodiment, the multiple spinning nozzles 51 are arranged in a row along the transverse direction (CD), but the present disclosure is not limited thereto. The multiple spinning nozzles 51 may be arranged in two or more rows along the transverse direction (CD).
[0073] (1.5.4.2) Gas nozzle The gas nozzle 52 injects the heated gas G near the opening of the spinning nozzle 51. As shown in Fig. 1, the gas nozzle 52 injects the heated gas G onto the material immediately after it is discharged from the spinning nozzle 51. The supply amount of the heated gas G (hereinafter also referred to as "stretching air amount") and the temperature of the heated gas G are not particularly limited and are appropriately selected depending on the application of the MB nonwoven fabric, etc.
[0074] (1.5.5) Gas heating equipment The gas heating device 60 supplies a heating gas G to the gas nozzle 52 of the die 50. The gas heating device 60 may have a known configuration.
[0075] (1.5.6) Collection mechanism The collection mechanism 70 collects the multiple fibers discharged from the die 50. The collection mechanism 70 includes a screen 71, a roller 72, an air suction unit 73 arranged on the back side of the collection surface of the screen 71, and a blower 74. The screen 71 is, for example, a porous belt. The distance DCD (see FIG. 1) between the screen 71 and the spinning nozzle 51 is not particularly limited and is appropriately selected depending on the application of the MB nonwoven fabric. The roller 72 supports the screen 71 and moves the screen 71 in the machine direction (MD). The air suction unit 73 sucks in the multiple fibers discharged from the die 50. The blower 74 is connected to the air suction unit 73. The blower 74 applies suction force to the air suction unit 73.
[0076] (1.5.7) Operation In the meltblown nonwoven fabric manufacturing apparatus 1, the solid of the resin composition (A) fed into the extruder 10 becomes a melt of the resin composition (A) and is supplied to the die 50 via the gear pump 20. The solid of the resin composition (B) fed into the extruder 30 becomes a melt of the resin composition (B) and is supplied to the die 50 via the gear pump 40. The melt of the resin composition (A) fed to the die 50 is extruded from the multiple spinning nozzles 51A into the high-speed flow of the high-temperature gas G and stretched to become multiple fibers (A). The melt of the resin composition (B) fed to the die 50 is extruded from the multiple spinning nozzles 51B into the high-speed flow of the high-temperature gas G and stretched to become multiple fibers (B). The multiple fibers (A) and the multiple fibers (B) are layered on the moving screen 71 to obtain an MB nonwoven fabric.
[0077] (2) Sanitary materials The sanitary material of the present disclosure includes the meltblown nonwoven fabric of the present disclosure. The sanitary material of the present disclosure may have any known configuration other than that it includes the meltblown nonwoven fabric of the present disclosure.
[0078] The sanitary material of the present disclosure is used in diapers, masks, disposable surgical gowns, rescue gowns, etc. Specifically, the sanitary material of the present disclosure is preferably used in top sheets, back sheets, waistbands (e.g., extension tapes, side flaps, etc.), fastening tapes, three-dimensional gathers, leg cuffs, etc. in flat-type disposable diapers or pants-type disposable diapers. The sanitary material is preferably used in parts such as side panels of pants-type disposable diapers. By using the meltblown nonwoven fabric of the present disclosure in these parts, it becomes possible to follow the movements of the wearer and fit the wearer's body, and a comfortable state is maintained even while wearing it.
[0079] (3)Water-resistant sheet The waterproof sheet of the present disclosure includes the meltblown nonwoven fabric of the present disclosure. The waterproof sheet of the present disclosure may have any known configuration, except that it includes the meltblown nonwoven fabric of the present disclosure. The waterproof sheet of the present disclosure may be made of the meltblown nonwoven fabric of the present disclosure. The waterproof sheet of the present disclosure may have a layer made of the meltblown nonwoven fabric of the present disclosure (hereinafter also referred to as the "meltblown nonwoven fabric layer") and a layer made of known fibers (e.g., cellulose fibers, etc.) (hereinafter also referred to as the "fiber layer"). The fiber layer is laminated on one main surface of the meltblown nonwoven fabric layer.
[0080] The waterproof sheet of the present disclosure can be suitably used for absorbent materials (e.g., disposable diapers, sanitary products, etc.), sanitary materials (e.g., sanitary masks, cosmetic materials, etc.), medical materials (e.g., bandages, etc.), daily materials (e.g., clothing materials, packaging materials, etc.), industrial materials (e.g., filters, etc.), etc.
[0081] (4) Medical Sheets The medical sheet of the present disclosure includes the meltblown nonwoven fabric of the present disclosure. The medical sheet of the present disclosure may have any known configuration other than including the meltblown nonwoven fabric of the present disclosure. For example, the medical sheet of the present disclosure may be made of a meltblown nonwoven fabric, or may have a meltblown nonwoven fabric layer and a fiber layer. The fiber layer is laminated on one main surface of the meltblown nonwoven fabric layer.
[0082] The medical sheet of the present disclosure is suitable for use as materials for gowns, caps, drapes, masks, gauze, bandages, various protective clothing, plaster base fabrics, poultices, wound dressings, wound tapes, etc. Furthermore, by using raw materials that are stable to electron beams and gamma rays irradiated during sterilization and disinfection, the medical sheet of the present disclosure is suitable for use as a sterilized medical sheet. EXAMPLES
[0083] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0084] [1] Measurement methods for physical properties The methods for measuring various physical properties are as follows.
[0085] [1.1] Mixed fiber ratio The supply mass of the molten resin composition (A) per unit time was determined from the supply volume per unit time of the molten resin composition (A) supplied from the gear pump 20 and the melt density of the molten resin composition (A). Similarly, the supply mass of the molten resin composition (B) per unit time was determined from the supply amount per unit time of the molten resin composition (B) supplied from the gear pump 40 and the melt density of the molten resin composition (B). The ratio (A / B) of these resin supply masses per unit time was defined as the "mixed fiber ratio (A / B)" of the resulting meltblown nonwoven fabric.
[0086] [1.2] Weight per unit area [g / m 2 〕 Ten test pieces measuring 100 mm (MD) x 100 mm (CD) were taken from the meltblown nonwoven fabric. The test pieces were taken from the center of the cross direction (CD) of the meltblown nonwoven fabric. The mass [g] of each test piece was then measured using a top-pan electronic balance (Kensei Kogyo Co., Ltd.) in an environment of 20°C and relative humidity of 50%. The average mass of each test piece was calculated. A distance of 1 m was calculated from the average mass. 2 The value is converted to mass per unit [g] and rounded off to the nearest tenth to obtain the value "weight per unit [g / m 2 〕".
[0087] [1.3] Average fiber diameter [g / m 2 〕 The average fiber diameter of the fibers was determined as follows. The meltblown nonwoven fabric to be measured was observed with a scanning electron microscope (KEYENCE Corporation, 3D real surface view microscope "VE9800 / 8800"). 100 fibers were selected from the multiple fibers forming the meltblown nonwoven fabric on the screen, and their fiber diameters were measured. The average value of the measured fiber diameters of the 100 fibers was taken as the "average fiber diameter."
[0088] [1.4] Tensile strength, elongation and toughness The tensile strength of the meltblown nonwoven fabric was measured in accordance with JIS L 1906 6.12.1 [Method A] (transitioned to JIS L 1913:2010, corresponding to ISO 9073-3:1989). Ten test pieces of 200 mm (MD) x 25 mm (CD) were taken from the meltblown nonwoven fabric. The test pieces were taken from five locations in the cross direction (CD). Using a tensile tester, a load was applied to the test piece in the machine direction (MD) with a chuck distance of 100 mm and a head speed of 100 mm / min until the test piece broke. The strength of the test piece at the maximum load was taken as the "tensile strength [N / 25 mm]". The "elongation rate [%]" was calculated from the elongation at the maximum load. In the stress-strain curve of the above tensile test (i.e., a graph of load (N / 25mm) against elongation (%)), the integral value of the curve from the time when the test piece starts to be pulled in the machine direction (MD) to the time when the test piece breaks is called "toughness (N / in 2 The average of the measured values of the MD tensile strength per unit area weight of 10 test pieces was taken as "MD tensile strength per unit area weight." The average of the measured values of the MD elongation of 10 test pieces was taken as "MD elongation." The average of the measured values of the MD toughness of 10 test pieces was taken as "MD toughness."
[0089] The MD tensile strength, MD elongation, and MD toughness per unit area weight were each evaluated based on the following evaluation criteria. The evaluation results are shown in Table 1. An acceptable evaluation result for MD tensile strength per unit area weight is "A1". An acceptable evaluation result for MD elongation is "A2". An acceptable evaluation result for MD toughness is "A3".
[0090] [1.5.1] Evaluation criteria for MD tensile strength per unit area "A1": MD tensile strength per unit area ≧ 0.28 [N m 2 / 25mm·g] "B1": MD tensile strength per unit area < 0.28 [N m 2 / 25mm·g]
[0091] [1.5.2] Evaluation criteria for MD elongation "A2": MD elongation rate ≧120 [%] "B2": MD elongation rate <120〔%〕
[0092] [1.5.3] MD Toughness Evaluation Criteria "A3":MD toughness ≧10 [N / in 2 〕 "B3":MD toughness <10 [N / in 2 〕
[0093] [1.5] Water pressure resistance [mmH2O] Ten test pieces measuring 150 mm (MD) x 150 mm (CD) were taken from the meltblown nonwoven fabric. The test pieces were taken from the center of the cross direction (CD) of the meltblown nonwoven fabric. Using a water pressure resistance tester, pressure was applied to the test pieces at an acceleration rate of 10 mbar / min, and the pressure at which water leaked from three points in the test piece (i.e., water pressure resistance) was measured. The average value of the measured water pressure resistance values of the 10 test pieces was recorded as the "water pressure resistance [mmH2O]."
[0094] The water pressure resistance was evaluated based on the following evaluation criteria. The evaluation results are shown in Table 1. The acceptable evaluation result for water pressure resistance is "A4".
[0095] [1.4.1] Water pressure resistance evaluation criteria "A4": Water pressure resistance ≧320 [mmH2O] "B4": Water pressure resistance <320 [mmH2O]
[0096] [1.6] Abrasion resistance Two test pieces of 150 mm (MD) × 150 mm (CD) were taken from the meltblown nonwoven fabric. The test pieces were taken from the center of the cross direction (CD) of the meltblown nonwoven fabric. A friction test was performed using a Gakushin-type friction fastness tester (manufactured by Daiei Scientific Instruments Manufacturing Co., Ltd., new model NR-100) in accordance with the friction fastness test method of JIS L 0849. A white cloth (No. 3-1) for dye fastness test conforming to JIS L 0803 was attached to the frictional element to obtain a cloth-attached frictional element. The cloth-attached frictional element was brought into contact with the nozzle side surface of the test piece (hereinafter also referred to as the "nozzle surface") without applying a load to the test piece, and the cloth-attached frictional element was moved back and forth in the machine direction (MD) to rub the nozzle surface. After every 10 reciprocations, visual observation was made to see whether fluffing (a phenomenon in which fibers fall off the meltblown nonwoven fabric and become fluffy) or nonwoven fabric destruction (a phenomenon in which the nonwoven fabric breaks and a hole is formed) occurred in the center part of the friction point on the nozzle surface. The friction test was performed until fluffing or nonwoven fabric destruction was observed. The number of reciprocations at which fluffing or nonwoven fabric destruction was first observed was taken as the wear resistance number. The average number of abrasion cycles for the two test pieces was taken as the "average number of abrasion cycles." The average number of abrasion cycles was used to evaluate the abrasion resistance based on the following evaluation criteria. The evaluation results and the state of the abrasion points on the nozzle surface after the number of abrasion cycles are shown in Table 1. An acceptable evaluation result for abrasion resistance is "A5".
[0097] [1.5.1] Evaluation criteria for wear resistance "A5": Average abrasion resistance ≥ 20 times "B5": Average abrasion resistance <20 times
[0098] [2] Preparation of meltblown nonwoven fabric [2.1] Example 1 The following materials were used for the meltblown nonwoven fabric:
[0099] <Thermoplastic non-elastomer (a)> · hPP(a1): Homopolypropylene product (Material: Homopolypropylene, Melting point: 166℃, MFR(230℃): 35g / 10min)
[0100] <Thermoplastic elastomer (b)> POE(b1): "Tafmer (registered trademark) PN20300" (manufactured by Mitsui Chemicals, Inc., material: polyolefin elastomer, melting point: 160°C, MFR (230°C): 30g / 10min)
[0101] A meltblown nonwoven fabric manufacturing apparatus 1 shown in Figures 1 and 2 was prepared. A single-screw extruder was used as the extruder 10. A twin-screw extruder was used as the extruder 30. The diameter L1 (see Figure 2) of the spinning nozzle 51 was 0.3 mm. The nozzle distance L2 (see Figure 2) was 1 mm. The distance DCD (see Figure 1) between the screen 71 and the spinning nozzle 51 was 400 mm.
[0102] A meltblown nonwoven fabric was produced as follows. A solid material of hPP (a1) was fed into an extruder 10 and dissolved therein. A solid material of POE (b1) was fed into an extruder 30 and dissolved therein. Each of the melts of hPP (a1) and POE (b1) was fed into a die 50.
[0103] The set temperature of the die 50 was 270°C. The supply rate of the molten hPP (a1) to the die 50 was adjusted so that the single-hole output rate of the spinning nozzle 51A was 0.083 g / min. The supply rate of the molten POE (b1) to the die 50 was adjusted so that the single-hole output rate of the spinning nozzle 51B was 0.027 g / min. By adjusting the supply rates in this way, the mixed fiber ratio was PP: 75 mass% and POE: 25 mass%.
[0104] The melt of hPP (a1) discharged from each of the multiple spinning nozzles 51A and the melt of POE (b1) discharged from each of the multiple spinning nozzles 51B were stretched by the high-temperature gas G and blown onto the moving screen 71 to become fibers. The temperature of the high-temperature gas G was 270°C, and the flow rate of the high-velocity gas G was 270 m 3 / hr.
[0105] The screen speed was adjusted to collect the fibers so that the basis weight was 30.4 gsm, and a meltblown nonwoven fabric was obtained. The average fiber diameter of the fibers contained in the meltblown nonwoven fabric was 5.0 μm. The MD maximum strength of the meltblown nonwoven fabric was 0.29 N / 25 mm gsm, the MD elongation was 151%, and the MD toughness was 12.6 N / in 2 The water resistance was 351mmH2O.
[0106] [2.2] Example 2, Example 3 and Comparative Examples 1 to 4 A meltblown nonwoven fabric was obtained in the same manner as in Example 1, except that the resin type and the single-hole discharge rate were changed as shown in Table 1. The evaluation results of the obtained meltblown nonwoven fabric are shown in Table 1. Furthermore, a graph showing the relationship between the tangle rate of POE (b1) and the MD tensile strength is shown in Figure 3.
[0107] [Table 1]
[0108] The meltblown nonwoven fabrics of Comparative Examples 1 to 3 contain fibers (A) containing hPP (a1) as a thermoplastic non-elastomer (a) and fibers (B) containing POE (b1) as a thermoplastic elastomer (b). The blend ratio (A / B) was outside the range of 60 / 40 to 99 / 1 in mass ratio. Therefore, in Comparative Examples 1 to 3, the evaluation results of MD maximum strength were "B1" and the evaluation results of water pressure resistance were "B4". The meltblown nonwoven fabric of Comparative Example 4 did not contain the fiber (B). Therefore, in Comparative Example 4, the evaluation result of the MD maximum strength was "B1", the evaluation result of the MD toughness was "B3", the evaluation result of the water pressure resistance was "B4", and the evaluation result of the abrasion resistance was "B5". These results show that the meltblown nonwoven fabrics of Comparative Examples 1 to 5 are not meltblown nonwoven fabrics excellent in tensile strength, elongation, toughness, water pressure resistance and abrasion resistance.
[0109] The meltblown nonwoven fabrics of Examples 1 to 3 contain fibers (A) containing hPP (a1) as a thermoplastic non-elastomer (a) and fibers (B) containing POE (b1) as a thermoplastic elastomer (b). The melting point of POE (b1) is lower than that of hPP (a1). The blend ratio (A / B) was within the range of 60 / 40 to 99 / 1 in mass ratio. Therefore, in Examples 1 to 5, the evaluation results of MD maximum strength were "A1", the evaluation result of MD elongation was "A2", the evaluation result of MD toughness was "A3", the evaluation result of water pressure resistance was "A4", and the evaluation result of abrasion resistance was "A5". As a result, it was found that the meltblown nonwoven fabrics of Examples 1 to 3 were meltblown nonwoven fabrics excellent in tensile strength, elongation, toughness, water pressure resistance and abrasion resistance. [Explanation of symbols]
[0110] 1. Meltblown nonwoven fabric manufacturing equipment 10,30 Extruder 11,31 Hopper 12,32 barrels 20,40 Gear pump 50 Die 51, 51A, 51B Spinning nozzle 52 Gas nozzle 60 Gas Heating Equipment 70 Collection mechanism 71 screens 72 Laura 73 Air suction section 74 Blower
Claims
1. The fiber (A) includes a thermoplastic non-elastomer (a) and a fiber (B) includes a thermoplastic elastomer (b), The melting point of the thermoplastic elastomer (b) is lower than the melting point of the thermoplastic non-elastomer (a); The meltblown nonwoven fabric has a blend ratio (A / B) of the fibers (A) and (B) of 60 / 40 to 99 / 1 by mass ratio.
2. The thermoplastic non-elastomer (a) comprises a propylene homopolymer, The meltblown nonwoven fabric according to claim 1 , wherein the thermoplastic elastomer (b) comprises a polyolefin-based elastomer.
3. The meltblown nonwoven fabric according to claim 1 or 2, wherein the mixed fiber ratio (A / B) is 65 / 35 to 72 / 28.
4. Tensile strength in the machine direction (MD) per unit weight is 0.28 N m 2 The meltblown nonwoven fabric according to claim 1 or claim 2, having a strength of 25 mm g or more.
5. Machine direction (MD) toughness is 12.5 N / in 2 The meltblown nonwoven fabric according to claim 1 or 2.
6. Water resistance: 320mmH 2 The meltblown nonwoven fabric according to claim 1 or 2, having a viscosity of 0 or more.
7. Tensile strength in the machine direction (MD) per unit weight is 0.28 N m 2 / 25 mm g or more, The elongation in the machine direction (MD) is 120% or more, Machine direction (MD) toughness is 10N / in 2 That's all. Water resistance: 320mmH 2 The meltblown nonwoven fabric according to claim 1 or 2, having a viscosity of 0 or more.
8. A sanitary material comprising the meltblown nonwoven fabric according to claim 1 or 2.
9. A waterproof sheet comprising the meltblown nonwoven fabric according to claim 1 or 2.
10. A medical sheet comprising the meltblown nonwoven fabric according to claim 1 or 2.
Citation Information
Patent Citations
Long-fiber nonwoven fabric and fiber product using the same
JP2004197291A