Polyester film roll and decorative molded body

The polyester film roll with optimized biomass-derived materials and controlled manufacturing processes addresses mechanical property gaps, enhancing decorative molding with clear design transfer and reduced environmental impact.

JP2024172813APending Publication Date: 2024-12-12MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023090797
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Biomass-derived polyester films lack mechanical properties equivalent to fossil fuel-derived polyester, particularly in decorative molding applications, with issues such as noticeable yellow tint and poor design transfer.

Method used

A polyester film roll composed of biomass-derived polyester with specific mechanical properties, including a y value less than 0.323, and a laminated structure with layers of biomass and fossil fuel-derived polyesters, optimized through controlled manufacturing conditions such as cooling, stretching, and catalyst use.

Benefits of technology

The film roll achieves improved design and clear pattern/color transfer for decorative molding, reducing environmental impact by using carbon-neutral materials while maintaining mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024172813000001_ABST
    Figure 2024172813000001_ABST
Patent Text Reader

Abstract

To provide a polyester film roll which enhances designability of a polyester film roll and is suitable for decorative molding.SOLUTION: There is provided a polyester film roll obtained by winding a polyester film which contains a biomass-derived polyester and has a y value of less than 0.323 as measured by the color tone reflection method.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester film roll and a decorated molded article. [Background technology]

[0002] Polyester films are excellent in properties such as heat resistance, weather resistance, mechanical strength, transparency, chemical resistance, and gas barrier properties, and are also readily available at low cost, making them highly versatile and used in a variety of applications such as packaging materials and optical applications. Polyesters are obtained by polycondensation of diols and dicarboxylic acids, and for example, polyethylene terephthalate is produced from ethylene glycol and terephthalic acid as raw materials. Conventionally, the raw material for polyesters has been produced from petroleum, a fossil fuel.

[0003] In recent years, global warming and marine pollution have become major problems. For example, greenhouse gases are generated when plastic is burned, and large amounts of plastic flow into the ocean and continue to accumulate as plastic waste, which has become a problem. In addition, petroleum resources are finite, and the depletion of resources due to the production of fossil fuel-based plastics is also a problem. For this reason, the use of biomass-derived raw materials has attracted attention in order to reduce the use of fossil fuels. Biomass is an organic resource derived from plants that is produced by living organisms through photosynthesis from water and carbon dioxide using solar energy. The carbon dioxide released when biomass is burned is different from the carbon dioxide released when fossil fuels are burned, and is carbon dioxide absorbed from the atmosphere through photosynthesis during the growth process of living organisms, so biomass is said to be a "carbon neutral" resource that does not increase new carbon dioxide in the atmosphere.

[0004] For example, Patent Document 1 discloses a laminate having at least two layers, the first layer being made of a resin composition mainly containing a polyester composed of diol units and dicarboxylic acid units, the resin composition being made of a polyester whose diol units are ethylene glycol derived from biomass and whose dicarboxylic acid units are dicarboxylic acid derived from fossil fuel, in an amount of 50 to 95% by mass based on the entire resin composition, and the second layer being made of a resin material containing a raw material derived from fossil fuel. Patent Document 2 also discloses a method for producing a biaxially stretched resin film made of a resin composition mainly containing a polyester composed of diol units and dicarboxylic acid units, the resin composition including a biomass-derived polyester whose diol units are ethylene glycol derived from biomass and whose dicarboxylic acid units are terephthalic acid derived from fossil fuel, and a recycled polyester obtained by recycling a product made of a polyester resin obtained by a polycondensation reaction using a diol unit whose diol unit is a diol derived from fossil fuel or ethylene glycol derived from biomass as the diol unit and a terephthalic acid derived from fossil fuel as the dicarboxylic acid unit. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-52125 A [Patent Document 2] JP 2022-97531 A Summary of the Invention [Problem to be solved by the invention]

[0006] Biomass-derived polyesters are required to have mechanical properties equivalent to those of fossil fuel-derived polyesters, but there is still room for improvement in the various mechanical properties of biomass-derived polyesters. For example, when a polyester film is used for decorative molding, it is required that the pattern or color tone is clearly transferred (printed) to the molded product, and in such cases, the polyester film is required to have a clear color tone with little yellowness. In addition, when the polyester film is rolled, the yellowness of the cut surface of the roll is noticeable, and when it is made into various molded products, the design may be poor, and improvement has been required. Therefore, in order to solve such problems of the conventional technology, the present invention aims to provide a polyester film roll that improves the design of the polyester film roll and is suitable for decorative molding. [Means for solving the problem]

[0007] Examples of specific embodiments of the present invention are given below.

[0008] [1] Contains biomass-derived polyester; A polyester film roll obtained by winding up a polyester film having a y value of less than 0.323 as measured by a color reflection method. [2] The polyester film roll according to [1], wherein the polyester film has a layer containing a biomass-derived polyester as a main component and a layer containing a fossil fuel-derived polyester as a main component. [3] The polyester film roll according to [1] or [2], wherein the polyester film has a layer containing a biomass-derived polyester as a main component as an intermediate layer and a layer containing a fossil fuel-derived polyester as a main component as a surface layer. [4] Polyesters contain diol units and dicarboxylic acid units. The polyester film roll according to any one of [1] to [3], wherein the diol unit is an ethylene glycol unit derived from biomass. [5] The polyester film roll according to [4], wherein the polyester contains 10 mol % or more of ethylene glycol units derived from biomass. [6] The polyester film roll according to any one of [1] to [5], wherein the polyester film is a biaxially stretched polyester film. [7] The polyester film roll according to any one of [1] to [6], which has a haze of 10% or less. [8] The polyester film roll according to any one of [1] to [7], which has a haze ratio of 10% or less when heated at 180° C. for 5 minutes. [9] The polyester film roll according to any one of [1] to [8], which is a film for decorative molding.

[10] A laminate film comprising the polyester film according to any one of [1] to [9] and a coating layer on at least one surface of the polyester film.

[11] A laminate film comprising the polyester film according to any one of [1] to

[10] and a printed layer on at least one surface of the polyester film.

[12] The laminate film according to

[10] or

[11] , which is a film for decorative molding.

[13] The laminate film according to any one of

[10] to

[12] , which is a film for simultaneous molding and transfer.

[14] A decorated molding decorated with the polyester film according to any one of [1] to

[13] .

[15] The decorated molded article according to

[14] , which is a mobile device, a home appliance, or a vehicle part.

[0009] [A] A decorative molding method using the polyester film according to any one of [1] to [9]. [B] Use of the polyester film according to any one of [1] to [9] for decorative molding of an object. [C] A decorative molding method using the laminate film according to any one of

[10] to

[13] . [D] Use of the laminate film according to any one of

[10] to

[13] for decorative molding of an object. Effect of the Invention

[0010] According to the present invention, it is possible to obtain a polyester film roll that is improved in design and is suitable for decorative molding. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a cross-sectional view showing a laminated structure of a polyester film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment or a specific example, but the present invention is not limited to such an embodiment. In this specification, when "X to Y" (X and Y are any numbers) is used, it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is any number) or "Y or less" (Y is any number), it also means "preferably greater than X" or "preferably less than Y". In the following description, "film" and "sheet" are not clearly distinguished from each other, and when "film" is used, it includes "sheet", and when "sheet" is used, it includes "film".

[0013] In this specification, the MD direction of the film is the extrusion direction (or take-up direction or flow direction) during film formation and is also called the machine direction, while the TD direction is the direction perpendicular to the MD direction and is also called the transverse direction or width direction.

[0014] (Polyester film roll) The polyester film roll of the present embodiment (hereinafter also referred to as "the present roll") relates to a polyester film roll obtained by winding up a polyester film that contains a biomass-derived polyester and has a y value of less than 0.323 as measured by a color reflection method.

[0015] Since the present roll contains a carbon-neutral polyester that does not newly increase carbon dioxide in the atmosphere, the burden on the environment can be reduced. The polyester film constituting the present roll has mechanical properties equivalent to those of polyester films produced using conventional fossil fuels. In addition, the polyester film constituting the present roll also has properties that could not be achieved by polyester films produced using conventional fossil fuels. For example, the y value of the polyester film constituting the present roll is smaller than 0.323 by a color reflection method. By making the y value of the polyester film smaller than 0.323, the design of the polyester film roll obtained by winding the polyester film on a roll can be improved. In particular, in the polyester film roll, the color of the cut surface of the roll is strongly recognized, but in this embodiment, the yellowness of the cut surface of the roll is also suppressed. In addition, when the present roll is used to produce products such as various molded products, the design can be improved. In addition, since the y value of the polyester film constituting the present roll is smaller than 0.323 by a color reflection method, when the polyester film is used for decorative molding, the pattern and color tone can be clearly transferred (printed) to the molded product. Therefore, the polyester film constituting the present roll is suitable for decorative molding.

[0016] The roll is formed by winding a polyester film around a core such as a paper tube, a metal tube, a plastic tube, etc. The diameter of the core is not particularly limited, but is preferably 10 mm or more, more preferably 20 mm or more, and even more preferably 30 mm or more. The upper limit of the diameter of the core is not particularly limited, but is preferably, for example, 500 mm or less.

[0017] The width of the roll is preferably 0.2 m or more, more preferably 0.3 m or more, and even more preferably 1 m or more. The upper limit of the width of the roll is not particularly limited, but is preferably, for example, 3 m or less. The length of the polyester film wound on the roll is not particularly limited, but is preferably, for example, 1000 m or more, more preferably, 2000 m or more, even more preferably, 4000 m or more, and particularly preferably, 6000 m or more. The upper limit of the length of the polyester film wound on the roll is not particularly limited, but is, for example, preferably, 65000 m or less, more preferably, 40000 m or less, and even more preferably, 20000 m or less.

[0018] <Polyester film> The polyester film may have a single layer structure or a laminated (multi-layer) structure. When the polyester film has a laminated structure, the polyester film may have a two-layer structure, a three-layer structure, or a four-layer structure or more. The number of layers to be laminated is not particularly limited, but is preferably 10 layers or less. When the polyester film has a laminated structure, the polyester film is preferably a co-extruded laminated polyester film.

[0019] When the polyester film has a laminated structure, the polyester film preferably has a layer containing a biomass-derived polyester as a main component, or may have a layer containing a biomass-derived polyester as a main component and a layer containing a fossil fuel-derived polyester as a main component.

[0020] When the polyester film has a laminated structure, a preferred form is a laminated structure consisting of at least three layers having a surface layer, an intermediate layer, and a surface layer in this order. Other layers may be provided between each layer, but in this embodiment, it is preferable that the surface layer, the intermediate layer, and the surface layer are directly laminated in this order. In addition, the laminated structure of the polyester film is preferably a two-kind three-layer structure or a three-kind three-layer structure, and more preferably a two-kind three-layer structure. As shown in FIG. 1, when the polyester film 100 has a two-kind three-layer structure, it is preferable that the surface layers 20 laminated on both sides of the intermediate layer 10 are the same type of layer, and only the intermediate layer 10 is a different type of layer.

[0021] When the polyester film has a laminated structure of at least three layers having a surface layer, an intermediate layer, and a surface layer in this order, the polyester film preferably has a layer containing a biomass-derived polyester as a main component as an intermediate layer. In this case, the surface layer may be a layer containing a biomass-derived polyester as a main component, or may be a layer containing a fossil fuel-derived polyester as a main component. As an embodiment, the polyester film has a layer containing a biomass-derived polyester as a main component as an intermediate layer, and a layer containing a fossil fuel-derived polyester as a main component as a surface layer.

[0022] The thickness (total thickness) of the polyester film is preferably 1 μm or more, more preferably 4 μm or more, even more preferably 8 μm or more, and particularly preferably 12 μm or more. The thickness of the polyester film is preferably 1000 μm or less, more preferably 800 μm or less, even more preferably 500 μm or less, even more preferably 200 μm or less, and particularly preferably 100 μm or less.

[0023] When the polyester film has a laminated structure, for example, a laminated structure consisting of at least three layers having a surface layer, an intermediate layer, and a surface layer in this order, the thickness of the surface layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, and particularly preferably 1 μm or more. The thickness of the surface layer is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 50 μm or less, even more preferably 30 μm or less, and particularly preferably 10 μm or less. In the above case, the thickness of the intermediate layer is preferably 1 μm or more, more preferably 3 μm or more, even more preferably 5 μm or more, even more preferably 10 μm or more, and particularly preferably 20 μm or more. The thickness of the intermediate layer is preferably 1000 μm or less, more preferably 800 μm or less, even more preferably 500 μm or less, even more preferably 300 μm or less, even more preferably 100 μm or less, and particularly preferably 80 μm or less. The layer structure and thickness of each layer of the polyester film can be determined by observing a cross section of a film freeze-fractured with an ultramicrotome at a magnification of 3,000 to 200,000 times using a transmission electron microscope and taking a photograph of the cross section.

[0024] When the polyester film has a laminated structure, the thickness of the layer containing biomass-derived polyester as a main component is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more of the total thickness of the polyester film.

[0025] The polyester film may be a non-stretched polyester film or a stretched polyester film. Among them, the polyester film is preferably a stretched polyester film, and more preferably a biaxially stretched polyester film. By making the polyester film a biaxially stretched polyester film, the mechanical properties and printability can be effectively improved.

[0026] <Physical properties of polyester film> The y value of the polyester film measured by the color reflection method is preferably smaller than 0.323, more preferably 0.321 or less, further preferably 0.319 or less, and particularly preferably 0.317 or less. The lower limit of the y value of the polyester film is not limited, but is preferably 0.310 or more, and may be 0.320 or more.

[0027] When measuring the y value of a polyester film, the polyester film is stacked and measured so that the thickness (total thickness at the time of measurement) is closest to 500 μm. A spectrophotometer can be used as the measuring device, and the measurement conditions are reflection conditions. The measurement is performed in an environment of 23°C.

[0028] By setting the y value of the polyester film within the above range, the design of the polyester film roll obtained by winding the polyester film on a roll can be improved. In particular, in the polyester film roll, the color of the cut surface of the roll is strongly noticeable, but in this embodiment, the yellowness of the cut surface of the roll is also suppressed. In addition, since the y value of the polyester film constituting this roll is within the above range, when the polyester film is used for decorative molding, the pattern and color tone can be clearly transferred (printed) onto the molded body. For this reason, the polyester film is suitable for decorative molding.

[0029] In order to set the y value of the polyester film within the above range, methods include adjusting the type and amount of biomass-derived raw materials in the polyester, adjusting melt mixing conditions during polyester film production such as shear rate and residence time to prevent resin deterioration, appropriately controlling the crystalline state of the film by adjusting cooling temperature conditions from the molten state, and appropriately controlling stretching conditions and manufacturing processes such as stretch ratio, stretching temperature, and heat treatment (heat setting) temperature after stretching. In particular, the y value of the polyester film tends to be easily reduced by appropriately controlling various manufacturing conditions in addition to adjusting the type and amount of biomass-derived raw materials in the polyester.

[0030] Cooling from the molten state can be carried out, for example, by using a cast roll as a cooling machine and bringing the extruded molten resin into contact with the cast roll, and specifically, a method in which the cooling temperature is set to a temperature 30 to 130°C higher than the glass transition temperature of the raw material resin component can be mentioned. The cooling temperature is more preferably 35 to 120°C higher, and particularly preferably 40 to 110°C higher, than the glass transition temperature of the resin component. By setting the cooling temperature within the above range, the cooling speed of the film, i.e., the relative crystallinity, can be adjusted, making it easy to adjust the y value.

[0031] In the case where the film is a biaxially stretched film, for example, it is also useful to adjust the conditions for biaxial stretching and heat setting. For example, the y value can be easily reduced by setting the heat setting temperature to a predetermined temperature or less or the treatment time to a predetermined time or less. For this reason, the treatment temperature and treatment time during heat setting may be appropriately adjusted in consideration of the type and blending ratio of the raw materials used in the film. It is also effective to avoid exposure to light, especially ultraviolet light, and in order to reduce the y value, it is also effective to pay attention to the storage conditions of the raw material resin before film formation.

[0032] The y value can also be controlled by the polymerization catalyst used when polymerizing the raw polyester. Antimony, titanium, germanium, and aluminum-based catalysts are known as polymerization catalysts for polyesters, and the y value of the polyester film obtained is easily reduced by using preferably antimony, germanium, or aluminum-based, and more preferably antimony-based, catalysts. In addition, it is also effective to suppress the activity of the catalyst residue so that the polyester polymerization catalyst residue does not remain in the film. For example, in the case of a titanium-based polymerization catalyst, it is also effective to suppress the catalyst activity by adding a phosphorus-based additive to the raw polyester in advance or by adding it separately when forming the film. The above-mentioned method for adjusting the y value is particularly effective when using a biomass-derived polyester.

[0033] Furthermore, it is possible to carry out a relaxation treatment to reduce the shrinkage rate in the width direction of the biaxially stretched film. In this case, the biaxially stretched film is preferably subjected to a relaxation treatment for reducing shrinkage, usually in the range of 0.1 to 10% of the tenter clip interval, in the maximum temperature region of the heat setting zone in the tenter or in a cooling zone at a temperature lower than that.

[0034] The tensile elongation at break in the MD direction of the polyester film is preferably 50% or more, more preferably 80% or more, even more preferably 120% or more, even more preferably 150% or more, even more preferably 170% or more, and particularly preferably 190% or more. The upper limit of the tensile elongation at break in the MD direction of the polyester film is not particularly limited, but is preferably, for example, 300% and more preferably 280%. The tensile elongation at break in the TD direction of the polyester film is preferably 50% or more, more preferably 80% or more, even more preferably 120% or more, and particularly preferably 150% or more. The upper limit of the tensile elongation at break in the TD direction of the polyester film is not particularly limited, but is preferably, for example, 300% and more preferably 250%. By setting the tensile elongation at break of the polyester film within the above range, a polyester film suitable for, for example, decorative molding can be obtained. In particular, when the tensile elongation at break of a polyester film is equal to or greater than a predetermined value, the film is more conformable to the adherend, and the film has good decorative formability even when the adherend has an uneven structure or the adherend has a large surface area. The tensile elongation at break of a polyester film can be measured by taking a sample piece having a width of 15 mm and a length of 150 mm, and performing a tensile test using a tensile tester with a gripping distance of 50 mm and a tensile speed of 200 mm / min. The elongation at break is measured and used as the tensile elongation at break.

[0035] The tensile breaking strength in the MD direction of the polyester film is preferably 100 MPa or more, more preferably 120 MPa or more, and even more preferably 150 MPa or more. The upper limit of the tensile breaking strength in the MD direction of the polyester film is not particularly limited, but is preferably 400 MPa, and more preferably 300 MPa, for example. The tensile breaking strength in the TD direction of the polyester film is preferably 100 MPa or more, more preferably 120 MPa or more, and even more preferably 150 MPa or more. The upper limit of the tensile breaking strength in the TD direction of the polyester film is not particularly limited, but is preferably 400 MPa, and more preferably 300 MPa, for example. By setting the tensile breaking strength of the polyester film within the above range, it is possible to obtain a polyester film suitable for, for example, decorative molding. In particular, when the tensile breaking strength of the polyester film is a predetermined value or more, it is possible to suppress the polyester film from breaking during decorative molding. The tensile breaking strength of polyester film can be measured by taking a sample piece of 15 mm wide and 150 mm long, and conducting a tensile test using a tensile tester with a gripping distance of 50 mm and a pulling speed of 200 mm / min. The load at the time of tensile breaking (when breaking) is measured and regarded as the tensile breaking strength.

[0036] The load at 5% elongation in the MD direction of the polyester film is preferably 150 MPa or less, more preferably 140 MPa or less, and even more preferably 130 MPa or less. The load at 5% elongation in the MD direction of the polyester film is not particularly limited, but is preferably 50 MPa or more, and more preferably 70 MPa or more. The load at 5% elongation in the TD direction of the polyester film is preferably 150 MPa or less, more preferably 140 MPa or less, and even more preferably 130 MPa or less. The load at 5% elongation in the TD direction of the polyester film is not particularly limited, but is preferably 50 MPa or more, and more preferably 70 MPa or more. The state in which the polyester film is 5% elongated is similar to the state of the polyester film during, for example, decorative molding. Therefore, by setting the load at 5% elongation within the above range, it becomes easier to control the force of shrinkage of the polyester film, and the occurrence of deviation of the decoration position and the printing position can be more effectively suppressed. The load at 5% elongation of polyester film can be measured by taking a sample piece of 15 mm wide and 150 mm long, and conducting a tensile test using a tensile tester with a gripping distance of 50 mm and a tensile speed of 200 mm / min. The load at 5% elongation is measured.

[0037] The heat shrinkage rate in the MD direction when the polyester film is heated at 180°C for 5 minutes is preferably 3% or less, more preferably 2.8% or less, even more preferably 2.5% or less, and particularly preferably 2.2% or less. The heat shrinkage rate in the MD direction may be about 0%, or may be about 0.3%. The heat shrinkage rate in the TD direction when the polyester film is heated at 180°C for 5 minutes is preferably 2% or less, more preferably 1.8% or less, even more preferably 1.5% or less, and particularly preferably 1% or less. The heat shrinkage rate in the TD direction may be about -1%, or may be about -0.7%.

[0038] The heat shrinkage rate in the MD direction when the polyester film is heated at 120°C for 5 minutes is preferably 3% or less, more preferably 2.8% or less, even more preferably 2.5% or less, and particularly preferably 2% or less. The heat shrinkage rate in the MD direction may be about 0%, or may be about 0.2%. The heat shrinkage rate in the TD direction when the polyester film is heated at 120°C for 5 minutes is preferably 2% or less, more preferably 1.8% or less, even more preferably 1.5% or less, and particularly preferably 1% or less. The heat shrinkage rate in the TD direction may be about -1%, or may be about -0.5%.

[0039] The heat shrinkage rate of a polyester film can be calculated by measuring a 1.5 cm x 15 cm polyester film in an untensioned state, heat treating it for 5 minutes in a hot air oven kept at a specified temperature (180°C or 120°C), measuring the length of the polyester film before and after the treatment, and using the following formula. Heat shrinkage rate (%) = {(sample length before heat treatment) - (sample length after heat treatment)} / (sample length before heat treatment) x 100

[0040] The haze of the polyester film is preferably 10% or less, more preferably 8% or less, even more preferably 7% or less, even more preferably 5% or less, and particularly preferably 4.5% or less. The lower limit of the haze of the polyester film is not particularly limited, and may be, for example, 0% or less, or may be 1%. The haze of the polyester film when heated at 180°C for 5 minutes is preferably 10% or less, more preferably 9% or less, and even more preferably 7% or less. The lower limit of the haze of the polyester film is not particularly limited, and may be, for example, 0% or less, or may be 1%. If the haze value of the polyester film after heat treatment is within the above range, it means that the transparency is maintained even after decorative molding. The haze of the polyester film is measured in accordance with JIS K 7136:2000.

[0041] The change in haze (ΔH) of the polyester film before and after the heat treatment is preferably 2% or less, more preferably 1.8% or less, even more preferably 1.5% or less, and particularly preferably 1.5% or less. The change in haze (ΔH) is particularly preferably 0%, but may be about 0.3%. The change in haze (ΔH) of the polyester film before and after the heat treatment is a value calculated by the following formula. Change (ΔH) (%) = (haze of film after heating at 180°C for 5 minutes) (%) - (haze of film before heating) (%) If the change in haze (ΔH) of the polyester film before and after the heat treatment is within the above range, it means that the transparency of the film is not reduced by the heat treatment, which means that the heat treatment causes little precipitation of oligomer components derived from polyester.

[0042] The total light transmittance of the polyester film is preferably 80% or more, more preferably 85% or more. The upper limit of the total light transmittance of the polyester film is not particularly limited, and may be, for example, 100% or 95%. The total light transmittance of the polyester film is measured in accordance with JIS K 7361-1:1997.

[0043] The maximum value of the sagging amount at the end of the polyester film is preferably less than 10 mm, more preferably 9.5 mm or less, even more preferably 9 mm or less, even more preferably 8 mm or less, and particularly preferably 7.5 mm or less. The lower limit of the maximum value of the sagging amount of the polyester film is not limited, and is particularly preferably 0 mm, but may be 1 mm. When measuring the sagging amount of the polyester film, the polyester film is unwound from the polyester film roll and hung over two rolls that are parallel and horizontally placed with a gap of 1.5 m so that the polyester film's longitudinal direction spans them. Then, a constant tension of 0.4 MPa is applied to the polyester film between the two rolls. When a constant tension is applied to the polyester film between the two rolls, one or both ends in the width direction may become loose and droop. In this case, the difference between the highest point and the lowest point of the sagging occurring at the end of the polyester film in the width direction (maximum depth of sagging) is measured with an ultrasonic displacement sensor (UD-500 manufactured by Keyence Corporation) and is taken as the sagging amount (mm). When the amount of sagging is different between the first end (the right end in the running direction) and the second end (the left end in the running direction) in the width direction of the polyester film, the larger value is regarded as the maximum amount of sagging. When the amount of sagging is the same between the first end and the second end in the width direction of the polyester film, the amount of sagging at each end is regarded as the maximum amount of sagging. Normally, the amount of sagging at the center of the film is rarely greater than the amount of sagging at the ends of the film, but even if the amount of sagging at the center is greater than the amount of sagging at the ends of the film, the above "amount of sagging" refers to the maximum amount of sagging that occurs at the ends in the width direction of the polyester film. The greater the width of the film roll, the greater the absolute value of the amount of sagging, so when the width of the polyester film is 1000 mm or more, the amount of sagging is regarded as the value proportional to the width of 1000 mm. For example, if the sag amount is 7.5 mm at a width of 1500 mm, converting it proportionally to a width of 1000 mm gives 7.5 mm x 1000 / 1500 = 5 mm, which is the same as a film roll with a width of 1000 m and a sag amount of 5 mm.

[0044] In order to adjust the amount of sagging in a polyester film, methods include adjusting the type and amount of biomass-derived raw materials in the polyester, and appropriately controlling the stretching conditions and manufacturing process during the production of the polyester film, such as the stretching ratio, stretching temperature, heat treatment (heat setting) temperature after stretching, cooling temperature after heat treatment, and tentering and relaxation treatment, tension during winding, etc. In particular, by appropriately controlling various manufacturing conditions in addition to adjusting the type and amount of biomass-derived raw materials in the polyester, the amount of sagging in the polyester film tends to be reduced.

[0045] Cooling from the molten state can be carried out, for example, by using a cast roll as a cooling machine and bringing the extruded molten resin into contact with the cast roll, and specifically, a method of setting the cooling temperature to a temperature 30 to 130°C higher than the glass transition temperature of the raw material resin component can be mentioned. The cooling temperature is more preferably 35 to 120°C higher, and particularly preferably 40 to 110°C higher, than the glass transition temperature of the resin component. By setting the cooling temperature within the above range, the cooling speed of the film, i.e., the relative crystallinity, can be adjusted, and the amount of sagging can be easily adjusted.

[0046] In the case where the film is a biaxially stretched film, for example, when the biaxially stretched and heat-set film is cooled, a method can be used in which a treatment is performed to slightly widen or shrink one or both side edges of the film, preferably in a temperature range of 100 to 160°C, depending on the shape of the sag (position of the sag) and the degree of sag. This treatment can usually be adjusted by moving the tenter clip spacing in a direction to widen it (hereinafter referred to as "spanning treatment") or in a direction to shrink it (hereinafter referred to as "relaxation treatment"). The amount of this width-widening or relaxation treatment can be adjusted by selecting from within a range of 0.1 to 2% of the length from the center of the film in the width direction to the side edge (i.e., half the length of the tenter clip spacing).

[0047] When the side edges of a film are tentered, the length (longitudinal dimension) of the side edges becomes longer than before tentering, and conversely, when they are relaxed, the length becomes shorter. It is believed that the change in film length due to tentering or relaxation is greatest at the side edges of the film, with only a small effect on the center of the film. Therefore, the choice of tentering or relaxation should be based on the film length at the center of the film, where the effect of the treatment is less likely to be felt. The above-mentioned method for adjusting the amount of sagging is particularly effective when using a biomass-derived polyester.

[0048] <Polyester> The polyester film contains a biomass-derived polyester. The polyester is a polymeric compound having a continuous ester bond in the main chain, specifically, obtained by polycondensation reaction of a dicarboxylic acid component and a diol component. Thus, the polyester contains a diol unit and a dicarboxylic acid unit. In this specification, the biomass-derived polyester is a polyester produced using a raw material derived from biomass, and may contain a biomass-derived unit, preferably 5 mol % or more, more preferably 10 mol % or more. Specifically, the dicarboxylic acid component and / or the diol component are preferably raw materials derived from biomass, and the biomass-derived polyester contains preferably 5 mol % or more, more preferably 10 mol % or more of a biomass-derived dicarboxylic acid unit and / or diol unit.

[0049] The polyester film is a film containing polyester as a main component. The content of polyester is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, based on the total mass of the polyester film. In this embodiment, at least a part of the polyester constituting the polyester film is a biomass-derived polyester, and the polyester film is preferably a film containing biomass-derived polyester as a main component. The content of biomass-derived polyester is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 70% by mass or more, based on the total mass of the polyester film.

[0050] The biomass-derived polyester may contain biomass-derived units, preferably at 5 mol% or more, more preferably at 10 mol% or more, even more preferably at 15 mol% or more, even more preferably at 20 mol% or more, even more preferably at 25 mol% or more, even more preferably at 30 mol% or more, particularly preferably at 35 mol% or more, even more particularly preferably at 40 mol% or more, and most preferably at 45 mol% or more. In addition, both the dicarboxylic acid component and the diol component may be biomass-derived raw materials, and the biomass-derived polyester may contain 100 mol% of biomass-derived units.

[0051] The biomass-derived polyester preferably contains 10 mol% or more of biomass-derived units relative to the total amount of diesel-derived units, more preferably 30 mol% or more, even more preferably 50 mol% or more, even more preferably 70 mol% or more, even more preferably 80 mol% or more, and even more preferably 90 mol% or more, and may contain 100 mol% of biomass-derived units.

[0052] In this embodiment, it is particularly preferable that the diol component is a biomass-derived raw material. Here, examples of the diol component include ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, and neopentyl glycol. Among them, it is preferable that the diol component is ethylene glycol, and it is preferable that ethylene glycol is a biomass-derived raw material. That is, in the biomass-derived polyester, it is preferable that the diol unit is a biomass-derived ethylene glycol unit.

[0053] Biomass-derived ethylene glycol can be obtained from ethanol (biomass ethanol) produced using biomass as a raw material. Specifically, biomass-derived ethylene glycol can be obtained by producing ethylene glycol from biomass ethanol via ethylene. In addition, commercially available biomass-derived ethylene glycol can also be used as the biomass-derived ethylene glycol.

[0054] The biomass-derived polyester preferably contains 5 mol% or more of biomass-derived ethylene glycol units, more preferably 10 mol% or more, even more preferably 15 mol% or more, even more preferably 20 mol% or more, even more preferably 25 mol% or more, even more preferably 30 mol% or more, particularly preferably 35 mol% or more, even more particularly preferably 40 mol% or more, and most preferably 45 mol% or more. The content of biomass-derived ethylene glycol units in the total polyester of the polyester film is preferably 5 mol% or more, more preferably 10 mol% or more, even more preferably 15 mol% or more, even more preferably 20 mol% or more, and most preferably 30 mol% or more. It is more preferably 40 mol % or more, even more preferably 40 mol % or more, and particularly preferably 45 mol % or more.

[0055] As the dicarboxylic acid component, aromatic dicarboxylic acid or aliphatic dicarboxylic acid can be used. As the aromatic dicarboxylic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, and other furandicarboxylic acids can be mentioned. As the aliphatic dicarboxylic acid, oxalic acid, succinic acid, glutaric acid, adipic acid, sebacic acid, dodecanedioic acid, dimer acid, and other acids can be mentioned. These may be used alone or in combination of two or more. Among them, the dicarboxylic acid component is preferably an aromatic dicarboxylic acid, and particularly preferably terephthalic acid. As the terephthalic acid, one made from paraxylene extracted from petroleum may be used.

[0056] The polyester may be a homopolyester or a copolymer polyester. In this specification, the homopolyester is a polyester obtained by polycondensation of one kind of diol component and one kind of dicarboxylic acid component. Representative examples of the homopolyester include polyethylene terephthalate (PET) and polybutylene terephthalate (PBT). On the other hand, the copolymer polyester is a polyester obtained by polycondensation of a third component. The third component is a component other than the compound that is the main component (i.e., the component with the highest content) of the dicarboxylic acid component constituting the polyester and the compound that is the main component (i.e., the component with the highest content) of the diol component. Examples of the dicarboxylic acid component of the third component include isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, and sebacic acid, and examples of the glycol component include ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, and neopentyl glycol. When the polyester is a copolymer polyester, the content of the third component is preferably 30 mol% or less.

[0057] In addition, when polyester is produced (polycondensed) using ethylene glycol as one of the raw materials, diethylene glycol is usually produced as a by-product from ethylene glycol. In this specification, this diethylene glycol is referred to as by-product diethylene glycol. The amount of diethylene glycol produced as a by-product from ethylene glycol varies depending on the type of polycondensation, but is about 5 mol% or less of ethylene glycol. In this specification, 5 mol% or less of diethylene glycol is defined as by-product diethylene glycol, and the by-product diethylene glycol is also included in ethylene glycol and is distinguished from the copolymerization component. However, when diethylene glycol is contained in an amount exceeding 5 mol%, diethylene glycol is treated as a copolymerization component and not as a by-product diethylene glycol.

[0058] In this embodiment, recycled raw materials may be used in combination with the polyester. Examples of recycled raw materials include the edges of polyester films that were not used in the polyester film production line, recycled polyesters derived from PET bottles, labels for PET bottles, binding labels for lunch boxes, and recycled polyesters derived from packaging materials. However, when the recycled raw materials are not polyesters derived from biomass, the amount of the recycled raw materials used is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total polyester mass of the polyester film.

[0059] In recent years, the use of mechanically recycled raw materials, especially mechanically recycled polyester, has been considered, but mechanically recycled raw materials have a problem of being strongly yellowish due to their thermal history. In order to effectively use mechanically recycled raw materials and reduce the burden on the environment, biomass-derived polyester and mechanically recycled raw materials, especially mechanically recycled polyester, may be combined. This makes it easier to adjust the yellowish color of the mechanically recycled raw materials, and makes it easier to produce a film that is environmentally friendly and has excellent appearance and design.

[0060] The biomass degree of the polyester film is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more. The upper limit of the biomass degree is not particularly limited, but may be 100%. The biomass degree in this specification can be calculated by the following method. "Biomass ratio" (%) = "Biomass ratio of biomass raw material" (%) x "mass ratio of biomass raw material in the film" (%) The biomass degree of a biomass feedstock is an index of the concentration of biomass-derived carbon in the biomass feedstock, and is a value measured by measuring the amount of biomass-derived carbon measured by radioactive carbon (C14). Carbon dioxide in the atmosphere contains a certain percentage (105.5 pMC) of C14, so it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere is about 105.5 pMC. It is also known that fossil fuels contain very little C14. Therefore, the biomass degree of a biomass feedstock can be calculated by measuring the percentage of C14 contained in the total carbon atoms in the biomass feedstock.

[0061] <Polycondensation catalyst> The polycondensation catalyst used in polycondensing the polyester is not particularly limited, and any conventionally known compound can be used. Examples of the polycondensation catalyst include titanium compounds, germanium compounds, antimony compounds, manganese compounds, aluminum compounds, magnesium compounds, and calcium compounds.

[0062] In this embodiment, in order to suppress the amount of oligomer components precipitated in the polyester film, the polyester film may be manufactured using a polyester having a low content of oligomer components as a raw material. As a method for manufacturing a polyester having a low content of oligomer components, various known methods can be used, such as a method of solid-phase polymerization after polyester production. In addition, the polyester may be obtained by melt polycondensation under reduced pressure at a higher reaction temperature after esterification or transesterification.

[0063] <Intrinsic viscosity> The intrinsic viscosity (IV) of the polyester is preferably 0.5 dL / g or more, more preferably 0.52 dL / g or more, and even more preferably 0.54 dL / g or more. The intrinsic viscosity (IV) of the polyester is, for example, 1 dL / g or less, preferably 0.8 dL / g or less. By setting the intrinsic viscosity of the polyester within the above range, it becomes easier to control the y value of the polyester film within a desired range. Furthermore, by setting the intrinsic viscosity of the polyester within the above range, the production efficiency of the polyester film can be more effectively improved.

[0064] <Optional ingredients> The polyester film may contain additives, such as colorants such as pigments and dyes, antistatic agents, flame retardants, ultraviolet absorbing agents, antibacterial agents, nucleating agents, plasticizers, release agents, antioxidants, inorganic particles, and organic particles, as necessary.

[0065] In this embodiment, it is also preferred that the polyester film contains a colorant such as a pigment or dye as an optional component. In this case, the polyester film preferably contains a blue colorant. By containing the blue colorant in the polyester film, the color tone and design of the film can be improved. In addition, such a polyester film is preferably used as a decorative molding film.

[0066] Examples of blue colorants include conventionally known blue dyes and blue pigments. Among them, it is preferable to use a blue dye, and examples of blue dyes include anthraquinone-based, azo-based, and phthalocyanine-based blue dyes. In addition, it is preferable that the blue colorant is halogen-free. If a halogen-free colorant is used, the adverse effect on the environment, i.e., the environmental load, can be reduced when the polyester film is discarded. Among them, it is preferable to use a halogen-free anthraquinone-based blue dye as the blue colorant. Specific examples of halogen-free anthraquinone blue dyes include Disperse Blue 3, Disperse Blue 5, Disperse Blue 14, Disperse Blue 26, Disperse Blue 28, Disperse Blue 35, Disperse Blue 334, Disperse Blue 359, Disperse Blue 60, Disperse Blue 72, Disperse Blue 73, Disperse Blue 77, Disperse Blue 214, Disperse Blue 167, Disperse Blue 54, Solvent Blue 101, Solvent Blue 102, Solvent Blue 104, Solvent Blue 122, Solvent Blue 35, Solvent Blue 36, Solvent Blue 59, Solvent Blue 63, Solvent Blue 68, Solvent Blue 78, and Solvent Blue 97.

[0067] The content of the colorant depends on the type of the colorant, but is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.03% by mass or more, based on the total mass of the polyester film. The content of the colorant is preferably 1% by mass or less, more preferably 0.8% by mass or less, even more preferably 0.6% by mass or less, and particularly preferably 0.5% by mass or less.

[0068] The polyester film may contain particles mainly for the purpose of imparting easy slippage and preventing scratches in each process. The type of particles contained in the polyester film is not particularly limited as long as it is a particle capable of imparting easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, as well as crosslinked polymers such as crosslinked silicone resin particles, crosslinked acrylic resin particles, crosslinked styrene-acrylic resin particles, and crosslinked polyester particles, and organic particles such as calcium oxalate and ion exchange resin. As the particles, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.

[0069] The shape of the particles to be used is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. In addition, there is no particular limit to the hardness, specific gravity, color, etc. of the particles. Two or more kinds of these series of particles may be used in combination as necessary.

[0070] The average particle size of the particles used is usually 5 μm or less, preferably 0.01 to 3 μm, more preferably 0.02 to 1.5 μm, and further preferably 0.03 to 1 μm. When the average particle size is within this range, the polyester film can have both easy handling and surface smoothness. In addition, when the particles are powder, the average particle size of the particles can be the particle size (d50) at an accumulated volume fraction of 50% in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device (e.g., Shimadzu Corporation's "SA-CP3 type"). The average particle size of the particles in the film, layer, or resin can be determined by observing 10 or more particles with a scanning electron microscope (SEM) to measure the diameters of the particles and calculating the average value. In this case, in the case of non-spherical particles, the average value of the longest diameter and the shortest diameter can be measured as the diameter of each particle.

[0071] When particles are incorporated into a polyester film, it is preferable to incorporate particles into the surface layer, for example, by providing a surface layer and an intermediate layer. When a two-type three-layer structure or a three-type three-layer structure is designed, it is also possible to incorporate particles into at least one of the surface layers.

[0072] The content of particles depends on the average particle size, but in the layer containing particles, it is preferably 10000 ppm or less, more preferably 8000 ppm or less, even more preferably 7000 ppm or less, more preferably 6000 ppm or less, based on mass. If it is within this range, the surface smoothness of the polyester film can be improved. In addition, the content of particles is preferably 50 ppm or more, more preferably 100 ppm or more.

[0073] The method of adding particles to the polyester film is not particularly limited, and any conventionally known method can be adopted. For example, in the case of a polyester film having a laminated structure, the particles can be added at any stage of manufacturing the polyester constituting each layer, but it is preferable to add the particles after the completion of the esterification or transesterification reaction.

[0074] The polyester film contains polyester as a main component, but may also contain other resins as long as the effects of the present invention are not impaired. Examples of other resins include polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, chlorinated polyethylene resins, polycarbonate resins, polyamide resins, polyacetal resins, acrylic resins, ethylene vinyl acetate copolymers, polymethylpentene resins, polyvinyl alcohol resins, cyclic olefin resins, polylactic acid resins, polybutylene succinate resins, polyacrylonitrile resins, polyethylene oxide resins, cellulose resins, polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, and fluorine-based resins.

[0075] <Laminated film> This embodiment may relate to a laminated film having an optional layer on at least one side of the above-mentioned polyester film. For example, this embodiment may relate to a laminated film having a coating layer on at least one side of the above-mentioned polyester film. The coating layer may be provided on at least one side of the polyester film, or on both sides. Examples of the coating layer include an easy-adhesion layer, a release layer, an antistatic layer, and an antiblocking layer. In addition, it is preferable that the physical properties such as the y value of the laminated film are equivalent to the physical properties such as the y value of the polyester film, and when measuring various physical properties of the laminated film, the various physical properties may be measured in the state of the laminated film.

[0076] For example, a laminate film including a coating layer may have the following layer structure: In the following, the term "antistatic layer / release layer" may refer to an antistatic layer, a release layer, or a release layer having an antistatic function. (1) Easy-adhesion layer: polyester film (2) Polyester film / antistatic layer / release layer (3) Polyester film / anti-blocking layer (4) Easy-adhesion layer / polyester film / antistatic layer / release layer (5) Release layer / adhesive layer / polyester film / antistatic layer / release layer (6) Release layer / polyester film / antistatic layer / release layer (7) Easy-adhesion layer / polyester film / easy-adhesion layer (8) Anti-blocking layer / easy-adhesion layer / polyester film / easy-adhesion layer (9) Anti-blocking layer / polyester film / easy adhesion layer (10) Anti-blocking layer / easy adhesion layer / polyester film / antistatic layer / release layer (11) Anti-blocking layer / polyester film / antistatic layer / release layer

[0077] The easy-adhesion layer preferably contains a polymer and a crosslinking agent. Examples of the polymer include polyurethane, polyester, and acrylic resin. Among them, the polymer is preferably polyurethane, and more preferably polyester polyurethane. The polymer preferably has a carboxylic acid residue, at least a part of which is hydrophilized using amine or ammonia. The glass transition temperature (Tg) of the polymer is preferably 0°C or higher, and more preferably 40°C or higher. Examples of the crosslinking agent contained in the easy-adhesion layer include melamine-based, epoxy-based, and oxazoline-based resins, and it is preferable to use melamine-based resins in terms of coatability and durable adhesion.

[0078] The release layer contains a release agent. Examples of the release agent include long-chain alkyl compounds, fluorine-based acrylic resins, silicones, waxes, and the like. The release layer may also contain a binder polymer in order to improve adhesion to the polyester film. Examples of the binder polymer include polyester resins, acrylic resins, urethane resins, polyvinyls (polyvinyl chloride, vinyl chloride-vinyl acetate copolymers, and the like), polyalkylene glycols, polyalkyleneimines, methylcellulose, starches, and the like. The release layer may also contain a crosslinking agent. Examples of the crosslinking agent include methylolated or alkylolated urea-based, melamine-based, guanamine-based, acrylamide-based, polyamide-based compounds, oxazoline compounds, epoxy compounds, aziridine compounds, blocked polyisocyanates, silane coupling agents, and the like. These crosslinking components may be bonded to the binder polymer in advance. The release layer may contain inactive particles for the purpose of improving slip properties, and specific examples thereof include silica, alumina, kaolin, calcium carbonate, titanium oxide, organic particles, and the like.

[0079] The antistatic layer contains an antistatic agent. Examples of the antistatic agent include cationic antistatic agents such as primary amine salts, tertiary amines, and quaternary ammonium compounds; anionic antistatic agents such as sulfurized oils, sulfated amide oils, sulfated ester oils, fatty alcohol sulfate salts, alkyl sulfate salts, fatty acid ethyl sulfonates, alkyl sulfonates, alkylnaphthalene sulfonates, alkylbenzene sulfonates, and phosphoric acid ester salts; nonionic antistatic agents such as partial fatty acid esters of polyhydric alcohols, ethylene oxide adducts of fatty alcohols, ethylene oxide adducts of fatty amines or fatty acid amides, ethylene oxide adducts of alkylphenols, ethylene oxide adducts of alkylnaphthols, polyethylene glycols, and fatty acid esters of alkyldiethanolamines; and amphoteric antistatic agents such as carboxylic acid derivatives and imidazoline derivatives. Among these, sodium alkylsulfonate, sodium alkylbenzenesulfonate, lithium alkylsulfonate, and lithium alkylbenzenesulfonate are preferably used from the viewpoints of antistatic performance and transparency. The antistatic agent may be contained in the adhesion layer or the release layer, and it is also preferable that the adhesion layer or the release layer also has antistatic properties.

[0080] The antiblocking layer preferably contains a water-dispersible polyolefin resin and a crosslinking agent. Examples of the polyolefin resin include compounds having the following compounds (1) to (5) as a basic skeleton. (1) Waxes, resins, and rubbers made of homopolymers or copolymers of α-olefin-based unsaturated hydrocarbons such as ethylene, propylene, 1-butene, 4-methyl-1-pentene, etc. Examples include polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymers, ethylene-1-butene copolymers, propylene-1-butene copolymers, etc. (2) Rubber-like copolymers of two or more of the above α-olefins with conjugated or non-conjugated dienes, such as ethylene-propylene-butadiene copolymers, ethylene-propylene-dicyclopentadiene copolymers, ethylene-propylene-ethylidenenorbornene copolymers, ethylene-propylene-1,5-hexadiene copolymers, and isobutene-isoprene copolymers. (3) Copolymers of the above α-olefins with conjugated or non-conjugated dienes, such as ethylene-butadiene copolymers and ethylene-ethylidenenorbornene copolymers. (4) Copolymers of the above α-olefins (especially ethylene) with vinyl acetate and their completely or partially saponified products. (5) Graft polymers in which the above-mentioned conjugated or non-conjugated dienes or vinyl acetate, etc. are grafted onto the homo- or copolymers of the above-mentioned α-olefins, and their completely or partially saponified products. Examples of the crosslinking agent include melamine-based, epoxy-based, amide-based, and acrylamide-based compounds, polyisocyanates, blocked polyisocyanates, carbodiimide compounds, etc. Examples of the melamine-based crosslinking agent include alkylol- or alkoxyalkylol-based melamine compounds such as methoxymethylated melamine and butoxymethylated melamine, and melamine partially co-condensed with urea or the like can also be used.

[0081] If necessary, antifoaming agents, coating property improvers, thickeners, organic lubricants, bactericides, inorganic particles, organic particles, antistatic agents, antioxidants, ultraviolet absorbers, foaming agents, and dyes can be added to the above-mentioned coating layer.

[0082] When forming a coating layer, a coating agent (coating agent) is applied to the surface of the polyester film. For example, a coating device such as a reverse roll coater, a gravure coater, a rod coater, or an air doctor coater can be used as the coating method. In addition, the polyester film may be subjected to a chemical treatment or a discharge treatment in order to modify the surface of the film before coating.

[0083] The thickness of the coating layer (thickness after drying) is preferably 0.01 μm or more, more preferably 0.02 μm or more, and is preferably 1 μm or less.

[0084] The coating layer is preferably formed during the stretching process of the polyester film, and is preferably formed by so-called in-line coating. When the coating layer is provided on the polyester film by in-line coating, it is possible to apply the coating simultaneously with stretching, and the thickness of the coating layer can be changed by the stretching ratio, so that a film suitable as a polyester film can be produced. When the coating layer is formed by in-line coating, for example, in the case of sequential biaxial stretching, it is preferable to perform the coating treatment after the longitudinal stretching and before the transverse stretching.

[0085] This embodiment may also relate to a laminated film having a printed layer on at least one side of the polyester film. When the laminated film has a printed layer, the printed layer is preferably laminated on the coating layer (e.g., an easy-adhesion layer) described above. For example, the laminated film including the printed layer may have the following layer structure. (1) Printing layer / polyester film (2) Printing layer / polyester film / coating layer (adhesive layer, antistatic layer, release layer, antiblocking layer, etc.) (3) Printing layer / coating layer (release layer) / polyester film / coating layer (easy-adhesion layer, antistatic layer, release layer, anti-blocking layer, etc.) (4) Printing layer / coating layer (release layer) / coating layer (easy adhesion layer) / polyester film / coating layer (easy adhesion layer, antistatic layer, release layer, antiblocking layer, etc.) (5) Coating layer (release layer) / printing layer / coating layer (easy adhesion layer) / polyester film / coating layer (easy adhesion layer, antistatic layer, release layer, antiblocking layer, etc.) (6) Coating layer (release layer) / printing layer / coating layer (release layer) / coating layer (easy adhesion layer) / polyester film / coating layer (easy adhesion layer, antistatic layer, release layer, antiblocking layer, etc.)

[0086] The printing layer can be formed using a conventionally known pigment or dye, and the method of forming the printing layer is not particularly limited. The printing layer preferably contains a binder polymer in addition to a colorant (pigment or dye). Examples of the binder polymer include polyurethane resin, vinyl resin, polyamide resin, polyester resin, acrylic resin, polyvinyl acetal resin, polyester urethane resin, cellulose ester resin, alkyd resin, and thermoplastic elastomer resin. As the colorant, it is preferable to use a colored ink containing a pigment or dye of an appropriate color as the colorant.

[0087] The printing layer can be formed by a known method, and it is preferable to use a printing method such as offset printing, gravure printing, or screen printing. In particular, when multicolor printing or gradation color is required, offset printing or gravure printing is preferably used. In addition, in the case of a single color, a coating method such as gravure coating, roll coating, or comma coating can also be used. Depending on the design, printing may be performed over the entire surface or part of the polyester film.

[0088] The laminated film may further have a functional layer such as a hard coat layer, an inorganic vapor deposition layer, etc. Examples of such laminated bodies include the following laminated structures. (1) Functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / Printed layer / Coating layer (easy adhesion layer) / Polyester film / Coating layer (easy adhesion layer) (2) Functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printed layer / coating layer (release layer) / polyester film / coating layer (antistatic layer, release layer, anti-blocking layer, etc.) (3) Functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printed layer / coating layer (release layer) / coating layer (easy adhesion layer) / polyester film / coating layer (antistatic layer, release layer, antiblocking layer, etc.) (4) Functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printed layer / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / coating layer (easy adhesion layer) / polyester film / coating layer (easy adhesion layer) (5) Functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printed layer / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / coating layer (release layer) / polyester film / coating layer (antistatic layer, release layer, antiblocking layer, etc.) (6) Functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printed layer / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / coating layer (release layer) / coating layer (easy adhesion layer) / polyester film / coating layer (antistatic layer, release layer, antiblocking layer, etc.) (7) Coating layer (release layer) / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printed layer / coating layer (easy adhesion layer) / polyester film / coating layer (easy adhesion layer) (8) Coating layer (release layer) / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printed layer / coating layer (release layer) / polyester film / coating layer (antistatic layer, release layer, anti-blocking layer, etc.) (9) Coating layer (release layer) / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printing layer / coating layer (release layer) / coating layer (easy adhesion layer) / polyester film / coating layer (antistatic layer, release layer, antiblocking layer, etc.) (10) Coating layer (release layer) / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printing layer / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / coating layer (easy adhesion layer) / polyester film / coating layer (easy adhesion layer) (11) Coating layer (release layer) / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printing layer / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / coating layer (release layer) / polyester film / coating layer (antistatic layer, release layer, antiblocking layer, etc.) (12) Coating layer (release layer) / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / printing layer / functional layer (hard coat layer, inorganic vapor deposition layer, etc.) / coating layer (release layer) / coating layer (easy adhesion layer) / polyester film / coating layer (antistatic layer, release layer, antiblocking layer, etc.)

[0089] <Manufacturing method of polyester film / polyester film roll> A specific example of the production of the polyester film in the present roll will be described below, but the production method is not limited to the following example.

[0090] When the polyester film is a biaxially stretched polyester film, a method is preferred in which the raw material polyester is extruded as a molten sheet from a die using an extruder, and cooled and solidified on a rotating cooling drum (casting drum) to obtain an unstretched sheet. When the polyester film has a multilayer structure, the raw material polyester constituting each layer is fed to each extruder, melted, co-extruded, and cooled and solidified. Here, the cooling is preferably performed to a temperature below the glass transition point of the polymer, for example, to obtain an unoriented sheet (unstretched sheet) in a substantially amorphous state. In addition, in order to improve the flatness of the sheet, it is preferable to increase the adhesion between the sheet and the cooling roll, and an electrostatic application adhesion method and / or a liquid application adhesion method are preferably adopted. The raw material polyester is preferably fed to the extruder after being appropriately dried as pellets or the like. In addition, particles, ultraviolet absorbers, other additives, etc. may be appropriately blended into the pellets.

[0091] Next, the obtained unstretched sheet is stretched in biaxial directions. In this case, the unstretched sheet is first stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 2.5 to 7 times, preferably 3 to 6 times.

[0092] Next, the film is stretched in a direction perpendicular to the first-stage stretching direction, in which case the stretching temperature is usually 70 to 170° C., and the stretching ratio is usually 3 to 7 times, preferably 3.5 to 6 times. When the coating layer is formed by in-line coating as described above, for example, the coating treatment may be carried out after the first-stage stretching is completed and before the second-stage stretching.

[0093] Then, the film is heat-treated under tension or relaxation of 30% or less at a temperature of 180 to 270° C. to obtain a biaxially stretched film. This heat treatment is also called a heat setting step. The heat treatment may be performed in two or more steps with different temperatures. After the heat treatment, the film may be cooled in a cooling zone. The cooling temperature is preferably higher than the glass transition temperature (Tg) of the polyester constituting the film, and more specifically, is preferably in the range of 100 to 160° C. This cooling may be performed in two or more steps at different temperatures. In the above stretching, a method of stretching in one direction in two or more stages can be adopted. In that case, it is preferable to perform the stretching so that the final stretch ratios in both directions are each within the above range.

[0094] A simultaneous biaxial stretching method can also be used to produce the polyester film. The simultaneous biaxial stretching method involves simultaneously stretching and orienting the unstretched sheet in the machine direction (longitudinal direction) and width direction (transverse direction) under a temperature controlled condition usually at 70 to 120° C., preferably 80 to 110° C., and the stretching ratio is preferably 4 to 50 times, more preferably 7 to 35 times, and even more preferably 10 to 25 times in terms of area ratio. Then, the film is subsequently heat-treated under tension or under relaxation of 30% or less at a temperature of 170 to 250° C. to obtain a stretched and oriented film. Regarding the simultaneous biaxial stretching device employing the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, or a linear drive method can be employed.

[0095] In addition, when using recycled raw materials as part of polyester raw materials, the recycled raw materials are sorted, pulverized, and then used as flakes and / or chipped flakes such as pellets. A conventionally known method can be used to obtain flakes, and an example of the method is to obtain flakes by pulverizing with a pulverizer. A conventionally known method can also be used to chip the flakes, and an example of the method is to melt-extrude the flakes and then cut the strand-shaped molten extrudate to obtain chipped raw material such as pellets.

[0096] The polyester film obtained as described above is wound up by a winder device to become a master roll. Then, in a slitting process, the biaxially oriented polyester film is unwound from the obtained master roll and cut to a predetermined width, while applying surface pressure to the film roll with a contact roll and tension to the film with a two-axis turret winder, and the polyester film roll can be wound up.

[0097] <Uses of polyester film> The polyester film or laminated film of the present embodiment can be suitably used for applications such as packaging products, various label materials, lid materials, sheet molded products, window clings, building materials, release films, agricultural greenhouses, composite parts for aircraft, beverage cans, furniture, medical, optical (process films such as OLET, polarizing plates, backlights for liquid crystal displays, and base films for touch panels), mobile devices such as smartphones and tablets, home appliances, vehicle parts for automobiles, dry films, films for sublimation and transfer, and films for decorative molding. Among these, the polyester film or laminated film is preferably a film for decorative molding. In particular, a laminated film having the above-mentioned coating layer or printing layer is preferably used as a film for decorative molding.

[0098] The decorative molding film can be used, for example, in film insert molding and film in-mold molding. In film insert molding, the decorative molding film is three-dimensionally processed by a method such as vacuum molding, and then the three-dimensionally processed insert film is set in a mold for injection molding, the mold is closed, molding resin is injected into the cavity, and the molding resin is solidified to form a resin molded product, and at the same time, the decorative molding film (insert film) is integrally bonded to the surface of the product, thereby decorating the resin molded product. In film insert molding, the film that has been included in the product is set in a mold, and resin is poured in to obtain a decorative molded product integrated with the film.

[0099] On the other hand, film in-mold molding is a method in which a decorative molding film having a printing layer is used, and only the printing layer is transferred and printed using the heat and pressure during plastic injection molding. In film in-mold molding, a laminated film (transfer film) is prepared by laminating a printing layer including a release layer on a polyester film (base film) in advance, and transfer printing is performed using the heat and pressure during resin injection molding. At this time, the transfer film is peeled off between the release layer surface and the printing layer surface and separated. In other words, after molding transfer, the printing layer is adhered to the surface of the molded product and taken out as a product, and the release layer is removed from the product while adhering to the surface of the base film. In this way, in film in-mold molding, molding and transfer are performed simultaneously, so it is also called simultaneous molding transfer method.

[0100] As described above, in film insert molding, the polyester film is also integrated with the molding resin to form a decorative molding, but in film in-mold molding, the polyester film is the substrate of the transfer film, and only the printing layer laminated on the substrate is transferred to the molding resin. The laminate film of this embodiment is preferably used for both film insert molding and film in-mold molding, and the laminate film may be an insert film or a film for transfer during molding.

[0101] Since the y value of the polyester film of this embodiment is suppressed to a predetermined value or less, the printing accuracy and color tone can be improved when decorating a molded resin. In addition, by setting the load at 5% elongation, tensile breaking strength, and tensile breaking elongation at 5% elongation in the polyester film of this embodiment within a predetermined range, the response follow-up to the molded resin is improved and the polyester film is prevented from breaking during decorative molding.

[0102] In addition to the above-mentioned molding method, the decorative molding film is also preferably used in heat press molding, vacuum / compressed air heat press molding, and the like.

[0103] (Decorative molding) This embodiment relates to a decorated molded body decorated with the above-mentioned polyester film (laminated film). When the decorative molding is formed by insert molding, the decorated molded body may contain the above-mentioned polyester film. When the decorative molding is formed by in-mold molding, the decorated molded body does not contain the above-mentioned polyester film, and the printed layer in the laminated sheet is transferred. The decorated molded body is used, for example, as a vehicle part for an automobile or the like, a housing equipment part, a home appliance, or a mobile device part for a smartphone or a tablet. EXAMPLES

[0104] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0105] (1) Measurement of intrinsic viscosity (IV) of polyester 1 g of polyester was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and measured at 30°C.

[0106] (2) Color (y value) The color tone (y value) of the polyester film was measured using a spectrophotometer CM-3700d manufactured by Konica Minolta Japan, Inc., as follows. A sample was punched out from a predetermined location of the polyester film with a round holder blade of about 60 mm in diameter to obtain a sample. The number of test sheets was determined to be the number whose layer thickness (total thickness at the time of measurement) was closest to 500 μm. For example, 20 sheets of film may be stacked for a 25 μm film, and 13 sheets of film may be stacked for a 38 μm film. The measurement conditions were reflective conditions. The color tone was measured in an environment of 23°C.

[0107] (3) Load, tensile strength and elongation at break at 5% elongation of polyester film Sample pieces measuring 15 mm wide and 150 mm long were taken from a designated location on the polyester film, and the tensile strength and elongation at break were measured using an autograph AGX-V manufactured by Shimadzu Corporation. Gauge marks were placed at 50 mm intervals in the center of each test piece, and a tensile test was performed using a tensile tester with a gripping distance of 50 mm and a tensile speed of 200 mm / min to measure the load at 5% elongation, the load at break (tensile strength at break), and the elongation (tensile elongation at break). The tensile test was performed in both the machine direction (MD) and the transverse direction (TD) of the film.

[0108] (4) Haze of polyester film (H0) The measurement was performed according to JIS K 7136:2000 using a haze meter NDH4000 manufactured by Nippon Denshoku Industries Co., Ltd.

[0109] (5) Haze of polyester film after heat treatment (H1) After the sample film was heat-treated under the specified conditions (180°C, 5 minutes), the film haze was measured in the same manner as above. The change in haze (ΔH) before and after heating was calculated using the following formula. ΔH(%)=(H1)(%)-(H0)(%)

[0110] (6) Heat shrinkage rate of polyester film A 1.5cm x 15cm polyester film was heat-treated for 5 minutes in a hot air oven maintained at a specified temperature (180°C or 120°C) in an untensioned state, and the length of the polyester film was measured before and after the treatment, and the heat shrinkage rate (%) was calculated using the following formula. The heat shrinkage rate (%) was calculated for both the machine direction (MD) and the transverse direction (TD) of the film. Heat shrinkage rate (%) = {(sample length before heat treatment) - (sample length after heat treatment)} / (sample length before heat treatment) x 100

[0111] [Polyester raw materials] Raw material A: Biomass-derived PET with a bio content of 30%, IV=0.63dL / g (98 mol% of biomass-derived ethylene glycol units and 2 mol% of biomass-derived diethylene glycol units out of all diol-derived units), biomass-derived units out of the total diol units and dicarboxylic acid units are 50 mol% Material B: Recycled materials of materials A, C and E, IV=0.57dL / g, biomass content 21% Raw material C: Fossil fuel-derived PET, IV = 0.82 dL / g (diethylene glycol units are 2 mol% of all diol-derived units) Raw material D: PET recycled raw material derived from fossil fuels (containing 0.06% by mass of silica particles with a particle size of 3 μm), IV = 0.57 dL / g Raw material E: Fossil fuel-derived PET (particle master batch) containing 0.7% by mass of silica particles (particle size 3 μm), IV = 0.59 dL / g

[0112] Example 1 The raw materials for both surface layers were made by mixing the manufacturing raw materials C and E at a ratio of 69% by mass and 31% by mass, respectively, and the raw materials for the intermediate layer were made by mixing the raw materials A and B at a ratio of 75% by mass and 25% by mass, respectively. The mixed raw materials for both surface layers and the intermediate layer were fed to two extruders, melted at 280°C, and then co-extruded onto a cooling roll set at 25°C in a layer structure of two types and three layers (extrusion rate of surface layer / intermediate layer / surface layer = 5.5 / 39 / 5.5), and cooled and solidified to obtain an unstretched sheet. Next, the obtained unstretched sheet was stretched 3.1 times in the machine direction (MD) at 88°C using a roll stretching machine. Furthermore, after preheating at 100°C in a tenter, it was stretched 4.1 times in the transverse direction (TD) at 135°C. Finally, it was heat-treated at 238°C, relaxed 7% in the transverse direction, and wound up into a roll using a winder to produce a master roll of biaxially stretched polyester film with a thickness of 50 μm (each surface layer: 5.5 μm, middle layer: 39 μm). The biaxially oriented polyester film was unwound from the obtained master roll and slit to a width of 1,300 mm onto a core having a diameter of 6 inches (152.2 mm). The film roll was wound up while applying surface pressure to the film roll with a contact roll and tension to the film with a two-axis turret winder.

[0113] Comparative Example 1 A biaxially oriented polyester film and a polyester film roll were obtained in the same manner as in Example 1, except that the production raw materials were changed as shown in the table below.

[0114] [Table 1]

[0115] [Table 2]

[0116] The polyester film rolls of the examples containing biomass-derived polyester had smaller y values ​​than the polyester film rolls of the comparative examples made of fossil fuel-derived polyester, and as a result, the decorative clarity tended to be better. [Explanation of symbols]

[0117] 10. Middle Class 20 Surface layer 100 Polyester film

Claims

1. Contains biomass-derived polyester, The polyester film roll is obtained by winding up a polyester film having a y value of less than 0.323 as measured by a color reflection method.

2. 2 . The polyester film roll according to claim 1 , wherein the polyester film has a layer containing a biomass-derived polyester as a main component and a layer containing a fossil fuel-derived polyester as a main component.

3. 3. The polyester film roll according to claim 2, wherein the polyester film has a layer containing the biomass-derived polyester as a main component as an intermediate layer, and a layer containing the fossil fuel-derived polyester as a main component as a surface layer.

4. The polyester comprises diol units and dicarboxylic acid units, 2. The polyester film roll of claim 1, wherein the diol units are ethylene glycol units derived from biomass.

5. The polyester film roll according to claim 4 , wherein the polyester contains 10 mol % or more of ethylene glycol units derived from the biomass.

6. 2. The polyester film roll of claim 1, wherein the polyester film is a biaxially oriented polyester film.

7. 2. The polyester film roll of claim 1, having a haze of 10% or less.

8. 2. The polyester film roll according to claim 1, which has a haze ratio of 10% or less when heated at 180° C. for 5 minutes.

9. 2. The polyester film roll according to claim 1, which is a decorative forming film.

10. A laminated film comprising the polyester film according to claim 1 and a coating layer on at least one surface of the polyester film.

11. A laminated film comprising the polyester film according to claim 1 and a printed layer on at least one surface of the polyester film.

12. The laminated film according to claim 10, which is a film for decorative molding.

13. The laminated film according to claim 11, which is a film for simultaneous molding and transfer.

14. A decorated molded article decorated with the polyester film according to any one of claims 1 to 13.

15. The decorated molded article according to claim 14, which is a mobile device, a home appliance, or a vehicle part.

Citation Information

Patent Citations

  • Laminate for molding

    JP2012040713A

  • Biaxially-stretched polyester film for luminance increasing sheet member

    JP2012250445A

  • Laminate and packaging bag including the same

    JP2019025722A

  • Biaxially stretched polyester film

    WO2022131360A1

  • Laminated body of polyester resin composition

    JP2018052125A

Cited By

  • Polyester film having furandicarboxylic acid unit and method for producing same

    WO2026211967A1