Method for preparing catalysts based on MFI-type zeolites with improved density and mechanical strength

JP2024500631A5Pending Publication Date: 2024-11-14IFP ENERGIES NOUVELLES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023530748
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-23
Filing Date
2021-11-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing catalysts face a trade-off between high zeolite content for high catalytic performance and binder content for mechanical strength, leading to brittleness or limited catalytic performance.

Method used

A method involving mixing MFI type zeolite with a binder, using peptizers and neutralizing agents, shaping by extrusion, and heat treatment in the presence of water vapor to create catalysts with optimized porosity and mechanical strength, allowing high zeolite content without compromising mechanical integrity.

Benefits of technology

The method results in catalysts with improved mechanical strength and controlled porosity, suitable for various hydrocarbon conversion processes, maintaining high zeolite content and enhancing catalytic performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a unique process for the preparation of a catalyst in the form of extrudates, comprising an acidic zeolite having an MFI structure code and a zeolite content between 45% and 90% relative to the total mass of the catalyst, and a binder, and optionally containing a hydrogenation active phase, said process comprising at least the steps: a) mixing the MFI zeolite with the binder, the average size of the elementary particles of the MFI zeolite being between 110 and 800 nm, b) adding a deflocculating agent to the mixture obtained in step a), c) adding a neutralizing agent to the mixture, d) forming a mixture by extrusion, e) optionally drying the solid, f) heat treating the solid obtained in the presence of water vapor at a temperature between 400 and 1000° C. in the presence of an air stream containing 1 to 60% by volume of water, g) optionally introducing on the solid one or more precursors of the hydrogenation active phase, at a temperature between 400 and 1000° C., in the presence of an air stream containing 1 to 60% by volume of water, at a temperature between 400 and 1000° C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention provides a unique method for preparing a catalyst based on an acidic MFI type zeolite (preferably H-ZSM-5) in the form of extrudates incorporated at a high content by a binder containing alumina, possibly containing a hydrogenation active phase. The catalyst of this type obtained can be used for many heterogeneous catalytic applications requiring acid functions, in particular for the conversion of hydrocarbons: Methanol conversion (to olefins, gasoline, etc.), olefin conversion (to olefins, gasoline, diesel, etc.), various processes for converting paraffins to aromatics, alkylation processes, dewaxing processes for diesel, oil, plastic pyrolysis, biomass pyrolysis, etc. [Background technology]

[0002] US Pat. No. 5,999,333 claims solid ZSM-5 and a method for its preparation.

[0003] US Pat. Nos. 5,993,333 and 5,293,623 disclose catalysts based inter alia on ZSM-5 zeolite having a zeolitic primary crystal structure and further having a specific aggregate size of the primary crystals of the zeolite.

[0004] US Pat. No. 5,399,633 discloses a catalyst based on a zeolite / binder matrix having improved attrition resistance.

[0005] US Pat. No. 5,399,633 discloses a method for preparing a hydrocracking catalyst containing ZSM-5 zeolite, a binder, and a hydrogenation phase.

[0006] Patent Document 6 discloses a catalyst for producing propylene by catalytic cracking, which contains ZSM-5 zeolite, a binder, and an element of the rare earth group.

[0007] US Pat. No. 5,399,633 discloses a process for producing olefins from alcohols using steam-treated ZSM-5 type zeolites.

[0008] To ensure high catalytic performance, it is often necessary to achieve a high zeolite content. The role of the binder in shaped zeolite catalysts is to ensure the cohesion of the units and therefore allow sufficient mechanical strength for catalytic use.

[0009] Therefore, a high content of zeolitic phases may lead to a weakening of the unit, and a high content of binder to ensure good mechanical strength may limit the catalytic performance. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] U.S. Pat. No. 3,702,886 [Patent Document 2] U.S. Pat. No. 5,063,187 [Patent Document 3] U.S. Patent No. 7,229,941 [Patent Document 4] U.S. Pat. No. 4,206,085 [Patent Document 5] US Patent Application Publication No. 2019 / 0247837 [Patent Document 6] Chinese Patent No. 106608779 [Patent Document 7] U.S. Pat. No. 4,788,377 Summary of the Invention [Means for solving the problem]

[0011] (Subject of the Invention) The present invention provides a unique process for the preparation of a catalyst in the form of extrudates comprising an acidic MFI type zeolite, preferably H-ZSM-5, and a binder, preferably alumina, with a zeolite content between 45% and 90% relative to the total mass of the catalyst, and optionally containing a hydrogenation active phase, said process comprising at least the following steps: a) mixing the MFI zeolite with a binder; the average size of the elementary particles of the MFI zeolite is 110-800 nm, preferably 120-700 nm, and highly preferably 150-500 nm, as measured by scanning electron microscopy; b) adding to the mixture obtained in step a) a deflocculating agent selected from nitric acid and a carboxylic acid selected from acetic acid, citric acid and butyric acid, either alone or in mixture; c) adding to the mixture obtained in step b) a neutralizing agent selected from an inorganic base selected from sodium hydroxide, potassium hydroxide, and ammonia, either alone or as a mixture, and an organic base in solution selected from an amine and a quaternary ammonium compound, either alone or as a mixture, d) shaping the mixture obtained in step c) by extrusion to obtain a solid; e) optionally drying the solid obtained in step d), f) heat treating the solid obtained in step d) or e) in the presence of water vapor at a temperature between 400° C. and 1000° C. in the presence of a stream of air containing 1% to 60% by volume of water, g) Optionally, introducing one or more precursors of a hydrogenation active phase into the solid obtained in step f).

[0012] The proposed preparation scheme allows to obtain catalysts with porosity different from that of the prior art, by combining in a unique way the various steps of the preparation of the support / catalyst. In particular, despite the high content of zeolite introduced, the method for preparing said catalyst allows to obtain an optimized pore volume (minimization of macroporosity and control of mesopore distribution) and to obtain a high zeolite volume content (i.e. density (kg / m)) in the reactor. 3 )) can be finely adjusted. The volumetric content of zeolite in the reactor is defined as the product of the TPD (tapped packing density) of the catalyst and the mass content of zeolite in the catalyst. Furthermore, the process according to the invention makes it possible to improve the mechanical properties, which are of great importance for supports with a high zeolite content.

[0013] This type of catalyst obtained according to the invention can be used for many heterogeneous catalytic applications requiring acid functionality, in particular for the conversion of hydrocarbons: conversion of methanol (to olefins, gasoline, etc.), conversion of olefins (to olefins, gasoline, diesel, etc.), conversion of paraffins to aromatics, alkylation processes, processes for dewaxing of diesel, oil, plastic pyrolysis, biomass pyrolysis products, etc.

[0014] (Terminology and Characterization Techniques) The catalysts and supports of the present invention have a particular pore distribution, the macropore and mesopore volumes being measured by mercury intrusion and the micropore volume by nitrogen adsorption.

[0015] The term "macropores" is understood to mean pores with an opening greater than 50 nm.

[0016] The term "mesopores" is understood to mean pores with openings in the range of 2 nm to 50 nm.

[0017] The term "micropores" is understood to mean pores with an opening of less than 2 nm.

[0018] In the following description of the invention, specific surface area is understood to mean the BET specific surface area determined by nitrogen adsorption according to standard ASTM D 3663-78 based on the Brunauer-Emmett-Teller method described in the journal "Journal of the American Society", 60, 309, (1938).

[0019] The macropore and mesopore volumes are measured by mercury intrusion porosimetry according to standard ASTM D4284-83, at a maximum pressure of 4000 bar (400 MPa), using a surface tension of 484 dyne / cm and a contact angle of 140°. The wetting angle used was considered equal to 140°, following the recommendation of the publication “Techniques de l'ingenieur, traite analyse et caracterisation” [Engineer's Techniques, Analysis and Characterisation Treatises], pp. 1050-5, authors Jean Charpin and Bernard Rasneur.

[0020] The value above which mercury fills all intergranular voids is set to 0.2 MPa, and it is believed that mercury penetrates into the pores of the sample above this value.

[0021] The macropore volume of a catalyst or support is defined as the cumulative volume of mercury introduced at a pressure between 0.2 MPa and 30 MPa, which corresponds to the volume contained in pores having an apparent diameter of more than 50 nm.

[0022] The mesopore volume of a catalyst or support is defined as the cumulative volume of mercury introduced at a pressure between 30 MPa and 400 MPa, and corresponds to the volume contained in pores having an apparent diameter between 3.6 nm and 50 nm.

[0023] The micropore volume is measured by nitrogen porosimetry. The quantitative analysis of the microporosity is carried out by the "t" method (Lippens-De Boer, 1965). This corresponds to the transformation of the onset adsorption isotherm, as described in the publication "Adsorption by powders and porous solids. Principles, methodology and applications", authors F. Rouquerol, J. Rouquerol, and K. Sing, Academic Press, 1999.

[0024] In the following description of the invention, the "total pore volume" of an alumina or support or catalyst is understood to mean the sum of the volumes of mesopores, macropores (measured by mercury intrusion porosimetry) and micropores (measured by nitrogen porosimetry).

[0025] The mechanical strength of the material according to the invention is determined by the single-pellet crush strength (SPCS) test. This is a standardized test (standard ASTM D4179-01) and consists in applying a compressive force at break to the material in the form of millimeter-sized units, for example beads, pellets or extrudates. The analysis is repeated on a given number of solids taken individually, typically a number between 10 and 200 solids. The average of the measured break side forces constitutes the average SPCS, which is expressed in units of force (N) in the case of granules and in units of force per unit length (daN / mm or decanewtons per millimeter of extrudate length) in the case of extrudates.

[0026] Loss on ignition (LOI) of a solid is the relative mass loss (expressed in %) of a solid after being heated to 1000° C. for 3 hours in a muffle furnace.

[0027] Tapped Packing Density (TPD) is defined as the bulk density of a sample after tapping. It is measured as follows: a given weight of carrier or mass is introduced into a graduated cylinder, which holds the aggregates in a given volume. The cylinder is then vibrated until all settling has ceased and a constant volume has been reached. The weight of the aggregates occupying a unit volume is then calculated. Tapped Packing Density (TPD) is determined according to standard NF EN ISO 787-11.

[0028] (Explanation of SEM for particle size measurement) The size of the zeolite particles is measured by scanning electron microscopy at a magnification of 10,000 to 100,000 on a Zeiss Supra 40 instrument. The equivalent diameter is calculated by any method known to those skilled in the art for a number of units greater than 200. Agglomerates are not taken into account, since the units are clearly separated from one another. The average size of the elementary zeolite particles is then calculated as the arithmetic mean of the measured equivalent diameters of each unit. The average size of the elementary particles is the number average size.

[0029] In the following text, the groups of chemical elements are given according to the CAS classification (CRC Handbook of Chemistry and Physics, published by CRC Press, editor in chief DR Lide, 81st edition, 2000-2001). For example, group VIII according to the CAS classification corresponds to the metals in columns 8, 9 and 10 according to the new IUPAC classification.

[0030] For the purposes of the present invention, the various embodiments presented may be used alone or in combination with one another, without any limitations on their combinations, where this is technically possible.

[0031] For purposes of the present invention, various ranges of parameters for a given process, such as pressure ranges and temperature ranges, may be employed alone or in combination, e.g., for purposes of the present invention, a preferred range of pressure values ​​may be combined with a more preferred range of temperature values. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] Detailed Description of the Invention The present invention provides an original method for preparing a catalyst in the form of extrudates comprising an acidic MFI type zeolite, preferably H-ZSM-5, and a binder, preferably alumina, the zeolite content being between 45% and 90% relative to the total mass of the catalyst, and optionally comprising a hydrogenation active phase.

[0033] (Catalyst Preparation) According to the invention, the catalyst comprises at least one MFI type zeolite and a binder.

[0034] According to step a), the MFI zeolite is mixed with a binder. According to a preferred preparation method, said MFI zeolite and binder may be mixed in the form of a powder, a crushed powder, a suspension or a suspension that has undergone a deagglomeration treatment, but this is not limiting. Said zeolite and binder may advantageously be mixed by mechanical mixing or suspension in a concentration adjusted to the target final zeolite content and the target final binder content in the catalyst prepared according to the invention.

[0035] (MFI type zeolite) MFI type zeolites are crystalline microporous solids and have been described in the literature (GT Kokotailo, SL Lawton, DH Olson, WM Meier, Nature, vol. 272, pp. 437-438, 1978; DH Olson, GT Kokotailo, SL Lawton, WM Meier, J. Phys. Chem., vol. 85, pp. 2238-2243, 1981; H. van Koningsveld, JC Jansen, H. van Bekkum, Zeolites, vol. 10, pp. 235-242, 1990). The crystal structures of these materials are described in the publications "Collection of simulated XRD powder patterns for zeolites", ed. MMJ Treacy and JB Higgins, Fifth Revised Edition, 2007, pp. 280-281 and "Atlas of zeolite framework types", C. Baerlocher, LB McCusker, DH Olson, sixth revised edition, 2007, pp. 212-213.

[0036] Also described in said document is a method for preparing MFI type zeolites.

[0037] Said MFI type zeolite has a chemical composition, expressed on an anhydrous basis, in moles of oxide defined by the following general formula: (96-a)XO2:a / 2Y2O3:a / 2M 2 / n O In the formula, X represents at least one tetravalent element, Y represents at least one trivalent element, M represents at least one alkali metal and / or alkaline earth metal of valence n, and x<27.

[0038] X is preferably selected from silicon, germanium, titanium, and at least two of these tetravalent elements, and highly preferably X is silicon, and Y is preferably selected from aluminum, boron, iron, indium, and gallium; highly preferably Y is aluminum. M is preferably selected from lithium, sodium, potassium, calcium, magnesium, and a mixture of at least two of these metals, and highly preferably M is sodium. Preferably, X represents silicon; the MFI zeolite according to the invention is a completely silicon solid when element Y is not present in the composition of the MFI zeolite. It is also advantageous to use a mixture of elements as element X, in particular a mixture of silicon and another element X selected from germanium and titanium, preferably germanium. Therefore, when silicon is present in a mixture with another element X, the MFI zeolite according to the invention is a crystalline metallosilicate and when it is in calcined form, it shows the same X-ray diffraction pattern as described in "Collection of simulated XRD powder patterns for zeolites", eds. MMJ Treacy and JB Higgins, Fifth Revised Edition, 2007, p. 280-281. Even more preferably, in the presence of element Y, X is silicon and Y is aluminum: the MFI zeolite according to the invention is an aluminosilicate. Preferably, the MFI zeolite according to the invention is in the form of an aluminosilicate.

[0039] Preferably, the average size of the elementary particles of the MFI type zeolite, as measured by scanning electron microscopy, is between 110 and 800 nm, preferably between 120 and 700 nm, highly preferably between 150 and 500 nm.

[0040] Preferably, the MFI type zeolite is ZSM-5.

[0041] Preferably, the molar ratio Si / Al of the number of silicon atoms to the number of aluminium atoms is less than 100, preferably less than 70, highly preferably less than 50.

[0042] The MFI zeolite contained in the composition of the catalyst according to the invention is advantageously subjected to at least one exchange by treatment with a solution of at least one ammonium salt to obtain the ammonium form of the MFI zeolite, which, once calcined, converts said MFI zeolite into the acid form (H + This exchange step may be carried out at any stage in the preparation of the catalyst, i.e. after the step of preparing the MFI zeolite, after the step of shaping the MFI zeolite with a porous mineral binder or after the optional step of introducing a hydrogenation-dehydrogenation phase.

[0043] The MFI type zeolite contained in the composition of the catalyst used in the process according to the invention is advantageously at least partially, preferably substantially completely, in acid form, i.e. H + It is a type.

[0044] According to the invention, the content of zeolite is between 45% and 90% by weight, preferably between 50% and 80% by weight and highly preferably between 55% and 75% by weight, relative to the total mass of the catalyst.

[0045] (Binder) According to the invention, the catalyst used also contains a binder. The binder may advantageously be amorphous or crystalline. Preferably, the binder is advantageously selected from the group consisting of the following oxides or their hydrated forms: alumina, silica, silica / alumina, clay, titanium oxide, boron oxide, and zirconia, employed alone or as a mixture. Preferably, the binder is alumina or aluminium hydroxide, alone or as a mixture. Preferably, the binder is in any of its forms known to the skilled person, for example α-, γ-, η- or δ-alumina or hydroxides, for example boehmite, bayerite or gibbsite. The aluminas differ in their specific surface area and in their pore volume. The loss on ignition of the binder is advantageously greater than 15%.

[0046] Preferably, the catalyst comprises from 10% to 60% by weight, preferably from 20% to 50% by weight, of a binder relative to the total mass of the catalyst.

[0047] According to step b), a deflocculating agent selected from nitric acid and a carboxylic acid selected from acetic acid, citric acid and butyric acid, either alone or in a mixture, is added to said mixture obtained from step a), preferably the deflocculating agent is nitric acid.

[0048] The amount of peptizer, which may advantageously be defined as the total acid content, expressed as a percentage relative to the mass of the dried binder introduced in step a), is between 0.1% and 12% by weight. Preferably, the total acid content is between 0.1% and 6% by weight, highly preferably between 0.1% and 4% by weight.

[0049] Water can also be introduced during step b) so that the loss on ignition of the mixture is between 20 and 80%, preferably between 30 and 70%.

[0050] According to step c), an inorganic base selected from sodium hydroxide, potassium hydroxide, and ammonia, alone or as a mixture, and an organic base in solution selected from amines and quaternary ammonium compounds, alone or as a mixture, are added to the mixture obtained from step b). Preferably, the organic base in solution is selected from alkylethanolamines and ethoxylated alkylamines. The organic base is preferably used as a solution in water. Highly preferably, the neutralizing agent is an inorganic base, preferably ammonia, preferably ammonia (NH4OH) in an aqueous solution.

[0051] The amount of neutralizing agent can be defined as the degree of neutralization expressed as the molar percentage of base relative to the amount of acid introduced in step b) and is between 1 and 200%. Preferably, the degree of neutralization expressed as the molar percentage of base relative to the amount of acid is between 10 and 100%.

[0052] According to step d), the mixture obtained in step c) is shaped by extrusion to obtain a solid. To facilitate this process, various additives may be added. Examples of additives include, inter alia, cellulose, carboxymethylcellulose, carboxyethylcellulose, tall oil, xanthan gum, surfactants, flocculants such as polyacrylamide, carbon black, starch, stearic acid, polyacryl alcohol, polyvinyl alcohol, biopolymers, glucose, polyethylene glycol, etc.

[0053] The extrusion may advantageously be carried out by any conventional commercially available tool. The mixture obtained from step c) is advantageously extruded through a die, for example using a piston or single or twin screw extruder. This extrusion step may advantageously be carried out in any manner known to the person skilled in the art, to obtain a solid or raw material.

[0054] The process according to the invention may optionally comprise a step e) of drying the solid obtained in the shaping step d), said drying step being advantageously carried out by any technique known to the person skilled in the art.

[0055] Preferably, drying is carried out in a stream of air, which may be dry or moist. The drying may advantageously be carried out in a stream of any oxidizing, reducing or inert gas. Preferably, drying is advantageously carried out at temperatures between 50° C. and 180° C., preferably between 60° C. and 150° C., highly preferably between 80° C. and 130° C. Preferably, the drying step is carried out for a period between 2 hours and 10 hours.

[0056] According to step f), the heat treatment in the presence of water vapor of the solid obtained in step d) or e) is carried out at a temperature between 400 and 1000° C., advantageously for a period of 1 to 24 hours, in the presence of a current of air containing 1% to 60% by volume of water.

[0057] Preferably, said step f) is carried out in the presence of a stream of air having a water content of 1% to 50% by volume, highly preferably 1% to 10% by volume. Preferably, said heat treatment step f) is carried out at a temperature of 450° C. to 850° C. Preferably, said heat treatment step f) is carried out for a period of 2 hours to 10 hours.

[0058] The process according to the invention may optionally comprise a step g) of introducing into the solid obtained in step f) one or more precursors of a hydrogenation active phase.

[0059] Preferably, the precursor(s) of the hydrogenation active phase comprises at least one group VIII element and optionally at least one group VIB element. Preferably, the group VIII element is selected from nickel and cobalt, and highly preferably, the group VIII element is nickel. When the hydrogenation phase comprises a group VIB element, it is preferably molybdenum or tungsten, and highly preferably, it is molybdenum.

[0060] The precursors of the hydrogenated phase may advantageously be introduced by any method known to those skilled in the art, such as dry impregnation, excess impregnation, ion exchange, etc.

[0061] Preferably, the precursor of the hydrogenation phase is introduced by dry impregnation. The precursor of the hydrogenation phase may advantageously be introduced by one or more operations of impregnating the solid obtained in step f) with a solution containing at least one precursor of at least one metal selected from the group consisting of group VIII elements and optionally at least one precursor of at least one metal selected from the group consisting of group VIB elements. If two or more precursors are used, they are preferably introduced simultaneously. In a preferred variant in which the group VIII element is nickel or cobalt and the group VIB element is molybdenum or tungsten, examples of precursors that may be used in the catalyst preparation step include nickel nitrate, nickel dihydroxide, nickel acetate, nickel carbonate, cobalt nitrate, cobalt dihydroxide, cobalt acetate, cobalt carbonate, ammonium heptamolybdate, molybdic acid, molybdenum oxide, ammonium metatungstate, tungstic acid or tungsten oxide. Any other compound known to the skilled person having sufficient solubility may also be used.

[0062] The impregnation of the precursor of the element selected from group VIII elements and optionally group VIB elements may advantageously be promoted by adding phosphoric acid to the aqueous solution.

[0063] In the case where step g) is included, the content of group VIII elements is advantageously between 0.1% and 10% by weight of oxide relative to the total mass of the catalyst, preferably between 0.5% and 8% by weight of oxide and highly preferably between 1% and 6% by weight of oxide.

[0064] In the variant in which the hydrogenation active phase comprises a group VIB element, the content of group VIB element is advantageously between 1% and 40% by weight of oxide relative to the total mass of said catalyst, preferably between 2% and 35% by weight of oxide and highly preferably between 5% and 30% by weight of oxide.

[0065] The catalyst may advantageously contain phosphorus: the phosphorus content is advantageously between 0.5% and 15% by weight of oxide P2O5 relative to the total mass of said catalyst, and preferably between 1% and 10% by weight of oxide.

[0066] After impregnation with the constituent elements of the hydrogenated phase, the solid thus charged with impregnation liquid may optionally undergo a step h) of maturation at room temperature for a period between 0.5 h and 24 h, preferably between 1 h and 6 h.

[0067] After the impregnation and, optionally, maturation step, the solid obtained undergoes a step i) of drying for a period between 0.5 h and 24 h, preferably between 1 h and 12 h. Preferably, the drying is carried out in a stream of air, said stream of air being either dry or moist. Preferably, the drying is carried out at a temperature advantageously between 50° C. and 180° C., preferably between 60° C. and 150° C.

[0068] The dried, optionally aged solid then undergoes a calcination step j), optionally for a period between 0.5 h and 24 h, preferably between 1 h and 12 h, said calcination step being advantageously carried out in the presence of molecular oxygen, for example by flushing with air, advantageously at a temperature between 200° C. and 600° C., preferably between 300° C. and 500° C., the air being either dry or moist.

[0069] The hydrogenation active phase of the catalyst used in the process according to the invention is preferably used in sulphurized form. The sulphurization of the catalyst may be carried out in situ or ex situ by any method known to the person skilled in the art. In the case of an in situ sulphurization step, the sulphurization of the catalyst is carried out by treating it with a feedstock containing at least one sulphur compound whose decomposition leads to the fixation of sulphur in the active phase. This feedstock may be in gaseous or liquid form, for example hydrogen containing H2S or a liquid containing at least one sulphur compound. In the case of ex situ sulphurization, the sulphur compound may be introduced into the catalyst, optionally in the presence of another compound. The catalyst is subsequently dried and then transferred to the reactor used to carry out the process of the invention. In this reactor, the catalyst is treated with hydrogen to convert at least a part of the main metals into sulphides. Particularly suitable procedures for use in the present invention are those described in patents FR-B-2 708 596 and FR-B-2 708 597.

[0070] (Characteristics of the obtained catalyst) The preparation process according to the invention has the remarkable advantage of resulting in a porous zeolite catalyst having quite satisfactory mechanical strength in relation to the pore volume characterizing it, said strength being embodied by a Single Pellet Crush Strength (SPCS) value, preferably of at least 0.8 daN / mm, highly preferably of at least 0.9 daN / mm.

[0071] The preparation process according to the invention makes it possible to obtain a catalyst with a high zeolite content, said catalyst advantageously having a total pore volume, measured by mercury intrusion porosimetry, of between 0.25 and 0.8 mL / g, preferably between 0.35 and 0.7 mL / g.

[0072] The mesopore volume of the catalyst prepared according to the invention, ie the volume contained in pores with a diameter of 2-50 nm, is 0.1-0.6 mL / g, preferably 0.2-0.5 mL / g, measured by mercury intrusion porosimetry.

[0073] The macropore volume of the catalyst prepared according to the invention, ie the volume contained in pores with a diameter of more than 50 nm, is between 0 and 0.4 mL / g, preferably between 0 and 0.2 mL / g, measured by mercury intrusion porosimetry.

[0074] The catalyst according to the present invention generally has a specific surface area of ​​250 m 2 / g, preferably 300m 2 / g, preferably 320m 2 / g.

[0075] According to the present invention, the content of MFI type zeolite in the catalyst according to the present invention is 45% by weight to 90% by weight, preferably 55% by weight to 80% by weight, relative to the total mass of said catalyst.

[0076] The volumetric zeolite content of the catalyst according to the invention is advantageously 350 kg / m 3 More than 400 kg / m 3 It's super.

[0077] The TPD of the catalyst according to the invention is advantageously between 0.5 and 1.0 g / mL, preferably between 0.6 and 0.9 g / mL.

[0078] The catalysts of this type obtained can be used in many heterogeneous catalytic applications requiring acid functionality, in particular for the conversion of hydrocarbons: methanol (to olefins, gasoline, etc.), olefins (to olefins, gasoline, diesel, etc.), various processes for the conversion of paraffins to aromatics, as well as alkylation processes, processes for the dewaxing of diesel, oil, plastic pyrolysis, biomass pyrolysis, etc.

[0079] The invention is illustrated by the following examples which are in no way limiting in nature.

[0080] (Example) Example 1: Preparation of Catalyst A (not of the present invention) For the preparation of catalyst A, ZSM-5 MFI type zeolite (Zeolyst®) with an average unit particle size of about 1-3.5 μm, a Si / Al atomic ratio of 22, and in the NH4 form is shaped with a boehmite binder (Sasol®). The boehmite powder and the zeolite powder are dry mixed in a mass percentage of 30 / 70, respectively. They are then introduced into the closed tank of an MX series double sigma blade kneader (Guittard®). The deflocculating agent nitric acid (HNO3) is added to achieve an acid level of 4%. Water is also gradually introduced to achieve an LOI of about 50%, its value being adjusted according to the formulation, to obtain a homogeneous and cohesive paste. After mixing for 30 minutes, the neutralizing agent ammonia (NH4OH) is added to the paste. The amount of neutralizing agent used is adjusted to achieve a neutralization level of 40%. The paste is kneaded for a further 15 minutes and then extruded using a piston extruder through a die with a diameter of 3 mm. The extrudates thus obtained are dried (overnight in air at 120° C. in a ventilated oven) and then calcined at 540° C. for 4 hours in moist air with a water content equal to 6% by volume.

[0081] The characteristics of the obtained catalyst are shown in Table 1 below.

[0082] Example 2: Preparation of Catalyst B (not of the present invention) For the preparation of catalyst B, ZSM-5 MFI type zeolite (Zeolyst®) in the NH4 form with an average unit particle size of about 150-500 nm and a Si / Al atomic ratio of 25 is shaped with a boehmite binder (Sasol®). The boehmite and zeolite powders are dry mixed in a mass percentage of 30 / 70, respectively. They are then introduced into the closed tank of a MX series double sigma blade kneader (Guittard®). A deflocculating agent (nitric acid (HNO3)) is added to achieve an acid level of 4%. Water is also gradually introduced to achieve an LOI of about 50%, its value being adjusted according to the recipe, to obtain a homogeneous and cohesive paste. No neutralizing agent is added to the paste. The paste is extruded through a die with a diameter of 3 mm using a piston extruder. The extrudates thus obtained are dried (overnight at 120° C. in air in a ventilated oven) and then calcined in moist air having a water content equal to 6% by volume at 540° C. for 4 hours.

[0083] The characteristics of the obtained catalyst are shown in Table 1 below.

[0084] Example 3: Preparation of Catalyst C (not of the present invention) For the preparation of catalyst C, ZSM-5 MFI type zeolite (Zeolyst®) with an average unit particle size of about 150-500 nm, a Si / Al atomic ratio of 25, and in the NH4 form is shaped with a boehmite binder (Sasol®). The boehmite powder and the zeolite powder are dry mixed in a mass percentage of 30 / 70, respectively. They are then introduced into the closed tank of an MX series double sigma blade kneader (Guittard®). A deflocculating agent (nitric acid (HNO3)) is added to achieve an acid level of 4%. Water is also gradually introduced to achieve an LOI of about 50%, its value being adjusted according to the recipe to obtain a homogeneous and cohesive paste. After mixing for 30 minutes, a neutralizing agent (ammonia (NH4OH)) is added to the paste. The amount of neutralizing agent used is adjusted to achieve a neutralization level of 40%. The paste is kneaded for a further 15 minutes and then extruded using a piston extruder through a die with a diameter of 3 mm. The extrudates thus obtained are dried (overnight at 120° C. in air in a ventilated oven) and then calcined in dry air at 540° C. for 4 hours.

[0085] The characteristics of the obtained catalyst are shown in Table 1 below.

[0086] Example 4: Preparation of Catalyst D (not of the present invention) For the preparation of catalyst D, ZSM-5 MFI type zeolite (Zeolyst®) in NH4 form with an average unit particle size of about 1-2 μm and a Si / Al atomic ratio of 22 is shaped with a boehmite binder (Sasol®). The boehmite and zeolite powders are dry mixed in a mass percentage of 40 / 60, respectively. They are then introduced into the closed tank of a MX series double sigma blade kneader (Guittard®). A deflocculating agent (nitric acid (HNO3)) is added to achieve an acid level of 4%. Water is also gradually introduced to achieve an LOI of about 50%, its value being adjusted according to the recipe to obtain a homogeneous and cohesive paste. After mixing for 30 minutes, a neutralizing agent (ammonia NH4OH) is added to the paste. The amount of neutralizing agent used is adjusted to achieve a neutralization level of 40%. The paste is kneaded for a further 15 minutes and then extruded using a piston extruder through a die with a diameter of 3 mm. The extrudates thus obtained are dried (overnight at 120° C. in air in a ventilated oven) and then calcined at 540° C. for 4 hours in moist air with a water content equal to 6% by volume.

[0087] The characteristics of the obtained catalyst are shown in Table 1 below.

[0088] Example 5: Preparation of Catalyst E (not of the present invention) For the preparation of catalyst E, ZSM-5 MFI type zeolite (Zeolyst®) with an average unit particle size of about 150-500 nm, a Si / Al atomic ratio of 25, and in the NH4 form is shaped with a boehmite binder (Sasol®). The boehmite and zeolite powders are dry mixed in a mass percentage of 50 / 50, respectively. They are then introduced into the closed tank of a MX series double sigma blade kneader (Guittard®). A deflocculating agent (nitric acid HNO3) is added to achieve an acid level of 4%. Water is also gradually introduced to achieve an LOI of about 50%, its value being adjusted according to the formulation to obtain a homogeneous and cohesive paste. After mixing for 30 minutes, a neutralizing agent (ammonia NH4OH) is added to the paste. The amount of neutralizing agent used is adjusted to achieve a neutralization level of 40%. The paste is kneaded for a further 15 minutes and then extruded using a piston extruder through a die with a diameter of 3 mm. The extrudates thus obtained are dried (overnight at 120° C. in air in a ventilated oven) and then calcined in dry air at 540° C. for 4 hours.

[0089] The characteristics of the obtained catalyst are shown in Table 1 below.

[0090] Example 6: Preparation of Catalyst F (not of the present invention) For the preparation of catalyst F, ZSM-5 MFI type zeolite (Zeolyst®) with an average unit particle size of about 150-500 nm, a Si / Al atomic ratio of 25, and in the NH4 form is shaped with a boehmite binder (Sasol®). The boehmite powder and the zeolite powder are dry mixed in a mass ratio of 30 / 70, respectively. They are then introduced into the closed tank of a MX series double sigma blade kneader (Guittard®). A deflocculating agent (nitric acid HNO3) is added to achieve an acid level of 4%. Water is also gradually introduced to achieve an LOI of about 50%, its value being adjusted according to the formulation to obtain a homogeneous and cohesive paste. After mixing for 30 minutes, a neutralizing agent (ammonia NH4OH) is added to the paste. The amount of neutralizing agent used is adjusted to achieve a neutralization level of 100%. The paste is kneaded for a further 15 minutes and then extruded using a piston extruder through a die with a diameter of 3 mm. The extrudates thus obtained are dried (overnight at 120° C. in air in a ventilated oven) and then calcined at 540° C. for 4 hours in moist air with a water content equal to 6% by volume.

[0091] The characteristics of the obtained catalyst are shown in Table 1 below.

[0092] Example 7: Preparation of Catalyst G (Invention) For the preparation of catalyst G, ZSM-5 MFI type zeolite (Zeolyst®) with an average unit particle size of about 150-500 nm, a Si / Al atomic ratio of 25, and in the NH4 form is shaped with a boehmite binder (Sasol®). The boehmite powder and the zeolite powder are dry mixed in a mass ratio of 40 / 60, respectively. They are then introduced into the closed tank of a MX series double sigma blade kneader (Guittard®). A deflocculating agent (nitric acid HNO3) is added to achieve an acid level of 4%. Water is also gradually introduced to achieve an LOI of about 50%, its value being adjusted according to the formulation, so as to obtain a homogeneous and cohesive paste. After mixing for 30 minutes, a neutralizing agent (ammonia NH4OH) is added to the paste. The amount of neutralizing agent used is adjusted to achieve a neutralization level of 40%. The paste is kneaded for a further 15 minutes and then extruded using a piston extruder through a die with a diameter of 3 mm. The extrudates thus obtained are dried (overnight at 120° C. in air in a ventilated oven) and then calcined at 540° C. for 4 hours in moist air with a water content equal to 6% by volume.

[0093] The characteristics of the obtained catalyst are shown in Table 1 below.

[0094] Example 8: Preparation of Catalyst H (present invention) The solid H obtained in the form of extrudates according to Example 7 is subjected to dry impregnation with an impregnation solution prepared by dissolving nickel nitrate (Ni(NO3)2·6H2O, Sigma®, >98%) in demineralized water. After dry impregnation, the extrudates are left to rest and age for 2 hours in a water-saturated atmosphere, then dried at 120°C for 12 hours and finally calcined at 450°C for 2 hours in a stream of dry air. The amount of nickel nitrate in the impregnation solution is adjusted to obtain a nickel content corresponding to 3% by weight NiO, calculated as oxide.

[0095] The characteristics of the obtained catalyst are shown in Table 1 below.

[0096] (Example 9: Characteristics of Catalysts A to H) Table 1 below summarizes the characteristics of the synthesized catalysts A to H.

[0097] [Table 1]

[0098] The measured characteristics of the various catalysts, shown in Table 1, show that the solids prepared according to the invention allow improvements compared to known methods of the prior art: in particular, the combination of a neutralization step (solids F, G, H versus B) and a steaming step (solids F, G, H versus C and E), coupled with the use of small-sized elementary particles of MFI type zeolite (solids F, G, H versus A and D), allows a higher zeolite loading per unit volume while maintaining good mechanical properties.

Claims

1. A process for preparing a catalyst in the form of extrudates, comprising an acidic MFI type zeolite, preferably H-ZSM-5, and a binder, preferably alumina, the zeolite content being between 45% and 90% relative to the total mass of the catalyst, and optionally containing a hydrogenation active phase, comprising at least the following steps: a) mixing said MFI zeolite with a binder; the average size of the elementary particles of said MFI zeolite is between 110 and 800 nm, preferably between 120 and 700 nm, highly preferably between 150 and 500 nm, as measured by scanning electron microscopy; b) adding to the mixture obtained in step a) a deflocculating agent selected from nitric acid and a carboxylic acid selected from acetic acid, citric acid and butyric acid, either alone or in mixture; c) adding to the mixture obtained in step b) a neutralizing agent selected from an inorganic base selected from sodium hydroxide, potassium hydroxide, and ammonia, either alone or as a mixture, and an organic base in solution selected from an amine and a quaternary ammonium compound, either alone or as a mixture; d) shaping the mixture obtained in step c) by extrusion to obtain a solid; e) optionally drying the solid obtained in step d); f) heat treating the solid obtained in step d) or e) in the presence of water vapor at a temperature between 400° C. and 1000° C. in the presence of a stream of air containing between 1% and 60% by volume of water, g) Optionally, introducing one or more precursors of a hydrogenation active phase into the solid obtained in step f).

2. 2. The method according to claim 1, wherein the average size of the elementary particles of MFI zeolite is between 120 and 700 nm, highly preferably between 150 and 500 nm, as measured by scanning electron microscopy.

3. The method according to claim 1 or 2, wherein the MFI zeolite is ZSM-5.

4. The process according to any one of claims 1 to 3, wherein the zeolite content is between 55% and 80% by weight relative to the total mass of the catalyst.

5. The method according to any one of claims 1 to 4, wherein the binder is alumina.

6. The method according to any one of claims 1 to 5, wherein the deflocculating agent used in step b) is nitric acid.

7. 7. The method according to claim 1, wherein the amount of deflocculating agent used in step b), defined as the total acid content expressed as a percentage relative to the mass of the dried binder introduced in step a), is between 0.1% and 12% by weight, preferably between 0.1% and 6% by weight, highly preferably between 0.1% and 4% by weight.

8. The neutralizing agent used in step c) is an inorganic base, preferably ammonia, preferably ammonia (NH 4 8. The method according to claim 1, wherein the aryl group is aryl, aryloxy ...

9. 9. The process according to any one of claims 1 to 8, wherein the amount of neutralizing agent used in step c), defined as the degree of neutralization expressed as the molar percentage of base relative to the amount of acid introduced in step b), is between 1 and 200%, preferably between 10 and 100%.

10. 10. The method according to claim 1, wherein step f) is carried out in the presence of a stream of air having a water content of 1% to 50% by volume, highly preferably 1% to 10% by volume, at a temperature of 450° C. to 850° C., for a period of 2 hours to 10 hours.

11. 11. The method according to claim 1, wherein in the case of comprising step g), the one or more precursors of the hydrogenation active phase comprise at least one group VIII element and optionally at least one group VIB element.

12. 12. The process according to claim 11, wherein the content of group VIII elements is between 0.1% and 10% by weight of oxide relative to the total mass of the catalyst, preferably between 0.5% and 8% by weight of oxide, highly preferably between 1% and 6% by weight of oxide.