Raw material for nitrided component, nitrided component, and method of manufacturing nitrided component

A tailored chemical composition and processing method for nitrided parts addresses deformation issues in complex shapes by enhancing machinability and fatigue strength, thus optimizing manufacturing efficiency.

JP2024179337APending Publication Date: 2024-12-26NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2023098095
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Existing nitriding technologies fail to adequately suppress deformation in mechanically complex parts with high bending and torsional deformation, leading to increased manufacturing costs and reduced yields due to the need for additional straightening processes.

Method used

A specific chemical composition and microstructure for nitrided parts, including controlled amounts of elements like Cr, C, and V, combined with low-temperature annealing and nitriding processes, to minimize deformation and enhance machinability and fatigue strength.

Benefits of technology

The solution effectively suppresses deformation during nitriding, ensuring high machinability and fatigue properties in complex-shaped parts, reducing manufacturing costs and improving yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024179337000003
    Figure 2024179337000003
  • Figure 2024179337000004
    Figure 2024179337000004
  • Figure 2024179337000005
    Figure 2024179337000005
Patent Text Reader

Abstract

To provide a raw material for nitrided component which has sufficiently low hardness and excellent machinability when performing cutting work, suppresses deformation of component during nitriding, and can obtain high fatigue characteristic after nitriding, a nitrided component, and a method of manufacturing a nitrided component.SOLUTION: Provided are a raw material for nitrided component which has a predetermined chemical composition, has a fine structure in which the sum of area ratios of bainite and martensite is less than 90% at the position of a depth 5 mm from a surface, the content of Crsol which is Cr of a solid solution state is 0.45% or more, and Fn expressed by the following formula (1) is 0.50 or more, and an application thereof. Fn=(Cr-Crsol) / (C×Cr)...(1) (in formula (1), Cr and C denote the content of each element in mass%, Crsol denotes the content of Crsol in mass%)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a preform for a nitrided component, a nitrided component, and a method for manufacturing a nitrided component. [Background technology]

[0002] Some mechanical structural parts used in automobiles, ships, industrial machines, etc. are repeatedly subjected to high bending stresses. In order to provide these parts with the necessary fatigue strength, various surface hardening heat treatments are sometimes performed. On the other hand, when parts are subjected to surface hardening heat treatment such as carburizing or induction hardening, the parts are deformed due to martensitic transformation during hardening. In order to suppress such deformation during hardening, nitriding is sometimes used instead of carburizing or induction hardening.

[0003] Nitriding is carried out at a relatively low temperature of 600°C or less, and since martensitic transformation does not occur, the deformation of the parts is small. Nitriding reduces the amount of deformation of parts compared to other surface hardening heat treatments, but it does not completely eliminate deformation. When nitriding is performed on parts that require extremely high dimensional accuracy, the deformation during nitriding cannot be ignored, which can lead to a decrease in yield and an increase in manufacturing costs due to the addition of processes such as straightening after nitriding. For this reason, technology to suppress deformation of nitrided parts has been developed.

[0004] A technique for suppressing deformation of nitrided parts is disclosed in, for example, Patent Document 1.

[0005] In the technology described in Patent Document 1, in order to suppress the formation of a compound layer, which is one of the causes of deformation, the steel composition is optimized and the nitriding temperature is controlled. By suppressing the formation of the compound layer, the change in the outer diameter of the ring-shaped test piece is suppressed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-49059 Summary of the Invention [Problem to be solved by the invention]

[0007] The technology described in Patent Document 1 focuses on suppressing the expansion of the nitrided layer. Therefore, although it is effective in cases where the deformation of a part is only an increase in diameter or axial length, such as a shaft with a perfectly axially symmetrical shape, it is not sufficiently effective in suppressing bending or twisting deformation of parts with complex shapes.

[0008] For shaft-shaped parts with flanges and keyways, thin-walled large ring-shaped parts that are prone to torsional deformation, and parts with complex shapes such as gears, it is desirable for bending and torsional deformation to be suppressed and for the material to have the fatigue strength and machinability required for machine structural parts.

[0009] An object of the present disclosure is to provide a base material for a nitrided part, a nitrided part, and a method for manufacturing a nitrided part, which have sufficiently low hardness and excellent machinability during cutting, which are suppressed in deformation of the part during nitriding, and which can obtain high fatigue characteristics after nitriding. [Means for solving the problem]

[0010] The above problems are solved by the following means. <1> In mass%, C: 0.04-0.18%, Si: 0.03 to 0.35%, Mn: 0.40-2.20%, P: 0.050% or less, S: 0.001~0.050%, Cu: 0.01-0.40%, Cr: 0.50~1.40%, Ni: 0.01 to 0.40%, Al: 0.001 to 0.080%, V: 0.10 to 0.40%, and N: 0.0040 to 0.0250%, with the balance being Fe and impurities; The microstructure has a sum of the area ratios of bainite and martensite of less than 90% at a depth of 5 mm from the surface, A base material for nitrided parts, wherein the content by mass of Crsol, which is Cr in a solid solution state, is 0.45% or more at a position 5 mm deep from the surface, and Fn, represented by the following formula (1), is 0.50 or more. Fn=(Cr-Crsol) / (C×Cr)...(1) (In formula (1), Cr and C represent the content of each element in mass%, and Crsol represents the content of Crsol in mass%).) <2> In mass%, C: 0.04-0.18%, Si: 0.03 to 0.35%, Mn: 0.40-2.20%, P: 0.050% or less, S: 0.001~0.050%, Cu: 0.01-0.40%, Cr: 0.50~1.40%, Ni: 0.01 to 0.40%, Al: 0.001 to 0.080%, V: 0.10 to 0.40%, and N: 0.0040 to 0.0250%, and further containing one or more elements selected from the group consisting of the following A group to C group, with the balance being Fe and impurities, (Group A) Mo: Less than 0.30% (Group B) Ca: 0.0050% or less, and Sn: 0.100% or less, one or two selected from the group consisting of (Group C) Ti: 0.050% or less, and Nb: 0.050% or less, one or two selected from the group consisting of The microstructure has a sum of the area ratios of bainite and martensite of less than 90% at a depth of 5 mm from the surface, A base material for nitrided parts, wherein the content by mass of Crsol, which is Cr in a solid solution state, is 0.45% or more at a position 5 mm deep from the surface, and Fn, represented by the following formula (1), is 0.50 or more. Fn=(Cr-Crsol) / (C×Cr)...(1) (In formula (1), Cr and C represent the content of each element in mass%, and Crsol represents the content of Crsol in mass%).) <3> It has a chemical composition containing the above-mentioned group A in mass %. <2> The base material for nitrided parts according to claim 1. <4> It has a chemical composition containing the above-mentioned B group in mass %. <2> The base material for nitrided parts according to claim 1. <5> It has a chemical composition containing the above C group in mass%. <2> The base material for nitrided parts according to claim 1. <6> Vickers hardness HV is 300 or less <1> ~ <5> 10. The base material for nitrided parts according to claim 9, <7> A component having a core portion that is deeper than 1.5 mm from the surface and a nitride layer that is present on the outside of the core portion, The core portion is <1> ~ <5> The chemical composition and the microstructure are as described in any one of the above. A nitrided part, in which the content by mass of Crsol, which is Cr in a solid solution state, is 0.40% or more at a position 5 mm deep from the surface, and Fn, represented by the following formula (1), is 1.00 or more. Fn=(Cr-Crsol) / (C×Cr)...(1) (In formula (1), Cr and C represent the content of each element in mass%, and Crsol represents the content of Crsol in mass%).) <8> <7> A method for manufacturing a nitrided component according to claim 1, comprising the steps of: <1> ~ <5> a steel bar having the chemical composition and the microstructure according to any one of the above items being forged into a steel bar; a low-temperature annealing step of holding the steel material at 500 to 630°C for 0.5 to 3.0 hours; a machining process in which the steel blank after the low-temperature annealing process is machined into a member having a part shape; a nitriding process for subjecting the member to a nitriding process at 550 to 620°C and at a temperature not higher than the low-temperature annealing temperature in the low-temperature annealing process +50°C for 1.0 to 10.0 hours; A method for producing a nitrided part, comprising: Effect of the Invention

[0011] The present disclosure provides a base material for nitrided parts, a nitrided part, and a method for manufacturing a nitrided part, which have sufficiently low hardness and excellent machinability during cutting, are suppressed in deformation of the part during nitriding, and can obtain high fatigue characteristics after nitriding. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic diagram of an Ono-type rotating bending fatigue test piece used in the bending fatigue test of the examples. [Diagram 2] FIG. 2 is a schematic diagram of a round bar test piece used in evaluating the amount of bending in the examples. [Diagram 3] FIG. 4 is a schematic diagram illustrating a method for measuring the amount of bending in the examples. [Figure 4] FIG. 2 is a diagram showing a part of an optical microscope photograph used to determine the area ratio of a metal structure in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment that is an example of the present disclosure will be described. In this disclosure, a numerical range expressed using "~" means a range that includes the numerical values ​​before and after "~" as the lower and upper limits. However, when a numerical value is followed by "more than" or "less than," it means a range that does not include the numerical value as the lower or upper limit. The content of an element in a chemical composition may be expressed by adding the "amount" to the element symbol (for example, C amount, Si amount, etc.). With respect to the contents of elements in chemical compositions, "%" means "mass %." When the content of an element in a chemical composition is described as "0~", it means that the element does not have to be contained. The term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.

[0014] One of the causes of bending and twisting deformation in parts with complex shapes is the residual stress introduced into the parts before nitriding. The inventors of the present disclosure created various distribution states of residual stress before nitriding and investigated the effects of these on bending deformation, and obtained the following findings. (a) Low-temperature annealing at a temperature above the nitriding temperature prior to nitriding reduces the amount of deformation during the subsequent nitriding. (b) If low-temperature annealing is performed at a temperature above the nitriding temperature before nitriding, the amount of hardening during nitriding is reduced, and fatigue properties are deteriorated. (c) The reason why the amount of hardening during nitriding is reduced by low-temperature annealing is that the alloying elements precipitate as alloy carbides or dissolve in cementite during low-temperature annealing, and therefore do not precipitate as alloy nitrides during the subsequent nitriding treatment. (d) In order to reduce the amount of deformation during nitriding without significantly deteriorating the fatigue properties after nitriding, it is necessary to optimize the amount of alloy components and the balance between C (carbon) and alloying elements, and to select optimal low-temperature annealing conditions to suppress the precipitation of alloy carbides and the concentration of alloying elements in cementite. (e) By controlling the dislocation density of the structure so as not to be too high, the generation of V carbides during low-temperature annealing can be suppressed. Therefore, the reduction in the amount of hardening during nitriding can also be suppressed. The invention according to the present disclosure has been completed based on the above findings.

[0015] [Materials for nitrided parts] (chemical composition) First, the chemical composition of the nitrided part material according to the present disclosure will be described. The chemical composition of the nitrided part preform according to the present disclosure and the chemical composition of the core of the nitrided part are the same as the chemical composition of the steel used as a raw material. In the following description, the nitrided part preform according to the present disclosure and the steel used in manufacturing the nitrided part may be referred to as the "steel in the present disclosure" or simply as the "steel". The steel material and the base material for nitrided parts in the present disclosure contain the following elements.

[0016] C: 0.04 to 0.18% Carbon (C) increases the core hardness of the steel material and increases the bending fatigue strength of the nitrided parts manufactured using the steel material as a raw material. If the C content is less than 0.04%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges disclosed herein. On the other hand, if the C content exceeds 0.18%, the alloy elements are excessively concentrated in cementite during low-temperature annealing, deteriorating fatigue properties. Also, machinability during machining is reduced. Therefore, the C content is 0.04 to 0.18%. The lower limit of the C content is preferably 0.05%, more preferably 0.06%, and further preferably 0.07%. The upper limit of the C content is preferably 0.17%, more preferably 0.16%, and further preferably 0.15%.

[0017] Silicon: 0.03 to 0.35% Silicon (Si) dissolves in the ferrite phase in pro-eutectoid ferrite and pearlite to increase the bending fatigue strength of the nitrided parts made of the steel material of the present disclosure. If the Si content is less than 0.03%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of the present disclosure. On the other hand, if the Si content exceeds 0.35%, the machinability of a steel preform made from the steel material decreases even if the contents of other elements are within the ranges of the present disclosure. Therefore, the Si content is 0.03 to 0.35%. The lower limit of the Si content is preferably 0.05%, more preferably 0.08%, and further preferably 0.10%. The upper limit of the Si content is preferably 0.32%, and more preferably 0.29%.

[0018] Mn: 0.40~2.20% Manganese (Mn) increases the core hardness of nitrided parts and improves fatigue strength. In nitriding, the fatigue strength is also improved by increasing the hardness of the nitrided layer through the formation of nitrides. Mn further combines with S to form MnS, improving the machinability of steel preforms made from steel. If the Mn content is less than 0.40%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges disclosed herein. On the other hand, if the Mn content exceeds 2.20%, even if the contents of other elements are within the ranges of the present disclosure, a compound layer of sufficient thickness cannot be obtained, and sliding properties and corrosion resistance may not be obtained. Therefore, the Mn content is 0.40 to 2.20%. The lower limit of the Mn content is preferably 0.45%, and more preferably 0.50%. The upper limit of the Mn content is preferably 2.00%, more preferably 1.80%, and further preferably 1.60%.

[0019] P:0.050% or less Phosphorus (P) is an element contained in steel as an impurity. If the P content exceeds 0.050%, the toughness of the steel deteriorates. Therefore, the P content is 0.050% or less. The P content may be as small as possible. The upper limit of the P content is preferably 0.045%, and more preferably 0.040%.

[0020] S: 0.001 to 0.050% Sulfur (S) combines with Mn to form MnS, which improves the machinability of steel preforms made from steel. If the S content is less than 0.001%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges disclosed herein. On the other hand, if the S content exceeds 0.050%, even if the contents of other elements are within the ranges of the present disclosure, coarse MnS will be formed. In this case, the bending fatigue strength of the nitrided part made of the steel preform will decrease. Therefore, the S content is 0.001 to 0.050%. The lower limit of the S content is preferably 0.005%, and more preferably 0.010%. The upper limit of the S content is preferably 0.045%, and more preferably 0.040%.

[0021] Cu: 0.01 to 0.40% Copper (Cu) dissolves in ferrite to increase the core hardness, thereby improving bending fatigue strength. If the Cu content is less than 0.01%, the above effect cannot be sufficiently obtained even if the contents of other elements are within the ranges of the present disclosure. On the other hand, if the Cu content exceeds 0.40%, even if the contents of other elements are within the ranges of the present disclosure, Cu may segregate at the grain boundaries of the steel material and cause hot cracks during the manufacturing process of the steel material or during the hot working process of the manufacturing process of the steel material using the steel material as a raw material. Therefore, the Cu content is 0.01 to 0.40%. The lower limit of the Cu content is preferably 0.03%, and more preferably 0.05%. The upper limit of the Cu content is preferably 0.35%, and more preferably 0.30%.

[0022] Cr: 0.50~1.40% Chromium (Cr) improves fatigue strength by forming nitrides and increasing the hardness of the nitrided layer. When low-temperature annealing is performed before nitriding, Cr is concentrated in cementite. Once concentrated in cementite, Cr no longer contributes to strengthening the nitrided layer. If the Cr content is less than 0.50%, the amount of strengthening during nitriding after low-temperature annealing is insufficient even if the contents of other elements are within the ranges disclosed in this disclosure. On the other hand, Cr forms nitrides to suppress the diffusion of nitrogen, so if the Cr content is high, the thickness of the hardened layer may become thin. If the Cr content exceeds 1.40%, even if the contents of other elements are within the ranges of the present disclosure, a nitrided layer of sufficient thickness may not be obtained, and fatigue properties may deteriorate. Therefore, the Cr content is 0.50 to 1.40%. The lower limit of the Cr content is preferably 0.55%, and more preferably 0.60%. The upper limit of the Cr content is preferably 1.35%, and more preferably 1.30%.

[0023] Ni: 0.01 to 0.40% Nickel (Ni) dissolves in ferrite to increase the core hardness, thereby improving bending fatigue strength. Ni also suppresses the occurrence of hot cracks caused by Cu when the steel material contains Cu. If the Ni content is less than 0.01%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges of the present disclosure. On the other hand, if the Ni content exceeds 0.40%, the above effects saturate and the manufacturing costs become high. Therefore, the Ni content is 0.40% or less. The lower limit of the Ni content is preferably 0.03%, and more preferably 0.05%. The upper limit of the Ni content is preferably 0.35%, and more preferably 0.30%.

[0024] Al: 0.001 to 0.080% Aluminum (Al) is used to deoxidize steel in the steelmaking process during the manufacturing process of steel material, and is also contained in the subsequent steel material. Al also has the effect of strengthening the nitride layer. If the Al content is less than 0.001%, the above effect cannot be sufficiently obtained. On the other hand, if the Al content exceeds 0.080%, there is a concern about nozzle clogging during casting, even if the contents of other elements are within the ranges of the present disclosure. Therefore, the Al content is 0.001 to 0.080%. The lower limit of the Al content is preferably 0.002%, more preferably 0.005%, and further preferably 0.010%. The lower limit of the Al content is preferably 0.070%, more preferably 0.060%, and further preferably 0.050%.

[0025] V: 0.10~0.40% Vanadium (V) improves fatigue strength by forming nitrides and increasing the hardness of the nitrided layer. When low-temperature annealing is performed before nitriding, V is concentrated in cementite. Once concentrated in cementite, V no longer contributes to strengthening the nitrided layer. If the V content is less than 0.10%, the amount of strengthening during nitriding after low-temperature annealing is insufficient even if the contents of other elements are within the ranges disclosed in this disclosure. On the other hand, V also precipitates as V carbide during low-temperature annealing. V carbide hardens the parent phase, so if the V content is too high, the machinability during machining deteriorates. In addition, V forms nitrides to suppress the diffusion of nitrogen, so if the V content is too high, the thickness of the hardened layer may become thin. If the V content exceeds 0.40%, sufficient machinability may not be obtained even if the contents of other elements are within the ranges of the present disclosure, and the fatigue properties may deteriorate due to the thin nitride layer. Therefore, the V content is 0.10 to 0.40%. The lower limit of the V content is preferably 0.11%, more preferably 0.13%, and further preferably 0.15%. The upper limit of the V content is preferably 0.35%, more preferably 0.30%, and further preferably 0.25%.

[0026] N: 0.0040~0.0250% Nitrogen (N) increases the core hardness of nitrided parts and improves fatigue strength. If the N content is less than 0.0040%, the above effects cannot be sufficiently obtained even if the contents of other elements are within the ranges disclosed herein. On the other hand, if the N content exceeds 0.0250%, even if the contents of other elements are within the ranges of the present disclosure, bubbles due to nitrogen gas may be generated in the nitrided component, which may reduce the bending fatigue strength. Therefore, the N content is 0.0040 to 0.0250%. The lower limit of the N content is preferably 0.0060%, and more preferably 0.0080%. The upper limit of the N content is preferably 0.0230%, and more preferably 0.0200%.

[0027] Remainder: Fe and impurities The balance of the chemical composition of the steel material in the present disclosure is composed of Fe and impurities. Here, the impurities in the chemical composition refer to those that are mixed in from raw materials such as ores, scraps, or the manufacturing environment when the steel material is industrially manufactured, and are not intentionally contained, but are allowed within a range that does not impair the effects of the nitrided part preform and nitrided part in the present disclosure. As an example, even if boron (B) is contained in an amount of 0.0005% or less as the upper limit, the properties of the steel are not significantly impaired, and the effects of the present invention can be obtained in the same manner.

[0028] <Optional Elements> The nitrided part preform according to the present disclosure may further contain, as an optional element, one or more elements selected from the group consisting of Group A, Group B, and Group C, in place of a portion of Fe. The optional elements will be described below.

[0029] In the present disclosure, in order to increase the bending fatigue strength of the steel, Mo may be further contained as an A group element in place of a portion of Fe.

[0030] (Group A) Mo: Less than 0.30% Molybdenum (Mo) is an optional element and may not be contained, that is, the Mo content may be 0%. When Mo is contained, that is, when the Mo content is more than 0%, Mo increases the core hardness and the hardness of the nitrided layer of the nitrided part, and increases the bending fatigue strength of the nitrided part. Even if even a small amount of Mo is contained, the above effects can be obtained to a certain extent. However, if the Mo content is 0.30% or more, the hardness during machining increases and the machinability deteriorates, so the Mo content is 0 to 0.30%. The lower limit of the Mo content is preferably more than 0%, more preferably 0.05%, and even more preferably 0.10%. The upper limit of the Mo content is preferably 0.25%, and more preferably 0.23%.

[0031] The chemical composition of the nitrided part preform according to the present disclosure may further contain one or two elements selected from Group B in place of a portion of Fe in order to improve the machinability of the steel.

[0032] (Group B) Ca: 0.0050% or less Sn: 0.100% or less

[0033] Ca: 0.0050% or less Calcium (Ca) is an optional element and may not be contained. In other words, the Ca content may be 0%. When Ca is contained, it improves the machinability of the steel material. However, if the Ca content is too high, coarse Ca oxides are generated, and the fatigue strength of the nitrided parts decreases. Therefore, the Ca content is 0 to 0.0050%. In order to stably obtain the above effects, the preferable lower limit of the Ca content is 0.0001%, and the preferable lower limit of the Ca content is 0.0003%.

[0034] Sn: 0.100% or less Tin (Sn) is an optional element and does not have to be contained. In other words, the Sn content may be 0%. When Sn is contained, that is, when the Sn content is more than 0%, Sn improves chip disposability during cutting processing, thereby improving the machinability of the steel material. If even a small amount of Sn is contained, the above effect can be obtained to a certain extent. However, if the Sn content exceeds 0.100%, the toughness of the steel material may deteriorate. Therefore, the Sn content is 0 to 0.100%. The lower limit of the Sn content is preferably 0.010%, and more preferably 0.020%.

[0035] The nitrided part preform according to the present disclosure may further contain one or two elements selected from the C group in place of a portion of Fe in order to increase the toughness of the steel.

[0036] (Group C) Ti: 0.050% or less Nb: 0.050% or less

[0037] Ti: 0.050% or less Titanium (Ti) is an optional element and may not be contained. In other words, the Ti content may be 0%. When Ti is contained, that is, when the Ti content is more than 0%, Ti refines the grain size and increases the toughness of the steel. If even a small amount of Ti is contained, the above effects can be obtained to some extent. However, if the Ti content exceeds 0.050%, coarse Ti carbonitrides are formed, which may deteriorate the fatigue properties. Therefore, the Ti content is 0 to 0.050%. The lower limit of the Ti content is preferably more than 0%, and more preferably 0.003%. The upper limit of the Ti content is preferably 0.030%, and more preferably 0.020%.

[0038] Nb: 0.05% or less Niobium (Nb) is an optional element and may not be contained. In other words, the Nb content may be 0%. When Nb is contained, that is, when the Nb content is more than 0%, Nb combines with C and N in the steel material in austenite to form carbonitrides, suppressing the coarsening of crystal grains during hot forging and homogenizing the structure. As a result, the variation in hardness after hot forging is reduced. However, if the Nb content is too high, the Nb carbonitrides become coarse and may deteriorate the fatigue properties. Therefore, the Nb content is 0 to 0.05%. The lower limit of the Nb content is preferably 0.005%, and more preferably 0.01%. The upper limit of the Nb content is preferably 0.04%, and more preferably 0.03%.

[0039] (Method of measuring chemical composition) The chemical composition of the steel material, the preform for nitrided parts, and the nitrided parts in the present disclosure can be measured by a known component analysis method in accordance with JIS G0321:2017. Specifically, chips are collected from the inside of the steel material to a depth of 1 mm or more from the surface using a drill. The collected chips are dissolved in acid to obtain a solution. An elemental analysis of the chemical composition is performed on the solution by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry). The C content and S content are determined by a known high-frequency combustion method (combustion-infrared absorption method). The N content is determined by a known inert gas fusion-thermal conductivity method.

[0040] The content of each element is determined by rounding off the measured value to the nearest digit based on the significant figures specified in this disclosure. For example, the C content of the steel material in this disclosure is determined to the second decimal place. Therefore, the C content is determined to the second decimal place by rounding off the measured value to the nearest digit.

[0041] Similarly, with respect to the contents of other elements than the C content of the nitrided part base material according to the present disclosure, the measured value is rounded off to the minimum digit specified in the present disclosure to obtain the content of that element.

[0042] In addition, rounding off means rounding down if the fraction is less than 5, and rounding up if the fraction is 5 or more.

[0043] Solute Cr content in nitrided part materials (Crsol content): 0.45% or more In order for Cr to form fine nitrides during nitriding and contribute to hardening of the nitrided layer, it must be in a solid solution state during nitriding. If low-temperature annealing is performed too much, the amount of dissolved Cr decreases, and sufficient fatigue properties cannot be obtained even if nitriding is performed. Specifically, the Crsol amount, which is the amount of dissolved Cr at a depth of 5 mm from the surface, must be 0.45% or more. The Crsol amount is preferably 0.50% or more, and more preferably 0.55% or more. The Crsol amount can be as high as possible. The amount of dissolved Cr (Crsol amount) in the preform for nitrided parts is measured by the method described in the examples below.

[0044] Fn in the base material for nitrided parts: 0.50 or more In the nitrided part preform according to the present disclosure, residual stresses introduced into the steel preform by forging or the like are released by low-temperature annealing in order to suppress deformation during nitriding. In the process of low-temperature annealing, Cr is concentrated in cementite. Therefore, the degree of progress of low-temperature annealing is expressed by the amount of Cr concentrated in cementite. Specifically, the degree of progress of low-temperature annealing needs to be such that Fn, expressed by the following formula (1), is 0.50 or more in the nitrided part preform. Fn=(Cr-Crsol) / (C×Cr)...(1) In formula (1), Cr and C represent the contents of each element, and Crsol represents the Crsol content at a position 5 mm deep from the surface. For example, if low-temperature annealing is not performed, the amount of dissolved Cr is approximately equal to the amount of contained Cr, and the value of Fn will be small. If a base material for nitrided parts with an Fn of 0.50 or more is nitrided under normal nitriding conditions, the Fn in the nitrided part will be 1.00 or more. The Fn at a depth of 5 mm of the nitrided part preform is preferably 0.55 or more, more preferably 0.60 or more, and even more preferably 0.65 or more. There is no particular upper limit for Fn, but if it exceeds 3.00, the amount of solute Cr is small, and there is concern about deterioration of fatigue properties. Therefore, Fn is preferably 3.00 or less, and more preferably 2.50 or less.

[0045] (microstructure) Area ratio of bainite + martensite at a depth of 5 mm from the surface: less than 90% The nitrided part preform according to the present disclosure is cut to form a part shape, and then nitrided to produce the nitrided part. Therefore, if the hardness of the steel preform (nitrided part preform) after low-temperature annealing is too high, the cost of cutting increases. In order to prevent the hardness after low-temperature annealing from being too high, it is necessary to control the content of alloying elements as well as the degree of quenching of the microstructure (metal structure). Specifically, bainite and martensite are hard in themselves, which deteriorates machinability, and also promote the nucleation of V carbides because they contain a large amount of dislocations. Therefore, in the nitrided part preform according to the present disclosure, the total ratio of bainite and martensite in the microstructure is limited. In order to have excellent machinability even after low-temperature annealing, the sum of the area ratios of bainite and martensite at a position 5 mm deep from the surface (sometimes referred to as the "5 mm deep position" in this disclosure) is set to less than 90%. The sum of the area ratios of bainite and martensite at a depth of 5 mm in the nitrided part preform is more preferably less than 80%, even more preferably less than 70%, and particularly preferably less than 50%. The area ratios of bainite and martensite may be as low as possible, even 0%. There are no particular limitations on the microstructures other than bainite and martensite, and examples include pearlite and ferrite.

[0046] The microstructure in the core of the nitrided part according to the present disclosure is similar to the microstructure at a depth of 5 mm in the preform for a nitrided part. The area ratios of bainite and martensite at a depth of 5 mm in the preform for nitrided parts and in the core of the nitrided parts are measured by the method described in the examples below.

[0047] (Hardness) The hardness of the nitrided part preform according to the present disclosure is not limited, but the higher the hardness, the lower the machinability. Therefore, it is preferable that the Vickers hardness HV is 300 or less. If the Vickers hardness HV is 300 or less, the preform has high machinability and the cost of machining the nitrided part preform into a part-shaped member can be kept low. From this viewpoint, the Vickers hardness of the nitrided part preform is more preferably 290 or less, further preferably 280 or less, and particularly preferably 270 or less. The Vickers hardness HV of the preform for nitrided parts is measured by the method described in the Examples below.

[0048] (shape) The shape of the nitrided part preform according to the present disclosure can be selected according to the application of the nitrided part obtained by cutting and nitriding the nitrided part preform. The nitrided part finally produced is not particularly limited, but examples thereof include gears, shaft parts, ring-shaped parts, pin-shaped parts, etc.

[0049] [Nitriding parts] The nitrided part according to the present disclosure comprises a nitrided layer formed on the surface and a core part located deeper than the nitrided layer, and the chemical composition of the core part is the same as the chemical composition of the steel material and the base material for nitrided parts according to the present disclosure described above. In this disclosure, the surface layer of a nitrided part means a region from the surface to a depth of 1.5 mm, and the core means a region deeper than 1.5 mm from the surface. The maximum depth of nitrogen that penetrates from the surface by nitriding is expected to be about 1.5 mm. In other words, the surface layer of a nitrided part here refers to a region into which nitrogen can penetrate, and the core refers to a region that cannot be penetrated by nitrogen by nitriding. The nitrided part according to this disclosure has a core that is a portion deeper than 1.5 mm from the surface, and a nitrided layer that exists on the outside (surface layer) of the core.

[0050] The chemical composition and microstructure in the core of the nitrided component according to the present disclosure are the same as the chemical composition and microstructure at a depth of 5 mm of the preform for nitrided components according to the present disclosure described above.

[0051] When steel is nitrided, a layer called a compound layer, mainly composed of iron nitride, is formed on the surface, and a layer called a diffusion layer, in which the matrix is ​​reinforced with solid-solution N or alloy nitride, is formed immediately below the compound layer. In the present disclosure, the nitride layer includes both the compound layer and the diffusion layer, and the N content of the compound layer is, for example, 2 to 11%, and the N content of the diffusion layer is, for example, 0.030 to 0.600%.

[0052] Solute Cr content in nitrided parts (Crsol content): 0.40% or more In order for Cr to form fine nitrides during nitriding and contribute to the hardening of the nitrided layer, it must be in a solid solution state during nitriding. The amount of Cr in a solid solution state during nitriding correlates with the amount of dissolved Cr in the unnitrided layer after nitriding. If a sufficient amount of Cr nitrides precipitates in the nitrided layer during nitriding, the amount of dissolved Cr in the unnitrided layer after nitriding will be 0.40% or more. Therefore, in order to obtain sufficient precipitation hardening in nitrided parts, the Crsol amount, which is the amount of dissolved Cr at a position 5 mm from the surface, must be 0.40% or more. The Crsol amount is preferably 0.45% or more, and more preferably 0.50% or more. The Crsol amount may be as high as possible.

[0053] Fn in nitrided parts: 1.00 or more The Fn of the nitrided component according to the present disclosure is 1.00 or more. If the effect of low-temperature annealing is sufficient, Fn will be high. From the viewpoint of suppressing distortion, the Fn of the nitrided component according to the present disclosure is preferably 1.3 or more, more preferably 1.5 or more, and even more preferably 1.7 or more. There is no particular upper limit to the Fn of the nitrided component according to the present disclosure, but a high Fn may reflect a state in which the hardening of the nitrided layer is insufficient. Therefore, Fn may be 5.0 or less, or may be 4.0 or less.

[0054] (Diffusion layer hardness) The hardness of the diffusion layer of the nitrided component according to the present disclosure is not particularly limited, while from the viewpoint of fatigue properties, the Vickers hardness HV of the diffusion layer of the nitrided component according to the present disclosure is preferably 450 HV or more, more preferably 500 HV or more, and even more preferably 550 HV or more. The Vickers hardness HV of the diffusion layer of the nitrided part is measured by the method described in the examples below.

[0055] (Application) The uses of the nitrided parts according to the present disclosure are not particularly limited, but because the nitriding treatment hardens the surface layer and increases the bending fatigue strength, the parts are suitable for use in, for example, gears, shaft parts, ring-shaped parts, pin-shaped parts, and the like.

[0056] [Steel manufacturing method] An example of a method for producing a steel material (steel material in the present disclosure) used in producing the nitrided part and the preform for nitrided parts according to the present disclosure includes the following steps. (Process 1) Material preparation process (Process 2) Hot processing process Each step will be described below.

[0057] (Process 1) Material preparation process In the material preparation step, a steel material according to the present disclosure is prepared. Specifically, molten steel satisfying the above-mentioned chemical composition is produced. The refining method is not particularly limited, and any known method may be used. For example, molten iron produced by a known method is subjected to refining (primary refining) in a converter. The molten steel tapped from the converter is subjected to known secondary refining. In the secondary refining, alloy elements are added to the molten steel to adjust the composition, and molten steel having the above-mentioned chemical composition is produced.

[0058] The molten steel produced by the above-mentioned refining method is used to produce a material by a well-known casting method. For example, the molten steel may be used to produce an ingot by an ingot casting method. Alternatively, the molten steel may be used to produce a bloom or billet by a continuous casting method. By the above-mentioned methods, a material (ingot, bloom, or billet) is produced.

[0059] (Process 2) Hot processing process The produced material is then hot worked to produce steel. In the hot working step, usually, one or more hot working steps are performed. When multiple hot working steps are performed, the first hot working step is, for example, rolling using blooming or hot forging, and the subsequent hot working steps may be rolling using a continuous rolling mill. The continuous rolling mill includes multiple rolling stands arranged in a line. The steel material after hot working is cooled to room temperature. A billet is produced by rough rolling and rolling using a continuous rolling mill, and then the billet is reheated and further subjected to finish rolling using a continuous rolling mill to produce a steel material of a desired size. Alternatively, the steel material may be produced from the material only by hot forging. The heating temperature of the material during hot working is not particularly limited, but is, for example, 1100 to 1300°C.

[0060] Through the above steps, a steel material for producing the nitrided part preform according to the present disclosure is produced.

[0061] [Manufacturing method of base material for nitrided parts] An example of a method for producing a nitrided component preform according to the present disclosure includes the following steps. (Process 3) Steel material forming process (Step 4) Low-temperature annealing step

[0062] (Process 3) Steel material forming process In the steel blank forming process, the steel material having the above-mentioned chemical composition is formed into a steel blank by, for example, hot forging. Specifically, first, the steel material is heated. The heating temperature is, for example, 1000 to 1300°C. If the heating temperature is too high, the sum of the area ratios of bainite and martensite will not be less than 90%, and if the heating temperature is too low, the die life will be reduced, resulting in increased manufacturing costs. In order to make the sum of the area ratios of bainite and martensite less than 90%, it is preferable to set the heating temperature before forging to 1300°C or less. In addition, it is preferable to set the forming completion temperature to 1100°C or less. The heated steel material is hot forged and formed into a steel preform having a predetermined shape corresponding to the nitrided part to be finally manufactured. The formed steel preform is air-cooled. In order to make the sum of the area ratios of bainite and martensite less than 90%, it is preferable to cool the steel preform to room temperature by air cooling after forming. The cooling rate during air cooling may be appropriately adjusted using a fan as long as the sum of the area ratios of bainite and martensite is less than 90%. If the cooling after forming is too fast, the sum of the area ratios of bainite and martensite will be 90% or more, and if the cooling after forming is too slow, the manufacturing cycle time will be long and productivity will deteriorate. In order to make the sum of the area ratios of bainite and martensite less than 90%, it is preferable to set the average cooling rate in the temperature range from 900°C to 500°C during cooling after forming to a range of 0.2 to 3.0°C / s.

[0063] (Step 4) Low-temperature annealing step The hot forged steel blank is subjected to low temperature annealing in order to remove residual stress introduced after forging. In order to release the residual stress before nitriding while not deteriorating the fatigue strength after nitriding, it is necessary to appropriately select the low-temperature annealing conditions. If the low-temperature annealing temperature is too low, Cr is not concentrated enough in the cementite, resulting in an insufficient amount of Fn, which means that the residual stress is not sufficiently released and deformation during nitriding cannot be suppressed. On the other hand, if the low-temperature annealing temperature is too high, Cr is excessively concentrated in the cementite, which reduces the amount of solid-solubilized Cr too much, which reduces the amount of hardening during nitriding and deteriorates the fatigue properties. From this perspective, the low-temperature annealing temperature is 500 to 630°C, and the low-temperature annealing time is 0.5 to 3.0 hours.

[0064] By the above-mentioned manufacturing process, the nitrided part base material according to the present disclosure can be manufactured.

[0065] [Manufacturing method for nitrided parts] An example of a method for manufacturing a nitrided part according to the present disclosure using the above-mentioned nitrided part base material includes the following steps. (Process 5) Machining process (Step 6) Nitriding process Each step will be described below.

[0066] (Process 5) Machining process In the machining process, machining is performed on the nitrided part preform to shape the nitrided part preform into a component having a shape close to that of the final product. Specifically, cutting and / or grinding is performed to shape the nitrided part preform into a component having the part shape.

[0067] (Step 6) Nitriding process In the nitriding process, the member after the machining process is subjected to nitriding. The nitriding process may be, for example, gas nitriding, gas soft nitriding, salt bath soft nitriding, plasma nitriding, etc. The gas used in the nitriding process is NH 3 It may be only NH 3 In addition, N 2 , H 2 , CO 2 Alternatively, the gas may be a mixed gas containing various hydrocarbons. In order to provide the nitrided parts with high fatigue strength, the nitriding conditions must be appropriately selected. If the nitriding temperature is too low, the hardened layer will not be sufficiently formed, and the fatigue properties will not improve. If the nitriding temperature is too high compared to the temperature of the immediately preceding low-temperature annealing, the residual stress that was not released during the low-temperature annealing will be released, and bending during nitriding cannot be suppressed. In addition, if the nitriding temperature is too high, the alloy nitrides may become coarse and the hardness of the diffusion layer may decrease. From this perspective, the nitriding temperature is 550 to 620°C, and is not more than the low-temperature annealing temperature +50°C, and the nitriding time is 1.0 to 10.0 hours. The cooling method after nitriding may be water cooling, oil cooling, or furnace cooling.

[0068] The nitrided component according to the present disclosure can be manufactured by the above manufacturing process. EXAMPLES

[0069] The preform for nitrided parts, the nitrided parts, and the manufacturing method for nitrided parts according to the present disclosure will be described in more detail with reference to examples. Note that the conditions in the following examples are examples of conditions adopted to confirm the feasibility and effectiveness of the preform for nitrided parts, the nitrided parts, and the manufacturing method for nitrided parts according to the present disclosure. Therefore, the preform for nitrided parts, the nitrided parts, and the manufacturing method for nitrided parts according to the present disclosure are not limited to the following examples.

[0070] [Steel manufacturing] Steel materials A to U having the chemical compositions (unit: mass%, balance: Fe and impurities) shown in Table 1 were produced by the following method. The underlined parts indicate that they are outside the scope of the present disclosure. In addition, "<0.01" for Mo indicates that it was not intentionally added. A 50 kg ingot was produced using a vacuum melting furnace. The ingot was heated to 1250°C and then hot worked to produce a steel material. Specifically, the ingot was hot forged into a steel bar having a cross section perpendicular to the axial direction of 60 mm x 60 mm. Next, the steel bar was heated again to 1250°C, and then hot forged into a steel bar having a cross section of 40 mm in diameter, and then allowed to cool to room temperature. Through the above manufacturing process, a steel material (steel bar) was manufactured.

[0071] [Table 1]

[0072] [Manufacturing of steel materials] Using each of the produced steel materials as a starting material, steel preforms having each test number were produced by the following method.

[0073] In order to simulate the steel preform forming process in the above-mentioned process 3, the steel was held at 1150°C, which is close to the finishing temperature of forging, for 60 minutes, and then cooled in the air to obtain the steel preform. In order to simulate the cooling rate of a general medium-sized nitrided part, a hot forging simulation process was performed in which the steel preform was cooled to room temperature while blowing air with a fan. The surface temperature of the steel preform during cooling was measured using a radiation thermometer. Except for test number 20 (steel T), the average cooling rate was about 1.5°C / sec, calculated by dividing the time required to cool the temperature in the range of 900 to 500°C by the temperature range of the range. For test number 20 (steel T), the fan was turned up to a high volume to cool the steel, and the average cooling rate was 3.2°C / sec, in order to evaluate the influence of the metal structure. In the hot forging simulation process here, no deformation processing was performed on the actual steel (bar steel), but the influence of the presence or absence of deformation processing on the microstructure, etc. is minor.

[0074] The steel preforms (with some exceptions) after the simulated hot forging process were subjected to low-temperature annealing treatment in which they were held at 400 to 700°C for 1.0 to 4.0 hours and then cooled to room temperature. Through the above manufacturing process, a steel preform simulating a preform for nitrided parts was manufactured.

[0075] [evaluation] The following evaluation tests (Tests 1 to 7) were carried out on the produced steel preforms having each test number. (Test 1) Microstructural observation of steel material (Test 2) Machinability evaluation of steel materials (Test 3) Measurement of Cr solid solution amount in steel materials (Test 4) Evaluation of bending fatigue strength after nitriding (Test 5) Evaluation of bending measurement during nitriding (Test 6) Measurement of Cr solid solution amount in nitrided parts (Test 7) ​​Measurement of diffusion layer hardness of nitrided parts

[0076] (Test 1) Microstructural observation of steel material Block-shaped test pieces for microstructure observation were cut out from a cross section perpendicular to the longitudinal direction of the steel blank of each test number so that the center of the test surface was 5 mm deep from the surface, embedded in resin, and mirror-polished. The polished surface was etched with nital, and four fields of view of 0.74 mm x 0.55 mm were photographed for each test number at 200x magnification using an optical microscope. The area ratio of each metal structure was calculated from the photographs using the point counting method, and the average of the area ratios obtained from the four optical microscope images was regarded as the area ratio of the metal structure for that test number.

[0077] FIG. 4 is a part of an optical microscope photograph of Steel J (Test No. 10) used to determine the area ratio of the metal structure. The white parts are ferrite, the gray parts are bainite, and the parts that are partly gray and mostly black are pearlite. It may be difficult to determine whether a structure containing carbides is pearlite or bainite. In this disclosure, pearlite and bainite show different contrasts in optical microscope images after etching with nital, and therefore what is etched darkly is pearlite and what is etched lightly is bainite. When it was difficult to judge based on contrast alone, the corresponding measurement point was excluded from the calculation of the area ratio.

[0078] (Test 2) Machinability evaluation of steel materials The Vickers hardness of the microstructure observation test pieces of each test number was measured. Vickers hardness tests were conducted in five random locations on the mirror-polished surface in accordance with JIS Z 2244:2009. The test force was 9.8 N. The arithmetic mean value of the five hardness values ​​obtained was defined as the Vickers hardness of the test number. It was determined that sufficient machinability was obtained when the Vickers hardness was 300 HV or less.

[0079] (Test 3) Measurement of Cr solid solution amount in steel materials A test piece for electrolytic analysis with a diameter of 10 mm and a length of 40 mm was prepared from the center position (R / 2 position) of the radius (R) of the cross section perpendicular to the axial direction of each steel blank (40 mm diameter steel bar) of each test number. The test piece was electrolytically analyzed in a 10% acetylacetone-1% tetramethylammonium chloride-methanol electrolyte at a current density of 20 mA / cm. 2 The electrolysis was performed at 600° C., and the solution after electrolysis was suction filtered through a Crypore filter with a mesh size of 0.2 μm. The amount of Cr in the obtained residue was analyzed using an inductively coupled plasma optical emission spectrometer. The value obtained by subtracting the amount of Cr from the amount of Cr contained was regarded as the amount of Cr dissolved in the steel material.

[0080] (Test 4) Evaluation of bending fatigue strength after nitriding An Ono-type rotating bending fatigue test specimen, as shown in Figure 1, was prepared from the radial center position (R / 2 position) of the cross section perpendicular to the axial direction of the steel blank (40 mm diameter steel bar) with each test number. The numbers in Figure 1 indicate dimensions (unit: mm). "φ" in Figure 1 means diameter. "R1" means that the radius of curvature at the notch bottom is 1 mm.

[0081] Specifically, the steel blanks of each test number were machined (cut) to produce intermediate pieces for the Ono-type rotating bending fatigue test specimens. The intermediate pieces were then subjected to a nitriding treatment to produce the Ono-type rotating bending fatigue test specimens shown in Figure 1. The nitriding treatment conditions were as follows: In the nitriding process, the intermediate product was held at 580°C for 2 hours in an atmosphere of 1:1 RX gas (endothermic conversion gas) and ammonia gas. After holding, the intermediate product was oil-cooled. Through the above process, an Ono-type rotating bending fatigue test specimen simulating a nitrided part was produced.

[0082] Ono-type rotating bending fatigue tests were conducted using Ono-type rotating bending fatigue test pieces with each test number. Multiple Ono-type rotating bending fatigue test pieces were prepared for each test number. Fatigue tests were conducted by changing the stress applied to each test piece, and the fatigue test was conducted for 10 million cycles (10 7The highest stress at which the material did not break after repeated cycles of 1000 times was taken as the bending fatigue strength (MPa). In the Ono-type rotating bending fatigue test, the rotation speed was 3000 rpm and the stress ratio was reversed. The obtained bending fatigue strength is shown in the "Bending fatigue strength (MPa)" column in the "Nitrided parts" section of Table 2. It was determined that a fatigue strength of 500 MPa or more was sufficient.

[0083] (Test 5) Evaluation of bending measurement during nitriding A φ15 × 100 mm test piece for bending measurement, shown in Figure 2, was prepared from the radial center position (R / 2 position) of the cross section perpendicular to the axial direction of the steel blank (40 mm diameter steel bar) of each test number. The test piece was subjected to nitriding treatment by holding it at 580°C for 2 hours in an atmosphere of 1:1 RX gas and ammonia gas, and then oil quenching. The amount of bending of the test piece after nitriding was measured by a contact-type three-dimensional measuring machine. Specifically, as shown in Figure 3, a reference circle was obtained from the cross section at three locations, 10 mm from both ends of the test piece and at the midpoint in the longitudinal direction, and the center of the reference circle was obtained. The distance between the line (A1) connecting the center coordinates of the reference circle at the 10 mm position from both ends and the center coordinate (A0) of the reference circle at the midpoint in the longitudinal direction was considered to be the amount of bending. The method of obtaining the reference circle is described below. At the position where the reference circle was to be obtained, the coordinates of eight points were measured at 45° intervals around the circumference. The coordinates of each of the eight points were used to approximate a perfect circle and the reference circle at that position was considered to be a sufficient amount of bending. When the amount of bending was 4.0 μm or less, it was considered that bending was sufficiently suppressed.

[0084] (Test 6) Measurement of Cr solid solution amount in nitrided parts A test piece for electrolytic analysis with a diameter of 10 mm and a length of 40 mm was prepared from the center of each bending test piece. The test piece was electrolytically analyzed in a 10% acetylacetone-1% tetramethylammonium chloride-methanol electrolyte at a current density of 20 mA / cm. 2 The solution after electrolysis was suction filtered through a Crypore filter with a mesh size of 0.2 μm, and the amount of Cr in the resulting residue was analyzed using a high-frequency inductively coupled plasma optical emission spectrometer. The value obtained by subtracting this amount of Cr from the amount of Cr contained was regarded as the amount of dissolved Cr in the nitrided parts.

[0085] (Test 7) ​​Measurement of diffusion layer hardness of nitrided parts The hardness of the diffusion layer was measured using a part of the Ono-type rotating bending fatigue test piece used in Test 4. The φ10 mm parallel part of the test piece was cut perpendicular to the longitudinal direction at a position 2 mm from the edge of the R1 notch, embedded in resin so that the cut surface could be observed, and then mirror-polished. Vickers hardness tests were performed in accordance with JIS Z 2244:2009 at five random locations 0.05 mm deep from the outermost surface. The test force was 2.94 N. The arithmetic mean value of the five hardness values ​​obtained was defined as the Vickers hardness of the diffusion layer of the test number. If the Vickers hardness was 450 HV or more, it was determined that the diffusion layer hardness was sufficiently high.

[0086] The heat treatment conditions after the hot forging simulation treatment and the evaluation results of Tests 2 to 7 are shown in Table 2. In Table 2, underlines indicate that the results are outside the scope of the present disclosure or that the evaluation results are insufficient. Note that since nitriding was performed at 630°C or less, the microstructure in the core of the steel preform (nitrided part) after nitriding is similar to the microstructure of the steel preform. The remainder of the microstructure is ferrite and / or pearlite.

[0087] [Table 2]

[0088] In test numbers 1 to 13 which met the requirements of the present disclosure, the steel preform had a hardness HV of 300 or less and excellent machinability, and the nitrided parts had a bending fatigue strength of 500 MPa or more and a bending amount of 4.0 μm or less. Test No. 15 had an insufficient C content and thus had insufficient bending fatigue strength. Test No. 16 had an excessively high C content, and was therefore inferior in machinability and insufficient in bending fatigue strength. In test number 17, the Cr content and the amount of dissolved Cr were too small, and the bending fatigue strength was insufficient. Test No. 18 had an insufficient V content and thus had insufficient bending fatigue strength. Test No. 19 had an excessively high V content and was poor in machinability. Test No. 20 had an excessively large total area ratio of bainite and martensite, and was poor in machinability. Test No. 21 had an excessively large Mo amount and an excessively large total area ratio of bainite and martensite, and was therefore inferior in machinability. In test numbers 22 and 23, the low-temperature annealing was insufficient, resulting in an insufficient Fn and a large amount of bending. In test number 24, the low-temperature annealing temperature was too high, resulting in an insufficient amount of dissolved Cr, and the bending fatigue strength was insufficient. In test numbers 25 and 26, the low-temperature annealing was insufficient, resulting in an insufficient Fn and a large amount of bending. In test number 27, the low-temperature annealing temperature was too high, resulting in an insufficient amount of dissolved Cr, and the bending fatigue strength was insufficient. Test No. 28 satisfied the requirements of the present disclosure as a steel preform, but the nitriding temperature was too high, resulting in an insufficient amount of dissolved Cr in the nitrided part, and the bending fatigue strength was insufficient.

Claims

1. In mass percent, C: 0.04-0.18%, Si: 0.03-0.35%, Mn: 0.40-2.20%, P: 0.050% or less, S: 0.001-0.050%, Cu: 0.01-0.40%, Cr: 0.50-1.40%, Ni: 0.01 to 0.40%, Al: 0.001-0.080%, V: 0.10 to 0.40%, and N: 0.0040 to 0.0250%, with the balance being Fe and impurities; The microstructure has a sum of the area ratios of bainite and martensite of less than 90% at a depth of 5 mm from the surface, A base material for nitrided parts, wherein the content by mass of Crsol, which is Cr in a solid solution state, is 0.45% or more at a position 5 mm deep from the surface, and Fn, which is represented by the following formula (1), is 0.50 or more. Fn=(Cr-Crsol) / (C×Cr)...(1) (In formula (1), Cr and C represent the content of each element in mass%, and Crsol represents the content of Crsol in mass%).

2. In mass percent, C: 0.04-0.18%, Si: 0.03-0.35%, Mn: 0.40-2.20%, P: 0.050% or less, S: 0.001-0.050%, Cu: 0.01-0.40%, Cr: 0.50-1.40%, Ni: 0.01 to 0.40%, Al: 0.001-0.080%, V: 0.10 to 0.40%, and N: 0.0040 to 0.0250%, and further containing one or more elements selected from the group consisting of the following A group to C group, with the balance being Fe and impurities; (Group A) Mo: less than 0.30% (Group B) Ca: 0.0050% or less, and Sn: 0.100% or less, one or two selected from the group consisting of (Group C) Ti: 0.050% or less, and Nb: 0.050% or less, one or two selected from the group consisting of The microstructure has a sum of the area ratios of bainite and martensite of less than 90% at a depth of 5 mm from the surface, A base material for nitrided parts, wherein the content by mass of Crsol, which is Cr in a solid solution state, is 0.45% or more at a position 5 mm deep from the surface, and Fn, which is represented by the following formula (1), is 0.50 or more. Fn=(Cr-Crsol) / (C×Cr)...(1) (In formula (1), Cr and C represent the contents of each element in mass%, and Crsol represents the content of Crsol in mass%).

3. 3. The preform for nitrided parts according to claim 2, having a chemical composition containing, in mass %, said Group A elements.

4. 3. The preform for nitrided parts according to claim 2, having a chemical composition containing, in mass %, the B group.

5. 3. The preform for nitrided parts according to claim 2, having a chemical composition containing, in mass %, the C group.

6. 3. The preform for nitrided parts according to claim 1 or 2, which has a Vickers hardness HV of 300 or less.

7. A component having a core portion that is a portion deeper than 1.5 mm from a surface and a nitride layer that is present on the outside of the core portion, The core portion has the chemical composition and the microstructure according to any one of claims 1 to 5, A nitrided component, in which the content by mass of Crsol, which is Cr in a solid solution state, is 0.40% or more at a position 5 mm deep from the surface, and Fn, represented by the following formula (1), is 1.00 or more. Fn=(Cr-Crsol) / (C×Cr)...(1) (In formula (1), Cr and C represent the contents of each element, and Crsol represents the content of Crsol.)

8. A method for manufacturing a nitrided component according to claim 7, comprising the steps of: a steel bar having the chemical composition and the microstructure according to any one of claims 1 to 5, being forged into a steel bar; a low-temperature annealing step of holding the steel blank at 500 to 630°C for 0.5 to 3.0 hours; a machining process in which the steel blank after the low-temperature annealing process is machined into a member having a part shape; a nitriding process for performing a nitriding process on the member at a temperature of 550 to 620°C and at a temperature equal to or lower than the low-temperature annealing temperature in the low-temperature annealing process + 50°C for 1.0 to 10.0 hours; A method for producing a nitrided part, comprising:

Citation Information

Patent Citations

  • Production of nitrided steel member small in heat treating strain

    JP1996049059A

Cited By

  • Steel material

    WO2026164171A1